Thermal insulation material and its manufacturing method

A permeable fire-resistant insulation material with plastic balls, sodium silicate, and aluminum hydroxide, coated with carbon black, addresses low thermal insulation and rapid deterioration issues, offering enhanced fire resistance, stability, and ease of application.

JP7576859B2Active Publication Date: 2024-11-01FIRST POINT AS
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022506591
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-07
Filing Date
2020-06-26
Publication Date
2024-11-01
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Existing insulation materials suffer from low thermal insulation properties, high flammability, rapid deterioration, and poor resistance to UV radiation, particularly in permeable fire-resistant systems.

Method used

A permeable fire-resistant insulation material comprising 2-40% plastic balls, 55-95% aqueous sodium silicate solution, 2-6% aluminum hydroxide, and 0.1-0.5% water glass stabilizer, with a surface-coated carbon black, is formulated and applied using a method that includes mixing, stirring, and pouring onto application sites to create flexible, durable, and UV-resistant insulation.

Benefits of technology

The material achieves improved fire resistance, thermal stability, UV resistance, and reduced deterioration, while maintaining permeability, flexibility, and ease of application, suitable for various surfaces and environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An insulating material, particularly a permeable fire-resistant insulating material containing water glass, comprising a curable compound containing 2-40% by weight of plastic balls, 55-95% by weight of an aqueous sodium silicate solution, 2-6% by weight of aluminum hydroxide, and 0.1-0.5% by weight of a water glass stabilizer. 11. A method for producing the insulating material, particularly a breathable fire-resistant insulating material containing water glass and plastic balls, comprising: first, mixing the plastic balls with an aqueous carbon black solution to coat their entire surfaces; then, adding the plastic balls to the aqueous sodium silicate solution and mixing the whole to form an insulating mixture; then, adding the water glass stabilizer to the aqueous sodium silicate solution; then, mixing the water glass hardener with the solution; and stirring the solution for another 1-10 minutes to form a binder solution; adding the insulating mixture to the binder solution while constantly stirring; then, mixing the whole; and finally, pouring the resulting mixture onto the application site.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an insulating material, in particular a permeable fire-resistant insulating material containing water glass, and a method for producing the same. [Background technology]

[0002] From the current state of the art it is known to use insulating materials for insulating various types of buildings.

[0003] For horizontal insulation, modern spray-on insulation made from PUR foam is used, as well as polystyrene panels. The disadvantages of this foam are its low fire resistance and rapid aging.

[0004] Another known method of insulating horizontal and vertical surfaces is mineral wool insulation. Mineral wool has higher fire resistance but is absorbent, which means it loses its insulating properties and mold grows in it.

[0005] From the Czech patent application CZ PV2017-127, a soundproofing and thermal insulation material for use in structures is known, which has a thermal insulation capacity of 300 kg / m 3 It consists of a slurry of an air-hardening mixture containing 5-76% by weight of bulk insulation material with a specific volume mass of less than 10 ...

[0006] Czech Utility Model CZ 31095 discloses a mixture for a permeable, fire-resistant, lightweight polystyrene insulation system. The mixture contains 10% by weight of expanded polystyrene beads with a diameter of 3 to 6 mm, 88% by weight of sodium silicate water glass, 1% by weight of carbon black, and 1% by weight of a water glass stabilizer - hydrophilic alkoxyalkyl-ammonium salt. The disadvantage of this mixture is that the carbon black is not provided as a protective material on the surface of the beads but is freely dispersed in the insulation material, which causes the insulation material to have a higher thermal conductivity and lower thermal stability, thus limiting its fire-resistant properties and making it less resistant to UV radiation, resulting in very rapid deterioration. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Czech Republic Patent Application No. CZ PV2017-127 [Patent Document 2] Czech Republic Utility Model No. CZ 31095 Summary of the Invention [Problem to be solved by the invention]

[0008] From the above current technology, it is clear that the main drawback of the current technology is the lower thermal insulation properties of the known materials and their faster degradation rate.

[0009] The object of the present invention is a lightweight insulating material structure that is highly fire resistant while at the same time being flexible, pliable, and resistant to degradation. [Means for solving the problem]

[0010] The above-mentioned drawbacks are largely eliminated and the object of the present invention is achieved in a first variant by an insulating material, in particular a permeable fire-resistant insulating material containing water glass, characterized in that according to the invention the material consists of a hardening mixture containing 2-40% by weight of plastic balls, 55-95.0% by weight of an aqueous sodium silicate solution, 2-6% by weight of aluminum hydroxide and 0.1-0.5% by weight of a water glass stabilizer.

