Anode active material for aqueous secondary battery, cathode for aqueous secondary battery and aqueous secondary battery
Non-graphitizable carbon with C-F bonding groups and optimized surface area ratios in the negative electrode active material enhances the charge/discharge efficiency and safety of aqueous secondary batteries by suppressing electrolyte decomposition and reducing irreversible lithium loss.
Patent Information
- Application Number
- JP2021574490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-31
- Filing Date
- 2020-12-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-12-01
AI Technical Summary
Conventional aqueous secondary batteries suffer from low charge/discharge efficiency and safety issues due to the use of organic solvent-based electrolytes, which are flammable and have low ionic conductivity, limiting rapid charging and discharging capabilities.
The use of a negative electrode active material composed of non-graphitizable carbon with C-F bonding groups on its surface, optimized by specific BET specific surface area and peak intensity ratios, to suppress reductive decomposition and enhance charge/discharge efficiency in aqueous secondary batteries.
This approach improves the charging and discharging efficiency of aqueous secondary batteries by forming a dense film on the non-graphitizable carbon surface, reducing irreversible lithium loss and enhancing overall battery performance.
Smart Images

Figure 0007576761000002 
Figure 0007576761000003 
Figure 0007576761000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative electrode active material for an aqueous secondary battery, a negative electrode for an aqueous secondary battery, and an aqueous secondary battery. [Background technology]
[0002] As a secondary battery with high output and high energy density, a lithium ion secondary battery is widely used, which includes a positive electrode, a negative electrode, and an electrolyte, and charges and discharges by transferring lithium ions between the positive electrode and the negative electrode. Conventional secondary batteries use an organic solvent-based electrolyte to achieve a high energy density.
[0003] However, organic solvents are generally flammable, making safety an important issue, and the ionic conductivity of organic solvents is lower than that of aqueous solutions, making rapid charge / discharge characteristics insufficient.
[0004] In view of such problems, secondary batteries using an electrolyte solution containing water (hereinafter, sometimes referred to as an aqueous electrolyte solution) have been studied. For example, Patent Documents 1 and 2 propose the use of an aqueous solution containing a high concentration of alkaline salt as the aqueous electrolyte solution of a secondary battery, and Patent Document 3 proposes the use of an aqueous electrolyte solution in which an organic carbonate is added to an aqueous solution containing a high concentration of alkaline salt. Patent Document 4 also proposes a secondary battery having a negative electrode, a positive electrode, and an aqueous electrolyte solution, and the negative electrode has a composite of a negative electrode active material and polytetrafluoroethylene. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6423453 [Patent Document 2] International Publication No. 2017 / 122597 [Patent Document 3] JP 2018-73819 A [Patent Document 4] JP 2019-57359 A Summary of the Invention
[0006] Conventional aqueous secondary batteries have the problem of only being able to achieve low charge / discharge efficiency.
[0007] One aspect of the present disclosure is a negative electrode active material that is applied to an aqueous secondary battery that uses an aqueous electrolyte solution containing water and a lithium salt, the negative electrode active material including non-graphitizable carbon, the non-graphitizable carbon having a C-F bond group on its surface, and the non-graphitizable carbon having a peak intensity of I at about 688 eV derived from a C-F bond in an XPS spectrum obtained by X-ray photoelectron spectroscopy measurement. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV As the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is X, and the BET specific surface area (m 2 When X and Y each satisfy Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2, the negative electrode active material for an aqueous secondary battery is a water-based secondary battery negative electrode active material, in which X and Y each satisfy Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2.
[0008] Another aspect of the present disclosure is a negative electrode for an aqueous secondary battery, comprising the above-mentioned negative electrode active material for an aqueous secondary battery.
[0009] Another aspect of the present disclosure is an aqueous secondary battery having the above-mentioned aqueous secondary battery negative electrode, a positive electrode, and an aqueous electrolyte solution containing water and a lithium salt.
[0010] According to the present disclosure, the charge / discharge efficiency of a water-based secondary battery can be improved. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the relationship between the I688eV / I284eV value (X) and the BET specific surface area (Y) in the non-graphitizable carbon of the present disclosure. [Diagram 2]FIG. 2 is a schematic cross-sectional view showing an example of the water-based secondary battery of this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In general, in an aqueous secondary battery using an aqueous electrolyte solution containing water and a lithium salt, when a carbon material is used as the negative electrode active material, the aqueous electrolyte solution is actively reductively decomposed on the carbon material, and the progress of the charging reaction of the negative electrode active material is inhibited. However, as a result of intensive research, the present inventors have found that by using a non-graphitizable carbon having a C-F bond group formed on its surface as the negative electrode active material, and optimizing the absolute amount of the C-F bond group on the surface of the non-graphitizable carbon and the BET specific surface area of the non-graphitizable carbon, the reductive decomposition of the aqueous electrolyte solution can be suppressed to advance the charging / discharging reaction of the negative electrode active material, thereby improving the charging / discharging efficiency of the aqueous secondary battery. Hereinafter, one embodiment of the present disclosure will be described.
[0013] The negative electrode active material for an aqueous secondary battery according to one embodiment of the present disclosure includes non-graphitizable carbon, the non-graphitizable carbon having a C—F bond group on its surface, and the non-graphitizable carbon has a peak intensity of I at about 688 eV derived from a C—F bond in an XPS spectrum obtained by X-ray photoelectron spectroscopy measurement. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV As the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is X, and the BET specific surface area (m 2 When the amount of X and Y in the negative electrode active material is 0.1 / g, the X and Y satisfy Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2. By using the negative electrode active material for a water-based secondary battery according to one embodiment of the present disclosure, the charge / discharge efficiency of a secondary battery can be improved. The mechanism by which this effect is achieved is not fully clear, but the following is presumed.
