Method for producing extruded thermoplastic resin foam
The extruded thermoplastic resin foam board, made with styrene-(meth)acrylic acid ester copolymer and polyester resin, addresses high air permeability issues by maintaining low thermal conductivity and flame retardancy, enhancing long-term heat insulation and safety.
Patent Information
- Application Number
- JP2021006353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-01-19
AI Technical Summary
Existing extruded thermoplastic resin foams exhibit high air permeability, leading to poor long-term heat insulation properties and inadequate flame retardancy.
A method for producing an extruded thermoplastic resin foam board using a base resin composed of styrene-(meth)acrylic acid ester copolymer and polyester resin, with specific ratios and a hydrofluoroolefin physical blowing agent, to achieve low thermal conductivity and excellent heat insulation and flame retardancy.
The method results in a foam board that maintains low thermal conductivity over a long period and meets flame retardancy standards, ensuring effective heat insulation and safety as a building material.
Smart Images

Figure 0007576984000001 
Figure 0007576984000002 
Figure 0007576984000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an extruded thermoplastic resin foam board and a manufacturing method thereof, and more particularly to an extruded thermoplastic resin foam board which can be suitably used as an insulating material for the walls, floors, roofs, etc. of buildings, and a manufacturing method thereof. [Background technology]
[0002] Polyester resin is known as a resin for forming a foam board. Polyester resin has a high performance of preventing air from entering the foam board, but it is difficult to mold polyester resin alone into a foam board.
[0003] On the other hand, styrene-(meth)acrylic acid ester copolymers are known as resins that have a high performance of preventing air from flowing into foam boards. However, although it is possible to manufacture foam boards using styrene-(meth)acrylic acid ester copolymers as the sole raw material, there is still room for further improvement in terms of reducing thermal conductivity.
[0004] Therefore, the present inventors proposed an extruded thermoplastic resin foam board (hereinafter, also referred to simply as extruded foam board) containing polystyrene resin and a specific polyester resin (including a styrene-(meth)acrylic acid ester copolymer) in a mass ratio of polystyrene resin to polyester resin of 95:5 to 50:50 in Patent Document 1. This extruded foam board had no uneven waviness on the foam surface, had a good appearance, was sufficiently thick, and had a high expansion ratio.
[0005] The present inventors also proposed a styrene-based resin foam consisting of a mixed resin of polystyrene resin, a styrene-(meth)acrylic acid ester copolymer, and an amorphous polyester resin (the content of the amorphous polyester resin in the examples is 22 to 44% by mass) in Patent Document 2. This extruded foam had little change in thermal conductivity over time and was excellent in flame retardancy and mechanical strength such as bending strain at break. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-082805 A [Patent Document 2] JP 2019-189666 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the extruded foams of Patent Documents 1 and 2 contain a specific ratio of ordinary polystyrene in the base resin, and since the polystyrene has a relatively high air permeability coefficient, there is still room for further improvement in terms of maintaining thermal insulation properties over a long period of time.
[0008] An object of the present invention is to provide an extruded thermoplastic resin foam board capable of maintaining low thermal conductivity for a long period of time and having excellent heat insulation and flame retardancy, and a method for producing the same. [Means for solving the problem]
[0009] The present invention provides the following extruded thermoplastic resin foam insulation board and a method for producing the same. <1> The foaming resin composition is extruded and foamed by kneading a base resin, a physical foaming agent, and a flame retardant, and molded into a plate shape using a molding tool. 3 A method for producing an extruded thermoplastic resin foam board having a thickness of 10 to 150 mm, comprising the steps of: the base resin contains a styrene-(meth)acrylic acid ester copolymer and a polyester resin having a heat of fusion based on JIS K7122-1987 of less than 5 J / g; the blending amount of the polyester resin in the base resin is 5 to 50 mass %, A method for producing an extruded thermoplastic resin foam board, wherein the content of a (meth)acrylic acid ester component derived from a styrene-(meth)acrylic acid ester copolymer in the base resin is 20 to 40 mass %. <2> The physical foaming agent contains a hydrofluoroolefin, and the amount of the hydrofluoroolefin added is 0.5 mol or more and 1.5 mol or less per 1 kg of the base resin. <1> A method for producing an extruded thermoplastic resin foam board according to claim 1. <3> The ratio of the amount of the hydrofluoroolefin added to the total amount of the physical foaming agents added (100 mol %) is 50 mol % or more. <2> A method for producing an extruded thermoplastic resin foam board according to claim 1. <4> The hydrofluoroolefin contains 1,3,3,3-tetrafluoropropene and 1-chloro-3,3,3-trifluoropropene, and the molar ratio of 1,3,3,3-tetrafluoropropene to 1-chloro-3,3,3-trifluoropropene is 20:80 to 80:20. <2> or <3> A method for producing an extruded thermoplastic resin foam board according to claim 1. <5> Contains flame retardant, apparent density 20-50kg / m 3 A thermoplastic resin extruded foam board having a thickness of 10 to 150 mm, The base resin of the extruded thermoplastic resin foam board is a mixture of a styrene-(meth)acrylic acid ester copolymer and a polyester resin having a heat of fusion of less than 5 J / g based on JIS K7122-1987; The polyester in the base resin resin The content is 5 to 50 mass %, The extruded thermoplastic resin foam board is characterized in that the content of a (meth)acrylic acid ester component derived from a styrene-(meth)acrylic acid ester copolymer in the base resin is 20 to 40 mass %. Effect of the Invention
[0010] The present invention provides a method for producing an extruded thermoplastic resin foam board, the base resin of which comprises a polyester resin having a heat of fusion of less than 5 J / g and a styrene-(meth)acrylic acid ester copolymer. By setting the ratio of the polyester resin in the base resin and the ratio of the (meth)acrylic acid ester component derived from the styrene-(meth)acrylic acid ester copolymer in the base resin within specific ranges, it is possible to provide a method for producing an extruded thermoplastic resin foam board that has excellent flame retardancy, can maintain low thermal conductivity over a long period of time, and has excellent thermal insulation properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The extruded thermoplastic resin foam board of the present invention and its manufacturing method will be described below. The extruded thermoplastic resin foam board (hereinafter also referred to as extruded foam board) manufactured by the present invention contains a foamable resin composition obtained by kneading a base resin, a physical foaming agent, and a flame retardant, and has an apparent density of 20 to 50 kg / m 3 The base resin contains a styrene-(meth)acrylic acid ester copolymer and a polyester resin having a heat of fusion of less than 5 J / g.
