Manufacturing method of non-magnetic stainless steel sheet and steel material for machine parts
Austenitic stainless steel with a specific chemical composition and processing method addresses the challenges of non-magnetic properties, shear workability, and wear resistance by ensuring large crystal grains and low work hardening, enhancing polishability and workability for precision mechanical parts.
Patent Information
- Application Number
- JP2020116336
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-06
AI Technical Summary
Existing austenitic stainless steels used in precision mechanical parts face challenges in achieving both non-magnetic properties, good shear workability, cold forgeability, and wear resistance, with annealed sheets sagging during press working and hard materials being difficult to polish.
Austenitic stainless steel with a specific chemical composition and processing method involving cold rolling and annealing to achieve large crystal grains, low work hardening index, and high hardness, ensuring non-magnetic properties and improved barrel polishability.
The solution results in a non-magnetic stainless steel with enhanced wear resistance, reduced sagging and burrs during processing, and improved polishability, maintaining high hardness and workability for precision mechanical parts.
Smart Images

Figure 0007576935000001 
Figure 0007576935000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a non-magnetic austenitic stainless steel sheet suitable for use as a material for machine parts manufactured by press working or barrel polishing, and also to a method for producing the non-magnetic austenitic stainless steel sheet. [Background technology]
[0002] Austenitic stainless steels are used in a variety of applications due to their excellent workability. When extensive processing is required, such as forging, it is advantageous to use stable austenitic stainless steels that contain a large amount of austenite-forming elements and thus are less likely to form processing-induced martensite.
[0003] On the other hand, for precision machine parts, the stronger the magnetism, the more easily dust is attracted to them, so materials that maintain their non-magnetic nature after processing are preferred. In addition, polishing is sometimes performed after press processing such as punching and forging to remove burrs and surface defects and to adjust the part shape.
[0004] Austenitic stainless steel with improved austenite stability is considered as a candidate for a material with excellent workability such as cold forgeability (coining property) suitable for manufacturing precision mechanical parts. For example, Patent Documents 1 and 2 disclose such austenitic stainless steel sheets. In the technology described in these documents, softening is attempted in order to emphasize cold forgeability, and the final processing history as a steel sheet is "annealing". However, such annealed steel sheets are soft, so that sagging becomes large during press processing, which is a factor that leads to a decrease in dimensional accuracy and productivity of parts. In addition, from the viewpoint of the life of mechanical parts, materials with less wear during sliding, that is, hard materials, are preferred. However, hard materials generally have poor polishing properties in the polishing process, so it has been difficult to achieve both wear resistance during sliding and polishing properties in the polishing process. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-371339 A [Patent Document 2] JP 2018-109215 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to provide a non-magnetic stainless steel material that has good shear workability, cold forgeability, barrel polishing property, and wear resistance and is suitable as a material for precision machine parts. It also aims to provide a steel material for machine parts obtained from the non-magnetic stainless steel material. Note that, unless otherwise specified, "wear resistance" in this specification does not mean high resistance to abrasive wear during barrel polishing (hard to be polished), but means hard to be worn due to sliding when used as a part. [Means for solving the problem]
[0007] In order to achieve excellent wear resistance in sliding parts, it is necessary to ensure sufficient hardness. In order to reduce sagging and burrs during shear processing and promote plastic flow during upsetting, it is advantageous to use a material with a low n-value (work hardening index). Refining the crystal grains is effective in reducing the n-value. However, it is difficult to ensure good barrel polishability in a structure state where the hardness is high and the crystal grain size is small. Therefore, the inventors have repeatedly studied various effective means for simultaneously providing barrel polishability. As a result, it was found that it is extremely effective to cold-roll a material with coarse crystal grains and ensure hardness by utilizing the work hardening imparted by the cold rolling. By increasing the crystal grains, the polishability in barrel polishing, which is largely due to abrasive wear, is improved, and the n-value of the material work-hardened by cold rolling is reduced compared to annealed material, and the negative contribution of increasing the crystal grains to the reduction in the n-value can be countered. In other words, it was found that the following methods (i) and (ii) are extremely effective. (i) It has a chemical composition that has high austenite stability, which allows it to maintain non-magnetic properties even after processing, and exhibits low work-hardening ability (hard to work-harden, low n value). (ii) After the crystal grains are coarsened by annealing at a relatively high temperature, the material is cold-rolled at a specific rolling ratio to give the material a structure having large crystal grain sizes and high hardness. This specification specifically discloses the following inventions.
