Sound-absorbing material, sound-absorbing panel using same, and method for manufacturing sound-absorbing material
The sound absorbing material with a polyester resin filling and polypropylene resin skin, featuring moisture discharge openings, addresses the issue of decreased sound absorption in humid environments by maintaining performance and durability in such conditions.
Patent Information
- Application Number
- JP2021154578
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-09-22
AI Technical Summary
Conventional sound absorbing materials made of polyethylene terephthalate resin fibers experience a decrease in sound absorption coefficient in humid environments due to moisture exposure.
A sound absorbing material composed of a filling material with polyester resin fibers encapsulated by a skin material made of polypropylene resin nonwoven fabric, featuring hydrophobic properties and strategically designed openings for moisture discharge, along with a layered nonwoven fabric structure for enhanced durability and sound absorption.
The material maintains excellent sound absorption coefficients in the low frequency range of 800 to 1250 Hz even in humid conditions, while also providing resistance to water and impact, ensuring longevity and effective moisture management.
Smart Images

Figure 0007576797000002 
Figure 0007576797000003 
Figure 0007576797000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a sound-absorbing material, a sound-absorbing panel using the same, and a method for manufacturing the sound-absorbing material. [Background technology]
[0002] Conventionally, there has been known a sound-absorbing material made of a laminated nonwoven fabric, in which a first nonwoven fabric made of polyethylene terephthalate resin fibers and having a specific range of density, thickness and breathability is used as a skin layer (skin material), and a second nonwoven fabric made of polyethylene terephthalate resin staple fibers and having a specific range of basis weight and thickness is used as a base layer (filling) (see, for example, Patent Document 1).
[0003] According to the sound-absorbing material described in Patent Document 1, the first nonwoven fabric and the second nonwoven fabric are laminated together, and thus the sound-absorbing material is provided with an excellent sound absorption coefficient in the low frequency range of 800 to 1250 Hz. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 143857 Summary of the Invention [Problem to be solved by the invention]
[0005] However, sound-absorbing materials made of short fibers of polyethylene terephthalate resin, such as the sound-absorbing material described in Patent Document 1, have the disadvantage that the sound absorption coefficient decreases in an environment with a lot of moisture.
[0006] Therefore, an object of the present invention is to provide a sound-absorbing material whose sound absorption coefficient is unlikely to decrease even in a moisture-rich environment. [Means for solving the problem]
[0007] In order to achieve this object, the sound absorbing material of the present invention comprises a padding containing fibers made of at least polyester resin, and a skin material enclosing the padding, Material The surface material is made of a nonwoven fabric containing fibers made of a polypropylene resin, and at least a part of the surface material is Water discharge It is characterized by having a mouth.
[0008] In addition, this is for the entire surface area of the skin, excluding the area under the seal. Open It is preferable that the ratio of the area of the openings be 10% or less, from the viewpoint of a balance between making it difficult for moisture to penetrate into the padding and efficiently discharging moisture that has penetrated into the padding to the outside of the sound-absorbing material.
[0009] Since fibers made of polypropylene-based resin are hydrophobic, the sound-absorbing material of the present invention does not come into contact with water because the filling is encapsulated in the skin material, and the sound absorption rate is less likely to decrease even in a humid environment.
[0010] Furthermore, since at least a portion of the skin material has an opening, even if water penetrates into the sound-absorbing material, specifically into the skin material, despite the hydrophobicity of the skin material, the water can be discharged to the outside of the skin material, specifically the sound-absorbing material, through an opening disposed, for example, in the bottom part of the skin material.
[0011] The sound-absorbing material of the present invention has an excellent sound absorption coefficient in the low frequency range of 800 to 1250 Hz because the padding contains fibers made of at least polyester-based resin, and it is preferable that the padding further contains fibers made of polypropylene-based resin.
[0012] In addition, in the sound-absorbing material of the present invention, the average fiber diameter of the filling is preferably in the range of 10 to 100 μm in order to provide excellent sound absorption coefficient in the low frequency range of 800 to 1250 Hz and to achieve both excellent drainage properties.
[0013] In the sound absorbing material of the present invention, the surface material has a thickness of 200 to 2000 mmH to prevent the padding from coming into contact with water. 2It is preferable that the surface material has a water pressure resistance in the range of 200 mmH. 2 If the temperature is less than 2000 mmH, it may not be possible to prevent the padding from coming into contact with water. 2 Even if it exceeds O, it is not easy to obtain any further effect.
[0014] However, when the sound-absorbing material of the present invention is used outdoors, it may be worn down and its lifespan may be shortened by the impact of solid objects such as hailstones, sleet, or pebbles. Therefore, it is desirable for the skin material to have abrasion resistance against the impact of solid objects (shot blast resistance) in addition to the water pressure resistance.
[0015] In the sound-absorbing material of the present invention, in order to combine the water pressure resistance within the above-mentioned range with the shot blast resistance, it is preferable that the surface layer includes a first spunbond nonwoven fabric, a meltblown nonwoven fabric located on the first spunbond nonwoven fabric, and a second spunbond nonwoven fabric located on the meltblown nonwoven fabric.
[0016] Generally, the average fiber diameter of the fibers contained in the meltblown nonwoven fabric is smaller than the average fiber diameter of the fibers contained in the spunbond nonwoven fabric, so that the meltblown nonwoven fabric provides water pressure resistance in the above-mentioned range, while the first or second spunbond nonwoven fabric located in the outer layer of the meltblown nonwoven fabric provides the shot blast resistance and protects the meltblown nonwoven fabric.
[0017] In this case, the meltblown nonwoven fabric preferably contains fibers having an average fiber diameter in the range of 0.5 to 5 μm in order to obtain the water pressure resistance in the above range, and the first or second spunbond nonwoven fabric preferably contains fibers having an average fiber diameter in the range of 25 to 50 μm in order to obtain the shot blast resistance.
[0018] In the sound absorbing material of the present invention, the surface material is, for example, a spunbond nonwoven fabric layer including a third spunbond nonwoven fabric. Consists of onlyThe third spunbond nonwoven fabric may be one having hydrophobic properties due to the inclusion of fibers made of a polypropylene-based resin, and thus capable of obtaining the water pressure resistance in the above-mentioned range. In this case, the third spunbond nonwoven fabric preferably contains fibers having an average fiber diameter in the range of 15 to 100 μm. If the average fiber diameter of the fibers contained in the third spunbond nonwoven fabric exceeds 100 μm, the water pressure resistance may not be obtained, and if it is less than 15 μm, the shot blast resistance may not be obtained.
[0019] In order to provide the shot blast resistance, it is further preferable that the fibers located on the surface of the spunbonded nonwoven fabric layer have an average fiber diameter in the range of more than 30 μm and not more than 100 μm. Since the spunbonded nonwoven fabric layer contains fibers having an average fiber diameter in the above range on the surface, it is preferable that the spunbonded nonwoven fabric layer has a welded area ratio of 20% or more, and the welded area ratio in the above range can be obtained, for example, by subjecting the spunbonded nonwoven fabric layer to an embossing process (thermocompression process).
[0020] The sound-absorbing panel of the present invention includes any one of the sound-absorbing materials described above and a frame that houses the sound-absorbing material, and is characterized in that the frame has openings in at least a portion of the shielding plate and side walls.