[0012] (1) Styrene-(meth)acrylic acid ester copolymer The styrene-(meth)acrylic acid ester copolymer used in the base resin is a copolymer of styrene and a lower alkyl ester of (meth)acrylic acid. Specific examples include styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-propyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, and styrene-propyl methacrylate copolymer. Among these, styrene-methyl acrylate copolymer and styrene-methyl methacrylate copolymer, which have a remarkable desired effect, are preferred, and styrene-methyl methacrylate copolymer is more preferred. These styrene-(meth)acrylic acid ester copolymers can be used alone or in combination of two or more. In this specification, "(meth)acrylic acid" is a concept that includes "acrylic acid" and "methacrylic acid", and means one or both of them.
[0013] The content of the (meth)acrylic acid ester component derived from the styrene-(meth)acrylic acid ester copolymer in the base resin is 20 to 40% by mass, preferably 25 to 38% by mass, and more preferably 30 to 36% by mass. Two or more types of styrene-(meth)acrylic acid ester copolymers having different contents of the (meth)acrylic acid ester component can be used in combination, and when two or more types of styrene-(meth)acrylic acid ester copolymers are used in combination, the total of the contents of the (meth)acrylic acid ester component contained in each styrene-(meth)acrylic acid ester copolymer is defined as the content of the (meth)acrylic acid ester component of the styrene-(meth)acrylic acid ester copolymer.
[0014] If the amount of the (meth)acrylic acid ester component in the base resin is too small, the effect of lowering the thermal conductivity of the extruded foam board is small. On the other hand, if the amount of the (meth)acrylic acid ester component is too large, the thermal conductivity of the extruded foam board is sufficient, but the flame retardancy is deteriorated and the flame retardancy standard required for building materials cannot be satisfied. However, the flame retardancy is also affected by the type and amount of the flame retardant used in the production, the density of the extruded foam, and the remaining amount of the blowing agent in the extruded foam. In addition, if the amount of the (meth)acrylic acid ester component in the base resin is within an appropriate range, the styrene-(meth)acrylic acid ester copolymer and the polyester resin with a heat of fusion of less than 5 J / g in the base resin are easily dispersed in layers, which is advantageous in that the thermal conductivity is easily reduced.
[0015] The thermal conductivity reduction effect of styrene-(meth)acrylic acid ester copolymer is due to the (meth)acrylic acid ester component's suppression of the escape of the blowing agent with low thermal conductivity from the extruded foam board and the suppression of the inflow of air with high thermal conductivity into the extruded foam board. Therefore, the thermal conductivity of the extruded foam board increases as the (meth)acrylic acid ester component in the styrene-(meth)acrylic acid ester copolymer decreases. However, if the extruded foam is manufactured using only styrene-(meth)acrylic acid ester copolymer with a high (meth)acrylic acid ester component, it becomes difficult to meet the flame retardant standard.
[0016] Therefore, when using a styrene-(meth)acrylic acid ester copolymer with a large amount of (meth)acrylic acid ester components, it is preferable to use a styrene-(meth)acrylic acid ester copolymer with a small amount of (meth)acrylic acid ester components in combination to set the content of the (meth)acrylic acid ester components within the range described above. The styrene-(meth)acrylic acid ester copolymer with a small amount of (meth)acrylic acid ester components has relatively excellent compatibility with both the styrene-(meth)acrylic acid ester copolymer with a large amount of (meth)acrylic acid ester components and the polyester resin. Therefore, in the case of a resin composition consisting of a styrene-(meth)acrylic acid ester copolymer with a large amount of (meth)acrylic acid ester components, a styrene-(meth)acrylic acid ester copolymer with a small amount of (meth)acrylic acid ester components, and a polyester resin, the resins constituting the obtained extruded foam board form a continuous layer with a complex dispersion state, and it is considered that it is possible to reduce the thermal conductivity of the extruded foam board while maintaining flame retardancy by efficiently suppressing the escape of the foaming agent from the extruded foam board and the inflow of air into the extruded foam board.
