Method for manufacturing solar cell and solar cell
A copper-based solar cell manufacturing method with insulating layers and selective etching prevents copper diffusion, ensuring performance and cost reduction without substrate damage.
Patent Information
- Application Number
- JP2020218895
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-12-28
AI Technical Summary
The use of copper (Cu) as a replacement for silver (Ag) in solar cell electrodes leads to performance deterioration due to etching solution penetration and diffusion into the semiconductor substrate, causing damage and reduced reliability.
A manufacturing method that uses copper electrodes with insulating layers and contact electrodes as masks during etching, avoiding contact with etching solutions and using hydrochloric acid for transparent electrode etching, thereby preventing copper diffusion.
The method maintains solar cell performance while reducing costs by using copper electrodes, preventing copper diffusion into the semiconductor substrate and maintaining contact properties.
Smart Images

Figure 0007576461000001 
Figure 0007576461000002 
Figure 0007576461000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a back electrode type (back contact type) solar cell, and to a back electrode type solar cell. [Background technology]
[0002] Patent documents 1 to 3 disclose techniques relating to the connection of electrodes of two polarities and wiring members in a back electrode type solar cell. The first wiring and the second wiring cross the first electrode and the second electrode, the first wiring is connected to the first electrode at a point where it intersects with the first electrode, and is insulated from the second electrode by an insulating layer at a point where it intersects with the second electrode; The second wiring is connected to the second electrode at a point where it intersects with the second electrode, and is insulated from the first electrode by an insulating layer at a point where it intersects with the first electrode; It is stated that:
[0003] In addition, Patent Document 3 describes a back electrode type solar cell as follows: A wiring for a p-electrode and a wiring for an n-electrode intersecting the p-electrode and the n-electrode are provided, -Insulating resin is formed on the back side, the p-electrode wiring is connected to the p-electrode by a conductive member in a hole in the insulating resin at a point where it intersects with the p-electrode, and is insulated from the n-electrode by the insulating resin at a point where it intersects with the n-electrode; The n-electrode wiring is connected to the n-electrode by a conductive member in a hole in the insulating resin at a point where it intersects with the n-electrode, and is insulated from the p-electrode by the insulating resin at a point where it intersects with the p-electrode. It is stated that: [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-133567 A [Patent Document 2] JP 2015-159286 A [Patent Document 3] JP 2014-127550 A Summary of the Invention [Problem to be solved by the invention]
[0005] In order to reduce the cost of such solar cells, the inventor(s) of the present application has devised the use of a relatively inexpensive metal, for example, Cu (for example, a film formed by a PVD method such as sputtering or a plating method, followed by wet etching) as the material for the metal electrode layer, instead of the relatively expensive known Ag paste. Note that a contact electrode made of Ag paste is used only in the portion that makes contact with the wiring member.
[0006] Furthermore, in order to simplify the manufacturing process of such solar cells, the inventor(s) of the present application have devised a method in which the insulating layer and contact electrode (Ag paste) for ensuring insulation and contact with the wiring members also serve as a resist for wet etching of the metal electrode layer (e.g., Cu) and transparent electrode layer.
[0007] However, according to the knowledge of the present inventors, such a solar cell and its manufacturing method may result in a decrease in the performance of the solar cell. This is considered as follows.
[0008] During wet etching of the metal electrode layer and the transparent electrode layer, the etching solution penetrates into the contact electrodes made of Ag paste. When the electrodes are subsequently annealed or heated in the operating environment, the etching solution that penetrates into the contact electrodes dissolves the metal electrode layer and the transparent electrode layer made of Cu. Then, for some reason, Cu diffuses into the semiconductor substrate through the semiconductor layer (for example, through local defects, etc.). This can cause damage to the semiconductor substrate, reducing the performance of the solar cell (reliability).
[0009] An object of the present invention is to provide a solar cell and a manufacturing method thereof that can suppress deterioration in the performance of the solar cell while reducing the cost of the solar cell. [Means for solving the problem]
[0010] The method for manufacturing a solar cell according to the present invention is a method for manufacturing a back electrode type solar cell including a semiconductor substrate, a first conductive type semiconductor layer, a first transparent electrode layer, and a first metal electrode layer which are laminated in this order in a first region which is a part of one main surface side of the semiconductor substrate, and a second conductive type semiconductor layer, a second transparent electrode layer, and a second metal electrode layer which are laminated in this order in a second region which is another part of the one main surface side of the semiconductor substrate, the method comprising the steps of: forming a series of transparent electrode layer material films on the first conductive type semiconductor layer and the second conductive type semiconductor layer on the one main surface side of the semiconductor substrate; a metal electrode layer material film forming step of forming a series of metal electrode layer material films, the metal electrode layer material film including copper, on the transparent electrode layer material film; an insulating layer forming step of forming a first insulating layer that entirely covers the metal electrode layer material film in the first region except for a first non-insulating region, and a second insulating layer that entirely covers the metal electrode layer material film in the second region except for a second non-insulating region, the first insulating layer and the second insulating layer being spaced apart from each other; and an insulating layer forming step of forming a first insulating layer and a second insulating layer between the first insulating layer and the second insulating layer by using an etching method using the first insulating layer and the second insulating layer as a mask. a metal electrode layer forming step of forming the first metal electrode layer patterned in the first region and the second metal electrode layer patterned in the second region by removing exposed portions of the metal electrode layer material film in the first non-insulating region and the second non-insulating region, and leaving the first insulating layer and the second insulating layer without removing it; a contact electrode forming step of forming a first contact electrode on the transparent electrode layer material film in the first non-insulating region so as to be in contact with a side surface of the first metal electrode layer and a side surface of the first insulating layer, and forming a second contact electrode on the transparent electrode layer material film in the second non-insulating region so as to be in contact with a side surface of the second metal electrode layer and a side surface of the second insulating layer; and a transparent electrode layer forming step of forming the first transparent electrode layer patterned in the first region by removing exposed portions of the transparent electrode layer material film using an etching method using the first insulating layer and the first contact electrode, and the second insulating layer and the second contact electrode as masks, and forming the second transparent electrode layer patterned in the second region, and leaving the first insulating layer and the second insulating layer without removing it.
[0011] The solar cell of the present invention is a back electrode type solar cell comprising a semiconductor substrate, a first conductive type semiconductor layer, a first transparent electrode layer and a first metal electrode layer stacked in sequence in a first region which is a part of one main surface side of the semiconductor substrate, and a second conductive type semiconductor layer, a second transparent electrode layer and a second metal electrode layer stacked in sequence in a second region which is the other part of the one main surface side of the semiconductor substrate, and comprises a first insulating layer formed in the first region so as to entirely cover the first metal electrode layer except for a first non-insulating region, a second insulating layer formed in the second region so as to entirely cover the second metal electrode layer except for a second non-insulating region, a first contact electrode formed in the first non-insulating region, and a second contact electrode formed in the second non-insulating region. The first metal electrode layer and the second metal electrode layer contain copper, the first transparent electrode layer is formed in the first non-insulating region, and the first metal electrode layer is not formed, the second transparent electrode layer is formed in the second non-insulating region, and the second metal electrode layer is not formed, the first contact electrode is in contact with a main surface of the first transparent electrode layer, a side surface of the first metal electrode layer, and a side surface of the first insulating layer, and the second contact electrode is in contact with a main surface of the second transparent electrode layer, a side surface of the second metal electrode layer, and a side surface of the second insulating layer.
[0012] Another solar cell manufacturing method according to the present invention is a method for manufacturing a back electrode type solar cell including a semiconductor substrate, a first conductive type semiconductor layer, a first transparent electrode layer, and a first metal electrode layer which are laminated in this order in a first region which is a part of one main surface side of the semiconductor substrate, and a second conductive type semiconductor layer, a second transparent electrode layer, and a second metal electrode layer which are laminated in this order in a second region which is another part of the one main surface side of the semiconductor substrate, the method including the steps of: forming a series of transparent electrode layer material films on the first conductive type semiconductor layer and the second conductive type semiconductor layer on the one main surface side of the semiconductor substrate; forming a series of metal electrode layer material films on the transparent electrode layer material film, the metal electrode layer material film including copper; forming a first insulating layer which entirely covers the metal electrode layer material film in the first region, and a second insulating layer which entirely covers the metal electrode layer material film in the second region, the first insulating layer and the second insulating layer being spaced apart from each other. the first insulating layer and the second insulating layer as masks, to remove exposed portions of the metal electrode layer material film, thereby forming the first metal electrode layer patterned in the first region, forming the second metal electrode layer patterned in the second region, and removing the first insulating layer and the second insulating layer; the contact electrode layer forming step of forming a first contact electrode layer on the first metal electrode layer and forming a second contact electrode layer on the second metal electrode layer; and the transparent electrode layer forming step of forming the first transparent electrode layer patterned in the first region, by removing exposed portions of the transparent electrode layer material film, using an etching method with the first contact electrode layer and the first metal electrode layer, and the second contact electrode layer and the second metal electrode layer as masks, to form the first transparent electrode layer patterned in the first region, and forming the second transparent electrode layer patterned in the second region.