[0021] The method for producing a sound-absorbing material of the present invention includes a fusing step of wrapping a filling material containing at least a fiber made of a polyester resin with a skin material which is a nonwoven fabric containing a fiber made of a polypropylene resin, and fusing an end of the skin material; and a fusing step of fusing the end of the skin material at least on the side of the skin material located below gravity when the sound-absorbing material is disposed. Water discharge and a drilling step for forming an opening. In the fusion step, the end portions of the skin are preferably fused by ultrasonic sealing. [Brief description of the drawings]
[0022] [Figure 1] 1 is an explanatory cross-sectional view showing the configuration of a first embodiment of a sound-absorbing material of the present invention. [Diagram 2]FIG. 4 is an explanatory cross-sectional view showing the configuration of a second embodiment of a sound-absorbing material of the present invention. [Diagram 3] FIG. 4 is an explanatory cross-sectional view showing the configuration of a modified example of an opening in the first embodiment. [Figure 4] FIG. 11 is an explanatory cross-sectional view showing the configuration of another modified example of the opening in the first embodiment. [Diagram 5] 6 is an explanatory cross-sectional view showing the configuration of another modified example of the opening in the first embodiment. FIG. [Figure 6] FIG. 11 is an explanatory cross-sectional view showing the configuration of still another modified example of the opening in the first embodiment. [Figure 7] FIG. 2 is an explanatory cross-sectional view showing one example of the configuration of the sound-absorbing panel of the present invention. [Figure 8] 11 is an explanatory cross-sectional view showing a configuration of a modified example of an opening in the sound-absorbing panel of the present invention. FIG. [Figure 9] FIG. 11 is an explanatory cross-sectional view showing the configuration of another modified example of the opening in the sound-absorbing panel of the present invention. [Figure 10] 13A to 13C are explanatory cross-sectional views showing the configurations of other modified examples of the openings in the sound-absorbing panel of the present invention. [Figure 11] FIG. 11 is an explanatory cross-sectional view showing the configuration of still another modified example of the opening in the sound-absorbing panel of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Next, embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0024] As shown in Fig. 1, a first embodiment of the sound-absorbing material 1 of this embodiment is composed of, for example, at least a filling 2 containing fibers made of polyester-based resin, and a single sheet of skin material 3 that is provided on both the front and back sides (upper and lower layers) of the filling 2 and contains the filling 2. The filling 2 is sandwiched between the skin material 3 that is folded in two, and the skin material 3 has seal portions 4 on three sides of its periphery. As a result, the filling 2 is surrounded by the folded portions of the skin material 3 and the seal portions 4, and is contained in the skin material 3.
[0025] It should be noted that the filling 2 needs to be enclosed within the skin material 3, and the configuration in which the filling 2 is enclosed within the skin material 3 is not limited to the configuration shown in FIG.
[0026] For example, as in the second embodiment of the sound-absorbing material 1 of this embodiment shown in Figure 2, it may be configured to include a filling 2 and two skin materials 3, 3 that are provided on both the front and back sides (upper and lower layers) of the filling 2 and encase the filling 2, and the skin materials 3, 3 have a sealing portion 4 at their peripheral portions that surround the filling 2.
[0027] The basis weight of the sound-absorbing material 1 is set to 500 to 3000 g / m from the viewpoint of further improving the sound absorption coefficient mainly in the range of 100 to 2000 Hz, preventing a decrease in workability due to an increase in the weight of the sound-absorbing material, and preventing the strength of the structure supporting the sound-absorbing material from being increased due to the increase in weight. 2 The range is preferably 1000 to 2800 g / m 2 More preferably, the range is 1300 to 2200 g / m 2 It is most preferable that the range is 100%.
[0028] The thickness of the sound-absorbing material 1 is preferably in the range of 10 to 100 mm, and more preferably in the range of 20 to 80 mm, from the viewpoint of further improving the sound absorption coefficient in the low frequency range, particularly in the range of 100 to 1000 Hz, and from the viewpoint of ensuring efficient space when installing it in a structure or the like.
[0029] The padding 2 may be made of only fibers made of polyester resin such as polyethylene terephthalate resin, or may further contain fibers made of polypropylene resin. By including fibers made of polyethylene terephthalate resin and fibers made of polypropylene resin, the padding 2 can have the effect of more easily maintaining an appropriate balance between bulkiness (ensuring sound absorption coefficient) and hydrophobicity.
[0030] As the filling 2, for example, a nonwoven fabric molding containing short fibers of the polyester (polyethylene terephthalate) resin and short fibers of the polypropylene resin can be used.
[0031] The weight of the padding 2 is set to 400 to 2900 g / m from the viewpoint of further improving the sound absorption coefficient in the range of 100 to 2000 Hz, preventing a decrease in workability due to an increase in the weight of the sound absorbing material, and preventing the strength of the structure supporting the sound absorbing material from being increased due to the increase in weight. 2 The range is preferably 900 to 2800 g / m 2 More preferably, the range is 1200 to 2500 g / m 2 It is most preferable that the range is 100%.
[0032] The polyester (polyethylene terephthalate) resin staple fibers and the polypropylene resin staple fibers may be produced by a known melt spinning method or may be commercially purchased. The polyester (polyethylene terephthalate) resin staple fibers may have an average fiber length in the range of 10 to 100 mm and an average fiber diameter in the range of 10 to 70 μm, for example, and the polypropylene resin staple fibers may have an average fiber length in the range of 10 to 100 μm and an average fiber diameter in the range of 10 to 50 μm, for example.
[0033] The inventors have discovered that the smaller (thinner) the average fiber diameter of the fibers contained in the filling 2, the denser it is and the better its sound absorption performance, particularly in the range of 800 Hz or less; however, it is desirable for the average fiber diameter of the fibers to be larger (thicker) from the standpoints of ease of discharging moisture absorbed in the filling 2, preventing the sound-absorbing material from bending when installed on a frame, maintaining the shape of the filling when it absorbs water, and long-term weather resistance.
[0034] Therefore, the average fiber diameter of the fibers contained in the filling 2 is preferably in the range of 10 to 100 μm, more preferably in the range of 10 to 70 μm, even more preferably in the range of 10 to 50 μm, even more preferably in the range of 15 to 45 μm, and particularly preferably in the range of 20 to 40 μm.
[0035] The "average fiber diameter of the fibers" referred to here is calculated from all the fibers contained in the filling 2. In other words, when the filling 2 is composed only of polyester such as polyethylene terephthalate, it means the average fiber diameter of the polyester, and when the filling 2 is composed of polyester and polypropylene-based resin, it means the average fiber diameter of all the fibers of the polyester fibers and polypropylene-based fibers.
[0036] The ratio of polyester-based resin staple fibers to polypropylene-based resin staple fibers in the nonwoven fabric molding is preferably, by mass, 99:1 to 5:95 (polyester-based resin staple fibers:polypropylene-based resin staple fibers), more preferably 95:5 to 10:90, and even more preferably 80:20 to 20:80, from the viewpoints of further improving the sound absorption coefficient and improving hydrophobicity and drainage properties.
[0037] The nonwoven fabric molding constituting the filling 2 can be obtained, for example, by mixing 1 to 95% by mass, for example 60% by mass, of the polypropylene-based resin staple fibers with 99 to 5% by mass, for example 40% by mass, of polyester (polyethylene terephthalate) binder staple fibers, forming a web using a fiber spreader and a carding machine, laminating the obtained web in multiple layers using a cross-layer machine, and treating it with a hot air treatment machine set to a predetermined gap distance to fuse the polyester (polyethylene terephthalate) binder staple fibers and the polypropylene-based resin staple fibers.