[0017] The styrene-(meth)acrylic acid ester copolymer having a high (meth)acrylic acid ester content preferably contains 40 to 75 mass %, more preferably 50 to 75 mass % of the (meth)acrylic acid ester component. The styrene-(meth)acrylic acid ester copolymer having a low (meth)acrylic acid ester content preferably contains 5 mass % or more and less than 40 mass %, more preferably 15 mass % or more and 30 mass % or less of the (meth)acrylic acid ester component.
[0018] The content of the (meth)acrylic acid ester component in the styrene-(meth)acrylic acid ester copolymer can be determined by a known method such as pyrolysis gas chromatography analysis.
[0019] The amount of the styrene-(meth)acrylic acid ester copolymer in the base resin is adjusted by the amount of the (meth)acrylic acid ester component contained in the styrene-(meth)acrylic acid ester copolymer, but is preferably 50% by mass or more, more preferably 60% by mass or more. From the viewpoint of maintaining a low thermal conductivity of the extruded foam board, the amount of the styrene-(meth)acrylic acid ester copolymer in the base resin is preferably 90% by mass or less, more preferably 80% by mass or less.
[0020] (2) Polyester resin Examples of the polyester resin used in the base resin include polyester copolymers produced by polycondensing a dicarboxylic acid component with a diol component, or by a transesterification reaction of a polyester homopolymer and / or a polyester copolymer.
[0021] The polyester resin satisfies the condition that the endothermic peak heat quantity accompanying melting of the polyester resin is less than 5 J / g (including 0) based on the DSC curve obtained by heating the polyester resin to a temperature 30° C. higher than the end of the glass transition at a heating rate of 10° C. / min using a heat flux differential scanning calorimeter (hereinafter referred to as DSC device) based on the heat flux differential scanning calorimetry method in JIS K7122 (1987) at a heating rate of 10° C. / min, maintaining the temperature at that temperature for 10 minutes, cooling the polyester resin to a temperature 50° C. lower than the glass transition temperature at a cooling rate of 10° C. / min, and heating the polyester resin again to a temperature 30° C. higher than the end of the glass transition at a heating rate of 10° C. / min. The endothermic peak heat quantity of this polyester resin is preferably less than 2 J / g (including 0), more preferably less than 1 J / g (including 0), from the viewpoint of the foaming properties of a base resin obtained by blending the polyester resin with a styrene-(meth)acrylic acid ester copolymer.
[0022] An example of the polyester resin is an amorphous polyethylene terephthalate copolymer in which a part of the ethylene glycol component units is replaced with a diol component bulkier than the ethylene glycol component in order to prevent crystallization of the polyethylene terephthalate.
[0023] As the diol component of the polyester resin, aliphatic and aromatic diols (including dihydric phenols) or ester-forming derivatives thereof can be used.
[0024] Examples of the diol component unit in the polyester resin include aliphatic diols such as ethylene glycol, propylene glycol, trimethylene glycol, diethylene glycol, 1,4-butanediol, and neopentyl glycol, alicyclic diols such as 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, and 1,6-cyclohexanediol, aromatic diols such as bisphenol A, and diols having a cyclic ether skeleton such as 3,9-bis(1,1-dimethyl-2-hydroxyethyl)2,4,8,10-tetraoxaspiro[5.5]undecane (hereinafter referred to as spiro glycol), 2-(5-ethyl-5-hydroxymethyl-1,3-dioxane-2-yl)-2-methylpropane-1-ol (hereinafter referred to as dioxane glycol). These diol components may be used alone or in combination of two or more kinds.
[0025] As the polyethylene terephthalate resin modified with the diol component, particularly preferred are spiroglycol-modified polyethylene terephthalate resin, dioxane glycol-modified polyethylene terephthalate resin, neopentyl glycol-modified polyethylene terephthalate resin, and 1,4-cyclohexanedimethanol-modified polyethylene terephthalate resin.
[0026] The polyester resin preferably contains, as a main dicarboxylic acid component unit, an acid component unit consisting of an aromatic dicarboxylic acid or its acid anhydride, or a derivative thereof, such as a terephthalic acid component unit, an isophthalic acid component unit, a naphthalenedicarboxylic acid component unit, or one or more of these dicarboxylic acid components.
[0027] The degree of crystallinity of the polyester resin can be adjusted by using two or more dicarboxylic acid components, such as terephthalic acid and isophthalic acid, and changing the molar ratio of the dicarboxylic acid component units, or by using two or more diol components, such as ethylene glycol and cyclohexanedimethanol, and changing the molar ratio of the diol component units.
[0028] In order for the base resin constituting the extruded foamed insulation board of the present invention to have a preferable morphology, the melt viscosity of the polyester resin is preferably close to the melt viscosity of the styrene-(meth)acrylic acid ester copolymer, and the melt viscosity is preferably 200° C. at a shear rate of 100 sec. -1 The melt viscosity (η) under these conditions is preferably in the range of 500 to 10,000 Pa·s, more preferably 700 to 8,000 Pa·s, and even more preferably 1,000 to 6,000 Pa·s.