[0014] The C-F bond group on the surface of the non-graphitizable carbon is a surface modification group in which fluorine is bonded to the non-graphitizable carbon or a functional group present on the surface of the non-graphitizable carbon, and is formed by subjecting the non-graphitizable carbon to a fluorine treatment described later. By forming the C-F bond group on the surface of the non-graphitizable carbon, the electrochemical catalytic activity at the defective site (electrochemically active site) on the surface of the non-graphitizable carbon can be suppressed. As a result, the growth rate of the film formed on the surface of the non-graphitizable carbon by the reductive decomposition of the aqueous electrolyte can be suppressed, and the denseness of the film can be improved. In addition, the water repellency of the C-F bond group can be expected to have the effect of keeping water molecules in the aqueous electrolyte away from the surface of the non-graphitizable carbon. However, since the C-F bond group on the surface of the non-graphitizable carbon can also become an irreversible site that traps lithium ions, if the absolute amount of the C-F bond group is too large, the amount of lithium released from the negative electrode active material during discharge decreases. Therefore, by optimizing the absolute amount of C—F bond groups on the surface of non-graphitizable carbon, a dense film can be formed and the decrease in the amount of lithium released due to the increase in irreversible sites can be suppressed, so that the charge / discharge reaction of the negative electrode active material can be promoted and the charge / discharge efficiency of the secondary battery can be improved. 284eV Peak intensity I 688eV The ratio (I 688eV / I 284eV When the BET specific surface area is defined as X and the BET specific surface area is defined as Y, the amount of C-F bond groups present on the non-graphitizable carbon surface becomes appropriate from the viewpoint of exerting the above-mentioned effect, by satisfying Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2, respectively.
[0015] FIG. 1 shows the I of the non-graphitizable carbon of the present disclosure. 688eV / I 284eV 1 is a graph showing the relationship between the I value (X) and the BET specific surface area (Y). As shown in FIG. 1, the area G filled with gray is 688eV / I 284eV The I value (X) and the BET specific surface area (Y) are in the ranges satisfying Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2. 688eV / I 284eV The value (X) and the BET specific surface area (Y) are included in the region G.688eV / I 284eV Even if the value (X) satisfies 0.1≦X≦5, when the BET specific surface area (Y) is Y<2, the absolute amount of CF bond groups on the non-graphitizable carbon surface is small, so a dense film is not formed, and when the BET specific surface area (Y) is Y≧-0.3X+3.75, the absolute amount of CF bond groups on the non-graphitizable carbon surface is large, so the amount of lithium released due to an increase in irreversible sites decreases. Also, even if the BET specific surface area (Y) satisfies Y<-0.3X+3.75 and Y≧2, the I 688eV / I 284eV When the value (X) is 0.1>X, the absolute amount of C—F bond groups on the surface of non-graphitizable carbon is small, so a dense film is not formed, and I 688eV / I 284eV When the value (X) is X>5, the absolute amount of C—F bond groups on the surface of the non-graphitizable carbon is large, and therefore the amount of lithium released decreases due to an increase in irreversible sites.
[0016] Hereinafter, an embodiment of the aqueous secondary battery according to the present disclosure will be described in detail.
[0017] The shape of the aqueous secondary battery of this embodiment is not particularly limited, and examples thereof include a coin type, a button type, a sheet type, a laminated type, a cylindrical type, a flat type, and a square type. FIG. 2 is a schematic cross-sectional view showing an example of the aqueous secondary battery of this embodiment. The aqueous secondary battery 20 shown in FIG. 2 includes a cup-shaped battery case 21, a positive electrode 22 provided on the upper part of the battery case 21, a negative electrode 23 provided at a position facing the positive electrode 22 via a separator 24, a gasket 25 formed of an insulating material, and a sealing plate 26 disposed at an opening of the battery case 21 and sealing the battery case 21 via the gasket 25. In the aqueous secondary battery 20 shown in FIG. 2, an electrolyte 27 is filled in the space between the positive electrode 22 and the negative electrode 23. The electrolyte 27, the positive electrode 22, the negative electrode 23, and the separator 24 will be described in detail below.
[0018] The electrolyte 27 is an aqueous electrolyte containing a solvent containing water and a lithium salt. Since the aqueous electrolyte contains water, which is not flammable, the safety of the aqueous secondary battery 20 can be improved. The solvent may be water alone, but the water content of the total amount of the solvent contained in the electrolyte 27 is preferably 50% or more by volume. By making the water content 50% or more by volume, the safety of the aqueous secondary battery 20 can be improved in some cases.
[0019] Furthermore, the amount of water relative to the lithium salt contained in the electrolyte solution 27 is preferably 1:4 or less, more preferably in the range of 1:0.5 to 1:4, and even more preferably in the range of 1:0.5 to 1:3, in terms of the molar ratio of lithium salt:water. When the amount of water relative to the lithium salt contained in the electrolyte solution 27 is within the above range, the potential window of the electrolyte solution 27 is expanded, for example, compared to when it is outside the above range, and the voltage applied to the aqueous secondary battery 20 may be increased.
[0020] The electrolytic solution 27 may contain a solvent other than water. Examples of the solvent other than water include organic solvents such as esters, ethers, nitriles, alcohols, ketones, amines, amides, sulfur compounds, and hydrocarbons. In addition, the solvent may be a halogen-substituted solvent in which at least a part of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. Specifically, in terms of improving the battery characteristics of the aqueous secondary battery, organic carbonates such as cyclic organic carbonates such as ethylene carbonate, propylene carbonate, vinylidene carbonate, and butylene carbonate, chain organic carbonates such as dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate, and fluorinated organic carbonates containing fluorine as a constituent element such as fluoroethylene carbonate, fluorodimethyl carbonate, and methyl fluoropropionate are preferred. Among the above-mentioned examples, cyclic organic carbonates and fluorinated organic carbonates containing fluorine as a constituent element are particularly preferred in terms of suppressing the self-discharge of the battery. Among the above-listed fluorinated organic carbonates, fluoroethylene carbonate is preferred. These organic solvents may be used alone or in combination of two or more.