[0038] The polyethylene terephthalate-based resin may be a copolymer of a polyhydric alcohol such as ethylene glycol and a dibasic acid such as terephthalic acid. Examples of such polyethylene terephthalate-based resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), polyethylene isophthalate (PEI), polybutylene isophthalate (PBI), polyhexamethylene terephthalate (PHT), polyhexamethylene isophthalate (PHI), and polyhexamethylene naphthalate (PHN).
[0039] The polypropylene-based resin may be a homopolymer of propylene, or a copolymer of propylene with other α-olefins copolymerizable with propylene. Examples of the α-olefin include α-olefins having 2 or more carbon atoms, preferably 2 to 8 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene. When the polypropylene-based resin is a copolymer of propylene and an α-olefin, it may be a copolymer of one or more α-olefins selected from the α-olefins. The polypropylene-based resin may have an MFR (melt flow rate) in the range of, for example, 1 to 500 g / min.
[0040] The polyester (polyethylene terephthalate) binder staple fiber may be, for example, one having a polyethylene terephthalate core and a binder component in the sheath. Examples of the binder component include copolymer polyesters made of terephthalic acid or its ester-forming derivatives, isophthalic acid or its ester-forming derivatives, lower alcohols, polyalkylene glycols or their monoethers.
[0041] The polyester-based resin staple fibers and the polypropylene-based resin staple fibers in the nonwoven fabric may have the form of composite fibers, hollow fibers, modified fibers, crimped fibers, split fibers, etc., within the scope of not impairing the effects of the present invention. In addition, they may contain heat stabilizers, ultraviolet absorbers, weather stabilizers, flame retardants, water repellents, oil agents, antistatic agents, colorants, inorganic substances, etc.
[0042] The skin material 3 is made of a nonwoven fabric containing fibers made of polypropylene resin. 2 It is preferable that the water pressure resistance is in the range of 200 to 1000 mmH 2 It is more preferable that the water pressure resistance is in the range of 250 to 500 mmH 2 It is more preferable that the water pressure resistance is in the range of 280 to 400 mmH 2 It is most preferable that the skin material 3 has a water pressure resistance in the range of O. The water pressure resistance of the skin material 3 can be increased by, for example, decreasing the average fiber diameter of the fibers constituting the skin material 3, increasing the density, and increasing the basis weight.
[0043] The basis weight of the skin material 3 is set to 50 to 200 g / m from the viewpoints of improving the water pressure resistance to prevent contact between the padding 2 and water, maintaining strength such as shot blast resistance, preventing a situation in which sound waves are difficult to transmit to the padding 2 side due to an excessively high basis weight, and preventing a situation in which workability such as ultrasonic sealing is reduced due to an excessively high basis weight. 2 The range is preferably 70 to 150 g / m 2 It is more preferable that the range is .
[0044] The air permeability of the skin material 3 is set to 5 to 200 cm from the viewpoint of improving the water pressure resistance and preventing the contact between the padding and water, and from the viewpoint of transmitting sound waves to the padding side to maintain a good sound absorption rate. 3 / cm 2 / sec, and preferably in the range of 7 to 150 cm 3 / cm 2 / sec, more preferably in the range of 10-50 cm 3 / cm 2 / sec range is most preferred.
[0045] The thickness of the skin material 3 is preferably in the range of 0.1 to 1.5 mm, and more preferably in the range of 0.3 to 1.0 mm, from the viewpoints of further improving the water pressure resistance and further preventing contact between the filling 2 and water, maintaining strength such as shot blast resistance, preventing the filling from being too thick and thus preventing sound waves from being difficult to transmit to the filling side, and preventing the filling from being too thick and thus reducing the ease of operation such as ultrasonic sealing.
[0046] The average fiber diameter of the fibers located near the surface of the skin material 3 (hereinafter sometimes referred to as the surface fiber diameter) is preferably in the range of 20 to 100 μm, and more preferably in the range of 30 to 50 μm, from the viewpoints of further improving the shot blast resistance and controlling the air permeability within an appropriate range.
[0047] The polypropylene resin used in the nonwoven fabric constituting the skin material 3 may be a homopolymer of propylene, similar to the polypropylene resin used in the filling 2, or may be a copolymer of propylene and other α-olefins copolymerizable with propylene. As the α-olefin, one or more of the same α-olefins as in the polypropylene resin used in the filling 2 can be used.
[0048] The fibers constituting the skin material 3 may contain heat stabilizers, ultraviolet absorbers, weather stabilizers, flame retardants, water repellents, oil agents, antistatic agents, colorants, inorganic substances, etc., within the scope of the invention.
[0049] The polypropylene resin used in the nonwoven fabric constituting the skin material 3 may have an MFR (melt flow rate) in the range of, for example, 10 to 1000 g / min, and more preferably 30 to 700 g / min.
[0050] In particular, when the skin material 3 is made of a spunbond nonwoven fabric or a meltblown nonwoven fabric, the MFR of the polypropylene resin used in the spunbond nonwoven fabric is preferably 15 to 80 g / min, and the MFR of the polypropylene resin used in the meltblown nonwoven fabric is preferably 100 to 700 g / min.
[0051] In the sound-absorbing material 1 of this embodiment, the skin material 3 has a water pressure resistance within the above-mentioned range, and the inside is sealed by the sealing part 4, so that the filling 2 does not come into contact with water, and the sound absorption rate is unlikely to decrease even in a humid environment.
[0052] The skin material 3 may be a single layer nonwoven fabric or a laminated nonwoven fabric in which multiple nonwoven fabrics are laminated. The nonwoven fabric constituting the skin material 3 is not particularly limited as long as it exhibits the effects of the present invention, and may be at least one type selected from the group consisting of spunbond nonwoven fabrics and meltblown nonwoven fabrics.
[0053] From the viewpoint of further improving the strength such as shot blast resistance as a sound absorbing material, the skin material 3 preferably includes at least one layer of spunbond nonwoven fabric. Also, from the viewpoint of controlling the water pressure resistance and air permeability within a preferred range, it preferably includes at least one layer of meltblown nonwoven fabric. Spunbond nonwoven fabric and meltblown nonwoven fabric can be distinguished by the average fiber diameter. In the embodiment of the present specification, the average fiber diameter of spunbond nonwoven fabric may be in the range of 15 to 100 μm, and the average fiber diameter of meltblown nonwoven fabric may be in the range of 0.5 to 5 μm.
[0054] The present inventors have found that, while the smaller (thinner) the average fiber diameter of the fibers contained in a nonwoven fabric, the denser it is and the better its water pressure resistance and sound absorption coefficient, from the viewpoint of abrasion resistance (shot blast resistance) against the impact of solids such as hail, sleet, or pebbles, it is desirable for the average fiber diameter to be large (thick), which is a trade-off relationship. In addition, the average fiber diameter of the fibers contained in a spunbonded nonwoven fabric is generally larger than the average fiber diameter of the fibers contained in a meltblown nonwoven fabric, which is smaller than the average fiber diameter of the fibers contained in a spunbonded nonwoven fabric.
[0055] Therefore, the skin material 3 may have at least a three-layer structure (hereinafter, the three-layer structure may be referred to as an SMS structure) of a first spunbond nonwoven fabric containing fibers made of polypropylene resin having an average fiber diameter in the range of 25 to 50 μm, a meltblown nonwoven fabric containing fibers made of polypropylene resin having an average fiber diameter in the range of 0.5 to 5 μm located on the first spunbond nonwoven fabric, and a second spunbond nonwoven fabric containing fibers made of polypropylene resin having an average fiber diameter in the range of 25 to 50 μm located on the meltblown nonwoven fabric, or may be composed only of a spunbond nonwoven fabric layer containing a third spunbond nonwoven fabric containing fibers made of polypropylene resin having an average fiber diameter in the range of 15 to 100 μm. Here, "composed only of a spunbond nonwoven fabric layer" means that it does not include nonwoven fabrics manufactured by other manufacturing methods such as meltblown nonwoven fabric, and does not exclude the inclusion of multiple spunbond nonwoven fabrics.