[0008] [1] A cold-rolled steel sheet having a chemical composition, in mass%, of C: 0.005-0.080%, Si: 0.10-1.00%, Mn: 1.00-4.00%, Ni: 7.00-14.00%, Cr: 15.00-19.00%, N: 0.001-0.060%, Mo: 0-0.50%, Cu: 2.00-4.00%, Ti: 0-0.20%, Al: 0-0.020%, the balance being Fe and unavoidable impurities, and an A value defined by the following formula (1) being 0 or less, wherein the Vickers hardness of the rolled surface is 220-285HV, the fracture elongation in the rolling direction is 3-15%, and the relative permeability μr is 1.030 or less, A non-magnetic stainless steel sheet having barrel polishability that is judged to pass in the evaluation method shown in (X) below. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo…(1) Here, the content value of the element expressed as mass% is substituted for the element symbol in formula (1). (X) A disk-shaped test piece with a diameter of 30 mm is taken from the steel plate to be evaluated by conventional punching with a one-side clearance of 3% and a processing speed of 30 spm. The test piece is subjected to centrifugal barrel polishing for 30 minutes at 300 rpm using a medium containing 10 g / L of ceramic media in water in the shape of a regular triangular prism with a height of 4 mm and a base of an equilateral triangle with a side length of 4 mm. After barrel polishing, the arithmetic mean roughness Ra over the entire diameter of both surfaces perpendicular to the thickness direction of the disk-shaped test piece is measured using a stylus roughness meter on two straight lines that pass through the center of the disk and are perpendicular to each other. If the Ra measured on a total of four straight lines on both sides is 1.0 μm or less, the test piece is judged to have passed the test. [2] The non-magnetic stainless steel sheet according to the above [1], having a sheet thickness of 0.8 to 1.5 mm. [3] A non-magnetic stainless steel sheet according to the above [1] or [2] for use in parts manufactured by subjecting the sheet to shearing and barrel polishing. [4] A "final annealing process" in which a cold-rolled steel sheet intermediate product having a chemical composition, in mass%, of C: 0.005-0.080%, Si: 0.10-1.00%, Mn: 1.00-4.00%, Ni: 7.00-14.00%, Cr: 15.00-19.00%, N: 0.001-0.060%, Mo: 0-0.50%, Cu: 2.00-4.00%, Ti: 0-0.20%, Al: 0-0.020%, the balance Fe and unavoidable impurities, and an A value defined by the following formula (1) is 0 or less, is annealed at a maximum temperature of 1075-1200 ° C and a holding time of 10 seconds or more at 1075 ° C or higher to obtain an annealed steel sheet; A "finish cold rolling process" in which the annealed steel sheet is cold rolled at a rolling ratio of 10 to 50% to obtain a cold-rolled steel sheet having a Vickers hardness of the rolled surface of 220 to 285 HV, a fracture elongation in the rolling direction of 3 to 15%, and a relative permeability μr of 1.030 or less; Includes and has barrel polishability that is judged to be acceptable in the evaluation method (X) described below. A method for manufacturing non-magnetic stainless steel sheets. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo…(1) Here, the content value of the element expressed as mass% is substituted for the element symbol in formula (1). (X) A disk-shaped test piece with a diameter of 30 mm is taken from the steel plate to be evaluated by conventional punching with a one-side clearance of 3% and a processing speed of 30 spm. The test piece is subjected to centrifugal barrel polishing for 30 minutes at 300 rpm using a medium containing 10 g / L of ceramic media in water in the shape of a regular triangular prism with a height of 4 mm and a base of an equilateral triangle with a side length of 4 mm. After barrel polishing, the arithmetic mean roughness Ra over the entire diameter of both surfaces perpendicular to the thickness direction of the disk-shaped test piece is measured using a stylus roughness meter on two straight lines that pass through the center of the disk and are perpendicular to each other. If the Ra measured on a total of four straight lines on both sides is 1.0 μm or less, the test piece is judged to have passed the test. [5] The method for producing a non-magnetic stainless steel sheet according to the above [4], wherein in the finish annealing step, a steel sheet is obtained having an average crystal grain size of 40 to 100 μm in a cross section (L cross section) parallel to the rolling direction and the sheet thickness direction. [6] The method for producing a non-magnetic stainless steel sheet according to the above [4] or [5], wherein in the finish cold rolling step, a steel sheet having a thickness of 0.8 to 1.5 mm is obtained. [7] A method for producing a steel material for machine parts, comprising processing the non-magnetic stainless steel plate obtained by the manufacturing method according to any one of the above items [4] to [6] through a step including shearing. [8] A method for producing steel material for mechanical parts, comprising processing a steel material having a sheared portion derived from a non-magnetic stainless steel plate obtained by the production method described in any one of [4] to [6] above, through a process including barrel polishing.