[0021] The amount of organic carbonate relative to the lithium salt contained in electrolytic solution 27, in terms of the molar ratio of lithium salt:organic carbonate, is preferably in the range of 1:0.01 to 1:2.5, and more preferably in the range of 1:0.05 to 1:2. When the amount of organic carbonate relative to the lithium salt contained in electrolytic solution 27 is within the above range, the battery characteristics of the aqueous secondary battery may be improved in some cases, compared to when the amount is outside the above range.
[0022] Any lithium salt can be used as long as it dissolves in a solvent containing water and dissociates to cause lithium ions to exist in the electrolyte solution 27. It is preferable that the lithium salt does not cause deterioration of battery characteristics due to reaction with materials constituting the positive and negative electrodes. Examples of such lithium salts include salts with inorganic acids such as perchloric acid, sulfuric acid, and nitric acid, salts with halide ions such as chloride ions and bromide ions, and salts with organic anions containing carbon atoms in their structures.
[0023] Examples of the organic anion constituting the lithium salt include anions represented by the following general formulas (i) to (vi). (R 1 SO 2 )(R 2 SO 2 )N - (i) (R 1 , R 2 are each independently selected from an alkyl group or a halogen-substituted alkyl group. 1 and R 2 may be bonded to each other to form a ring. R 3 SO 3 - (ii) (R 3 is selected from an alkyl group or a halogen-substituted alkyl group. R 4 CO 2 - (iii) (R 4is selected from an alkyl group or a halogen-substituted alkyl group. (R 5 SO 2 ) 3 C - (iv) (R 5 is selected from an alkyl group or a halogen-substituted alkyl group. [(R 6 SO 2 )N(SO 2 )N(R 7 SO 2 )] 2- (v) (R 6 , R 7 is selected from an alkyl group or a halogen-substituted alkyl group. [(R 8 SO 2 )N(CO)N(R 9 SO 2 )] 2- (vi) (R 8 , R 9 is selected from an alkyl group or a halogen-substituted alkyl group. In the above general formulas (i) to (vi), the number of carbon atoms in the alkyl group or the halogen-substituted alkyl group is preferably 1 to 6, more preferably 1 to 3, and further preferably 1 to 2. The halogen in the halogen-substituted alkyl group is preferably fluorine. The number of halogen substitutions in the halogen-substituted alkyl group is equal to or less than the number of hydrogen atoms in the original alkyl group.
[0024] R 1 ~R 9 Each of the above is, for example, a group represented by the following general formula (vii):
[0025] C n H a F b Cl c Br d I e (vii) (n is an integer greater than or equal to 1, a, b, c, d, and e are integers greater than or equal to 0, and 2n+1=a+b+c+d+e is satisfied.) Specific examples of the organic anion represented by the above general formula (i) include bis(trifluoromethanesulfonyl)imide (TFSI; [N(CF 3 SO 2 ) 2 ] - ), bis(perfluoroethanesulfonyl)imide (BETI; [N(C 2 F 5 SO 2 ) 2 ] - ), (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([N(C 2 F 5 SO 2 )(CF 3 SO 2 )] - Specific examples of the organic anion represented by the general formula (ii) include, for example, CF 3 SO 3 - , C 2 F 5 SO 3 - Specific examples of the organic anion represented by the general formula (iii) include, for example, CF 3 CO 2 - , C 2 F 5 CO 2 - Specific examples of the organic anion represented by the general formula (iv) include tris(trifluoromethanesulfonyl)carbonate ([(CF 3 SO 2 ) 3 C] - ), tris(perfluoroethanesulfonyl)carbonic acid ([(C 2 F 5 SO 2 ) 3 C] - ) and the like. Specific examples of the organic anion represented by the above general formula (V) include sulfonylbis(trifluoromethanesulfonyl)imide ([(CF 3 SO 2 )N(SO 2 )N(CF 3 SO2 )] 2- ), sulfonylbis(perfluoroethanesulfonyl)imide ([(C 2 F 5 SO 2 )N(SO 2 )N(C 2 F 5 SO 2 )] 2- ), sulfonyl(perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([(C 2 F 5 SO 2 )N(SO 2 )N(CF 3 SO 2 )] 2- ) and the like. Specific examples of the organic anion represented by the above general formula (vi) include carbonylbis(trifluoromethanesulfonyl)imide ([(CF 3 SO 2 )N(CO)N(CF 3 SO 2 )] 2- ), carbonylbis(perfluoroethanesulfonyl)imide ([(C2F5SO2)N(CO)N(C 2 F 5 SO 2 )] 2- ), carbonyl(perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([(C 2 F 5 SO 2 )N(CO)N(CF 3 SO 2 )] 2- ) etc.
[0026] Examples of organic anions other than those represented by the above general formulas (i) to (vi) include anions such as bis(1,2-benzenediolate(2-)-O,O') borate, bis(2,3-naphthalenediolate(2-)-O,O') borate, bis(2,2'-biphenyldiolate(2-)-O,O') borate, and bis(5-fluoro-2-oleate-1-benzenesulfonic acid-O,O') borate.
[0027] The anion constituting the lithium salt is preferably an imide anion. Specific examples of suitable imide anions include the imide anions exemplified as the organic anion represented by the general formula (i) above, as well as bis(fluorosulfonyl)imide (FSI; [N(FSO 2 ) 2 ] - ), (fluorosulfonyl)(trifluoromethanesulfonyl)imide (FTI; [N(FSO 2 )(CF 3 SO 2 )] - ) etc.
[0028] The lithium salt having a lithium ion and an imide anion is preferably, for example, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(perfluoroethanesulfonyl)imide (LiBETI), lithium (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide (LiFSI), or lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide (LiFTI), in terms of being able to effectively suppress self-discharge of the battery, and more preferably lithium bis(trifluoromethanesulfonyl)imide (LiTFSI). These may be used alone or in combination of two or more kinds.