[0056] When the skin material 3 has a structure of at least three layers, the average fiber diameter of the meltblown nonwoven fabric forming the inner layer is small and dense, thereby ensuring the water pressure resistance within the above range. On the other hand, since the average fiber diameter of the fibers contained in the meltblown nonwoven fabric is small, the meltblown nonwoven fabric may be prone to fluffing and may have poor shot blast resistance, so by using the first or second spunbond nonwoven fabric as the outer layer, the meltblown nonwoven fabric can be protected and tends to have better shot blast resistance.
[0057] Furthermore, the skin material 3 may have at least a four-layer structure (hereinafter, the four-layer structure may be referred to as an SSMS structure or an SMSS structure) including a fourth spunbond nonwoven fabric containing fibers having an average fiber diameter in the range of 25 to 100 μm located on the second spunbond nonwoven fabric, and the fourth spunbond nonwoven fabric can provide better shot blast resistance. The fourth spunbond nonwoven fabric may have an average fiber diameter in the range of 30 to 50 μm and a basis weight of 70 to 150 g / m, for example. 2 It is preferable that the range is .
[0058] When the skin material 3 is made of only a spunbond nonwoven fabric layer, the average fiber diameter is in the range of 10 to 100 μm, for example, in the range of 20 to 40 μm, and the basis weight is 70 to 200 g / m 2 By including the third spunbond nonwoven fabric in the range, it is possible to achieve both the water pressure resistance in the range and the shot blast resistance. The spunbond nonwoven fabric layer may be composed of a single layer of the third spunbond nonwoven fabric, or another spunbond nonwoven fabric may be laminated on the third spunbond nonwoven fabric.
[0059] In addition, when the skin material 3 is composed of only a spunbonded nonwoven fabric layer, the average fiber diameter of the fibers located near the surface (hereinafter, sometimes referred to as the surface fiber diameter) tends to be in the range of 25 to 100 μm, for example, in the range of more than 30 μm and not more than 100 μm, so that excellent shot blast resistance can be obtained. In the spunbonded nonwoven fabric layer, for example, by setting the temperature of the embossing roll in the range of 140 to 170 ° C. and the temperature of the mirror roll in the range of 140 to 170 ° C. and performing embossing (thermocompression processing) to set the welding area ratio to 15% or more, the surface fiber diameter can be set to the above range, and the fusion between fibers in the non-embossed part is promoted, so that the apparent fiber diameter becomes thick. For the same reason, the welding area ratio during embossing can be set to 20% or more, or a large embossing pattern of 0.7 mm square or more can be used even with the same welding area ratio, thereby improving the shot blast resistance.
[0060] The spunbonded nonwoven fabric can be produced by using a known spunbonded nonwoven fabric molding machine. More specifically, the spunbonded nonwoven fabric can be produced, for example, by melting a raw material polypropylene resin using an extruder, discharging the molten composition from a plurality of spinnerets, cooling and stretching the fibrous resin as necessary, depositing it on a collecting surface, and subjecting it to a heating and pressurizing treatment using an embossing roll.
[0061] The meltblown nonwoven fabric can be produced by using a known meltblown nonwoven fabric molding machine. More specifically, the meltblown nonwoven fabric can be produced by, for example, melting a raw material polypropylene resin, discharging it from a spinning nozzle, and pulling it with high-temperature, high-pressure gas to produce fine polypropylene ultrafine fibers, which are then collected and accumulated on a collector such as a perforated belt or perforated drum.
[0062] Generally, when high-pressure water is applied to the skin material 3 or when the sound-absorbing material 1 is exposed to an environment where moisture is present for a long period of time, the moisture may reach the padding portion 2 and adversely affect the sound-absorbing performance. Therefore, the inventors have discovered that by providing an opening in part of the skin material 3, the moisture absorbed in the padding portion 2 can be easily discharged to the outside of the sound-absorbing material 1.
[0063] The openings may be provided anywhere in the skin material 3, but from the viewpoint of striking a balance between making it difficult for moisture to penetrate into the padding portion 2 and efficiently discharging moisture that has penetrated into the padding 2 to the outside of the sound-absorbing material, in the first and second embodiments, as shown in Figures 1 and 2, openings 3a are provided in the surface of the skin material 3 that is located at the bottom when the sound-absorbing material 1 is installed (including the corners if it is rectangular) (in these embodiments, the four corners).
[0064] Furthermore, when the sound-absorbing material 1 is a rectangular parallelepiped, it is preferable to provide the openings 3a at the corners from the viewpoints of maintaining the shape of the sound-absorbing material 1, facilitating installation of openings, and drainage. Note that the rectangular parallelepiped does not have to be a perfect rectangle, and may be slightly deformed from a rectangle.
[0065] From the viewpoint of a balance between preventing moisture from penetrating the padding portion 2 and efficiently discharging moisture that has penetrated the padding portion 2 to the outside of the sound-absorbing material 1, the opening rate (the ratio of the area of the openings to the area of the entire skin material (excluding the sealing portion 4)) is preferably 10% or less, more preferably 5% or less, even more preferably 1 to 0.005%, and particularly preferably 0.8 to 0.01%.
[0066] Of the above, the ratio of the area of the opening 3a provided on the surface located at the bottom when the sound-absorbing material 1 is installed to the surface area of the skin material located at the bottom (not including the sealing portion 4) is preferably 10% or less, more preferably 7% or less, and even more preferably 5 to 0.05%.
[0067] The shape of the opening 3a is not particularly limited, and may be circular or polygonal. However, from the viewpoint of workability in providing the opening and efficient drainage, it is more preferable that the opening is a square or a linear slit. Note that the square does not necessarily have to be rectangular, and the opening may be a shape that is slightly deformed from a rectangle.
[0068] 1 and 2, an opening is formed in each of the four corners of the bottom surface of the skin material 3, for a total of four openings, but the number of openings is not particularly limited. It may be one, two or more, three or more, or four or more.
[0069] Furthermore, as shown in the first and second embodiments in FIG. 1 and FIG. 2, it is not necessary to form openings in each of the four corners of the bottom surface of the skin material 3, and openings may be formed in any one to three corners selected from the three corners.
[0070] Furthermore, instead of forming openings at the four corners of the bottom surface of the skin 3 as shown in the first and second embodiments in Fig. 1 and Fig. 2, openings 3a may be formed on the entire bottom surface of the skin 3 as shown in Fig. 3. Also, as shown in Fig. 4, openings 3a may be formed on the top and side surfaces in addition to the bottom surface of the skin 3. Furthermore, as shown in Fig. 5, openings 3a may be formed in the approximate center of the top and bottom surfaces in addition to the four corners of the bottom surface of the skin 3. Also, as shown in Fig. 6, openings 3a may be formed inwardly on the top and bottom surfaces in addition to the four corners of the bottom surface of the skin 3.
[0071] The sealed portion 4 can be formed by thermocompression or ultrasonic sealing. The sealed portion 4 may be formed continuously or discontinuously around the peripheral portion of the skin material 3, 3 so as to surround the padding 2. When the sealed portion 4 is formed discontinuously, it is preferable that a plurality of parallel sealed portions 4 are formed so that a discontinuous portion of one sealed portion 4 is complemented by a continuous portion of another sealed portion 4.