[0009] Of the above elements, Mo, Ti, and Al are optional elements. Effect of the Invention
[0010] The non-magnetic stainless steel sheet according to the present invention has the following advantages. Although the material is work-hardened by finish cold rolling, its low n-value promotes plastic flow during harsh press punching and upsetting processes, resulting in good workability. - The elongation is kept moderately low, so sagging and burrs in the press punched parts are reduced. This reduces the load during barrel polishing. In barrel polishing, it is believed that contact with the media (abrasive) leads to surface smoothing through a mechanism similar to three-dimensional abrasive wear. However, because the crystal grains are large, polishing due to abrasive wear progresses easily, and good barrel polishability can be obtained even though the steel is already work-hardened. When finally used as a sliding part, the high hardness achieved by finish cold rolling provides excellent wear resistance, and the highly austenitic chemical composition maintains non-magnetic properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] [Chemical composition of steel] Hereinafter, "%" in the steel composition means mass% unless otherwise specified.
[0012] C and N are elements necessary to improve austenite stability. The C content must be 0.005% or more. The N content must be 0.001% or more, and is preferably 0.005% or more. On the other hand, these elements have the effect of hardening the steel by solid solution strengthening. In the present invention, the hardness of the steel material is increased by work hardening in temper rolling. If the hardness increase by solid solution strengthening is excessively added, the workability decreases, which is not preferable. The C content is limited to 0.080% or less, and is more preferably 0.050% or less. The N content is limited to 0.060% or less.
[0013] Silicon is useful for deoxidization and for adjusting the stability of austenite during processing (reducing the A value described later), while it also has the effect of hardening steel through solid solution strengthening. The silicon content must be in the range of 0.10 to 1.00%, and is more preferably in the range of 0.40 to 0.90%.
[0014] Mn is useful for deoxidization and for adjusting the austenite stability during processing (reducing the A value described later). However, excessive Mn content reduces stacking fault energy, making it difficult to adjust the composition to obtain properties that are less susceptible to work hardening. The Mn content is limited to the range of 1.00 to 4.00%, and more preferably 1.30 to 1.90%.
[0015] The Ni content must be 7.00% or more in order to improve the austenite stability. A large amount of Ni content is a factor that leads to an increase in the price of steel materials. The present invention targets steel with a Ni content of 14.00% or less. Steel with a Ni content of 11.50 to 13.50% is more suitable.
[0016] Cr is an essential element for ensuring the corrosion resistance of stainless steel. Considering the usage environment of various precision machine parts, the Cr content must be 15.00% or more. It is more preferable to make it 15.50% or more. However, Cr has the effect of hardening steel by solid solution strengthening. The Cr content is limited to 19.00 or less, and may be controlled to 17.00% or less.
[0017] Mo is an element effective in improving corrosion resistance, and can be added as necessary. In that case, it is more effective to ensure a content of 0.01% or more. However, Mo has the effect of hardening the steel by solid solution strengthening. Since the steel sheet according to the present invention is work-hardened by finish cold rolling, unlike the case of annealed steel sheet, if a large amount of Mo is added, solid solution strengthening is exerted, the material becomes excessively hard, and workability is impaired. When Mo is added, the content must be 0.50% or less, and may be limited to a range of 0.10% or less, or 0.05% or less.