[0029] Other examples of lithium salts include CF 3 SO 3 Li, C. 2 F 5 SO 3 Li, C.F. 3 CO 2 Li, C. 2 F 5 CO 2 Li, (CF 3 SO 2 ) 3 CLi, (C 2 F 5 SO 2 ) 3 CLi, (C 2 F 5 SO 2 ) 2 (CF3 SO 2 )CLi, (C 2 F 5 SO 2 )(CF 3 SO 2 ) 2 CLi, [(CF 3 SO 2 )N(SO 2 )N(CF 3 SO 2 )]Li 2 , [(C 2 F 5 SO 2 )N(SO 2 )N(C 2 F 5 SO 2 )]Li 2 , [(C 2 F 5 SO 2 )N(SO 2 )N(CF 3 SO 2 )]Li 2 , [(CF 3 SO 2 )N(CO)N(CF 3 SO 2 )]Li 2 , [(C 2 F 5 SO 2 )N(CO)N(C 2 F 5 SO 2 )]Li 2 , [(C 2 F 5 SO 2 )N(CO)N(CF 3 SO 2 )]Li 2 , lithium bis(1,2-benzenedioleate(2-)-O,O')borate, lithium bis(2,3-naphthalenediolate(2-)-O,O')borate, lithium bis(2,2'-biphenyldioleate(2-)-O,O')borate, lithium bis(5-fluoro-2-oleate-1-benzenesulfonic acid-O,O')borate, lithium perchlorate (LiClO 4 ), lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium nitrate (LiNO3 ), lithium sulfate (Li 2 SO 4 ), lithium sulfide (Li 2 S), lithium hydroxide (LiOH), etc. These may be used alone or in combination of two or more.
[0030] The electrolyte 27 preferably contains an additive. The additive is added, for example, to improve the battery performance, and any additive known in the art can be used. In particular, a dicarbonyl group-containing compound is preferred in that it can form an electrochemically stable film on the negative electrode by the reduction reaction of the electrolyte 27 and effectively suppress the reduction decomposition reaction of the electrolyte 27.
[0031] Examples of the dicarbonyl group-containing compound include succinic acid, glutaric acid, phthalic acid, maleic acid, citraconic acid, glutaconic acid, itaconic acid, and diglycolic acid. The dicarbonyl group-containing compound may be an anhydride, and examples thereof include succinic anhydride, glutaric anhydride, phthalic anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and diglycolic anhydride. Among the above, succinic acid, succinic anhydride, maleic acid, maleic anhydride, diglycolic acid, and glutaric acid are preferred in that they form an electrochemically stable film on the negative electrode and can more effectively suppress the reductive decomposition reaction of the electrolyte 27. Among these, succinic acid and maleic anhydride are preferred. These may be used alone or in combination of two or more.
[0032] The content of the additive is, for example, preferably 0.1% by mass to 5.0% by mass, and more preferably 0.5% by mass to 3.0% by mass, relative to the total amount of the electrolytic solution 27. By setting the content within the above range, the reductive decomposition reaction of the electrolytic solution 27 may be more effectively suppressed than when the content is outside the above range.
[0033] The positive electrode 22 includes, for example, a positive electrode current collector and a positive electrode composite layer formed on the positive electrode current collector. As the positive electrode current collector, a foil of a metal that is electrochemically and chemically stable in the potential range of the positive electrode, a film having the metal disposed on the surface layer, or the like can be used. The form of the positive electrode current collector is not particularly limited, and for example, a mesh body of the metal, a punching sheet, an expanded metal, or other porous body may be used. As the material of the positive electrode current collector, a known metal that can be used in a secondary battery using an aqueous electrolyte can be used. Examples of such metals include stainless steel, Al, aluminum alloy, and Ti. The thickness of the positive electrode current collector is preferably, for example, 3 μm or more and 50 μm or less from the viewpoint of current collecting properties, mechanical strength, and the like.
[0034] The positive electrode mixture layer contains a positive electrode active material. The positive electrode mixture layer may also contain a binder, a conductive material, etc. The positive electrode 22 can be manufactured, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive material, etc., onto a positive electrode current collector, drying and rolling the coating, and forming a positive electrode mixture layer on the positive electrode current collector.
[0035] Examples of the positive electrode active material include lithium-containing transition metal oxides that contain lithium (Li) and transition metal elements such as cobalt (Co), manganese (Mn), and nickel (Ni). Other examples of the positive electrode active material include transition metal sulfides, metal oxides, and lithium iron phosphate (LiFePO 4 ) and lithium iron pyrophosphate (Li 2 FeP 2 O 7 Lithium-containing polyanion compounds containing one or more transition metals such as sulfur-based compounds (Li 2 S), oxygen, and oxygen-containing metal salts such as lithium oxide. The positive electrode active material is preferably a lithium-containing transition metal oxide, which preferably contains at least one of Co, Mn, and Ni as a transition metal element.
[0036] The lithium-containing transition metal oxide may contain other additive elements besides Co, Mn, and Ni. For example, it may contain aluminum (Al), zirconium (Zr), boron (B), magnesium (Mg), scandium (Sc), yttrium (Y), titanium (Ti), iron (Fe), copper (Cu), zinc (Zn), chromium (Cr), lead (Pb), tin (Sn), sodium (Na), potassium (K), barium (Ba), strontium (Sr), calcium (Ca), tungsten (W), molybdenum (Mo), niobium (Nb), and silicon (Si), etc.
[0037] Specific examples of the lithium-containing transition metal oxide include, for example, Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 , LiMPO 4 , Li 2 MPO 4 F (in each chemical formula, M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0 < x ≦ 1.2, 0 < y ≦ 0.9, 2.0 ≦ z ≦ 2.3). The lithium-containing transition metal oxide may be used alone or in combination of multiple kinds. From the viewpoint of increasing the capacity, it is preferable that the lithium-containing transition metal oxide contains 80 mol% or more of Ni with respect to the total amount of transition metals other than lithium. Also, from the viewpoint of the stability of the crystal structure, the lithium-containing transition metal oxide is Lia Ni b Co c Al d O 2 It is more preferable that (0 < a ≤ 1.2, 0.8 ≤ b < 1, 0 < c < 0.2, 0 < d ≤ 0.1, b + c + d = 1).