[0072] The water pressure resistance of the seal portion 4 is not particularly limited as long as the effects of the present invention are achieved. From the viewpoint of further suppressing the intrusion of water, however, a water pressure resistance of 100 mmH 2 O or higher is preferable, 150mmH 2 More than 0 is preferable, 200mmH 2 More preferably 0 or more, 250mmH 2 O or more is particularly preferable, 300mmH 2 The upper limit of the water pressure resistance of the seal portion 4 is not particularly limited, but is, for example, 2000 mmH 2 O or less, 1000mmH 2 O or less and 500mmH 2 It can be set to O or less.
[0073] The sealing conditions are not particularly limited, but in the case of ultrasonic sealing, they can be arbitrarily adjusted by the pressure during sealing, output voltage, sealing time, sealing pattern, etc. If the seal is too strong, the water pressure resistance tends to decrease, so by appropriately adjusting the above factors, it is possible to maintain a good water pressure resistance.
[0074] The width of the sealed portion 4 is not particularly limited as long as the effects of the present invention can be achieved, but from the viewpoint of further improving the water pressure resistance of the sealed portion and suppressing breakage, it is preferable that the width is in the range of 0.1 to 5.0 mm. The width of the sealed portion 4 can be, for example, 0.3 mm.
[0075] Next, the sound-absorbing panel of this embodiment will be described with reference to FIG.
[0076] 7, the sound-absorbing panel 11 of this embodiment includes a sound-absorbing material 1 and a frame 14 that houses the sound-absorbing material 1. The frame 14 is a box-shaped body that includes a rectangular shielding plate 12 that forms the bottom and side walls 13 that rise from the four sides of the shielding plate 12 and has an open end at the top, and includes a protection panel 15 that is placed at the open end of the frame 14 when the sound-absorbing material 1 is housed in the frame 14, and a support part 16 that is placed on the back surface of the frame 14 and supports the sound-absorbing panel 11 when the sound-absorbing panel 11 is attached to a building or the like.
[0077] The frame 14 may be formed by integrally forming the shielding plate 12, the side wall 13, and the support portion 16, or may be formed by connecting separate members. The material of the frame 14 is not particularly limited as long as it is a material that is durable against weather, moisture, etc., and may be made of metal or resin. As the metal, a lightweight metal such as aluminum or stainless steel is preferably used.
[0078] It is preferable that the protective panel 15 protects the sound absorbing material 1 from solid objects such as hail, sleet, or pebbles while facilitating the penetration of sound waves. For this reason, in this embodiment, a punched plate having a large number of through holes 15a arranged on the surface is preferably used as the protective panel 15, but the protective panel is not limited to a punched plate as long as it protects the sound absorbing material 1 while facilitating the penetration of sound waves. The total area of the through holes 15a relative to the total area of the surface of the protective panel 15 is not particularly limited, but is, for example, in the range of 20% to 80%.
[0079] The material of the protective panel 15 is not particularly limited as long as it can protect the sound-absorbing material 1 and is durable against the intrusion of sound waves, weather, moisture, etc., and can be made of metal or resin. As the metal, a lightweight metal such as aluminum or stainless steel is preferably used.
[0080] In this embodiment, an opening 13a is formed in the frame 14 so that moisture absorbed in the padding portion 2 of the sound-absorbing material 1 can be discharged to the outside of the sound-absorbing material 1. The opening 13a may be provided anywhere in the frame 14, but from the viewpoint of a balance between making it difficult for moisture to enter the padding portion 2 and efficiently discharging moisture that has entered the padding portion 2 to the outside of the sound-absorbing material 1, it is preferable to provide the opening 13a in the side wall 13 of the frame 14 and / or the shielding plate 12.
[0081] 7, a total of eight openings 13a are formed in each of the four corners of both side walls 13, but this is not limited to this. From the viewpoint of a balance between making it difficult for moisture to enter the sound-absorbing material 1 and improving drainage, the number of openings 13a is preferably 4 to 6, and more preferably 2 to 3 openings 13a are formed in each of both side walls 13.
[0082] Furthermore, from the viewpoint of making it difficult for water to enter the sound-absorbing material 1 from the outside, it is preferable that the openings 13a of the frame 14 are not present on the surfaces of the frame 14, i.e., on the top and bottom surfaces. Therefore, particularly when the sound-absorbing panel 11 is a rectangular parallelepiped as in this embodiment, it is more preferable that the openings 13a are present on the left and right side surfaces.
[0083] The shape of the opening 13a is not particularly limited, and may be circular or polygonal. However, from the viewpoint of workability in providing the opening 13a and efficient drainage, it is more preferable that the opening is square or semicircular. Note that the square does not necessarily have to be rectangular, and the opening may be a shape that is slightly deformed from a rectangle.
[0084] 3, a total of eight openings 13a are formed in each of the four corners of the side wall 13, but the number of openings 13a is not particularly limited. It may be one, two or more, three or more, or four or more.
[0085] Also, instead of forming the openings 13a at the corners of both side walls 13 as shown in the embodiment of Fig. 7, the openings 13a may be formed at both ends and the center of the shielding plate 12 as shown in Fig. 8. Also, as shown in Fig. 9, the openings 13a may be formed in the entirety of both side walls 13 in addition to the shielding plate 12. Furthermore, as shown in Fig. 10, in addition to forming the openings 13a at the corners of both side walls 13, the openings 13a may be formed at the center of both side walls 13. Also, as shown in Fig. 11, the openings 13a may be formed at the upper corners of both side walls 13 and both ends and the center of the shielding plate 12.
[0086] Next, a method for manufacturing the sound-absorbing material 1 of the present embodiment shown in FIG. 1 or FIG. 2 will be described.
[0087] The sound-absorbing material 1 can be produced, for example, by a production method including a fusion step of wrapping a filling 2 containing fibers made of at least polyester-based resin with a skin material 3 which is a nonwoven fabric containing fibers made of polypropylene-based resin, and fusing the ends of the skin material 3.
[0088] The method for fusing the ends is not limited as long as the effects of the present invention are achieved, but examples include a method in which a heat source such as an iron is applied to heat the resin to melt it and then pressure-bond it, an ultrasonic sealing method in which ultrasonic waves are applied to melt the resin while pressure-bonding it, a laser welding method, a vibration welding method, a high-frequency welding method, and a hot plate welding method. Among these, it is preferable to fuse the ends using the ultrasonic sealing method.
[0089] The fusion temperature is not particularly limited as long as it is a temperature at which the resin of the skin material 3 can be fused, but from the viewpoint of further improving the water pressure resistance and preventing peeling of the fused portion, it is preferably in the range of 130 to 160°C, and more preferably in the range of 140 to 155°C.
[0090] When the fusion step is performed by an ultrasonic sealing method, the output of the ultrasonic sealing device is not particularly limited as long as it can fuse the resin of the skin material 3. It can be appropriately adjusted from the viewpoint of further improving the water pressure resistance and suppressing peeling of the fused portion (sealed portion 4). The pressure in the pressure bonding is not particularly limited as long as it can fuse the resin of the skin material 3, but it is preferably in the range of 0.1 to 5 MPa from the viewpoint of further improving the water pressure resistance and suppressing peeling of the fused portion. The speed of forming the fused portion is preferably 0.5 to 30 m / min from the viewpoint of improving the work efficiency while suppressing peeling of the fused portion.