[0018] Cu is an important element in the present invention because it has the effect of increasing austenite stability and increasing stacking fault energy. By increasing the austenite stability, good non-magnetic properties can be maintained in the steel sheet finished by cold rolling. By increasing the stacking fault energy, the property of being resistant to work hardening is imparted. In order to fully obtain these effects, the Cu content is set to 2.00% or more, and more preferably 3.00% or more. A high Cu content has an adverse effect on hot workability. The Cu content is limited to a range of 4.00% or less. It may be controlled to 3.70% or less.
[0019] Ti fixes C and N, so it is effective in preventing excessive hardening. Ti can be added as needed. In that case, it is more effective to set the Ti content to 0.005% or more. If the Ti content is high, inclusions may be formed, which may deteriorate the workability. If Ti is added, the content must be 0.20% or less. It may be limited to 0.10% or less.
[0020] Al is effective as a deoxidizer and can be added as necessary. In order to fully utilize the deoxidizing effect of Al, it is more effective to add Al so that the Al content is 0.001% or more. If the Al content is high, inclusions may form, which may deteriorate the workability. The Al content is limited to 0.020% or less.
[0021] P is permitted up to 0.050% and S is permitted up to 0.005%.
[0022] The A value determined by the following formula (1) is an index showing the stability of the austenite phase. The smaller the A value, the more stable the austenite phase is, and the less likely it is that the deformation-induced martensite phase will form, which is advantageous for improving workability and maintaining non-magnetic properties. As a result of various investigations, a chemical composition with a low A value of 0 or less has been adopted here. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo…(1) Here, the content value of the element expressed as mass% is substituted for the element symbol in formula (1).
[0023] [Manufacturing method] The stainless steel sheet according to the present invention can be manufactured by melting steel having the above-mentioned chemical composition and by a process including "casting, hot rolling, hot-rolled sheet annealing, cold rolling, finish annealing, and finish cold rolling" in the above order. Although not described in the above steps, pickling is usually performed after annealing. The "annealed steel sheet" referred to in this specification includes so-called "annealed pickled steel sheet" that has been subjected to pickling after annealing. In addition, in this specification, the cold-rolled steel sheet to be subjected to finish annealing is called "cold-rolled steel sheet intermediate product". The cold rolling process before the finish annealing can be performed by multiple cold rolling including intermediate annealing as necessary. It is desirable that the cold-rolled steel sheet intermediate product is a cold steel sheet with a cold rolling reduction ratio of about 40 to 60%.
[0024] (finish annealing) The intermediate cold-rolled steel sheet is annealed at a maximum temperature of 1075 to 1200°C and for a holding time of 10 seconds or more at 1075°C or higher to obtain an annealed steel sheet. This makes it possible to obtain a steel sheet having an average crystal grain size of 40 to 100 μm in a cross section (L cross section) parallel to the rolling direction and the sheet thickness direction. If the average crystal grain size at this stage exceeds 100 μm and becomes too coarse, the steel sheet may be too soft and may not have sufficient hardness after finish cold rolling. The upper limit of the maximum temperature may be controlled to 1175°C or 1150°C. There is no particular restriction on the upper limit of the holding time at 1075°C or higher, but considering the implementation in a continuous annealing furnace, it is preferable to set it in the range of 60 seconds or less. There is no particular restriction on the atmosphere in the furnace for the finish annealing. Except when annealing is performed in a non-oxidizing atmosphere, pickling is usually performed after the finish annealing.
[0025] The average crystal grain size can be measured as follows. (Method of measuring average crystal grain size) The L-section of the steel plate is polished and then etched with hydrofluoric acid, nitric acid, and glycerin (hydrofluoric acid:nitric acid:glycerin = 1:1:2) to expose the austenite grain boundaries and prepare an observation surface, and a microscope image of the observation surface is obtained. On the microscope image, a straight test line is drawn parallel to the plate thickness direction, passing through the center of the plate thickness and having a length of at least half the plate thickness, and the number n of intersections between the test line and the grain boundaries is counted to determine the average line length L (μm) per grain of the test line that crosses the grain. The average line length L is the distance L between the intersection closest to one end of the test line and the intersection closest to the other end. 0 (μm) divided by the value of n-1. One or more test lines are set at randomly selected positions in the L direction so that the total number of crystal grains crossing the test lines is 250 or more. When multiple test lines are set, a single crystal grain is not crossed by multiple test lines. The arithmetic mean of the average line segment length L (μm) obtained for each test line is the average crystal grain size (μm) of the steel plate.