[0038] As the conductive material, known conductive materials that enhance the electrical conductivity of the positive electrode composite layer can be used. For example, carbon materials such as carbon black, acetylene black, ketjen black, graphite, carbon nanofibers, carbon nanotubes, and graphene can be mentioned. As the binder, known binders that maintain a good contact state between the positive electrode active material and the conductive material and enhance the binding property of the positive electrode active material and the like to the surface of the positive electrode current collector can be used. For example, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, carboxymethyl cellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), etc. can be mentioned.
[0039] The negative electrode 23 includes, for example, a negative electrode current collector and a negative electrode composite layer formed on the negative electrode current collector. As the negative electrode current collector, a foil of a metal that is electrochemically and chemically stable within the potential range of the negative electrode, and a film having the metal disposed on the surface layer, etc. can be used. The form of the negative electrode current collector is not particularly limited. For example, a porous body such as a mesh body, a punching sheet, or an expanded metal of the metal may be used. As the material of the negative electrode current collector, known metals that can be used in aqueous secondary batteries can be used. Such metals include, for example, Al, Ti, Mg, Zn, Pb, Sn, Zr, In, etc. These may be used alone or as an alloy of two or more, and it is sufficient that they are composed of a material having at least one as the main component. Also, when two or more elements are included, it is not necessarily required to be alloyed. From the viewpoints of current collection property, mechanical strength, etc., the thickness of the negative electrode current collector is preferably, for example, 3 μm or more and 50 μm or less.
[0040] The negative electrode mixture layer contains a negative electrode active material. The negative electrode mixture layer may also contain a binder, a conductive material, and the like. The conductive material and binder can be the same as those on the positive electrode side. The negative electrode 23 can be manufactured, for example, by applying a negative electrode mixture slurry containing a negative electrode active material, a binder, a conductive material, and the like onto a negative electrode current collector, drying and rolling the coating, and forming a negative electrode mixture layer on the negative electrode current collector.
[0041] The negative electrode active material contains non-graphitizable carbon having a C-F bond group on the surface. Hereinafter, the non-graphitizable carbon may be referred to as surface-modified non-graphitizable carbon. In terms of improving the charge / discharge efficiency of aqueous secondary batteries, surface-modified non-graphitizable carbon is characterized by a peak intensity of I at about 688 eV derived from C-F bonds in an XPS spectrum obtained by X-ray photoelectron spectroscopy measurement. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV As the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is X, and the BET specific surface area (m 2 When X is 0.1≦X≦5 and Y≧2, it is sufficient that X and Y satisfy Y<−0.3X+3.75, 0.1≦X≦2 and Y≧3.
[0042] Peak intensities from XPS spectra measured by X-ray photoelectron spectroscopy I 688eV and peak intensity I 284eV is obtained under the following conditions:
[0043] Measurement equipment: PHI Quantera SXM, manufactured by ULVAC-PHI X-ray source used: Al-mono (1486.6eV), 20kV / 100W Analysis area: 100μmφ Photoelectron take-off angle: 45° Neutralization conditions: Electron + floating ion neutralization Measurement range (eV): 1300~0 Step (eV): 1.0 Pass E(eV):280.0 Measurement time (msec / step): 60 The BET specific surface area is obtained under the following measurement conditions.
[0044] Measurement equipment: Quantachrome, Autosorb iQ-MP Pre-drying (degassing conditions): in vacuum, 100℃, 1 hour Adsorption gas: N 2 The surface-modified non-graphitizable carbon is obtained by subjecting non-graphitizable carbon to a fluorine treatment. The fluorine treatment of non-graphitizable carbon can be performed, for example, by a dry method or a wet method. In the dry method, a gaseous fluorinating agent is used to subject the non-graphitizable carbon to a fluorine treatment in a gas phase. In the wet method, a liquid fluorinating agent is used to subject the non-graphitizable carbon to a fluorine treatment in a liquid phase. Among these methods, the dry method is preferred from the viewpoints of ease of operation, ease of forming a C-F bond group on the surface of the non-graphitizable carbon, and difficulty in doping F into the interior of the non-graphitizable carbon.
[0045] The fluorinating agent is, for example, fluorine (F 2 ), nitrogen trifluoride, chlorine trifluoride, etc. are included among the fluorinating agents. Among them, fluorine (F 2 In addition, when the fluorination treatment is carried out by a dry method, the fluorinating agent may be diluted with a diluent gas such as an inert gas, such as nitrogen gas, helium gas, neon gas, argon gas, or xenon gas.
[0046] In the following, a case where non-graphitizable carbon is subjected to a fluorine treatment by a dry method will be described.
[0047] When non-graphitizable carbon is fluorinated by a dry method, the non-graphitizable carbon can be fluorinated by contacting the non-graphitizable carbon with a fluorinating agent gas. Examples of the method for contacting the non-graphitizable carbon with a fluorinating agent gas include a method in which the non-graphitizable carbon is placed in a closed atmosphere of the fluorinating agent gas and the non-graphitizable carbon is contacted with the fluorinating agent gas (called a batch method), and a method in which the non-graphitizable carbon is contacted with the fluorinating agent gas by supplying the fluorinating agent gas to the non-graphitizable carbon (flow method).
[0048] When the non-graphitizable carbon is brought into contact with the fluorinating agent gas, it is preferable to heat the non-graphitizable carbon in order to increase the efficiency of the fluorination treatment, etc. The heating temperature is, for example, preferably 200° C. or more and 500° C. or less, and more preferably 300° C. or more and 400° C. or less.
[0049] The longer the contact time of non-graphitizable carbon with the fluorinating agent gas, the greater the peak intensity I 688eV In addition, the longer the time for which the non-graphitizable carbon is in contact with the fluorinating agent gas, the smaller the BET specific surface area of the fluorinated surface-modified non-graphitizable carbon. Therefore, the time for which the non-graphitizable carbon is in contact with the fluorinating agent gas is I 688eV / I 284eV Value X and BET specific surface area (m 2 / g)Y must be set to satisfy Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2. Note that the fluorination treatment of non-graphitizable carbon reduces the BET specific surface area of the surface-modified non-graphitizable carbon, so the BET specific surface area (m 2 / g) Y does not have to satisfy the above.