[0013] Another solar cell according to the present invention is a back electrode type solar cell including a semiconductor substrate, a first conductive type semiconductor layer, a first transparent electrode layer, and a first metal electrode layer, which are stacked in this order in a first region that is a part of one main surface side of the semiconductor substrate, and a second conductive type semiconductor layer, a second transparent electrode layer, and a second metal electrode layer, which are stacked in this order in a second region that is another part of the one main surface side of the semiconductor substrate, and further including a first contact electrode layer stacked on the first metal electrode layer and a second contact electrode layer stacked on the second metal electrode layer. The first metal electrode layer and the second metal electrode layer contain copper. Effect of the Invention
[0014] According to the present invention, it is possible to suppress deterioration in the performance of solar cells even when the cost of the solar cells is reduced. [Brief description of the drawings]
[0015] [Figure 1] 1 is a diagram showing the solar cell according to the first embodiment as viewed from the back surface side. [Figure 2A] 2 is a cross-sectional view taken along line IIA-IIA of the solar cell of FIG. 1. [Figure 2B] 2 is a cross-sectional view of the solar cell shown in FIG. 1 taken along line IIB-IIB. [Figure 3A] 3A to 3C are diagrams illustrating a semiconductor layer forming step in the method for manufacturing the solar cell according to the first embodiment. [Figure 3B] 3A to 3C are diagrams illustrating an electrode layer material film forming step in the method for manufacturing the solar cell according to the first embodiment, that is, a transparent electrode layer material film forming step and a metal electrode layer material film forming step. [Figure 3C] 3A to 3C are diagrams illustrating an insulating layer forming step in the method for manufacturing the solar cell according to the first embodiment. [Figure 3D] FIG. 3 is a diagram showing a metal electrode layer forming step (electrode layer forming step) in the method for manufacturing the solar cell according to the first embodiment. [Figure 3E] 5A to 5C are diagrams illustrating a contact electrode forming step in the method for manufacturing the solar cell according to the first embodiment. [Figure 3F]FIG. 3 is a diagram showing a transparent electrode layer forming step (electrode layer forming step) in the method for manufacturing the solar cell according to the first embodiment. [Figure 4A] 2 is a cross-sectional view of a solar cell according to Comparative Example 1, taken along line IIA-IIA in FIG. [Figure 4B] 2 is a cross-sectional view of a solar cell according to Comparative Example 1, taken along line IIB-IIB in FIG. [Figure 5A] 1 is a diagram showing a transparent electrode layer material film forming step, a metal electrode layer material film forming step, and an insulating layer forming step in a solar cell manufacturing method according to Comparative Example 1. FIG. [Figure 5B] 10 is a diagram showing a contact electrode forming step in the solar cell manufacturing method according to Comparative Example 1. FIG. [Figure 5C] 1 is a diagram showing an electrode layer forming step, that is, a transparent electrode layer forming step and a metal electrode layer forming step, in a solar cell manufacturing method according to Comparative Example 1. FIG. [Figure 6] FIG. 11 is a diagram showing a solar cell according to a second embodiment as viewed from the back surface side. [Figure 7] 7 is a cross-sectional view of the solar cell shown in FIG. 6 taken along line VII-VII. [Figure 8A] 10A to 10C are diagrams illustrating a semiconductor layer forming step in a method for manufacturing a solar cell according to a second embodiment. [Figure 8B] 11A to 11C are diagrams illustrating an electrode layer material film forming step, that is, a transparent electrode layer material film forming step and a metal electrode layer material film forming step, in a manufacturing method for a solar cell according to a second embodiment. [Figure 8C] 11A to 11C are diagrams illustrating an insulating layer forming step in the method for manufacturing a solar cell according to a second embodiment. [Figure 8D] FIG. 11 is a diagram showing a metal electrode layer forming step (electrode layer forming step) in the method for manufacturing a solar cell according to a second embodiment. [Figure 8E] 11A to 11C are diagrams illustrating an insulating layer removal and formation step in the method for manufacturing a solar cell according to a second embodiment. [Figure 8F] 11A to 11C are diagrams illustrating a contact electrode layer forming step in the method for manufacturing a solar cell according to a second embodiment. [Figure 8G]FIG. 11 is a diagram showing a transparent electrode layer forming step (electrode layer forming step) in the method for manufacturing a solar cell according to the second embodiment. [Figure 9] 7 is a cross-sectional view of a solar cell according to Comparative Example 2, taken along line VII-VII in FIG. [Figure 10A] 13 is a diagram showing a transparent electrode layer material film forming step, a metal electrode layer material film forming step, and a contact electrode layer forming step in a solar cell manufacturing method according to Comparative Example 2. FIG. [Figure 10B] 11 is a diagram showing an electrode layer forming step, that is, a transparent electrode layer forming step and a metal electrode layer forming step, in a solar cell manufacturing method according to Comparative Example 2. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals. For convenience, hatching and reference numerals may be omitted, in which case other drawings shall be referred to.
[0017] (Solar cell of the first embodiment) Fig. 1 is a view of the solar cell according to the first embodiment as viewed from the back surface side. Fig. 2A is a cross-sectional view of the solar cell in Fig. 1 taken along line IIA-IIA, and Fig. 2B is a cross-sectional view of the solar cell in Fig. 1 taken along line IIB-IIB. The solar cell 1 shown in Figs. 1, 2A, and 2B is a back electrode type (also called a back contact type or back junction type) heterojunction solar cell.
[0018] Solar cell 1 includes a semiconductor substrate 11 with two main surfaces, and the main surface of semiconductor substrate 11 has a first region 7 and a second region 8. In the following, the main surface of semiconductor substrate 11 that receives light is referred to as the light-receiving surface, and the main surface of semiconductor substrate 11 opposite the light-receiving surface (one main surface) is referred to as the back surface.
[0019] The first regions 7 are strip-shaped and extend in the Y direction (second direction). Similarly, the second regions 8 are strip-shaped and extend in the Y direction. The first regions 7 and the second regions 8 are alternately provided in the X direction (first direction) that intersects with the Y direction.
[0020] As shown in FIG. 2A and FIG. 2B, the solar cell 1 includes a passivation layer 13 and an optical adjustment layer 15, which are laminated in this order on the light-receiving surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 23, a first conductive type semiconductor layer 25, a first electrode layer 27, and a first insulating layer 41, which are laminated in this order on a portion (first region 7) of the back surface side of the semiconductor substrate 11. The solar cell 1 also includes a passivation layer 33, a second conductive type semiconductor layer 35, a second electrode layer 37, and a second insulating layer 42, which are laminated in this order on another portion (second region 8) of the back surface side of the semiconductor substrate 11. The solar cell 1 also includes a first contact electrode 51 corresponding to the first electrode layer 27, and a second contact electrode 52 corresponding to the second electrode layer 37.
[0021] The semiconductor substrate 11 is formed of a crystalline silicon material such as single crystal silicon or polycrystalline silicon. The semiconductor substrate 11 is, for example, an n-type semiconductor substrate in which a crystalline silicon material is doped with an n-type dopant. The semiconductor substrate 11 may be, for example, a p-type semiconductor substrate in which a crystalline silicon material is doped with a p-type dopant. An example of the n-type dopant is phosphorus (P). An example of the p-type dopant is boron (B). The semiconductor substrate 11 functions as a photoelectric conversion substrate that absorbs incident light from the light-receiving surface side and generates photocarriers (electrons and holes).
[0022] By using crystalline silicon as the material for the semiconductor substrate 11, the dark current is relatively small, and a relatively high output (stable output regardless of illuminance) can be obtained even when the intensity of incident light is low.
[0023] The passivation layer 13 is formed on the light-receiving surface side of the semiconductor substrate 11. The passivation layer 23 is formed in a first region 7 on the back surface side of the semiconductor substrate 11. The passivation layer 33 is formed in a second region 8 on the back surface side of the semiconductor substrate 11. The passivation layers 13, 23, and 33 are formed of a material containing, for example, an intrinsic (i-type) amorphous silicon material as a main component. The passivation layers 13, 23, and 33 suppress recombination of carriers generated in the semiconductor substrate 11 and increase the carrier collection efficiency.
[0024] The optical adjustment layer 15 is formed on the passivation layer 13 on the light-receiving surface side of the semiconductor substrate 11. The optical adjustment layer 15 functions as an anti-reflection layer that prevents reflection of incident light, and also functions as a protective layer that protects the light-receiving surface side of the semiconductor substrate 11 and the passivation layer 13. The optical adjustment layer 15 is formed of an insulating material, for example, silicon oxide (SiO), silicon nitride (SiN), or a composite thereof such as silicon oxynitride (SiON).