[0026] (Finish cold rolling) The annealed steel sheet having the structure obtained by the above-mentioned finish annealing is cold-rolled at a rolling reduction ratio in the range of 10 to 50% to obtain a stainless steel sheet according to the present invention. In order to realize excellent wear resistance in precision machine parts, it is desirable to adjust the hardness to 220 HV or more at the stage of the steel sheet material before parts processing. If it is too hard, it becomes difficult to process it into parts, but the target steel of the present invention has a chemical composition that is not prone to solid solution strengthening and has high stacking fault energy and is not prone to work hardening, so as long as the hardness increase by finish cold rolling is in the range of up to 285 HV, good workability can be enjoyed. The tensile strength in the rolling direction is 850 N / mm 2 It is preferable that the ductility is less than 1.0%. In order to realize good shear processing with less burrs and burrs in severe press punching, it is desirable that the ductility is moderately suppressed. Specifically, in the case of an austenitic stainless steel sheet having the above-mentioned chemical composition, it has been confirmed that good results can be obtained in severe press punching if the breaking elongation in the rolling direction evaluated by a tensile test is in the range of 3 to 15%. It is more preferable that the breaking elongation is in the range of 5 to 15%. In addition, considering that it may be installed near an electronic circuit and that it is necessary to prevent dust from being attracted, it is necessary to suppress the relative permeability μr to be 1.030 or less and non-magnetic at the stage of the steel sheet material before part processing. In terms of the proportion of magnetic phases such as processing-induced martensite phases, it is desirable that the volume fraction of the magnetic phase is 3.0% or less as measured by a ferrite scope (ferrite content meter). In the case of an annealed steel sheet having the above-mentioned chemical composition, the optimal rolling conditions for imparting the above-mentioned desired characteristics can be set within a rolling ratio range of 10 to 50%. If the rolling reduction ratio is less than 10%, it becomes difficult to stably obtain a cold-rolled steel sheet having a sufficiently low n value (which is less susceptible to work hardening) In this manner, a cold-rolled steel sheet having a thickness of, for example, 0.8 to 1.5 mm is obtained. EXAMPLES
[0027] A continuous cast slab of the steel shown in Table 1 was manufactured, and after being held at a heating temperature set in the range of 1100 to 1300°C, it was extracted and hot rolled, and hot-rolled sheet annealed at 1100°C. After that, multiple cold rolling with intermediate annealing was performed to obtain a cold-rolled steel sheet intermediate product with a cold rolling reduction rate of 40 to 60% after the final intermediate annealing.
[0028] Each cold-rolled steel sheet intermediate product was subjected to finish annealing in a continuous annealing furnace. Finish annealing was performed at the maximum temperature shown in Table 2, and all conditions, except for the cases in which the maximum temperature was lower than 1075°C, were such that the holding time for the material temperature to reach 1075°C or higher was ensured to be 10 seconds or more. For samples taken from the annealed steel sheets after finish annealing, the average grain size of the L cross section was examined according to the "Method for measuring average grain size" described above.
[0029] Each annealed steel sheet was subjected to finish cold rolling at the rolling ratio shown in Table 2 to obtain a cold-rolled steel sheet. After each annealing, pickling was performed. The obtained cold-rolled steel sheets were used as test materials and the following investigations were carried out.
[0030] [Hardness] The surface (rolled surface) perpendicular to the thickness direction of the steel plate was measured for Vickers hardness HV30 (test force 294.2 N) based on JIS Z2244:2009.
[0031] [Tensile strength, elongation at break] Based on JIS Z2241:2011, a tensile test was carried out in the rolling direction using No. 13B test pieces to measure the tensile strength and breaking elongation (butt joint elongation).