[0050] In the XPS spectrum obtained by X-ray photoelectron spectroscopy, it is preferable that the surface-modified non-graphitizable carbon does not have a peak at about 685 eV (for example, in the range of 683.5 eV to 686.5 eV) derived from the Me-F bond (Me: alkali metal, alkaline earth metal). However, the peak derived from the Me-F bond in the XPS spectrum measured by X-ray photoelectron spectroscopy is confirmed for the surface-modified non-graphitizable carbon before charging and discharging the secondary battery. This is because a film having an Me-F bond such as LiF may be formed on the surface of the surface-modified non-graphitizable carbon after charging and discharging the secondary battery. By using the surface-modified non-graphitizable carbon that does not have a Me-F bond group on the surface, for example, since there is no insulator such as LiF on the surface of the surface-modified graphite during initial charging, local non-uniformity of the current density during charging can be suppressed, and a thinner and denser film can be formed. Therefore, the contact resistance between the surface-modified non-graphitizable carbons can be suppressed, and the battery characteristics such as output characteristics can be improved in some cases.
[0051] The conditions for measuring the peaks derived from Me-F bonds in the XPS spectrum measured by X-ray photoelectron spectroscopy are as follows.
[0052] Measurement equipment: PHI Quantera SXM, manufactured by ULVAC-PHI X-ray source used: Al-mono (1486.6eV), 20kV / 100W Analysis area: 100μmφ Photoelectron take-off angle: 45° Neutralization conditions: Electron + floating ion neutralization Measuring element: F1s Measurement range (eV): 695-675 Step (eV): 0.05 Path E(eV):55 Measurement time (msec / step): 60 The surface-modified non-graphitizable carbon preferably has an A atomic % / B atomic % ratio of 3 to 30, where A atomic % is the percentage of fluorine present on the surface of the surface-modified non-graphitizable carbon, and B atomic % is the percentage of fluorine present in the entire surface-modified non-graphitizable carbon. When A atomic % / B atomic % ratio is less than 3, the number of C-F bond groups on the surface of the surface-modified non-graphitizable carbon may be small, and the density of the film formed on the surface may be reduced, or there may be many F atoms inside the surface-modified non-graphitizable carbon, and there may be an increase in irreversible sites that trap lithium ions inside the surface-modified non-graphitizable carbon. Therefore, the charge / discharge efficiency of the secondary battery may be reduced compared to when A atomic % / B atomic % ratio satisfies the above range. In addition, when A atomic % / B atomic % ratio exceeds 30, the number of C-F bond groups on the surface of the surface-modified non-graphitizable carbon may be large, and there may be an increase in irreversible sites that trap lithium ions on the surface, and there may be an increase in the charge / discharge efficiency of the secondary battery. In order to increase the amount of fluorine present on the surface of the surface-modified non-graphitizable carbon, it is preferable to carry out the fluorine treatment by the above-mentioned dry method.
[0053] The fluorine percentage (A atomic %) of the surface-modified non-graphitizable carbon is a value calculated by X-ray photoelectron spectroscopy. Specifically, the fluorine amount (atomic %), carbon amount (atomic %), and oxygen amount (atomic %) are determined by X-ray photoelectron spectroscopy, and the fluorine percentage is calculated by setting the total amount of these to 100, and this value is the fluorine percentage (A atomic %) of the surface-modified non-graphitizable carbon. The fluorine percentage (B atomic %) of the entire surface-modified non-graphitizable carbon is a value calculated using the following elemental analyzer. The fluorine percentage (weight %) of the entire surface-modified non-graphitizable carbon is determined by an organic elemental analysis system (XS-2100H, manufactured by Mitsubishi Chemical Analytical Co., Ltd.), and then the carbon percentage (weight %) of the entire surface-modified non-graphitizable carbon is determined by an elemental analyzer (JM11, manufactured by J Science Lab Co., Ltd.). The total of the fluorine amount (weight %), carbon amount (weight %) and oxygen amount (weight %) of the entire surface-modified non-graphitizable carbon is taken as 100, and the above-mentioned fluorine percentage (weight %) and carbon percentage (weight %) are subtracted to determine the oxygen percentage (weight %) of the entire surface-modified non-graphitizable carbon. The fluorine percentage (weight %) is then converted to a fluorine percentage (atomic %), and this value is taken as the fluorine percentage (B atomic %) of the entire surface-modified non-graphitizable carbon.
[0054] The average particle size (D50) of the surface-modified non-graphitizable carbon is preferably, for example, 3 μm or more and 20 μm or less. When the average particle size (D50) of the surface-modified non-graphitizable carbon satisfies the above range, the packing density of the negative electrode is improved and good battery characteristics may be obtained compared to when the average particle size (D50) does not satisfy the above range. The average particle size (D50) means the volume average particle size at which the volume integrated value is 50% in the particle size distribution obtained by the laser diffraction scattering method.
[0055] The non-graphitizable carbon subjected to the fluorine treatment is a carbon material in which minute graphite crystals are arranged in random directions and further graphitization hardly progresses, and for example, the average lattice spacing (d002) of the (002) plane obtained by X-ray diffraction measurement is 0.37 nm or more, and the half-width of the peak near the diffraction angle 2θ=22.5° (for example, 21.0° to 24.0°) is 5° or more. The peak near the diffraction angle 2θ=22.5° is a peak derived from the (002) plane of the non-graphitizable carbon.
[0056] The conditions for the X-ray diffraction measurement are as follows.