[0011] In an advantageous embodiment, the plastic ball is a hollow plastic ball.

[0012] The advantages of this insulating material are significantly improved fire resistance, significantly higher thermal stability, high resistance to UV radiation, and significantly lower degradation. Another advantage is very good transparency. To improve flame retardancy, the mixture contains aluminum hydroxide.

[0013] Preferably, the plastic ball has a diameter of 1 to 50 mm, most preferably made of polypropylene. In other advantageous variations, the plastic ball material may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon. The advantage is the possibility of optimizing the structure of the material for optimal placement.

[0014] It is highly advantageous if the surface of the plastic ball is provided with carbon black, with pure carbon black comprising 0.025 to 0.25% by weight of the total weight. The carbon black provided in this manner has the advantage of reducing radiation transmittance and not increasing thermal conductivity. Another advantage is that carbon black acts as a flame retardant, reducing the flame retardancy of the plastic.

[0015] It is also advantageous that the water glass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt.

[0016] In this case, the sodium silicate solution is 1370 to 1400 kg / m 3 It is highly advantageous to have a density in the range of 1000 to 10000, and a molar ratio of SiO2 to Na2O in the range of 3.2 to 3.4. The molar mass ratio of silica to sodium oxide and the associated solution density and concentration have a significant effect on the rheological properties of the water glass as a polymer mixture, its electrical properties in electrolytes, compressibility and adhesive strength, as well as its hardness and strength. The advantage of the above parameters is that the resulting insulating material is partially flexible and pliable after curing.

[0017] The insulating material further advantageously comprises a hardening agent, which may be glycerol monoacetate-triacetate or a combination thereof.

[0018] The above drawbacks are largely eliminated, and the object of the present invention is achieved by a method for producing an insulating material, particularly a permeable fire-resistant insulating material containing water glass and plastic balls. According to the present invention, the method first mixes plastic balls with an aqueous carbon black solution so that their entire surface is coated, then adds aluminum hydroxide and mixes the whole to form an insulating mixture. Next, a water glass stabilizer is added to an aqueous sodium silicate solution, and then a water glass hardener is mixed into the solution. This solution is stirred for 1 to 10 minutes to form a binder solution. After this, the insulating mixture is poured into the binder solution while constantly stirring, and after mixing, the resulting mixture is poured onto the application site. The advantage of this method is that it can produce both solid products, such as insulating panels and building materials, and the insulating material can also be applied in its liquid form. [Effects of the Invention]

[0019] The resulting compound is then poured into a mold, which is the application site, and a sufficient amount of binder solution is then extruded from the resulting compound by means of a press to produce the desired ratio of insulating compound and binder solution. The advantage of this is that it is possible to easily produce products with precise parameters.

[0020] It is also advantageous to finally leave the mixture obtained until it hardens, the advantage of which is that the resulting insulation can be precisely tailored with respect to the geometric parameters of the insulating space: due to the fact that the hardening length can be regulated, the insulation material can be precisely molded to the desired shape.

[0021] The main advantage of the insulating material and its manufacturing method according to the present invention is that it has insulating properties comparable to those of previously used insulating materials, while, unlike existing materials, it is non-flammable, vapor-permeable, resistant to rainwater and moisture, antifungal, strong, flexible, and resistant to external influences such as ultraviolet radiation. Another advantage is the simple method of application. Both covering boards and building materials can be made from the insulating material, which can be easily applied as a liquid mixture by drawing, casting, or spraying. Therefore, the insulating material is suitable for floors and ceilings, horizontal and slightly sloped roofs, and replaces mineral wool, polystyrene concrete, or polyurethane foam. Unlike mineral wool or polystyrene board insulation, it is successfully applied in hard-to-reach places and on uneven edges of surfaces. It has good adhesion to various substrates, including trapezoidal and folded sheets, eternit, or asphalt, which are commonly found on roofs. At the same time, the insulating material is sufficiently strong and walkable. Another major advantage of the insulating material according to the present invention over existing materials is the ability to combine the board with the liquid mixture. One of the problems associated with fastening conventional polystyrene boards is the filling of the joints between the board and the holes around the dowels. Thanks to the possibility of filling these gaps and openings with liquid insulating material, a uniform surface with no heat escape route can be created very easily and quickly. Another major advantage is that semi-finished insulating material in the form of a liquid mixture can be used as an insulating lining in industries such as household appliances, electrical engineering, and automobiles. DETAILED DESCRIPTION OF THE INVENTION

[0022] Example 1

[0023] The permeable fire-resistant heat insulating material consists of an air-hardening compound containing 12% by weight of hollow plastic balls, which are polypropylene balls with a diameter of 5 to 10 mm, and 81.0% by weight of an aqueous sodium silicate solution.