[0025] The first conductive type semiconductor layer 25 is formed on the passivation layer 23, that is, in a first region 7 on the back surface side of the semiconductor substrate 11. On the other hand, the second conductive type semiconductor layer 35 is formed on the passivation layer 33, that is, in a second region 8 on the back surface side of the semiconductor substrate 11. That is, the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 have a strip shape and extend in the Y direction. The first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 are alternately arranged in the X direction. A part of the second conductive type semiconductor layer 35 may overlap a part of the adjacent first conductive type semiconductor layer 25 (not shown).
[0026] The first conductive type semiconductor layer 25 is formed of, for example, an amorphous silicon material. The first conductive type semiconductor layer 25 is, for example, a p-type semiconductor layer in which an amorphous silicon material is doped with a p-type dopant (for example, the above-mentioned boron (B)).
[0027] The second conductive type semiconductor layer 35 is formed of, for example, an amorphous silicon material. The second conductive type semiconductor layer 35 is, for example, an n-type semiconductor layer in which an amorphous silicon material is doped with an n-type dopant (for example, the above-mentioned phosphorus (P)). Note that the first conductive type semiconductor layer 25 may be an n-type semiconductor layer, and the second conductive type semiconductor layer 35 may be a p-type semiconductor layer.
[0028] The first electrode layer 27 is formed on the first conductive type semiconductor layer 25, i.e., in a first region 7 on the back surface side of the semiconductor substrate 11. On the other hand, the second electrode layer 37 is formed on the second conductive type semiconductor layer 35, i.e., in a second region 8 on the back surface side of the semiconductor substrate 11. That is, the first electrode layer 27 and the second electrode layer 37 have a strip-like shape and extend in the Y direction. The first electrode layer 27 and the second electrode layer 37 are alternately provided in the X direction.
[0029] The first electrode layer 27 has a first transparent electrode layer 28 and a first metal electrode layer 29 laminated in this order on the first conductivity type semiconductor layer 25. On the other hand, the second electrode layer 37 has a second transparent electrode layer 38 and a second metal electrode layer 39 laminated in this order on the second conductivity type semiconductor layer 35.
[0030] The first transparent electrode layer 28 and the second transparent electrode layer 38 are formed of a transparent conductive material. Examples of the transparent conductive material include ITO (Indium Tin Oxide: a composite oxide of indium oxide and tin oxide), ZnO (Zinc Oxide: zinc oxide), etc.
[0031] The first metal electrode layer 29 and the second metal electrode layer 39 contain Cu as a metal material, which is less expensive than a known conductive paste material containing Ag powder. For example, the first metal electrode layer 29 and the second metal electrode layer 39 are formed by using a PVD method such as sputtering, or a plating method.
[0032] The first insulating layer 41 is formed on the first metal electrode layer 29, i.e., in a first region 7 on the back surface side of the semiconductor substrate 11. The second insulating layer 42 is formed on the second metal electrode layer 39, i.e., in a second region 8 on the back surface side of the semiconductor substrate 11. That is, the first insulating layer 41 and the second insulating layer 42 have a band-like shape and extend in the Y direction, as shown in Fig. 1. The first insulating layer 41 and the second insulating layer 42 are provided alternately in the X direction.
[0033] The first insulating layer 41 entirely covers the first metal electrode layer 29 except for a first non-insulating region 41a. Similarly, the second insulating layer 42 entirely covers the second metal electrode layer 39 except for a second non-insulating region 42a.
[0034] The first non-insulating region 41a is free of the first insulating layer 41 and the first metal electrode layer 29. That is, the first non-insulating region 41a is composed of openings that expose the surface of the first transparent electrode layer 28 and the side surface of the first metal electrode layer 29. The first non-insulating region 41a is disposed on a first straight line X1 that extends in the X direction (first direction).
[0035] Similarly, the second non-insulating region 42a is not provided with the second insulating layer 42 or the second metal electrode layer 39. That is, the second non-insulating region 42a is formed with openings that expose the surface of the second transparent electrode layer 38 and the side surface of the second metal electrode layer 39. The second non-insulating region 42a is disposed on a second straight line X2 that is different from a first straight line X1 that extends in the X direction (first direction).
[0036] The first straight lines X1 and the second straight lines X2 intersect the first electrode layer 27 and the second electrode layer 37, and are arranged alternately in the Y direction (second direction).
[0037] Examples of materials for the first insulating layer 41 and the second insulating layer 42 include silicon oxide (SiO), silicon nitride (SiN), and composites thereof such as silicon oxynitride (SiON). Thermosetting resins such as epoxy resins or resin esters that can be applied by screen printing and baked can also be used. Inorganic particles such as silica or talc may be mixed into these resins to improve printability or chemical resistance.
[0038] A first contact electrode 51 is formed in the first non-insulating region 41a of the first insulating layer 41, and a second contact electrode 52 is formed in the second non-insulating region 42a of the second insulating layer 42. That is, the first contact electrode 51 is disposed on a first straight line X1, and the second contact electrode 52 is disposed on a second straight line X2.
[0039] The first contact electrode 51 is in contact with the surface of the first transparent electrode layer 28, the side surface of the first metal electrode layer 29, and the side surface of the first insulating layer 41. On the other hand, the second contact electrode 52 is in contact with the surface of the second transparent electrode layer 38, the side surface of the second metal electrode layer 39, and the side surface of the second insulating layer 42.
[0040] The first contact electrode 51 and the second contact electrode 52 are formed by printing and curing a printing material containing a particulate metal material such as Cu, Ag, Al, or the like, a resin material, and a solvent. Among these, the Ag paste material is preferable as the printing material from the viewpoint of contact with the solder for connection to the wiring member.
[0041] The width in the Y direction (second direction) of the first non-insulating region 41a of the first insulating layer 41, i.e., the width in the Y direction (second direction) of the first contact electrode 51, is greater than the width of the first wiring member 91. Similarly, the width in the Y direction (second direction) of the second non-insulating region 42a, i.e., the width in the Y direction (second direction) of the second contact electrode 52, is greater than the width of the second wiring member 92. For example, the widths of the first non-insulating region 41a and the second non-insulating region 42a, i.e., the widths of the first contact electrode 51 and the second contact electrode 52, are 1 mm or more and 50 mm or less. This makes it possible to ensure alignment clearance when connecting the wiring members.
[0042] 1, 2A, and 2B, the first electrode layer 27 and the second electrode layer 37 are separated at the boundary between the first region 7 and the second region 8. That is, the first transparent electrode layer 28 and the second transparent electrode layer 38 are separated, and the first metal electrode layer 29 and the second metal electrode layer 39 are separated. In addition, the first insulating layer 41 and the second insulating layer 42 are separated.
[0043] The region between the first transparent electrode layer 28 and the second transparent electrode layer 38, ie, the region between the first metal electrode layer 29 and the second metal electrode layer 39, is not covered with the first insulating layer 41 and the second insulating layer 42.
[0044] In the first metal electrode layer 29, the principal surface opposite to the principal surface in contact with the first transparent electrode layer 28 is covered with a first insulating layer 41. Similarly, in the second metal electrode layer 39, the principal surface opposite to the principal surface in contact with the second transparent electrode layer 38 is covered with a second insulating layer 42.
[0045] On the other hand, the side surfaces of the first metal electrode layer 29 and the first transparent electrode layer 28 are not covered with the first insulating layer 41. Similarly, the side surfaces of the second metal electrode layer 39 and the second transparent electrode layer 38 are not covered with the second insulating layer 42.
[0046] 1, the first wiring member 91 extends in the X direction (first direction) along a first straight line X1. Similarly, the second wiring member 92 extends in the X direction (first direction) along a second straight line X2. That is, the first wiring member 91 and the second wiring member 92 intersect the first electrode layer 27 and the second electrode layer 37, and are alternately arranged in the Y direction (second direction).
[0047] The first wiring member 91 is electrically connected to the first electrode layer 27 by a first contact electrode 51 in the first non-insulating region 41a of the first insulating layer 41, and is electrically insulated from the second electrode layer 37 by the second insulating layer 42. Similarly, the second wiring member 92 is electrically connected to the second electrode layer 37 by a second contact electrode 52 in the second non-insulating region 42a of the second insulating layer 42, and is electrically insulated from the first electrode layer 27 by the first insulating layer 41.
[0048] The center-to-center distance (pitch) in the Y direction between the first wiring member 91 and the second wiring member 92 is greater than the center-to-center distance (pitch) in the X direction between the first electrode layer 27 and the second electrode layer 37. For example, the center-to-center distance (pitch) between the first wiring member 91 and the second wiring member 92 is 5 mm or more and 50 mm or less. This makes it possible to shorten the current path flowing through the electrode layers, reduce output loss caused by electrode resistance, and improve the power generation efficiency of the solar cell.
[0049] The first wiring member 91 and the second wiring member 92 may be a known tab wire or the like.
[0050] Here, in order to reduce the cost of such solar cells, the inventor(s) of the present application have devised the use of a relatively inexpensive metal, for example, Cu (for example, a film formed by a PVD method such as sputtering or a plating method, followed by wet etching) instead of the relatively expensive known Ag paste as the material for the metal electrode layers 29, 39. Note that contact electrodes 51, 52 made of Ag paste are used only in the portions that make contact with the wiring members 91, 92.