[0057] Measurement device: PANalytical, X'PertPRO Target / monochrome: Cu / C Sample state: Powder Tube voltage / current: 45kV / 40mA Scanning mode: Continuous Step width: 0.01° Scanning speed: 5s / step Slit width (DS / SS / RS): 0.5° / None / 0.1mm Measurement range: 10°~120° Measurement temperature: room temperature Analysis software: PANalytical, HighScore Plus Lattice constant calculation method: Calculated using regression analysis from peak positions and plane indices calculated by local profile fitting analysis In addition to the surface-modified non-graphitizable carbon, the negative electrode active material may contain a material that can be used as a negative electrode active material in a conventional lithium ion secondary battery, as long as the effect of the present disclosure is not impaired. For example, an alloy containing lithium element, a metal oxide, a metal sulfide, a metal nitride, or other metal compound, silicon, etc., can be mentioned. Examples of the alloy containing lithium element include lithium aluminum alloy, lithium tin alloy, lithium lead alloy, and lithium silicon alloy. Examples of the metal oxide containing lithium element include lithium titanate (Li 4 Ti 5 O 12Examples of metal nitrides containing lithium include lithium cobalt nitride, lithium iron nitride, and lithium manganese nitride. Examples of sulfur-based compounds are also included.
[0058] The separator 24 is not particularly limited as long as it is permeable to lithium ions and has the function of electrically separating the positive electrode and the negative electrode, and for example, a porous sheet composed of a resin or an inorganic material is used. Specific examples of the porous sheet include a microporous thin film, a woven fabric, a nonwoven fabric, and the like. Examples of the material of the separator 24 include olefin resins such as polyethylene and polypropylene, polyamide, polyamideimide, cellulose, and the like. Examples of the inorganic material constituting the separator 24 include glass and ceramics such as borosilicate glass, silica, alumina, and titania. The separator 24 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. The separator 24 may also be a multilayer separator including a polyethylene layer and a polypropylene layer, and a separator having a material such as an aramid resin or ceramic applied to the surface of the separator may also be used.
[0059] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0060] <Example 1> [Negative electrode] Surface-modified non-graphitizable carbon was produced by subjecting non-graphitizable carbon to fluorine treatment. Specifically, the Ni crucible containing the non-graphitizable carbon was placed in a heating furnace, and N 2 Gas (flow rate: 2.7 L / min) was supplied for 1.5 hours. Then, N 2 While continuing the gas supply, the temperature inside the heating furnace was raised to 300°C over 3.5 hours. Next, the temperature inside the heating furnace was maintained at 300°C and N 2 Gas (flow rate: 2.0 L / min) 2A mixed gas containing N2 gas (1.9 mol / h) was fed into the heating furnace for 2 minutes. After that, the heating in the heating furnace was stopped and N2 gas was fed into the heating furnace. 2 Gas (flow rate: 2.7 L / min) was supplied and the mixture was allowed to cool to obtain a surface-modified non-graphitizable carbon. The physical properties of the obtained surface-modified non-graphitizable carbon were measured, and the results are shown in Table 1.
[0061] The surface-modified non-graphitizable carbon (negative electrode active material) and PVDF as a binder were mixed in N-methyl-2-pyrrolidone (NMP) at a solid content mass ratio of 96:4 to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied onto a negative electrode current collector made of copper foil, and the coating was dried and then rolled with a rolling roller. Then, the negative electrode was obtained by cutting into a predetermined electrode size. The application amount of the negative electrode composite slurry and the packing density of the negative electrode active material layer were 32.3 g / m, respectively. 2 , 1.0gcm -3 It was.
[0062] [Positive electrode] LiCoO as a positive electrode active material 2 The positive electrode mixture slurry was prepared by mixing the carbon black as a conductive material and the PVdF as a binder in a mass ratio of 94:3:3 in NMP. The positive electrode mixture slurry was then applied onto a positive electrode current collector made of Ti foil, the coating was dried, and then rolled with a rolling roller. The positive electrode was then cut into a predetermined electrode size to obtain a positive electrode. The application amount of the positive electrode mixture slurry and the packing density of the positive electrode active material layer were 65.0 g / cm. 2 , 2.8gcm -3 It was.
[0063] [Aqueous electrolyte] LITFSI, LIBETI, water, dimethyl carbonate (DMC), and fluoroethylene carbonate (FEC) were mixed in a molar ratio of 0.7:0.3:2.0:0.13:0.11 to prepare an aqueous electrolyte solution with a water volume ratio of 68% in the solvent.
[0064] [Test cell] A three-electrode cell (test cell) containing the above electrolyte was constructed, with the above negative electrode as a working electrode, the above positive electrode as a counter electrode, and Ag / AgCl (3M NaCl) as a reference electrode.
[0065] <Example 2> In the preparation of surface-modified non-graphitizable carbon, N 2 Gas and F 2 A surface-modified non-graphitizable carbon was produced in the same manner as in Example 1, except that the mixed gas of the gases was supplied into the heating furnace for 10 minutes. The physical properties of the obtained surface-modified non-graphitizable carbon were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified non-graphitizable carbon was used as the negative electrode active material.
[0066] <Comparative Example 1> Non-fluorinated non-graphitizable carbon was used as the negative electrode active material. The physical properties of the non-graphitizable carbon were measured, and the results are summarized in Table 1. A test cell was constructed in the same manner as in Example 1 using this non-graphitizable carbon as the negative electrode active material.
[0067] <Comparative Example 2> In the preparation of surface-modified non-graphitizable carbon, the temperature in the heating furnace was raised to 400°C over 4.5 hours. The temperature in the heating furnace was maintained at 400°C. 2 Gas and F 2 Surface-modified non-graphitizable carbon was produced in the same manner as in Example 1, except that the mixed gas of the gases was supplied into the heating furnace for 2 minutes. The physical properties of the obtained surface-modified non-graphitizable carbon were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified non-graphitizable carbon was used as the negative electrode active material.
[0068] <Comparative Example 3> In the preparation of surface-modified non-graphitizable carbon, N 2 Gas and F 2A surface-modified non-graphitizable carbon was produced in the same manner as in Comparative Example 2, except that the mixed gas of the gases was supplied into the heating furnace for 10 minutes. The physical properties of the obtained surface-modified non-graphitizable carbon were measured, and the results are summarized in Table 1. Then, a test cell was constructed in the same manner as in Example 1, except that this surface-modified non-graphitizable carbon was used as the negative electrode active material.