[0029] The blending amount of the polyester resin in the base resin is 5 to 50% by mass. If the blending amount of the polyester resin is too small, it is difficult to obtain an extruded foamed insulation board having a large cross-sectional area. On the other hand, if the blending amount of the polyester resin is too large, the melt tension of the base resin decreases, making foam molding difficult, and there is a risk that an extruded foamed insulation board with a high expansion ratio cannot be obtained. In addition, depending on the type of polyester resin, there is a risk that the heat resistance of the obtained extruded foamed insulation board is inferior to that of a conventional general polystyrene resin foamed insulation board. In addition, from the viewpoint of obtaining an extruded foamed insulation board with a large cross-sectional area and having both a high expansion ratio and a high closed cell ratio, the blending amount of the polyester resin in the base resin is preferably 10 to 45% by mass, more preferably 20 to 40% by mass.
[0030] The mass ratio of the styrene-(meth)acrylic acid ester copolymer to the polyester resin in the base resin (styrene-(meth)acrylic acid ester copolymer:polyester resin) is preferably 95:5 to 50:50, more preferably 85:15 to 45:55, and even more preferably 80:20 to 40:60.
[0031] In the present invention, other polymers such as polystyrene resin, polyolefin resin, styrene-based elastomer, and polyphenylene ether resin can be mixed into the base resin according to the purpose of blending, within the scope that does not impair the object of the present invention. The amount of such other polymers used in the base resin (base resin being 100% by mass) is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5% by mass or less. The polystyrene resin refers to a polystyrene resin in which the (meth)acrylic acid ester component is less than 5% by mass and the styrene component is more than 50% by mass.
[0032] (3) Physical foaming agents The physical foaming agent preferably has zero or extremely low ozone depletion potential and low global warming potential. For the purpose of reducing the thermal conductivity of the extruded thermoplastic resin foam insulation board, it is preferable to use at least hydrofluoroolefin (HFO) as the physical foaming agent.
[0033] Specific examples of the HFO include 1,3,3,3-tetrafluoropropene (hereinafter also referred to as HFO1234ze), 1-chloro-3,3,3-trifluoropropene (hereinafter also referred to as HFO1233zd), 1-chloro-2,3,3,3-tetrafluoropropene (hereinafter also referred to as HFO1224yd), 2,3,3,3-tetrafluoropropene (HFO-1234yf), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz), and the like. These blowing agents can be used alone or in combination of two or more. The hydrofluoroolefins have an ozone depletion potential of zero, a very small global warming potential, a low thermal conductivity in a gaseous state, and are non-flammable.
[0034] The HFO is more effective at plasticizing the (meth)acrylic acid ester component derived from the styrene-(meth)acrylic acid ester copolymer in the base resin than a hydrocarbon-based blowing agent, which is thought to facilitate the adjustment of the foaming suitability to a good range in relation to the content of the (meth)acrylic acid ester component, and facilitate the formation of a complex continuous layer between the styrene-(meth)acrylic acid ester copolymer and the polyester resin.
[0035] Furthermore, among the above-mentioned HFOs, from the viewpoint of obtaining an extruded foam board having particularly low thermal conductivity, it is preferable to use one or more HFOs selected from HFO1234ze, HFO1233zd, and HFO1224yd, which are HFOs having low permeability into styrene-(meth)acrylic acid ester copolymers and low thermal conductivity.
[0036] When HFO1234z and HFO1233zd are used as the HFOs, from the viewpoint of an effective amount of HFO remaining in the foamed insulation board after extrusion foaming and providing an extruded foam board with long-term insulation properties, the molar ratio of HFO1234ze to HFO1233zd (HFO1234ze:HFO1233zd) is preferably 20:80 to 80:20, and more preferably 30:70 to 70:30.
[0037] The amount of the HFO added is preferably 0.5 mol or more and 1.5 mol or less per 1 kg of the base resin. Within this range, an effective amount of HFO remains in the foamed insulation board after extrusion foaming, resulting in an extruded foam board with long-term insulation properties. From this viewpoint, the amount of the HFO added is more preferably 0.7 mol or more and 1.4 mol or less, and even more preferably 0.8 mol or more and 1.3 mol or less per 1 kg of the base resin.
[0038] Furthermore, the ratio of the amount of the hydrofluoroolefin added to the total amount of the physical foaming agents added (100 mol %) is preferably 50 mol % or more, more preferably 60 mol % or more, and even more preferably 70 mol % or more.
[0039] It is also preferable to use, as the physical blowing agent, an aliphatic alcohol having 1 to 5 carbon atoms, water, a dialkyl ether having an alkyl chain with 1 to 3 carbon atoms, carbon dioxide, or the like in combination, within a range that does not impair long-term heat insulating properties, because this reduces the amount of HFO added and allows for more inexpensive production.