[0091] The opening 3a may be made before or after the above-mentioned end portions are fused, but from the viewpoint of providing an opening of a more accurate size, it is preferable to make the opening after all of the fusion steps are completed. There are no particular limitations on the opening method, but if the sound-absorbing material is a rectangular parallelepiped and openings are to be made at the four corners, it is preferable to cut only the skin material 3 along the sides that make up the four corners with scissors, a cutter, or the like to provide the openings (for example, slit-shaped openings). At this time, care must be taken to cut only the skin and not to affect the filling. From this viewpoint, it is preferable to make the cut with scissors or a tool equivalent thereto.
[0092] Next, examples of the present invention and comparative examples will be described. EXAMPLES
[0093] In the following Examples and Comparative Examples, the physical properties and performance of the sound absorbing materials were measured or evaluated as follows.
[0094] [Weight (g / m 2 )〕 Five 10 cm square samples were taken from the sound absorbing material, not including the side surfaces. The weight of each sample was measured, and the total weight was divided by the total area to obtain the basis weight (g / m 2 ) was calculated.
[0095] [Thickness (mm)] For the five samples used in calculating the weight per unit area, the thickness of the center of each of the four sides of each sample was measured with a steel ruler, and the average value was taken as the thickness (mm).
[0096] [Water pressure resistance of surface material] The skin material used for the sound-absorbing material (if there is no skin material, five 15 cm square samples were taken from the surface area sliced to a thickness of 5 mm or less) and the water resistance was measured using JIS L 1096 (2010) Method A (low water pressure method), and the average value was taken as the water resistance of the skin material.
[0097] [Water pressure resistance of seal part] When the skin was taken from the sound-absorbing material, the seal was taken so as to be included in the centre of the 15 cm square sample, and the water pressure resistance of the seal was calculated to be the same as that of the skin.
[0098] [Breathability (cm 3 / cm 2 / sec)〕 From the skin material used for the sound absorbing material, five 15 cm square samples were taken with the same water pressure resistance as the skin material. The air permeability was measured using a Frazier air permeability measuring device in accordance with JIS L 1096 (2010), and the average value was calculated as the air permeability (cm 3 / cm 2 / sec).
[0099] [Shot blast resistance] A 25cm square sound-absorbing material was used as a sample, and a shot blast test was carried out under conditions of S30 (steel ball), a spray nozzle diameter of 5mm, a distance of 150mm from the nozzle tip to the top surface of the sample, and a spray air pressure of 0.1MPa. After 4 seconds of spraying, if the skin material was torn, it was marked as ×, if not torn, it was marked as ◯, and if there was no tear but damage was visible over an area of more than half the thickness of the skin material, it was marked as △.
[0100] [Average fiber diameter] For spunbond nonwoven fabric, ten test pieces measuring 10 mm x 10 mm were taken, and using a microscope (Nikon Corporation, product name: ECLIPSE E400) at a magnification of 50x, the diameters of 30 random points on each test piece were read in μm units to the first decimal place, and the average value was taken as the average fiber diameter. For the filling, 10 test pieces were sliced to 10 mm x 10 mm x 5 mm and 10 test pieces were taken. Using a microscope (Nikon Corporation, product name: ECLIPSE E400) at a magnification of 50x, the diameters of 30 random points on each test piece were read in μm units to the first decimal place and the average value was taken as the average fiber diameter. For meltblown nonwoven fabrics, the fiber diameters (μm) of 30 constituent fibers of the sampled specimen were measured at a magnification of 500x or 1000x using a scanning electron microscope (manufactured by Hitachi, Ltd., model name: SU3500), and the average value was taken as the average fiber diameter.
[0101] [Surface fiber diameter] The fiber diameters (μm) of 30 constituent fibers of a sample piece taken from a spunbond nonwoven fabric were measured at 50x or 100x magnification using a scanning electron microscope (manufactured by Hitachi, Ltd., model name: SU3500), and the average value was taken as the surface fiber diameter. Areas where the fibers were fused together and the interface was unclear, making it impossible to identify the diameter of each fiber, were excluded. Note that when the cross section of the skin material was observed with a scanning electron microscope, if no fusion was observed in the non-embossed area, the average fiber diameter was taken as the surface fiber diameter.
[0102] [Fusion between fibers in non-embossed portion] The surface of the spunbond nonwoven fabric on the outermost surface of the skin material was observed using a scanning electron microscope (manufactured by Hitachi, Ltd., model name: SU3500), and if the fusion shape was different from the embossed shape, it was determined that there was fusion between the fibers in the non-embossed part. Also, if the fusion shape was the same as the embossed shape, it was determined that there was no fusion between the fibers in the non-embossed part.
[0103] [Sound absorption coefficient] The normal incidence sound absorption coefficient was measured using an acoustic tube with an inner diameter of 100 mm in accordance with JIS A 1405-2 (transfer function method). The samples were prepared by cutting out the skin and the padding from the sound absorbing material with a 100mm diameter punching blade to obtain a circle with a diameter of 100mm, and then stacking the skin and padding in the original order to measure the normal incidence sound absorption coefficient. Note that the normal incidence sound absorption coefficient was measured after tap water was dripped onto the above sample so that the water retention rate after water absorption was the same as that in the drainage test shown below.
[0104] [Drainage test] The sample was a sound-absorbing material measuring 210 mm (length) x 297 mm (width) x 50 mm (thickness). Before submerging, the sample was placed on a 25 cm square metal net (a 25 mesh wire net surrounded by a 5 mm frame) and its weight was measured, which was taken as the dry weight (excluding the weight of the metal net). This was then submerged horizontally in a stainless steel bat (width 30 cm x length 50 cm x depth 10 cm) filled with tap water. At this time, pressure was applied little by little so as not to damage the seals of the sound-absorbing material, and the air contained inside was completely expelled and the inside of the sound-absorbing material was completely filled with water. Five minutes after submerging, the sample was pulled out of the water together with the sound-absorbing material on top while holding the metal net, and the weight was measured without delay. This was taken as the initial weight.
[0105] Next, the sound-absorbing material sample was submerged in water for 5 minutes in the same manner as above, then pulled out of the water so that the long side of the sound-absorbing material was vertical, and left to stand in that vertical position for 1 minute, after which the weight of the sample was measured and recorded as the weight after 1 minute. Five samples were prepared and the above drainage test was carried out on each, and the average of the results was recorded as the measured value. The water retention rate and drainage rate were calculated using the following formula:
[0106] [Water retention rate and drainage rate] Water retention rate (%) = (weight after 1 minute - dry weight) ÷ (initial weight - dry weight) x 100 Drainage rate (%)=100-water retention rate
[0107] [Sound absorption performance maintenance rate] The sound absorption performance after the drainage test was calculated as the sound absorption rate maintenance rate using the following formula. Sound absorption performance maintenance rate (%) = (sound absorption coefficient of sound absorbing material after drainage test) ÷ (sound absorption coefficient of sound absorbing material when dry) × 100
[0108] [Aperture ratio] When providing openings, only the surface layer was cut with scissors along the four corners of the sound-absorbing material sample measuring 210 mm (length) x 297 mm (width) x 50 mm (thickness). In a dry state, the area of the openings was measured using a steel ruler to determine the opening ratio as described below. Opening rate (%) = (area of opening) ÷ (total surface area of epidermis) × 100
[0109] Example 1 In this example, the sound absorbing material was obtained as follows.
[0110] <Preparation of skin material> A propylene homopolymer with a melt flow rate (MFR) of 60 g / 10 min was used to perform melt spinning at 230°C by a conventional spunbond method using a spunbond nonwoven fabric molding machine with a spinneret with a diameter of 0.6 mm. The fibers obtained by spinning were deposited on a collection surface, and the average fiber diameter was 16 μm and the basis weight was 10 g / m. 2 Thus, a first spunbond nonwoven fabric A-1 was obtained.