[0032] [Relative permeability μr] A sample with a diameter of 5 mm and a thickness of 1 mm was taken from the steel plate of the test material and magnetized by applying a magnetic field of 5 kOe (397.9 kA / m) at a sweep rate of 1 kOe / min using a sample vibration type magnetometer (Riken Denshi Co., Ltd., BHV525). The magnetic permeability was calculated from the slope of the magnetic field-magnetization curve obtained, and the magnetic permeability in vacuum was 4π×10 -7 The relative permeability μr was calculated by dividing by H / m. For each example, measurements were performed for five tests (n=5), and the average value of the five tests was calculated as the relative permeability μr of the test material.
[0033] [Volume fraction of magnetic phase] The volume fraction of the magnetic phase was determined using a ferrite scope (Fischer, FMP30). The volume fraction of the magnetic phase corresponds roughly to the volume fraction of the deformation-induced martensite phase.
[0034] [Barrel polishing ability] Barrel polishing was evaluated using the test method shown in (X) above. The media (abrasive) used was a ceramic regular triangular prism (MT4x4, manufactured by TKX) 4mm high with an equilateral triangular base with sides each measuring 4mm. The barrel polishing machine used was the SKC-32S, manufactured by Shinto Kogyo Co., Ltd. Cases that were deemed acceptable were marked with an ◯, and others with an ×. The above results are shown in Table 2.
[0035] [Table 1]
[0036] [Table 2]
[0037] The steel plate of the present invention has a hardness of 220HV or more, and is therefore believed to exhibit excellent wear resistance. It is adjusted to a chemical composition that is resistant to work hardening, and the n value is reduced by finish cold rolling, so it is believed to have good workability in the processing of various parts. It is adjusted to a ductility of 15% or less at break by cold rolling, so it also has good shear workability. It also has good barrel polishability and non-magnetic properties.
[0038] In contrast, the comparative example No. 5 had a low final annealing temperature, which resulted in insufficient grain coarsening and poor barrel polishability. No. 6 used steel with low austenite stability, so the desired non-magnetic properties could not be obtained. In addition, the composition of the steel was such that processing-induced martensite was easily generated and the steel was easily hardened, so the barrel polishability was poor. No. 7 used steel with an excessive Cu content, so edge cuts occurred during hot rolling, and the experiment was discontinued thereafter. No. 8 used a low final annealing temperature, which resulted in insufficient grain coarsening, and in addition, the rolling ratio of the final cold rolling was low, so the ductility became too high and burrs and burrs became large during shear processing. As a result, the barrel polishability was poor. No. 9 used a too high final annealing temperature, so the grains became excessively coarsened and the ductility decreased. In this case, the barrel polishability was good, but the n value was high, which may cause processing defects during severe upsetting processing, etc.
Claims
1. A cold-rolled steel sheet having a chemical composition, in mass%, of C: 0.005-0.080%, Si: 0.10-1.00%, Mn: 1.00-4.00%, Ni: 7.00-14.00%, Cr: 15.00-19.00%, N: 0.001-0.060%, Mo: 0-0.50%, Cu: 2.00-4.00%, Ti: 0-0.20%, Al: 0-0.020%, the balance being Fe and unavoidable impurities, and an A value defined by the following formula (1) being 0 or less, wherein the Vickers hardness of the rolled surface is 220-285HV, the breaking elongation in the rolling direction is 3-15%, and the relative magnetic permeability μr is 1.030 or less, A non-magnetic stainless steel sheet having barrel polishability that is judged to be acceptable in the evaluation method shown in (X) below. A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo...(1) Here, the content value of the element expressed as mass % is substituted for the element symbol in formula (1). (X) A disk-shaped test piece having a diameter of 30 mm is taken from the steel plate to be evaluated by conventional punching with a one-side clearance of 3% and a processing speed of 30 spm. The test piece is subjected to centrifugal barrel polishing for 30 minutes at 300 rpm using a medium containing 10 g / L of ceramic media in water, the ceramic media being in the shape of a regular triangular prism having a height of 4 mm and a base of an equilateral triangle with a side length of 4 mm. After barrel polishing, the arithmetic mean roughness Ra over the entire diameter of both surfaces perpendicular to the thickness direction of the disk-shaped test piece is measured using a stylus roughness meter on two straight lines passing through the center of the disk and perpendicular to each other. If the Ra measured on a total of four straight lines on both sides is 1.0 μm or less, the test piece is judged to have passed the test.