[0040] In addition, from the viewpoint of easily obtaining an extruded foam board having a low apparent density and a high closed cell ratio, the amount of saturated hydrocarbons having 3 to 5 carbon atoms added as the physical foaming agent is preferably 0.3 mol or less per kg of the base resin, more preferably 0.2 mol or less per kg of the base resin, and even more preferably 0.1 mol% or less per kg of the base resin. Saturated hydrocarbons having 3 to 5 carbon atoms have a weak effect of plasticizing the styrene-(meth)acrylic acid ester copolymer contained in the base resin. Therefore, in the present invention, it is considered that an extruded foam board having a low apparent density and a high closed cell ratio can be easily obtained by reducing the amount of saturated hydrocarbons having 3 to 5 carbon atoms added or not adding them at all.
[0041] (4) Flame retardants As the flame retardant, a bromine-based flame retardant can be suitably used. Examples of the bromine-based flame retardant include tetrabromobisphenol A, tetrabromobisphenol-A-bis(2,3-dibromopropyl ether), tetrabromobisphenol-A-bis(2-bromoethyl ether), tetrabromobisphenol-A-bis(allyl ether), tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol S, tetrabromobisphenol-S-bis(2,3-dibromopropyl ether), hexabromocyclododecane, tetrabromocyclooctane, tris(2,3-dibromopropyl)isocyanurate, tribromophenol, decabromodiphenyl oxide, tris(tribromoneopentyl)phosphate, brominated polystyrene, and brominated styrene-butadiene copolymer. These compounds can be used alone or in combination of two or more. Among the brominated flame retardants, it is particularly preferable to use tetrabromobisphenol-A-bis(2,3-dibromopropyl ether), tetrabromobisphenol-A-bis(2,3-dibromo-2-methylpropyl ether), tris(2,3-dibromopropyl)isocyanurate, and brominated styrene-butadiene copolymers from the viewpoint of high thermal stability and high flame retardancy. These compounds can be used alone or in combination of two or more kinds.
[0042] The amount of the flame retardant is preferably 1 part by mass, more preferably 3 parts by mass, per 100 parts by mass of the base resin, from the viewpoint of satisfying a high level of flame retardancy such as the flammability standard for extruded polystyrene foam insulation boards described in "Test Method A" in the flammability test method of JIS A9521: 2017. Also, from the viewpoint of minimizing the decrease in foamability during extrusion and the decrease in the mechanical properties of the thermoplastic resin foam, the upper limit of the amount of the flame retardant is preferably 10 parts by mass, more preferably 7 parts by mass, per 100 parts by mass of the thermoplastic resin.
[0043] Furthermore, in the present invention, a flame retardant auxiliary can be blended in combination with the flame retardant for the purpose of further improving the flame retardancy of the extruded foam board. Examples of the flame retardant auxiliary include diphenylalkanes and diphenylalkenes such as 2,3-dimethyl-2,3-diphenylbutane, 2,3-diethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 2,4-diphenyl-4-methyl-1-pentene, and 2,4-diphenyl-4-ethyl-1-pentene, triphenylphosphate, cresyl di-2,6-xylenyl phosphate, antimony trioxide, diantimony pentoxide, ammonium sulfate, zinc stannate, cyanuric acid, isocyanuric acid, triallyl isocyanurate, melamine cyanurate, melamine, melam, and melem, as well as inorganic compounds such as silicone compounds, boron oxide, zinc borate, and zinc sulfide, as well as red phosphorus, ammonium polyphosphate, and phosphorus compounds such as phosphazene. These compounds can be used alone or in combination of two or more.
[0044] The method of blending the flame retardant into the thermoplastic resin includes a method of feeding a predetermined proportion of the flame retardant together with the thermoplastic resin to a raw material feed section provided upstream of the extruder and kneading the flame retardant together with the thermoplastic resin in the extruder. In addition, the flame retardant can be fed into the thermoplastic resin melt from a flame retardant feed section provided in the extruder. When feeding the flame retardant into the extruder, a method of feeding a dry blend of the flame retardant and the thermoplastic resin into the extruder, a method of feeding a liquid flame retardant that has been heated and melted in advance into the extruder, or a method of preparing a master batch containing the flame retardant and the thermoplastic resin as the base resin and feeding the master batch into the extruder can be adopted. In particular, from the viewpoint of dispersibility, it is preferable to adopt a method of preparing a master batch containing the flame retardant and feeding the master batch into the extruder. The blending method of the flame retardant auxiliary is the same as the above method.
[0045] (5) Heat insulation improver In the present invention, the heat insulation can be further improved by blending a heat insulation improver with the base resin. Examples of heat insulation improvers include metal oxides such as titanium oxide, metals such as aluminum, ceramics, fine powders such as carbon black and graphite, infrared shielding pigments, and hydrotalcite. These can be used alone or in combination. The amount of the heat insulation improver added is in the range of 0.5 to 5 parts by mass, preferably 1 to 4 parts by mass, per 100 parts by mass of the base resin.
[0046] (6) Other additives In the present invention, various additives such as cell regulators, colorants such as pigments and dyes, heat stabilizers, and fillers may be appropriately blended with the base resin, if necessary.