[0051] Furthermore, for the purpose of simplifying the manufacturing process of such a solar cell, the inventor(s) have devised a method of using the insulating layers 41, 42 and the contact electrodes 51, 52 (Ag paste) for ensuring insulation and contact with the wiring members 91, 92 also as resists for wet etching of the metal electrode layers 29, 39 (e.g., Cu) and the transparent electrode layers 28, 38. Below, such a solar cell devised by the inventor(s) and a manufacturing method thereof will be described as Comparative Example 1.
[0052] (Solar cell of Comparative Example 1) 4A is a cross-sectional view of a solar cell according to comparative example 1, which is a cross-sectional view corresponding to line IIA-IIA in FIG. 1, and FIG. 4B is a cross-sectional view of a solar cell according to comparative example 1, which is a cross-sectional view corresponding to line IIB-IIB in FIG. 1. The solar cell 1X of Comparative Example 1 shown in Figures 4A and 4B differs from the solar cell 1 shown in Figures 2A and 2B mainly in that a first electrode layer 27X, i.e., a first transparent electrode layer 28X and a first metal electrode layer 29X, are also formed in the first non-insulating region 41a of the first insulating layer 41X, and a first contact electrode 51X is formed on the first metal electrode layer 29X of the first electrode layer 27X in the first non-insulating region 41a, and that a second electrode layer 37X, i.e., a second transparent electrode layer 38X and a second metal electrode layer 39X, are also formed in the second non-insulating region 42a of the second insulating layer 42X, and a second contact electrode 52X is formed on the second metal electrode layer 39X of the second electrode layer 37X in the second non-insulating region 42a.
[0053] (Method of manufacturing solar cell of Comparative Example 1) 5A to 5C, a description will be given below mainly of a manufacturing process for the electrode layers 27X, 37X in the manufacturing method for the solar cell of Comparative Example 1. In the manufacturing process for the electrode layers 27X, 37X in Comparative Example 1, after forming the insulating layers 41X, 42X, the contact electrodes 51X, 52X are formed, and then the electrode layers 27X, 37X, i.e., the metal electrode layers 29X, 39X and the transparent electrode layers 28X, 38X, are simultaneously patterned using the insulating layers 41X, 42X and the contact electrodes 51X, 52X as masks.
[0054] Fig. 5A is a diagram showing a transparent electrode layer material film forming step, a metal electrode layer material film forming step, and an insulating layer forming step in the manufacturing method for a solar cell according to Comparative Example 1, and Fig. 5B is a diagram showing a contact electrode forming step in the manufacturing method for a solar cell according to Comparative Example 1. Fig. 5C is a diagram showing an electrode layer forming step, i.e., a transparent electrode layer forming step and a metal electrode layer forming step, in the manufacturing method for a solar cell according to Comparative Example 1. Figs. 5A to 5C show the back side of semiconductor substrate 11, and omit the front side of semiconductor substrate 11.
[0055] 5A, a series of transparent electrode layer material films 28Z are formed on and across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 by, for example, a CVD method or a PVD method (transparent electrode layer material film forming step). Next, a series of metal electrode layer material films 29Z are formed on the transparent electrode layer material film 28Z, i.e., across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 by, for example, a PVD method such as sputtering or a plating method (metal electrode layer material film forming step).
[0056] Next, a first insulating layer 41X is formed on the first conductive type semiconductor layer 25 via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z, i.e., in the first region 7, except for the first non-insulating region 41a. Also, a second insulating layer 42X is formed on the second conductive type semiconductor layer 35 via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z, i.e., in the second region 8, except for the second non-insulating region 42a (insulating layer forming step). Note that the first insulating layer 41X and the second insulating layer 42X are formed to be spaced apart from each other.
[0057] For example, the first insulating layer 41X and the second insulating layer 42X are formed by printing and baking (curing) a printing material containing a resin material and a solvent using a pattern printing method such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing.
[0058] 5B, a first contact electrode 51X is formed in the first non-insulating region 41a of the first insulating layer 41X, and a second contact electrode 52X is formed in the second non-insulating region 42a of the second insulating layer 42X (contact electrode forming process). For example, a printing material containing Ag particles, a resin material, and a solvent, i.e., an Ag paste material, is printed and baked (cured) using a pattern printing method such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing, to form the first contact electrode 51X and the second contact electrode 52X.
[0059] Next, as shown in FIG. 5C, the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z are simultaneously patterned using an etching method with the first insulating layer 41X and the first contact electrode 51X, and the second insulating layer 42X and the second contact electrode 52X as masks, to form the first transparent electrode layer 28X and the second transparent electrode layer 38X, which are separated from each other, and the first metal electrode layer 29X and the second metal electrode layer 39X, which are separated from each other (electrode layer forming process). As a result, the first electrode layer 27X and the second electrode layer 37X are formed. At this time, the first insulating layer 41X and the second insulating layer 42X are left without being removed.
[0060] An example of an etching solution for simultaneous etching of the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z is a mixed solution of an oxidizing agent such as ammonium persulfate and hydrochloric acid (HCl).
[0061] According to the knowledge of the present inventors, the performance of solar cell 1X may be degraded in the manufacturing method of solar cell 1X in Comparative Example 1. This is considered as follows.
[0062] First, during wet etching of the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z, the etching solution penetrates into the contact electrodes 51X, 52X made of Ag paste. When subsequently annealed or heated in the usage environment, the etching solution that penetrated into the contact electrodes 51X, 52X dissolves the metal electrode layers 29X, 39X and the transparent electrode layers 28X, 38X made of Cu. Then, due to some factor, Cu diffuses into the semiconductor substrate 11 via the semiconductor layers 25, 23, 35, 33 (for example, via local defects, etc.). This may cause damage to the semiconductor substrate 11, resulting in a decrease in the performance of the solar cell 1X (reliability).
[0063] Secondly, a mixed solution of an oxidizing agent and hydrochloric acid is used as an etching solution for the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z. In this etching solution, chlorine is generated from hydrochloric acid by a reduction reaction of the oxidizing agent. Then, the contact electrodes 51X, 52X made of Ag paste are transformed into silver chloride by this chlorine. This may cause the contact property of the contact electrodes 51X, 52X with the wiring member to decrease, and the performance of the solar cell 1X may decrease (contact property).
[0064] In this regard, the inventor(s) of the present application devised a method of etching a metal electrode layer made of Cu, which requires the use of a mixed solution of an oxidizing agent and hydrochloric acid, followed by forming a contact electrode made of Ag, and then etching the transparent electrode layer using only hydrochloric acid.
[0065] (Method for manufacturing solar cell according to the first embodiment) Hereinafter, the method for manufacturing a solar cell according to the first embodiment will be described with reference to Figs. 3A to 3F. Fig. 3A is a diagram showing a semiconductor layer forming step in the method for manufacturing a solar cell according to the first embodiment, and Fig. 3B is a diagram showing a transparent electrode layer material film forming step and a metal electrode layer material film forming step (electrode layer material film forming step) in the method for manufacturing a solar cell according to the first embodiment. Fig. 3C is a diagram showing an insulating layer forming step in the method for manufacturing a solar cell according to the first embodiment, and Fig. 3D is a diagram showing a metal electrode layer forming step (electrode layer forming step) in the method for manufacturing a solar cell according to the first embodiment. Fig. 3E is a diagram showing a contact electrode forming step in the method for manufacturing a solar cell according to the first embodiment, and Fig. 3F is a diagram showing a transparent electrode layer forming step (electrode layer forming step) in the method for manufacturing a solar cell according to the first embodiment. Figs. 3A to 3F show the back side of the semiconductor substrate 11, and the front side of the semiconductor substrate 11 is omitted.
[0066] 3A, a passivation layer 23 and a first conductive type semiconductor layer 25 are formed on a part of the back surface side of the semiconductor substrate 11, specifically, on the first region 7 (semiconductor layer formation step). For example, after a passivation layer material film and a first conductive type semiconductor layer material film are formed on the entire back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 23 and the first conductive type semiconductor layer 25 may be patterned using an etching method that uses a resist generated using a photolithography technique or a printing technique, or a metal mask.
[0067] In addition, examples of the etching solution for the p-type semiconductor layer material film include an acidic solution such as hydrofluoric acid containing ozone or a mixture of nitric acid and hydrofluoric acid, and examples of the etching solution for the n-type semiconductor layer material film include an alkaline solution such as an aqueous solution of potassium hydroxide.
[0068] Alternatively, when a passivation layer and a first conductive type semiconductor layer are laminated on the back side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 23 and the first conductive type semiconductor layer 25 may be deposited and patterned simultaneously using a mask.
[0069] Next, a passivation layer 33 and a second conductive type semiconductor layer 35 are formed on another part of the back surface side of the semiconductor substrate 11, specifically, on the second region 8 (semiconductor layer formation step). For example, as described above, a passivation layer material film and a second conductive type semiconductor layer material film may be formed on the entire back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, and then the passivation layer 33 and the second conductive type semiconductor layer 35 may be patterned using an etching method that uses a resist generated using a photolithography technique or a printing technique, or a metal mask.