[0024] The surface of the hollow plastic ball is provided with carbon black, which constitutes 0.4% by weight of the total weight.

[0025] Alternatively, the material of the hollow plastic beads may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon.

[0026] The waterglass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in the form of a 98% aqueous solution.

[0027] The density of sodium silicate solution is 1390 kg / m 3 and the molar ratio of SiO2 to Na2O is 3.3.

[0028] The waterglass hardener is a compound of pure glycerol diacetate / triacetate in a volume ratio of 7:3, with a concentration of 2.8% by weight relative to the clear waterglass.

[0029] According to the manufacturing method of this heat insulating material, first, hollow plastic balls are mixed with an aqueous solution of 25% by weight of carbon black, and the entire surface is coated with carbon black. After that, aluminum hydroxide is added and the whole is mixed to form a heat insulating compound. Next, a water glass stabilizer is added to an aqueous solution of sodium silicate, and a water glass hardener is added to this solution. This solution is mixed for 5 minutes to form a binder solution. Next, the heat insulating mixture is added to the binder solution while constantly stirring, and the whole is mixed. The resulting mixture is poured into the application site, which is a silicone mold. Furthermore, from the resulting mixture, an amount of binder solution is extruded by means of a press so as to obtain a desired ratio of the heat insulating mixture to the binder solution.

[0030] Finally, the mixture is left to harden. The resulting product is an insulation board, or more precisely, an insulation layer placed on an OSB board, or between two OSB boards.

[0031] Example 2

[0032] The permeable fire-resistant insulating material is composed of an air-hardening compound containing 2% by weight of hollow plastic balls, which are polypropylene spheres with a diameter of 1 to 5 mm, 95.0% by weight of an aqueous sodium silicate solution, 2% by weight of aluminum hydroxide, 0.1% by weight of a water glass stabilizer, and 0.8% by weight of a hardener.

[0033] The surface of the hollow plastic ball is provided with carbon black, and the carbon black accounts for 0.1% by weight of the total weight.

[0034] Alternatively, the material of the hollow plastic ball may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon.

[0035] The waterglass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in the form of a 98% aqueous solution.

[0036] Density is 1370 kg / m 3 and the molar ratio of SiO2 to Na2O is within 3.2.

[0037] The waterglass hardener is a compound of pure glycerol diacetate / triacetate in a volume ratio of 7:3, with a concentration of 0.8% by weight relative to the transparent waterglass.

[0038] According to the manufacturing method of this insulating material, first, hollow plastic balls are mixed with an aqueous solution with a carbon black concentration of 25% by weight, and their entire surfaces are coated with carbon black. After that, aluminum hydroxide is added and the whole is mixed to form an insulating mixture; next, a water glass stabilizer is added to a sodium silicate aqueous solution, and a water glass hardener is added to this solution. This solution is mixed for 1 minute to form a binder solution; then, the insulating mixture is added to the binder solution with constant stirring, and the whole is mixed; the resulting mixture is poured into a flat divided attic space, spread, surface-treated, and left to harden.

[0039] Example 3

[0040] The permeable fire-resistant insulating material is made of an air-hardening compound containing 39% by weight of hollow plastic balls with a diameter of 10 to 50 mm, 55% by weight of sodium silicate aqueous solution, 2.5% by weight of aluminum hydroxide, 0.5% by weight of water glass stabilizer, and 2% by weight of hardener.

[0041] The hollow plastic ball is made of polypropylene.

[0042] Alternatively, the material of the hollow plastic beads may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon.

[0043] The surface of the hollow plastic ball is provided with carbon black, which constitutes 1% by weight of the total weight.

[0044] The waterglass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in the form of a 98% aqueous solution.

[0045] Density is 1400 kg / m 3 and the molar ratio of SiO2 to Na2O is in the range of 3.4.

[0046] The waterglass hardener is a compound of pure glycerol diacetate / triacetate in a volume ratio of 7:3, with a concentration of 4.5% by weight relative to the clear waterglass.