[0047] As the bubble regulator, for example, inorganic powders such as talc, kaolin, mica, silica, calcium carbonate, barium sulfate, aluminum oxide, clay, bentonite, diatomaceous earth, and conventionally known chemical foaming agents such as azodicarbodiamide can be used. Among them, talc is preferable because it does not inhibit flame retardancy and is easy to adjust the bubble size. In particular, it is preferable to use talc having a particle size of 0.1 to 20 μm, more preferably 0.5 to 15 μm, as specified in JIS Z8901 (2006). The amount of the bubble regulator to be added varies depending on the type of the bubble regulator, the target bubble size, and the like, but is generally 0.01 to 8 parts by mass, more preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the base resin.
[0048] The method for producing the extruded thermoplastic resin foam plate of the present invention is, for example, a method for producing an extruded thermoplastic resin foam plate by extruding and foaming the foamable resin composition obtained by kneading the thermoplastic resin, the physical foaming agent, and the flame retardant through a die attached to the outlet of an extruder, and forming it into a plate shape. Specifically, the extruded thermoplastic resin foam plate is produced by feeding the thermoplastic resin and additives added as necessary to an extruder, further feeding a physical foaming agent through a physical foaming agent supply port, extruding the molten kneaded product obtained by melt-kneading them from a die lip at the tip of the extruder under atmospheric pressure, and then forming it into a predetermined shape (plate shape) with a forming tool (such as a guider). The forming tool can be, for example, a shaping device consisting of a pair of upper and lower polytetrafluoroethylene plates.
[0049] The physical properties of the extruded thermoplastic resin foam board will be described in detail below. [Apparent Density] The apparent density of the extruded thermoplastic resin foam board of the present invention has a lower limit of 20 kg / m from the viewpoint of improving the production stability and mechanical strength of the foam board. 3 It is preferable that the thickness is 25 kg / m 3 More preferably, it is 30 kg / m 3 From the viewpoint of improving the heat insulating property and ensuring the light weight, the upper limit of the apparent density is 50 kg / m 3 Preferably, it is 45 kg / m 3 More preferably, it is 40 kg / m 3 It is even more preferable that:
[0050] Thickness The thickness of the extruded foam board is appropriately set according to the purpose of use, and is not particularly limited, but from the viewpoint of use as a heat insulating material, it is preferably 25 mm or more, more preferably 35 mm or more, and even more preferably 45 mm or more. The upper limit of the thickness is about 150 mm. In the present invention, since the base resin contains a polyester resin, it is easy to obtain the above-mentioned thick extruded foam board.
[0051] [Closed bubble rate] From the viewpoint of long-term heat insulation, the closed cell ratio of the extruded foam board is preferably 85% or more, more preferably 90% or more, and even more preferably 92% or more.
[0052] The closed cell ratio of the extruded foam board is measured by cutting out cut samples from a total of five randomly selected locations of the extruded foam board, determining the closed cell ratio for each measurement sample, and adopting the arithmetic average value of the closed cell ratio at the five locations. The cut sample is a sample without a skin cut into a size of 45 mm length x 20 mm width x 25 mm thickness from the extruded foam board. If the sample is too thin to cut out a 25 mm sample in the thickness direction, for example, two samples (cut samples) cut into a size of 45 mm length x 20 mm width x 12.5 mm thickness are stacked and measured. The closed cell ratio S (%) is calculated by the following formula (1) using the true volume Vx of the thermoplastic resin foam measured using an air comparison specific gravity meter (for example, Toshiba Beckman Co., Ltd., air comparison specific gravity meter, model: 930) according to procedure C of ASTM-D2856-70.
[0053] S(%)=(Vx-W / ρ)×100 / (VA-W / ρ)···(1) Vx: The true volume (cm) of the cut sample determined by measurement using an air-comparison type hydrometer 3 ) (This corresponds to the sum of the volume of the resin constituting the cut sample of the foam and the total volume of the air bubbles in the closed cell portion of the cut sample.) VA: Apparent volume (cm) of the cut sample calculated from the outer dimensions of the cut sample used in the measurement 3 ) W: Total weight of cut sample used for measurement (g) ρ: Density of the base resin constituting the thermoplastic resin foam (g / cm 3 )
[0054] [Thermal Conductivity] The thermal conductivity of the extruded foam board of the present invention 10 days after production is preferably 0.024 W / (m·K) or less, more preferably 0.023 W / (m·K) or less, and even more preferably 0.022 W / (m·K) or less.
[0055] The extruded foam of the present invention preferably has a thermal conductivity of 0.028 W / (m K) or less 1500 days after production, more preferably 0.027 W / (m K) or less, and even more preferably 0.026 W / (m K) or less. From the viewpoint of the long-term insulation properties of the extruded foam board, the smaller the difference between the thermal conductivity 10 days after production, 1500 days after production, and the thermal conductivity 10 days after production, the better.
[0056] The thermal conductivity is measured by cutting test pieces (length 200 mm × width 200 mm × thickness) without any skin from the extruded foam board immediately after production, storing the test pieces for 10 days in an atmosphere of 23°C and 50% humidity, and storing the test pieces for 10 days and 1500 days in accordance with the flat plate heat flow meter method (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C) described in JIS A 1412-2 (1999).