[0111] Next, a propylene homopolymer having an MFR of 400 g / 10 min was melted at 280° C. using an extruder, and the resulting molten material was extruded from a spinneret while being blown with heated air at 280° C. by a conventional melt-blowing method to deposit fibers having an average fiber diameter of 3 μm on the first spunbond nonwoven fabric A-1, resulting in a basis weight of 5 g / m 2 Thus, meltblown nonwoven fabric B-1 was formed.
[0112] Next, fibers were deposited on the meltblown nonwoven fabric B-1 in the same manner as the first spunbond nonwoven fabric A-1, and the average fiber diameter was 16 μm and the basis weight was 10 g / m 2 A second spunbond nonwoven fabric A-2 was formed.
[0113] Next, the laminate of the first spunbond nonwoven fabric A-1, the meltblown nonwoven fabric B-1, and the second spunbond nonwoven fabric A-2 was integrated by a hot embossing roll with an imprint area ratio of 18% set at a temperature of 145°C for the embossing roll and 150°C for the mirror roll, to obtain a three-layer structure (hereinafter referred to as SMS structure) nonwoven fabric in which the first spunbond nonwoven fabric and the second spunbond nonwoven fabric were laminated on both the front and back sides of the meltblown nonwoven fabric. The basis weight of the SMS structure nonwoven fabric was 25 g / m 2 It was.
[0114] Next, a propylene homopolymer having an MFR of 60 g / 10 min was used to perform melt spinning by a conventional spunbonding method at 230° C. in a spunbonding nonwoven fabric molding machine having a spinneret with a diameter of 1.3 mm, and the fibers obtained by spinning were deposited on the SMS structure nonwoven fabric to obtain a fiber having an average fiber diameter of 35 μm and a basis weight of 100 g / m. 2 A fourth spunbond nonwoven fabric C was formed. Next, the laminate of the SMS nonwoven fabric and the fourth spunbond nonwoven fabric C was integrated with a hot embossing roll (embossed pattern 0.9 mm square) with an imprint area ratio of 18% and an embossing roll temperature of 155°C and a mirror roll temperature of 160°C, to obtain a skin material made of a four-layered nonwoven fabric (hereinafter referred to as SSMS structure) in which the fourth spunbond nonwoven fabric C was laminated on the SMS nonwoven fabric. The structure of the skin material is sometimes referred to as PP-SSMS.
[0115] <Preparation of filling> 10 parts by mass of polypropylene staple fibers (manufactured by Ube Exsymo Co., Ltd., product name: UC Fiber, average fiber diameter 21 μm, average fiber length 51 mm), 30 parts by mass of polyethylene terephthalate (polyester) binder staple fibers (manufactured by Unitika Ltd., product name: Melty 4080, average fiber diameter 14 μm, average fiber length 51 mm), 40 parts by mass of polyethylene terephthalate-based (average fiber diameter 14 μm, average fiber length 51 mm) general-purpose staple fibers, and 20 parts by mass of polyethylene terephthalate-based (average fiber diameter 25 μm, average fiber length 51 mm) general-purpose staple fibers were mixed and formed into a web using a fiber spreader and a carding machine. The web was then multi-layered using a cross-layer machine and treated with a hot air treatment machine set to a gap distance of approximately 50 mm, to obtain a filling consisting of a sheet-like nonwoven fabric molding containing polypropylene staple fibers and polyethylene terephthalate staple fibers and having a thickness of approximately 50 mm.
[0116] <Preparation of sound absorbing material> Next, the filling was cut to 210 mm (length) x 297 mm (width) x 49 mm (thickness) (size for drainage test). Next, the skin material was placed on both sides of the cut filling so that the fourth spunbond nonwoven fabric C was on the outermost surface, and the peripheral portion of the skin material around the filling was fused with an ultrasonic sealer (manufactured by Seidensha Electronics Co., Ltd., product name: JII430SA) under conditions of output 2.0 V, pressure 0.3 MPa, and speed 5 m / min to form a continuous seal portion with a width of 0.3 mm, thereby obtaining a sound absorbing material in which the filling is enclosed in the skin material. The excess portion on the outer periphery of the seal portion was cut and removed. In the four corners of the obtained A4-sized rectangular parallelepiped, only the skin portion was cut according to the example table to provide slit openings.
[0117] Next, the physical properties and performance of the sound-absorbing material obtained in this example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0118] Example 2 <Preparation of skin material> In this example, the skin material was prepared in exactly the same manner as in Example 1.
[0119] <Preparation of filling> The filling was prepared in exactly the same manner as in Example 1, except that 5 parts by mass of polypropylene-based short fibers (manufactured by Ube Exsymo Co., Ltd., product name: UC Fiber, average fiber diameter 20 μm, average fiber length 51 mm), 35 parts by mass of polyethylene terephthalate (polyester)-based binder short fibers (manufactured by Unitika Ltd., product name: Melty 4080, average fiber diameter 14 μm, average fiber length 51 mm), 30 parts by mass of polyethylene terephthalate-based (average fiber diameter 25 μm, average fiber length 51 mm) general-purpose short fibers, and 30 parts by mass of polyethylene terephthalate-based (average fiber diameter 45 μm, average fiber length 51 mm) general-purpose short fibers were mixed.
[0120] <Preparation of sound absorbing material> The sound absorbing material was prepared in exactly the same manner as in Example 1.
[0121] Next, the physical properties and performance of the sound-absorbing material obtained in this example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0122] Example 3 <Preparation of skin material> In this example, the skin material was prepared in exactly the same manner as in Example 1.
[0123] <Preparation of filling> The filling was prepared in exactly the same manner as in Example 1, except that 5 parts by mass of polypropylene-based short fibers (manufactured by Ube Exsymo Co., Ltd., product name: UC Fiber, average fiber diameter 20 μm, average fiber length 51 mm), 35 parts by mass of polyethylene terephthalate (polyester)-based binder short fibers (manufactured by Unitika Ltd., product name: Melty 4080, average fiber diameter 14 μm, average fiber length 51 mm), and 60 parts by mass of polyethylene terephthalate-based (average fiber diameter 54 μm, average fiber length 51 mm) general-purpose short fibers were mixed.
[0124] <Preparation of sound absorbing material> The sound absorbing material was prepared in exactly the same manner as in Example 1.
[0125] Next, the physical properties and performance of the sound-absorbing material obtained in this example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0126] Example 4 <Preparation of skin material> In this example, the first spunbond nonwoven fabric A-1 and the second spunbond nonwoven fabric A-2 each have a basis weight of 18.5 g / m 2 The meltblown nonwoven fabric B-1 is made of a propylene homopolymer with an MFR of 1500 g / 10 min and has a basis weight of 8 g / m 2 A skin material was prepared in exactly the same manner as in Example 1, except for the above.
[0127] <Preparation of filling> In this example, the filling was prepared in exactly the same manner as in Example 1.
[0128] <Preparation of sound absorbing material> The sound absorbing material was prepared in exactly the same manner as in Example 1.
[0129] Next, the physical properties and performance of the sound-absorbing material obtained in this example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0130] Comparative Example 1 <Preparation of skin material> In this comparative example, the skin material was prepared in exactly the same manner as in Example 1.
[0131] <Adjusting the filling> In this comparative example, the filling was prepared in exactly the same manner as in Example 1.