[0070] Alternatively, when a passivation layer and a second conductive type semiconductor layer are laminated on the back surface side of the semiconductor substrate 11 using a CVD method or a PVD method, the passivation layer 33 and the second conductive type semiconductor layer 35 may be deposited and patterned simultaneously using a mask.
[0071] In this semiconductor layer forming step, a passivation layer 13 (not shown) may be formed on the entire light-receiving surface side of the semiconductor substrate 11.
[0072] 3B, a series of transparent electrode layer material films 28Z are formed on and across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 (transparent electrode layer material film forming process). The transparent electrode layer material film 28Z can be formed by, for example, a CVD method or a PVD method.
[0073] Next, a series of metal electrode layer material films 29Z (e.g., Cu) is formed on the transparent electrode layer material film 28Z, i.e., across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 (metal electrode layer material film formation process). The metal electrode layer material film 29Z can be formed by, for example, a PVD method such as sputtering or a plating method.
[0074] 3C, a first insulating layer 41 is formed on the first conductive type semiconductor layer 25 via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z, i.e., in the first region 7, except for the first non-insulating region 41a. Also, a second insulating layer 42 is formed on the second conductive type semiconductor layer 35 via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z, i.e., in the second region 8, except for the second non-insulating region 42a (insulating layer forming step). Note that the first insulating layer 41 and the second insulating layer 42 are formed to be spaced apart from each other.
[0075] Methods for forming the first insulating layer 41 and the second insulating layer 42 include a PVD method, a CVD method, a screen printing method, an inkjet method, a gravure coating method, a dispenser method, etc. Among these, it is preferable to form the first insulating layer 41 and the second insulating layer 42 by printing and baking (curing) a printing material containing a resin material and a solvent using a pattern printing method such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing.
[0076] Next, as shown in FIG. 3D, an etching method using the first insulating layer 41 and the second insulating layer 42 as a mask is used to remove exposed portions of the metal electrode layer material film 29Z between the first insulating layer 41 and the second insulating layer 42 and in the first non-insulating region 41a and the second non-insulating region 42a, thereby forming a patterned first metal electrode layer 29 in the first region 7 and a patterned second metal electrode layer 39 in the second region 8 (metal electrode layer formation process: electrode layer formation process).
[0077] The etching solution for etching the metal electrode layer material film 29Z may be a mixed solution of an oxidizing agent such as ammonium persulfate and hydrochloric acid (HCl). At this time, since no contact electrode made of Ag is formed, the etching solution is not included in the contact electrode. In addition, the contact electrode is not denatured.
[0078] 3E, a first contact electrode 51 is formed in the first non-insulating region 41a of the first insulating layer 41, and a second contact electrode 52 is formed in the second non-insulating region 42a of the second insulating layer 42 (contact electrode forming process). As a result, the first contact electrode 51 contacts the surface of the first transparent electrode layer 28, the side surface of the first metal electrode layer 29, and the side surface of the first insulating layer 41. In addition, the second contact electrode 52 contacts the surface of the second transparent electrode layer 38, the side surface of the second metal electrode layer 39, and the side surface of the second insulating layer.
[0079] Examples of a method for forming the first contact electrode 51 and the second contact electrode 52 include press printing such as screen printing or gravure printing, and pattern printing such as ejection printing such as inkjet printing. In the pattern printing method, the first contact electrode 51 and the second contact electrode 52 are formed by printing and baking (curing) a printing material containing Ag particles, a resin material, and a solvent, i.e., an Ag paste material.
[0080] Next, as shown in Fig. 3F, an etching method using the first insulating layer 41 and the first contact electrode 51, and the second insulating layer 42 and the second contact electrode 52 as a mask is used to remove exposed portions of the transparent electrode layer material film 28Z between the first insulating layer 41 and the second insulating layer 42, thereby forming a patterned first transparent electrode layer 28 in the first region 7, and forming a patterned second transparent electrode layer 38 in the second region 8 (electrode layer forming process: transparent electrode layer forming process). As a result, the first electrode layer 27 and the second electrode layer 37 are formed. At this time, the first insulating layer 41 and the second insulating layer 42 are left without being removed.
[0081] An example of an etching solution for the transparent electrode layer material film 28Z is hydrochloric acid (HCl). At this time, since a mixed solution of an oxidizing agent and hydrochloric acid is not used, the metal electrode layers 29 and 39 made of Cu are not dissolved, and Cu is not diffused into the semiconductor substrate 11 through the semiconductor layers 25, 23, 35 and 33 (for example, through local defects) due to some factor. Therefore, the semiconductor substrate 11 is not damaged. In addition, the contact electrodes 51 and 52 are not degenerated.
[0082] Thereafter, optical adjustment layer 15 (not shown) is formed on the entire light-receiving surface side of semiconductor substrate 11. Through the above steps, back electrode type solar cell 1 of this embodiment shown in Figures 1, 2A and 2B is obtained.
[0083] As described above, according to the method for manufacturing a solar cell of this embodiment, a relatively inexpensive metal, for example, Cu (for example, a film formed by a PVD method such as sputtering or a plating method, followed by wet etching) is used as the material for the metal electrode layers 29, 39 instead of the relatively expensive known Ag paste. This makes it possible to reduce the cost of the solar cell 1.
[0084] Furthermore, according to the manufacturing method of the solar cell of this embodiment, the insulating layers 41, 42 and the contact electrodes 51, 52 (Ag paste) for ensuring insulation and contact with the wiring members 91, 92 also serve as resists for wet etching of the metal electrode layers 29, 39 (e.g., Cu) and the transparent electrode layers 28, 38. This makes it possible to eliminate the steps of forming and removing the resists for wet etching of the metal electrode layers 29, 39 and the transparent electrode layers 28, 38, and thus simplifies the manufacturing process of the solar cell.
[0085] Furthermore, according to the manufacturing method of the solar cell of this embodiment, it is necessary to use a mixed solution of an oxidizing agent and hydrochloric acid, and after etching the metal electrode layers 29, 39 made of Cu, the contact electrodes 51, 52 made of Ag are formed, and then the transparent electrode layers 28, 38 are etched using only hydrochloric acid. This makes it possible to suppress a decrease in the performance of the solar cell 1, as will be described in detail below.
[0086] First, contact electrodes 51, 52 made of Ag paste are not exposed to a mixed solution of an oxidizing agent and hydrochloric acid used for wet etching of metal electrode layers 29, 39. As a result, unlike the above-mentioned Comparative Example 1, there is no diffusion of Cu into semiconductor substrate 11 due to the etching solution penetrating into contact electrodes 51, 52 made of Ag paste. This prevents damage to semiconductor substrate 11 caused by Cu, and can suppress deterioration in performance of solar cell 1 caused by this (reliability).
[0087] Secondly, the contact electrodes 51, 52 made of Ag are not exposed to a mixed solution of an oxidizing agent and hydrochloric acid and are not denatured. This prevents deterioration in the contact of the contact electrodes 51, 52 with the wiring member caused by denaturation of the contact electrodes 51, 52 made of Ag, and suppresses deterioration in the performance of the solar cell 1 caused by this (contact).
[0088] As described above, according to the method for manufacturing a solar cell of the present embodiment, it is possible to suppress deterioration in the performance of the solar cell even while simplifying the manufacturing process and reducing the cost of the solar cell.
[0089] (Solar Cell of Second Embodiment) In the first embodiment, a configuration in which a wiring member is disposed on the rear surface of a solar cell is described. In the second embodiment, a configuration in which a wiring member is not disposed on the rear surface of a solar cell, that is, a configuration in which an insulating layer does not need to be disposed on the rear surface of a solar cell is described.
[0090] Fig. 6 is a view of the solar cell according to the second embodiment as viewed from the back surface side, and Fig. 7 is a cross-sectional view of the solar cell taken along line VII-VII in Fig. 6. Solar cell 1A shown in Figs. 6 and 7 is also a back surface electrode type (also called a back contact type or back surface junction type) heterojunction solar cell.
[0091] Solar cell 1A includes a semiconductor substrate 11 having two main surfaces, and has a first region 7 and a second region 8 on the main surfaces (light-receiving surface and back surface) of semiconductor substrate 11.
[0092] The first region 7 has a so-called comb shape and includes a plurality of finger portions 7f corresponding to the teeth of the comb and busbar portions 7b corresponding to supports for the teeth of the comb. The busbar portions 7b extend in a first direction (X direction) along one side of the semiconductor substrate 11, and the finger portions 7f extend from the busbar portions 7b in a second direction (Y direction) intersecting the first direction.
[0093] Similarly, the second region 8 has a so-called comb shape and has a plurality of finger portions 8f corresponding to the teeth of the comb and busbar portions 8b corresponding to supports for the teeth of the comb. The busbar portions 8b extend in a first direction (X direction) along one side portion of the semiconductor substrate 11 that faces the other side portion, and the finger portions 8f extend in a second direction (Y direction) from the busbar portions 8b.