[0057] The thermal conductivity 1500 days after production is measured on samples that have been subjected to accelerated testing in accordance with JIS A1486 (2014). According to this method, for example, the thermal conductivity measured 60 days after production using a sample obtained by slicing a 50 mm thick extruded foam board to a thickness of 10 mm corresponds to the thermal conductivity of the extruded foam board approximately 1500 days after production. EXAMPLES
[0058] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way. The thermoplastic resins, flame retardants, cell regulators and physical foaming agents used in the examples and comparative examples are shown below.
[0059] <Thermoplastic resin> (Styrene-(meth)acrylic acid ester copolymer) (MS raw material) (Hereinafter, the (meth)acrylic acid ester component derived from the styrene-(meth)acrylic acid ester copolymer may be referred to as the M component.) MS1: styrene-methyl (meth)acrylate copolymer, manufactured by Toyo Styrene Co., Ltd., MS600 M component-60% by mass / styrene component-40% by mass, melt viscosity (200°C, 100 sec -1 ) 2570 Pa·s, air permeability coefficient 5.9 (cc·mm / (m 2 ·day·atm)) MS2: Styrene-methyl (meth)acrylate copolymer, manufactured by Toyo Styrene Co., Ltd., MS200 M component-20% by mass / styrene component-80% by mass, melt viscosity (200°C, 100 sec -1 ) 1750 Pa·s, air permeability coefficient 22.9 (cc·mm / (m 2 ·day·atm))
[0060] (Polyester resin) (PET raw material) PET1: (spiroglycol) modified PET, Mitsubishi Gas Chemical Co., Ltd. Altester 3012, dicarboxylic acid component - terephthalic acid 100% by mass, glycol component - spiroglycol (SPG) / ethylene glycol (EG) = 30% by mass / 70% by mass, endothermic peak heat quantity 0 J / g, melt viscosity (200 ° C, 100 sec -1 ) 2000 Pa·s, air permeability coefficient 4.1 (cc·mm / (m 2 ·day·atm)) PET2: Glycol-modified PET, SK Chemicals PN100, dicarboxylic acid component - terephthalic acid 100% by mass, glycol component - 1,4-cyclohexanedimethanol (CHDM) / ethylene glycol (EG) = 43% by mass / 57% by mass, endothermic peak heat quantity 0 J / g, melt viscosity 3170 Pa s, air permeability coefficient 2.4 (cc mm / (m 2 ·day·atm))
[0061] Tables 1 and 2 show the type, manufacturer, product name, melt viscosity, and air permeability coefficient of each of the above resins.
[0062] [Table 1]
[0063] [Table 2]
[0064] The melt viscosity of the resin was measured by the following method using a Capillograph 1D manufactured by Toyo Seiki Seisakusho Co., Ltd. A capillary with a hole diameter of 1.0 mm and a length of 10.0 mm was attached to the tip of a cylinder with a diameter of 9.55 mm and a length of 350 mm. After heating the cylinder and the capillary to 200°C, the cylinder was filled with a measurement sample (resin pellets), which was then sufficiently melted by preheating for 4 minutes and then heated at a shear rate of 100 sec. -1 The melt viscosity of the resin was measured under the above conditions.
[0065] The air permeability coefficient of the resin was measured using a gas permeability tester BT-3 manufactured by Toyo Seiki Co., Ltd. in accordance with JIS K7126-1:2006 Plastics - Films and sheets - Gas permeability test method - Part 1: Differential pressure method.
[0066] <Flame retardants> As a flame retardant, a bromide butadiene-styrene block copolymer, "Emerald Innovation 3000" manufactured by LANXESS KK, was used.
[0067] <Foam regulator> Talc "Hi-Filler #12" manufactured by Matsumura Sangyo Co., Ltd. was used as the bubble adjusting agent.
[0068] <Physical foaming agent> Blowing agent 1: Hydrofluoroolefin (HFO): 1,3,3,3-tetrafluoropropene (HFO-1234ze) Blowing agent 2: Hydrofluoroolefin (HFO): 1-chloro-3,3,3-trifluoropropene (HFO1233zd) Blowing agent 3: Ethanol (EtOH) Blowing agent 4: Water
[0069] The mixed resin, flame retardant, and cell regulator were fed to the extruder in the blending ratios shown in Tables 3 and 4 below (where the total blending amount of the MS raw material and the PET raw material is 100% by mass), and the physical foaming agent was fed from the physical foaming agent feed port, melted and kneaded, and the melt-kneaded product was extruded from the die lip at the tip of the extruder under atmospheric pressure under the conditions shown in Tables 3 and 4, and then molded into a predetermined shape (plate-like) by a shaping device (guider), which is a molding tool, to obtain a base plate with a thickness of 55 mm. The surface skins on both sides of the base plate were then evenly scraped to produce the plate-like thermoplastic resin extruded foam plates of Examples 1 to 6 and Comparative Examples 1 to 3, each with a width of 600 mm, a length of 2000 mm, and a thickness of 50 mm.