[0047] According to this method of manufacturing the insulating material, hollow plastic balls are first mixed with an aqueous solution containing 25% by weight of carbon black, and their entire surfaces are coated with carbon black. After that, aluminum hydroxide is added and the whole is mixed to form an insulating mixture. Next, a water glass stabilizer is added to an aqueous sodium silicate solution, and a water glass hardener is added to this solution. This solution is mixed for 10 minutes to form a binder solution. Next, the insulating mixture is added to the binder solution with constant stirring, and the whole is mixed. The resulting mixture is poured onto the exterior wall of a building equipped with a formwork having a silicone surface. Finally, the resulting mixture is left to harden, and then the formwork is removed.

[0048] Example 4

[0049] The permeable fire-resistant insulating material is composed of an air-hardening compound containing 12% by weight of plastic balls, which are polypropylene balls with a diameter of 5 to 10 mm, 81.0% by weight of sodium silicate aqueous solution, 4% by weight of aluminum hydroxide, 0.3% by weight of water glass stabilizer, and 2.3% by weight of hardener.

[0050] The surface of the plastic ball is provided with carbon black, which constitutes 0.4% by weight of the total weight.

[0051] Alternatively, the material of the plastic sphere may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon.

[0052] The waterglass stabilizer is a hydrophilic alkoxyalkylammonium salt of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in the form of a 98% aqueous solution.

[0053] The density of sodium silicate solution is 1390 kg / m 3 and the molar ratio of SiO2 to Na2O was 3.3.

[0054] The waterglass hardener is a compound of pure glycerol diacetate / triacetate in a volume ratio of 7:3, with a concentration of 2.8% by weight relative to the clear waterglass.

[0055] According to the manufacturing method of the heat insulating material, firstly, plastic balls are mixed with an aqueous solution of carbon black with a concentration of 25% by weight, and the entire surface is coated with carbon black, then aluminum hydroxide is added, and the whole is mixed to form a heat insulating mixture, then a water glass stabilizer is added to an aqueous solution of sodium silicate, and a water glass hardener is added to this solution, and this solution is mixed for 5 minutes to form a binder solution, then the heat insulating mixture is added to the binder solution with constant stirring, and the whole is mixed, then the obtained mixture is poured into the application site, which is a silicone mold, and further, from the obtained mixture, such an amount of binder solution is extruded by means of a press so as to obtain a desired ratio of the heat insulating mixture to the binder solution.

[0056] Finally, the resulting mixture is left to harden. The resulting product is an insulation board, or more precisely, an insulation layer placed on an OSB board, or between two OSB boards.

[0057] Example 5

[0058] The permeable fire-resistant insulating material is composed of 2% by weight of plastic balls, which are polypropylene balls with a diameter of 1 to 5 mm, an air-hardening compound containing 95.0% by weight of sodium silicate aqueous solution, 2% by weight of aluminum hydroxide, 0.1% by weight of water glass stabilizer, and 0.8% by weight of hardener.

[0059] The surface of the plastic ball is provided with carbon black, which constitutes 0.1% by weight of the total weight.

[0060] Alternatively, the material of the plastic sphere may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon.

[0061] The waterglass stabilizer is a hydrophilic alkoxyalkylammonium salt of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in the form of a 98% aqueous solution.

[0062] Density is 1370 kg / m 3 and the molar ratio of SiO2 to Na2O is within 3.2.

[0063] The waterglass hardener is a compound of pure glycerol diacetate / triacetate in a volume ratio of 7:3, with a concentration of 0.8% by weight relative to the transparent waterglass.

[0064] According to the manufacturing method of the insulating material, firstly, plastic balls are mixed into an aqueous solution with a carbon black concentration of 25% by weight, and the entire surface is coated with carbon black, then aluminum hydroxide is added and the whole is mixed to form an insulating mixture, then a water glass stabilizer is added to the sodium silicate aqueous solution, and a water glass hardener is added to this solution, and this solution is mixed for 1 minute to form a binder solution, then the insulating mixture is added to the binder solution with constant stirring, and the whole is mixed, and the resulting mixture is poured into a flat divided attic space, spread, surface treated, and left to harden.

[0065] Example 6

[0066] The permeable fire-resistant insulating material is made of an air-hardening compound containing 39% by weight of plastic balls with a diameter of 10 to 50 mm, 55% by weight of sodium silicate aqueous solution, 2.5% by weight of aluminum hydroxide, 0.5% by weight of water glass stabilizer, and 2% by weight of hardener.