[0094] The finger portions 7f and 8f are strip-shaped and extend in the second direction (Y direction), and are provided alternately in the first direction (X direction).
[0095] As shown in Fig. 7, solar cell 1A includes a passivation layer 13 and an optical adjustment layer 15, which are laminated in this order on the light-receiving surface side of semiconductor substrate 11. Solar cell 1A also includes a passivation layer 23, a first conductive type semiconductor layer 25, and a first electrode layer 27A, which are laminated in this order on a portion (first region 7) of the back surface side of semiconductor substrate 11. Solar cell 1A also includes a passivation layer 33, a second conductive type semiconductor layer 35, and a second electrode layer 37A, which are laminated in this order on another portion (second region 8) of the back surface side of semiconductor substrate 11. Solar cell 1A also includes a first contact electrode layer 51A corresponding to first electrode layer 27A, and a second contact electrode layer 52A corresponding to second electrode layer 37A.
[0096] The first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 are shaped like a comb and have a plurality of finger portions corresponding to the teeth of the comb and busbar portions corresponding to the supports of the teeth of the comb. The busbar portions extend in a first direction (X direction) along one side of the semiconductor substrate 11, and the finger portions extend from the busbar portions in a second direction (Y direction) intersecting the first direction.
[0097] The first electrode layer 27A is formed on the first conductive type semiconductor layer 25, that is, in a first region 7 on the back surface side of the semiconductor substrate 11. On the other hand, the second electrode layer 37A is formed on the second conductive type semiconductor layer 35, that is, in a second region 8 on the back surface side of the semiconductor substrate 11. That is, the first electrode layer 27A and the second electrode layer 37A have a so-called comb shape and have a plurality of finger portions corresponding to the teeth of the comb and a busbar portion corresponding to the support portion of the teeth of the comb. The busbar portion extends in a first direction (X direction) along one side portion of the semiconductor substrate 11, and the finger portion extends from the busbar portion in a second direction (Y direction) intersecting the first direction.
[0098] The first electrode layer 27A has a first transparent electrode layer 28A and a first metal electrode layer 29A laminated in this order on the first conductivity type semiconductor layer 25. On the other hand, the second electrode layer 37A has a second transparent electrode layer 38A and a second metal electrode layer 39A laminated in this order on the second conductivity type semiconductor layer 35.
[0099] The first transparent electrode layer 28A and the second transparent electrode layer 38A are formed of a transparent conductive material such as ITO (Indium Tin Oxide: a composite oxide of indium oxide and tin oxide), ZnO (Zinc Oxide), etc.
[0100] The first metal electrode layer 29A and the second metal electrode layer 39A contain Cu as a metal material, which is less expensive than a known conductive paste material containing Ag powder. For example, the first metal electrode layer 29A and the second metal electrode layer 39A are formed by using a PVD method such as sputtering or a plating method.
[0101] The first contact electrode layer 51A is formed on the first metal electrode layer 29A, that is, in a first region 7 on the back surface side of the semiconductor substrate 11. The second contact electrode layer 52A is formed on the second metal electrode layer 39A, that is, in a second region 8 on the back surface side of the semiconductor substrate 11. That is, as shown in FIG. 6, the first contact electrode layer 51A and the second contact electrode layer 52A have a so-called comb shape and have a plurality of finger portions corresponding to the teeth of the comb and a busbar portion corresponding to the support portion of the teeth of the comb. The busbar portion extends in a first direction (X direction) along one side portion of the semiconductor substrate 11, and the finger portion extends from the busbar portion in a second direction (Y direction) intersecting the first direction.
[0102] The first contact electrode layer 51A and the second contact electrode layer 52A are formed by printing and curing a printing material containing a particulate metal material such as Cu, Ag, Al, etc., a resin material, and a solvent. Among these, the Ag paste material is preferable as the printing material from the viewpoint of contact with the solder for connection to the wiring member.
[0103] 6, the first wiring member 91 is electrically connected to the busbar portion of the first electrode layer 27A via the first contact electrode layer 51A. On the other hand, the second wiring member 92 is electrically connected to the busbar portion of the second electrode layer 37A via the second contact electrode layer 52A.
[0104] Here, in order to reduce the cost of such solar cells, the inventor(s) of the present application have devised the use of a relatively inexpensive metal, for example, Cu (for example, a film formed by a PVD method such as sputtering or a plating method, followed by wet etching) as the material for the metal electrode layers 29A, 39A, instead of the relatively expensive known Ag paste. In addition, in consideration of the contact with the wiring members 91, 92, contact electrode layers 51A, 52A made of Ag paste are used on the metal electrode layers 29A, 39A.
[0105] Furthermore, in order to simplify the manufacturing process of such a solar cell, the inventor(s) have devised a method of using the contact electrode layers 51A, 52A (Ag paste) for ensuring contact with the wiring members 91, 92 as a resist for wet etching of the metal electrode layers 29A, 39A (e.g., Cu) and the transparent electrode layers 28A, 38A. The solar cell and its manufacturing method devised by the inventor(s) will be described below as Comparative Example 2.
[0106] (Solar cell of Comparative Example 2) Fig. 9 is a cross-sectional view of a solar cell according to Comparative Example 2, taken along line VII-VII in Fig. 6. Solar cell 1Y of Comparative Example 2 shown in Fig. 9 differs from solar cell 1A shown in Fig. 7 mainly in that the width of first electrode layer 27Y, i.e., the width of first metal electrode layer 29Y and first transparent electrode layer 28Y, is the same as or narrower than the width of first contact electrode layer 51Y, and in that the width of second electrode layer 37Y, i.e., the width of second metal electrode layer 39Y and second transparent electrode layer 38Y, is the same as or narrower than the width of second contact electrode layer 52Y.
[0107] (Method of manufacturing solar cell of Comparative Example 2) 10A to 10B, a description will be given mainly of a manufacturing process of the electrode layers 27Y, 37Y in the manufacturing method of the solar cell of Comparative Example 2. In the manufacturing process of the electrode layers 27Y, 37Y of Comparative Example 2, the contact electrode layers 51Y, 52Y are formed, and then the electrode layers 27Y, 37Y, i.e., the metal electrode layers 29Y, 39Y and the transparent electrode layers 28Y, 38Y, are simultaneously patterned using the contact electrode layers 51Y, 52Y as masks.
[0108] Fig. 10A is a diagram showing a transparent electrode layer material film forming step, a metal electrode layer material film forming step, and a contact electrode layer forming step in the manufacturing method for a solar cell according to Comparative Example 2, and Fig. 10B is a diagram showing the electrode layer forming step, i.e., the transparent electrode layer forming step and the metal electrode layer forming step, in the manufacturing method for a solar cell according to Comparative Example 2. In Figs. 10A and 10B, the back surface side of semiconductor substrate 11 is shown, and the front surface side of semiconductor substrate 11 is omitted.
[0109] 10A, a series of transparent electrode layer material films 28Z are formed on and across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 by, for example, a CVD method or a PVD method (transparent electrode layer material film forming step). Next, a series of metal electrode layer material films 29Z are formed on the transparent electrode layer material film 28Z, i.e., across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 by, for example, a PVD method such as sputtering or a plating method (metal electrode layer material film forming step).
[0110] Next, a first contact electrode layer 51Y is formed on the first conductive type semiconductor layer 25, i.e., in the first region 7, via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z. Also, a second contact electrode layer 52Y is formed on the second conductive type semiconductor layer 35, i.e., in the second region 8, via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z (contact electrode layer forming process). The first contact electrode layer 51Y and the second contact electrode layer 52Y are formed to be spaced apart from each other.
[0111] For example, using a pattern printing method such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing, a printing material containing Ag particles, a resin material and a solvent, i.e., an Ag paste material, is printed and baked (cured) to form the first contact electrode layer 51Y and the second contact electrode layer 52Y.
[0112] 10B, the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z are simultaneously patterned using an etching method with the first contact electrode layer 51Y and the second contact electrode layer 52Y as masks to form the first transparent electrode layer 28Y and the second transparent electrode layer 38Y separated from each other, and the first metal electrode layer 29Y and the second metal electrode layer 39Y separated from each other (transparent electrode layer forming step, metal electrode layer forming step). As a result, the first electrode layer 27Y and the second electrode layer 37Y are formed.
[0113] An example of an etching solution for simultaneous etching of the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z is a mixed solution of an oxidizing agent such as ammonium persulfate and hydrochloric acid (HCl).
[0114] According to the knowledge of the present inventors, even with the method for manufacturing solar cell 1Y of Comparative Example 2, the performance of solar cell 1X may deteriorate. This is considered as follows.