2. 2. The non-magnetic stainless steel sheet according to claim 1, wherein the sheet has a thickness of 0.8 to 1.5 mm.
3. 3. The non-magnetic stainless steel sheet according to claim 1 or 2, which is for use in a part manufactured by subjecting the part to shearing and barrel polishing.
4. A "finish annealing process" in which a cold-rolled steel sheet intermediate product having a chemical composition in which, in mass%, C: 0.005 to 0.080%, Si: 0.10 to 1.00%, Mn: 1.00 to 4.00%, Ni: 7.00 to 14.00%, Cr: 15.00 to 19.00%, N: 0.001 to 0.060%, Mo: 0 to 0.50%, Cu: 2.00 to 4.00%, Ti: 0 to 0.20%, Al: 0 to 0.020%, the balance Fe and inevitable impurities, and the A value defined by the following formula (1) is 0 or less, is subjected to annealing at a maximum temperature of 1075 to 1200 ° C. and a holding time of 10 seconds or more at 1075 ° C. or higher to obtain an annealed steel sheet; A "finish cold rolling process" in which the annealed steel sheet is subjected to cold rolling at a rolling ratio in the range of 10 to 50% to obtain a cold-rolled steel sheet having a Vickers hardness of the rolled surface of 220 to 285 HV, a fracture elongation in the rolling direction of 3 to 15%, and a relative magnetic permeability μr of 1.030 or less; The method for producing a non-magnetic stainless steel sheet having barrel polishability that is judged to be pass in the evaluation method shown in (X) below, comprising: A value=551-462(C+N)-9.2Si-8.1Mn-29(Ni+Cu)-13.7Cr-18.5Mo...(1) Here, the content value of the element expressed as mass % is substituted for the element symbol in formula (1). (X) A disk-shaped test piece having a diameter of 30 mm is taken from the steel plate to be evaluated by conventional punching with a one-side clearance of 3% and a processing speed of 30 spm. The test piece is subjected to centrifugal barrel polishing for 30 minutes at 300 rpm using a medium containing 10 g / L of ceramic media in water, the ceramic media being in the shape of a regular triangular prism having a height of 4 mm and a base of an equilateral triangle with a side length of 4 mm. After barrel polishing, the arithmetic mean roughness Ra over the entire diameter of both surfaces perpendicular to the thickness direction of the disk-shaped test piece is measured using a stylus roughness meter on two straight lines passing through the center of the disk and perpendicular to each other. If the Ra measured on a total of four straight lines on both sides is 1.0 μm or less, the test piece is judged to have passed the test.
5. 5. The method for producing a non-magnetic stainless steel sheet according to claim 4, wherein in the finish annealing step, a steel sheet is obtained having an average crystal grain size of 40 to 100 μm in a cross section (L cross section) parallel to the rolling direction and the sheet thickness direction.
6. The method for producing a non-magnetic stainless steel sheet according to claim 4 or 5, wherein in the finish cold rolling step, a steel sheet having a thickness of 0.8 to 1.5 mm is obtained.
7. A method for producing a steel material for machine parts, comprising processing the non-magnetic stainless steel plate obtained by the method according to any one of claims 4 to 6 through a step including shearing.
8. A method for producing a steel material for mechanical parts, comprising processing a steel material having a sheared portion derived from a non-magnetic stainless steel plate obtained by the production method according to any one of claims 4 to 6, by a process including barrel polishing.
Citation Information
Patent Citations
Non-magnetic austenitic stainless steel for quality dinnerware
JP1991087336A
Austenitic stainless steel plate for safety valve, and safety valve for hermetically sealed type battery using the same
JP1996158016A
Soft stainless steel sheet superior in workability and cold-forging property
JP2002371339A
Austenitic stainless steel superior in fine blanking property
JP2003113450A
Electric wiring terminal-manufacturing stainless steel plate excellent in surface contact electric resistance and punchability