[0132] <Preparation of sound absorbing material> This comparative example was the same as Example 1, except that the sound absorbing material was adjusted without providing slit openings at the four corners of the obtained A4 size rectangular parallelepiped.
[0133] Next, the physical properties and performance of the sound-absorbing material obtained in this comparative example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0134] Comparative Example 2 <Preparation of skin material> In this comparative example, the skin material was prepared in exactly the same manner as in Example 1.
[0135] <Adjusting the filling> In this comparative example, the filling was prepared in exactly the same manner as in Example 2.
[0136] <Preparation of sound absorbing material> This comparative example was the same as Example 2, except that the sound absorbing material was adjusted without providing slit openings at the four corners of the obtained A4 size rectangular parallelepiped.
[0137] Next, the physical properties and performance of the sound-absorbing material obtained in this comparative example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0138] Comparative Example 3 <Preparation of skin material> In this comparative example, the skin material was prepared in exactly the same manner as in Example 1.
[0139] <Adjusting the filling> In this comparative example, the filling was prepared in exactly the same manner as in Example 3.
[0140] <Preparation of sound absorbing material> This comparative example was the same as Example 3, except that the sound absorbing material was adjusted without providing slit openings at the four corners of the obtained A4 size rectangular parallelepiped.
[0141] Next, the physical properties and performance of the sound-absorbing material obtained in this comparative example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0142] Comparative Example 4 <Preparation of skin material> In this comparative example, the skin material was prepared in exactly the same manner as in Example 4.
[0143] <Adjusting the filling> In this comparative example, the filling was prepared in exactly the same manner as in Example 4.
[0144] <Preparation of sound absorbing material> This comparative example was the same as Example 4, except that the sound absorbing material was adjusted without providing slit openings at the four corners of the obtained A4 size rectangular parallelepiped.
[0145] Next, the physical properties and performance of the sound-absorbing material obtained in this comparative example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0146] Comparative Example 5 <Preparation of skin material> The skin material was a polyester (polyethylene terephthalate) nonwoven fabric (manufactured by Toyobo Co., Ltd., product name: Heim, fiber diameter 15 μm, basis weight 120 g / m 2 A skin material was prepared in the same manner as in Example 1, except that a single-layer spunbond nonwoven fabric (PET-SB) made of
[0147] <Adjusting the filling> In this comparative example, the filling was prepared in exactly the same manner as in Example 1, except that 60 parts by mass of polyethylene terephthalate (polyester)-based short fibers (manufactured by Teijin Frontier Co., Ltd., product name: Tetoron, average fiber diameter 30 μm, average fiber length 51 mm) were mixed with 40 parts by mass of the same polyethylene terephthalate (polyester)-based binder short fibers as in Example 1.
[0148] <Preparation of sound absorbing material> The skin material was laminated with the filling material using spray adhesive (3M, product number: 77) to obtain a sound-absorbing material with a skin on one side.
[0149] Next, the physical properties and performance of the sound-absorbing material obtained in this comparative example were measured or evaluated as described above. The physical properties, sound absorption coefficient in a dry state, sound absorption coefficient after a drainage test, and sound absorption performance retention rate are shown in Table 1.
[0150] [Table 1]
[0151] From Table 1, it is clear that the sound absorption coefficient of the sound absorbing materials of Examples 1, 2, 3 and 4, in which a filling containing at least polyester-based resin fibers is enclosed in a skin material made of nonwoven fabric containing polypropylene-based resin fibers and in which slit openings are provided at the four corners of the skin material, does not decrease even in a moist environment. In contrast, it is clear that the sound absorption coefficient of the sound absorbing materials of Comparative Examples 1, 2, 3 and 4, which do not have slit openings, or the sound absorbing material of Comparative Example 5, in which the skin material is made of nonwoven fabric containing polyester-based resin fibers, decreases in a moist environment. [Explanation of symbols]
[0152] REFERENCE SIGNS LIST 1...sound-absorbing material, 2...filling, 3...skin material, 3a...opening, 4...sealing portion, 11...sound-absorbing panel, 12...shielding plate, 13...side wall, 13a...opening, 14...frame, 15...protective panel, 16...support portion.
Claims
1. The padding includes a fiber made of at least a polyester resin, and a skin material that contains the padding. The skin material is made of a nonwoven fabric containing fibers made of a polypropylene-based resin, A sound-absorbing material having a water outlet in at least a part of said skin material.
2. 2. The sound absorbing material according to claim 1, wherein the padding contains fibers made of polypropylene resin.
3. In the sound absorbing material according to claim 1 or 2, the skin material has a sound absorption coefficient of 200 to 2000 mmH 2 A sound-absorbing material characterized by having a water pressure resistance in the range of O.
4. 4. The sound absorbing material according to claim 1, wherein the surface material includes a spunbond nonwoven fabric.
5. In the sound-absorbing material according to any one of claims 1 to 4, the skin material includes a first spunbond nonwoven fabric, a meltblown nonwoven fabric located on the first spunbond nonwoven fabric, and a second spunbond nonwoven fabric located on the meltblown nonwoven fabric. Sound-absorbing material characterized in that it includes a second spunbond nonwoven fabric.
6. 6. The sound-absorbing material according to claim 5, wherein the first or second spunbond nonwoven fabric contains fibers having an average fiber diameter in the range of 25 to 50 μm.
7. The sound-absorbing material according to claim 5, wherein the meltblown nonwoven fabric contains fibers having an average fiber diameter in the range of 0.5 to 5 μm.
8. 5. The sound absorbing material according to claim 1, wherein the surface material is made of only a spunbond nonwoven fabric layer including a third spunbond nonwoven fabric.
9. 9. The sound-absorbing material according to claim 8, wherein the third spunbond nonwoven fabric contains fibers having an average fiber diameter in the range of 15 to 100 μm.
10. 10. The sound-absorbing material according to claim 8 or 9, wherein the fibers located on the surface of the spunbond nonwoven fabric layer have an average fiber diameter in the range of more than 30 μm and not more than 100 μm.
11. 11. The sound-absorbing material according to claim 8, wherein the spunbond nonwoven fabric layer has a welded area ratio of 20% or more.
12. The sound absorbing material according to any one of claims 1 to 11, The sound-absorbing material is characterized in that the average fiber diameter of the fibers constituting the padding is 10 to 100 μm.
13. The sound absorbing material according to any one of claims 1 to 12, A sound-absorbing material characterized in that the ratio of the area of the openings to the area of the entire skin excluding the area below the seal portion is 10% or less.
14. A sound-absorbing material according to any one of claims 1 to 13, and a frame that houses the sound-absorbing material, A sound-absorbing panel having openings in at least a portion of the shielding plate and side walls of the frame.
15. A method for producing a sound-absorbing material, comprising the steps of: a fusing step of wrapping a filling material containing at least a fiber made of a polyester-based resin with a skin material which is a nonwoven fabric containing a fiber made of a polypropylene-based resin, and fusing an end portion of the skin material; a drilling step for forming a water outlet on at least a side of the skin material that is located below gravity when the sound absorbing material is disposed; A method for producing a sound-absorbing material, comprising:
16. 16. The method for producing a sound-absorbing material according to claim 15, wherein in the fusing step, the end portion of the skin material is fused by an ultrasonic sealing method.
Citation Information
Patent Citations
Silencer structure
JP2000080925A
Sound absorbing material
JP2000305574A
Sound absorbing material for vehicle
JP2004148906A
Sound absorptive object
JP2004197404A
Laminated sound absorbing material including nanofibers
JP2018169555A