[0069] Cyclic voltammetry (CV) measurements were performed using the test cells of Examples 1-2 and Comparative Examples 1-3, and the oxidation and reduction electricity quantities in the first cycle were measured. Specifically, the X (potential)-Y (current) curve obtained by the above CV measurement was converted to an X (time)-Y (current) curve using analysis software attached to the electrochemical measurement device, and the reduction electricity quantity (C) was calculated by integrating the entire period from the time when the reduction reaction started to the time when the oxidation reaction started, and the oxidation electricity quantity (C) was calculated by integrating the entire period from the time when the oxidation reaction started to the time when the reduction reaction started. When calculating the reduction electricity quantity, if the oxidation reaction did not start, the reduction electricity quantity (C) was calculated by integrating the entire period until the end of the first cycle, and the oxidation electricity quantity (C) was set to 0. Also, when calculating the oxidation electricity quantity, if the reduction reaction did not start, the oxidation electricity quantity (C) was calculated by integrating the entire period until the end of the first cycle. Then, the initial efficiency (%) was calculated using the following formula. Initial efficiency (%) = (amount of oxidation electricity (C)) / (amount of reduction electricity (C)) x 100 The measurement conditions for cyclic voltammetry are shown below.
[0070] Starting potential: OCV First folding potential: -2.950V vs. Ag / AgCl (3M NaCl) (0.288V based on Li) Second folding potential: -0.238V vs. Ag / AgCl (3M NaCl) (3V based on Li) Number of cycles: 2 cycles Sweep speed: 0.5mV / sec Measurement temperature: 25℃ The initial efficiency shown in Table 1 is a value showing the charge / discharge efficiency in the first cycle of Comparative Example 1 relatively to the charge / discharge efficiency in the first cycle of the other Examples and Comparative Examples, taking the charge / discharge efficiency in the first cycle of Comparative Example 1 as 100.
[0071] [Table 1]
[0072] I 688eV / I 284eV Examples 1 and 2, which used surface-modified non-graphitizable carbon in which the BET specific surface area (Y) and the BET specific surface area (X) are within the region satisfying Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2 (region G shown in FIG. 1), showed increased charge-discharge efficiency compared to Comparative Examples 1 to 3, which used negative electrode active materials not within region G shown in FIG. 1. [Explanation of symbols]
[0073] 20 Water-based secondary battery 21 Battery case 22 Positive electrode 23 Negative electrode 24 Separator 25 Gasket 26 Sealing plate 27 Electrolyte.
Claims
1. A negative electrode active material for use in an aqueous secondary battery using an aqueous electrolyte solution containing water and a lithium salt, The negative electrode active material contains non-graphitizable carbon, The non-graphitizable carbon has a C—F bond group on its surface, The non-graphitizable carbon has a peak intensity of I near 688 eV derived from a C—F bond in an XPS spectrum obtained by X-ray photoelectron spectroscopy. 688eV The peak intensity at around 284 eV due to the C-C bond is I 284eV As the peak intensity I 284eV The peak intensity I 688eV The ratio (I 688eV / I 284eV value) is X, and the BET specific surface area (m 2 / g) is defined as Y, and the X and Y satisfy Y<-0.3X+3.75, 0.1≦X≦5, and Y≧2.
2. 2. The negative electrode active material for an aqueous secondary battery according to claim 1, wherein, when a fluorine percentage present on a surface of the non-graphitizable carbon is defined as A atomic %, and a fluorine percentage present in the entire non-graphitizable carbon is defined as B atomic %, the A atomic % / B atomic % is 3 or more and 30 or less.
3. 3. The negative electrode active material for a water-based secondary battery according to claim 1, wherein the non-graphitizable carbon has an average particle size (D50) of 3 μm or more and 20 μm or less.
4. A negative electrode for use in an aqueous secondary battery using an aqueous electrolyte solution containing water and a lithium salt, The negative electrode comprises the negative electrode active material for an aqueous secondary battery according to any one of claims 1 to 3. Negative electrode for water-based secondary batteries.
5. 5. An aqueous secondary battery comprising a negative electrode, a positive electrode, and an aqueous electrolyte solution containing water and a lithium salt, the negative electrode being the aqueous secondary battery negative electrode according to claim 4.
6. The aqueous secondary battery of claim 5 , wherein the lithium salt comprises a salt having a lithium ion and an imide anion.
7. 7. The aqueous secondary battery of claim 6, wherein the lithium salt comprises lithium bis(trifluoromethanesulfonyl)imide.
8. 8. The aqueous secondary battery according to claim 5, wherein the content of the water relative to the lithium salt contained in the aqueous electrolyte is 1:4 or less in terms of a molar ratio of the lithium salt:water.
9. The aqueous secondary battery according to any one of claims 5 to 8, wherein the aqueous electrolyte solution contains an organic carbonate.
10. The aqueous secondary battery according to claim 9, wherein a content of the organic carbonate relative to the lithium salt contained in the aqueous electrolyte solution is in a range of 1:0.01 to 1:2.5 in terms of a molar ratio of the lithium salt:the organic carbonate, and a content of the water relative to the lithium salt contained in the aqueous electrolyte solution is in a range of 1:0.5 to 1:4 in terms of a molar ratio of the lithium salt:the water.
11. The aqueous secondary battery according to claim 9 or 10, wherein the organic carbonate comprises a cyclic organic carbonate.
12. The aqueous secondary battery according to claim 11 , wherein the cyclic organic carbonate contains fluorine as a constituent element.
13. 13. The aqueous secondary battery of claim 12, wherein the cyclic organic carbonate comprises fluoroethylene carbonate.
Citation Information
Patent Citations
Aqueous battery using carbon fluoride as anode
CN102903921A
Method for preparing graphite fluoride at low temperature
CN103043641A
Rotation controller for rotary head
JP1989023453A
Activating agent for lead storage battery and lead storage battery using same
JP2003059527A