[0115] First, as in Comparative Example 1, during wet etching of the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z, the etching solution penetrates into the contact electrode layers 51Y, 52Y made of Ag paste. Thereafter, when annealing or heating in the usage environment is performed, the etching solution that penetrates into the contact electrode layers 51Y, 52Y dissolves the metal electrode layers 29Y, 39Y and the transparent electrode layers 28Y, 38Y made of Cu. Then, due to some factor, Cu diffuses into the semiconductor substrate 11 through the semiconductor layers 25, 23, 35, 33 (for example, through local defects, etc.). This may cause damage to the semiconductor substrate 11, resulting in a decrease in the performance of the solar cell 1Y (reliability).
[0116] Secondly, as in Comparative Example 1, a mixed solution of an oxidizing agent and hydrochloric acid is used as an etching solution for the metal electrode layer material film 29Z and the transparent electrode layer material film 28Z, and in this etching solution, chlorine is generated from hydrochloric acid by a reduction reaction of the oxidizing agent. Then, the contact electrode layers 51Y, 52Y made of Ag paste are modified to silver chloride by this chlorine. This may cause a decrease in the contact property of the contact electrode layers 51Y, 52Y with the wiring member, and may cause a decrease in the performance of the solar cell 1Y (contact property).
[0117] In this regard, the inventor(s) of the present application devised a method of etching a metal electrode layer made of Cu, which requires the use of a mixed solution of an oxidizing agent and hydrochloric acid, followed by forming a contact electrode layer made of Ag, and then etching the transparent electrode layer using only hydrochloric acid.
[0118] (Method for manufacturing solar cell according to second embodiment) Hereinafter, the method for manufacturing a solar cell according to the second embodiment will be described with reference to Figs. 8A to 8G. Fig. 8A is a diagram showing a semiconductor layer forming step in the method for manufacturing a solar cell according to the second embodiment, and Fig. 8B is a diagram showing a transparent electrode layer material film forming step and a metal electrode layer material film forming step (electrode layer material film forming step) in the method for manufacturing a solar cell according to the second embodiment. Fig. 8C is a diagram showing an insulating layer forming step in the method for manufacturing a solar cell according to the second embodiment, Fig. 8D is a diagram showing a metal electrode layer forming step (electrode layer forming step) in the method for manufacturing a solar cell according to the second embodiment, and Fig. 8E is a diagram showing an insulating layer removing step in the method for manufacturing a solar cell according to the second embodiment. Fig. 8F is a diagram showing a contact electrode layer forming step in the method for manufacturing a solar cell according to the second embodiment, and Fig. 8G is a diagram showing a transparent electrode layer forming step (electrode layer forming step) in the method for manufacturing a solar cell according to the second embodiment. Figs. 8A to 8G also show the back side of the semiconductor substrate 11, and the front side of the semiconductor substrate 11 is omitted.
[0119] 8A, in the same manner as described above, a passivation layer 23 and a first conductive type semiconductor layer 25 are formed on a part of the back surface side of the semiconductor substrate 11, specifically in the first region 7 (semiconductor layer forming step). Next, in the same manner as described above, a passivation layer 33 and a second conductive type semiconductor layer 35 are formed on another part of the back surface side of the semiconductor substrate 11, specifically in the second region 8 (semiconductor layer forming step). Note that in this semiconductor layer forming step, a passivation layer 13 may be formed on the entire light receiving surface side of the semiconductor substrate 11 (not shown).
[0120] 8B, in the same manner as described above, a series of transparent electrode layer material films 28Z are formed on and across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 (transparent electrode layer material film forming process). The transparent electrode layer material film 28Z can be formed by, for example, a CVD method or a PVD method.
[0121] Next, in the same manner as described above, a series of metal electrode layer material films 29Z (e.g., Cu) is formed on the transparent electrode layer material film 28Z, i.e., across the first conductive type semiconductor layer 25 and the second conductive type semiconductor layer 35 (metal electrode layer material film forming step). The metal electrode layer material film 29Z can be formed by, for example, a PVD method such as sputtering or a plating method.
[0122] 8C, in the same manner as described above, a first insulating layer 41A is formed on the first conductive type semiconductor layer 25, i.e., in the first region 7, via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z. A second insulating layer 42A is formed on the second conductive type semiconductor layer 35, i.e., in the second region 8, via the transparent electrode layer material film 28Z and the metal electrode layer material film 29Z (insulating layer forming step). The first insulating layer 41A and the second insulating layer 42A are formed to be spaced apart from each other.
[0123] Methods for forming the first insulating layer 41A and the second insulating layer 42A include a PVD method, a CVD method, a screen printing method, an inkjet method, a gravure coating method, a dispenser method, etc. Among these, it is preferable to form the first insulating layer 41A and the second insulating layer 42A by printing and baking (curing) a printing material containing a resin material and a solvent using a pattern printing method such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing.
[0124] Next, as shown in FIG. 8D, an etching method using the first insulating layer 41A and the second insulating layer 42A as a mask is used to remove exposed portions of the metal electrode layer material film 29Z between the first insulating layer 41A and the second insulating layer 42A to form a patterned first metal electrode layer 29A in the first region 7 and a patterned second metal electrode layer 39A in the second region 8 (metal electrode layer formation process: electrode layer formation process).
[0125] The etching solution for etching the metal electrode layer material film 29Z may be a mixed solution of an oxidizing agent such as ammonium persulfate and hydrochloric acid (HCl). At this time, since the contact electrode layer made of Ag is not formed, the etching solution is not included in the contact electrode layer. In addition, the contact electrode layer is not denatured.
[0126] Next, as shown in Fig. 8E, first insulating layer 41A and second insulating layer 42A are removed. Examples of the removal solution include an organic solvent such as acetone, or an alkaline solution such as a sodium hydroxide solution.
[0127] Next, as shown in FIG. 8F, a first contact electrode layer 51A is formed on the first insulating layer 41A, and a second contact electrode layer 52A is formed on the second insulating layer 42A (contact electrode layer forming step).
[0128] The first contact electrode layer 51A and the second contact electrode layer 52A can be formed by a pattern printing method such as press printing, such as screen printing or gravure printing, or ejection printing, such as inkjet printing. In the pattern printing method, a printing material containing Ag particles, a resin material, and a solvent, i.e., an Ag paste material, is printed and baked (cured) to form the first contact electrode layer 51A and the second contact electrode layer 52A.
[0129] 8G, an etching method using the first contact electrode layer 51A and the first metal electrode layer 29A, and the second contact electrode layer 52A and the second metal electrode layer 39A as masks is used to remove exposed portions of the transparent electrode layer material film 28Z between the first metal electrode layer 29A and the second metal electrode layer 39A, thereby forming a patterned first transparent electrode layer 28A in the first region 7 and a patterned second transparent electrode layer 38A in the second region 8 (transparent electrode layer forming step: electrode layer forming step). As a result, the first electrode layer 27A and the second electrode layer 37A are formed.
[0130] An example of an etching solution for the transparent electrode layer material film 28Z is hydrochloric acid (HCl). At this time, since a mixed solution of an oxidizing agent and hydrochloric acid is not used, the metal electrode layers 29A and 39A made of Cu are not dissolved, and Cu is not diffused into the semiconductor substrate 11 through the semiconductor layers 25, 23, 35, and 33 (for example, through local defects) due to some factor. Therefore, the semiconductor substrate 11 is not damaged. In addition, the contact electrode layers 51A and 52A are not denatured.
[0131] Thereafter, optical adjustment layer 15 (not shown) is formed on the entire light-receiving surface side of semiconductor substrate 11. Through the above steps, back electrode type solar cell 1A of this embodiment shown in Figs.
[0132] As described above, in the method for manufacturing the solar cell of this embodiment, a relatively inexpensive metal, such as Cu (for example, a film formed by a PVD method such as sputtering or a plating method, followed by wet etching) is used as the material for the metal electrode layers 29A, 39A instead of the relatively expensive known Ag paste, which allows the cost of the solar cell 1A to be reduced.
[0133] Furthermore, in the manufacturing method of the solar cell of this embodiment, it is necessary to use a mixed solution of an oxidizing agent and hydrochloric acid. After etching the metal electrode layers 29A, 39A made of Cu, the contact electrode layers 51A, 52A made of Ag are formed, and then the transparent electrode layers 28A, 38A are etched using only hydrochloric acid. This makes it possible to suppress the deterioration of the performance of the solar cell 1A, as will be described in detail below.
[0134] First, the contact electrode layers 51A, 52A made of Ag paste are not exposed to the mixed solution of oxidizing agent and hydrochloric acid used for wet etching of the metal electrode layers 29A, 39A. As a result, unlike the above-mentioned Comparative Example 2, there is no diffusion of Cu into the semiconductor substrate 11 due to the etching solution penetrating into the contact electrode layers 51A, 52A made of Ag paste. This prevents damage to the semiconductor substrate 11 caused by Cu, and can suppress the deterioration of the performance of the solar cell 1A caused by this (reliability).