[0067] The plastic ball is made of polypropylene.

[0068] Alternatively, the material of the plastic sphere may be polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, aminoplast or Teflon.

[0069] The surface of the plastic ball is provided with carbon black, which constitutes 1% by weight of the total weight.

[0070] The waterglass stabilizer is a hydrophilic alkoxyalkylammonium salt of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in the form of a 98% aqueous solution.

[0071] Density is 1400 kg / m 3 and the molar ratio of SiO2 to Na2O is in the range of 3.4.

[0072] The waterglass hardener is a compound of pure glycerol diacetate / triacetate in a volume ratio of 7:3, with a concentration of 4.5% by weight relative to the clear waterglass.

[0073] According to the manufacturing method of the insulating material, first, plastic balls are mixed into an aqueous solution with a carbon black concentration of 25% by weight, and their entire surfaces are coated with carbon black. After that, aluminum hydroxide is added and the whole is mixed to form an insulating mixture. Next, a water glass stabilizer is added to an aqueous solution of sodium silicate, and a water glass hardener is added to this solution. This solution is mixed for 10 minutes to form a binder solution. Next, the insulating mixture is added to the binder solution with constant stirring, and the whole is mixed. Then, the resulting mixture is poured onto the exterior wall of a building equipped with a formwork having a silicone surface. Finally, the resulting mixture is left to harden, and then the formwork is removed. [Industrial Applicability]

[0074] The insulating material according to the invention can in particular be used in the building industry to make permeable fire-resistant insulation systems.

Claims

1. A permeable fire-resistant heat insulating material comprising water glass, 2 to 40% by weight of hollow plastic balls; 55 to 95.0% by weight of an aqueous solution of sodium silicate; 2 to 6% by weight of aluminum hydroxide; 0.1 to 0.5% by weight of a water glass stabilizer; and a hardening compound containing the same. The entire surface of the plastic ball is provided with carbon black, which constitutes 0.1 to 1% by weight of the total weight of the ball; A heat insulating material, characterized in that the water glass stabilizer is a hydrophilic alkoxyalkyl-ammonium salt.

2. 2. The heat insulating material according to claim 1, wherein the plastic balls have a diameter of 1 to 50 mm.

3. 3. The heat insulating material according to claim 1, wherein the material of the plastic balls is polypropylene.

4. 3. The heat insulating material according to claim 1, wherein the material of the plastic balls is polyethylene, polyurethane, polymethyl methacrylate, polyamide, polyvinyl chloride, polyester, phenolic resin, or polytetrafluoroethylene.

5. The heat insulating material according to any one of claims 1 to 4, characterized in that the density of the sodium silicate aqueous solution is in the range of 1370 to 1400 kg / m3.

6. The insulating material according to any one of claims 1 to 5, characterized in that the molar ratio of SiO2 to Na2O in the sodium silicate aqueous solution is within a range of 3.2 to 3.

4.

7. The insulating material according to any one of claims 1 to 6, further comprising a compound of glycerol diacetate / triacetate.

8. A method for producing a breathable fireproof material containing water glass and plastic balls according to any one of claims 1 to 6, comprising the steps of: First, the plastic ball is mixed with an aqueous solution of carbon black to coat the entire surface of the ball, Then, add to the aqueous sodium silicate solution and mix the whole to form an adiabatic mixture; Then, a water glass stabilizer is added to the aqueous sodium silicate solution; Then, the glycerol diacetate / triacetate compound is mixed and stirred for an additional 1-10 minutes to form a binder solution, and the adiabatic mixture is added to the binder solution with constant stirring and mixed throughout; The method for producing an insulating material comprises pouring the mixture into a mold.

9. A method for producing an insulating material as described in claim 8, characterized in that from the mixture obtained by pouring into the mold, such an amount of binder solution is extruded by a pressing means so as to obtain a desired ratio of insulating mixture and binder solution.

10. A method for producing an insulating material, comprising leaving the insulating material obtained by the method for producing an insulating material described in claim 8 or claim 9 to harden.

Citation Information

Patent Citations

  • Toughening heat-resistant PPR tubular product and preparation method thereof

    CN109796682A

  • A mixture for a breathable, fire retardant lightweight polystyrene thermal insulation system

    CZ31095U1

  • CZPV2017-127

  • Manufacture of flame retardant heat insulating material

    JP1984141454A

  • Binder composition, non-combustible formed material, non-combustible sheet and non-combustible honeycomb structure material

    JP2001019733A