[0135] Secondly, the contact electrode layers 51A, 52A made of Ag are not exposed to a mixed solution of an oxidizing agent and hydrochloric acid and are not denatured. This prevents deterioration in the contact of the contact electrode layers 51A, 52A with the wiring member caused by denaturation of the contact electrode layers 51A, 52A made of Ag, and suppresses deterioration in the performance of the solar cell 1A caused by this (contact).
[0136] In this way, even with the method for manufacturing a solar cell according to this embodiment, it is possible to suppress deterioration in the performance of the solar cell while reducing the cost of the solar cell.
[0137] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments, and various changes and modifications are possible. For example, in the above-mentioned embodiments, a manufacturing method of the solar cell 1, 1A using a crystalline silicon-based material is illustrated. However, the present invention is not limited to this, and can be applied to a manufacturing method of a solar cell using various materials such as gallium arsenide (GaAs).
[0138] In the above-described embodiment, the manufacturing method of the heterojunction solar cells 1, 1A has been illustrated, but the present invention is not limited thereto and can be applied to manufacturing methods of various solar cells such as homojunction solar cells. [Explanation of symbols]
[0139] 1,1A,1X,1Y solar cell 7 First area 8 Second area 11 Semiconductor substrate 13,23,33 Passivation layer 15 Optical adjustment layer 25 First conductive type semiconductor layer 27,27A,27X,27Y 1st electrode layer 28,28A,28X,28Y 1st transparent electrode layer 28Z Transparent electrode layer material film 29,29A,29X,29Y 1st metal electrode layer 29Z Metal electrode layer material film 35 Second conductive type semiconductor layer 37,37A,37X,37Y 2nd electrode layer 38,38A,38X,38Y 2nd transparent electrode layer 39,39,39X,39Y 2nd metal electrode layer 41, 41A, 41X First insulating layer 41a First non-insulated area 42, 42A, 42X Second insulating layer 42a Second non-insulated area 51, 51A, 51X, 51Y First contact electrode 51A, 51Y First contact electrode layer 52, 52A, 52X, 52Y Second contact electrode 52A, 52Y Second contact electrode layer 91, 91A First wiring member 92, 92A Second wiring member X1 1st straight line X2 2nd straight line
Claims
1. A method for manufacturing a back electrode type solar cell comprising: a semiconductor substrate; a first conductivity type semiconductor layer, a first transparent electrode layer, and a first metal electrode layer, which are laminated in this order in a first region, which is a part of one main surface side of the semiconductor substrate; and a second conductivity type semiconductor layer, a second transparent electrode layer, and a second metal electrode layer, which are laminated in this order in a second region, which is another part of the one main surface side of the semiconductor substrate, a transparent electrode layer material film forming step of forming a series of transparent electrode layer material films on the first conductive type semiconductor layer and the second conductive type semiconductor layer on the one main surface side of the semiconductor substrate; a metal electrode layer material film forming step of forming a series of metal electrode layer material films, the metal electrode layer material film including copper, on the transparent electrode layer material film; an insulating layer forming step of forming a first insulating layer that entirely covers the metal electrode layer material film in the first region except for a first non-insulating region, and a second insulating layer that entirely covers the metal electrode layer material film in the second region except for a second non-insulating region, the first insulating layer and the second insulating layer being spaced apart from each other; a metal electrode layer forming process, in which exposed portions of the metal electrode layer material film between the first insulating layer and the second insulating layer and in the first non-insulating region and the second non-insulating region are removed using an etching method using the first insulating layer and the second insulating layer as a mask, thereby forming the first metal electrode layer patterned in the first region, forming the second metal electrode layer patterned in the second region, and leaving the first insulating layer and the second insulating layer unremoved; a contact electrode forming step of forming a first contact electrode on the transparent electrode layer material film in the first non-insulating region so as to contact a side surface of the first metal electrode layer and a side surface of the first insulating layer, and forming a second contact electrode on the transparent electrode layer material film in the second non-insulating region so as to contact a side surface of the second metal electrode layer and a side surface of the second insulating layer; a transparent electrode layer forming process for forming the first transparent electrode layer patterned in the first region by removing exposed portions of the transparent electrode layer material film using an etching method in which the first insulating layer and the first contact electrode, and the second insulating layer and the second contact electrode are used as masks, and forming the second transparent electrode layer patterned in the second region, and leaving the first insulating layer and the second insulating layer unremoved; A method for manufacturing a solar cell, comprising:
2. 2. The method for manufacturing a solar cell according to claim 1, wherein in the contact electrode formation process, the first contact electrode and the second contact electrode are formed by printing and curing a printing material containing particulate metal material, a resin material and a solvent.
3. The method for manufacturing a solar cell according to claim 2 , wherein the printing material is a silver paste containing particulate silver material.
4. In the metal electrode layer forming step, a mixed solution of an oxidizing agent and hydrochloric acid is used as an etching solution, In the transparent electrode layer forming step, hydrochloric acid is used as an etching solution. The method for producing a solar cell according to any one of claims 1 to 3.
5. A back electrode type solar cell comprising: a semiconductor substrate; a first conductive type semiconductor layer, a first transparent electrode layer, and a first metal electrode layer, which are laminated in this order in a first region, which is a part of one main surface side of the semiconductor substrate; and a second conductive type semiconductor layer, a second transparent electrode layer, and a second metal electrode layer, which are laminated in this order in a second region, which is another part of the one main surface side of the semiconductor substrate; a first insulating layer formed in the first region so as to entirely cover the first metal electrode layer except for a first non-insulating region; a second insulating layer formed in the second region so as to entirely cover the second metal electrode layer except for a second non-insulating region; a first contact electrode formed in the first non-insulating region; a second contact electrode formed in the second non-insulating region; Equipped with the first metal electrode layer and the second metal electrode layer include copper; The first non-insulating region has the first transparent electrode layer formed therein and the first metal electrode layer not formed therein; the second transparent electrode layer is formed in the second non-insulating region, and the second metal electrode layer is not formed in the second non-insulating region; the first contact electrode is in contact with a main surface of the first transparent electrode layer, a side surface of the first metal electrode layer, and a side surface of the first insulating layer; the second contact electrode is in contact with a main surface of the second transparent electrode layer, a side surface of the second metal electrode layer, and a side surface of the second insulating layer; Solar cell.
6. The solar cell of claim 5 , wherein the first contact electrode and the second contact electrode contain particulate silver.
7. A method for manufacturing a back electrode type solar cell comprising: a semiconductor substrate; a first conductivity type semiconductor layer, a first transparent electrode layer, and a first metal electrode layer, which are laminated in this order in a first region, which is a part of one main surface side of the semiconductor substrate; and a second conductivity type semiconductor layer, a second transparent electrode layer, and a second metal electrode layer, which are laminated in this order in a second region, which is another part of the one main surface side of the semiconductor substrate, a transparent electrode layer material film forming step of forming a series of transparent electrode layer material films on the first conductive type semiconductor layer and the second conductive type semiconductor layer on the one main surface side of the semiconductor substrate; a metal electrode layer material film forming step of forming a series of metal electrode layer material films, the metal electrode layer material film including copper, on the transparent electrode layer material film; an insulating layer forming step of forming a first insulating layer that entirely covers the metal electrode layer material film in the first region and a second insulating layer that entirely covers the metal electrode layer material film in the second region, the first insulating layer and the second insulating layer being spaced apart from each other; a metal electrode layer forming step of forming the first metal electrode layer patterned in the first region by removing exposed portions of the metal electrode layer material film using an etching method with the first insulating layer and the second insulating layer as a mask, forming the second metal electrode layer patterned in the second region, and removing the first insulating layer and the second insulating layer; a contact electrode layer forming step of forming a first contact electrode layer on the first metal electrode layer and forming a second contact electrode layer on the second metal electrode layer; a transparent electrode layer forming step of removing exposed portions of the transparent electrode layer material film by an etching method using the first contact electrode layer, the first metal electrode layer, and the second contact electrode layer, and the second metal electrode layer as a mask, thereby forming the first transparent electrode layer patterned in the first region, and forming the second transparent electrode layer patterned in the second region; A method for manufacturing a solar cell, comprising:
8. 8. The method for manufacturing a solar cell according to claim 7, wherein in the contact electrode layer formation step, the first contact electrode layer and the second contact electrode layer are formed by printing and curing a printing material containing a particulate metal material, a resin material and a solvent.
9. The method for manufacturing a solar cell according to claim 8 , wherein the printing material is a silver paste containing particulate silver material.
10. In the metal electrode layer forming step, a mixed solution of an oxidizing agent and hydrochloric acid is used as an etching solution, In the transparent electrode layer forming step, hydrochloric acid is used as an etching solution. The method for producing a solar cell according to any one of claims 7 to 9.
Citation Information
Patent Citations
Crossed net-shaped electric contact back contact heterojunction battery and assembly manufacturing method
CN111834470A
Solar battery
JP2014127550A
Solar cell module and method for manufacturing the same
JP2015159286A
Solar cell with improved structure and solar cell module using the same
JP2018133567A
Interdigitated back contact heterojunction photovoltaic device with a floating junction front surface field
US20140224306A1