[0070] [Table 3]
[0071] [Table 4]
[0072] The extruded foam boards thus produced were measured for apparent density, closed cell ratio, and cell structure (cell diameter in the thickness direction, cell deformation rate) by the following methods. <Apparent density> The apparent density was measured in accordance with JIS K6767 (1999). Rectangular samples measuring 50 mm long x 50 mm wide x 50 mm thick were cut from three locations, namely the widthwise center and both widthwise ends, of each extruded foam board, and the apparent density of each sample was measured. The arithmetic mean of the measurements at the three locations was used as the apparent density.
[0073] <Closed bubble rate> The cut samples were cut from three locations, the center and both ends of the width direction of the extruded foam plate, to prepare measurement samples, and the closed cell ratio of each measurement sample was measured, and the arithmetic average value of the closed cell ratio of the three locations was used. The cut samples were cut from the extruded foam plate to a size of 25 mm length x 25 mm width x 25 mm thickness. The independent bubble ratio of the sample was measured using an air comparison pycnometer (Model: 930, manufactured by Toshiba Beckman Co., Ltd.) in accordance with Procedure C of ASTM-D2856-70, and was determined from the above formula (1). The arithmetic mean value at three locations was taken as the independent bubble ratio.
[0074] <Flammability evaluation> For the thermoplastic resin extruded foam board after 7 days from manufacturing, a flammability test was conducted in accordance with Measuring Method A of the flammability test method of JIS A9521:2017. For the measurement, 5 test pieces were randomly cut out from one extruded foam board, and the flammability was evaluated according to the following criteria. 〇: In all test pieces, the flame goes out within 3 seconds, there is no remaining dust, and it does not burn beyond the combustion limit line. ×: The average combustion time of the 5 test pieces exceeds 3 seconds.
[0075] <Surface property> The following evaluation was visually conducted for the surface property. 〇: A raw board with a smooth surface was stably manufactured, and a good extruded foam board was obtained. ×: Cracks were observed on the surface of the raw board, and a good extruded foam board could not be stably obtained.
[0076] <LOI (Oxygen index)> The extruded foam board immediately after manufacturing was transferred to a room with a temperature of 23°C and a relative humidity of 50%, and after leaving it in that room for 4 weeks, a test piece was cut out from the extruded foam board, measured in accordance with JIS K7201-2007, and the flammability was evaluated. As the type of heat source of the igniter, liquefied petroleum gas (LPG) was used, the ignition procedure used Method A, and the test piece was made to stand independently at a predetermined position in the testing machine. The test was conducted at a temperature of 23°C and a humidity of 50% at the test location.
[0077] <Thermal conductivity> From the extruded foam board immediately after manufacturing, a test piece with no skin having a length of 200 mm × width of 200 mm × thickness of 50 mm was cut out, and for the test piece stored for 10 days in an atmosphere with a temperature of 23°C and a humidity of 50%, the thermal conductivity was measured based on JIS A1412-2 (1999) Flat plate heat flow meter method (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C).
[0078] The thermal conductivity after 1500 days of manufacture was measured on a test piece subjected to test method A of the long-term accelerated change test of thermal resistance in accordance with JIS A1486 (2014). Specifically, a test piece without a molded skin measuring 200 mm x 200 mm x 10 mm was cut evenly from both sides of the center of a 50 mm-thick extruded foam board immediately after manufacture, and stored in a constant temperature and humidity room at a temperature of 23°C and a relative humidity of 50%. The thermal conductivity of the test piece after 60 days of manufacture (corresponding to 1500 days after the manufacture of a 50 mm-thick extruded foam board) was measured based on the flat plate heat flow meter method (two heat flow meter method, high temperature side 38°C, low temperature side 8°C, average temperature 23°C) described in JIS A1412-2 (1999).
[0079] [Table 5]
[0080] [Table 6]
[0081] <Evaluation Results> From the evaluation and measurement results of the physical properties shown in Table 5, it was confirmed that the extruded foam boards of Examples 1 to 6 exhibited good flame retardancy and maintained low thermal conductivity even after 1,500 days, because the base resin contained a styrene-(meth)acrylic acid ester copolymer and a polyester resin having a heat of fusion of less than 5 J / g based on JIS K7122-1987, the content of the polyester resin in the base resin was within the range of 5 to 50 mass%, and the content of the (meth)acrylic acid ester component in the base resin was within the range of 20 to 40 mass%, as shown in Table 3.
[0082] In contrast, the extruded foams of Comparative Examples 1 to 3, in which the content of the (meth)acrylic acid ester component in the base resin was not within the range of 20 to 40% by mass, either had poor flame retardancy or were unmoldable.
Claims
1. The foamable resin composition is extruded and foamed by kneading a base resin, a physical foaming agent, and a flame retardant, and molded into a plate shape using a molding tool. 3 A method for producing an extruded thermoplastic resin foam board having a thickness of 10 to 150 mm, comprising the steps of: the base resin comprises a styrene-(meth)acrylic acid ester copolymer and a polyester resin having a heat of fusion of less than 5 J / g based on JIS K7122-1987; The blending amount of the polyester resin in the base resin is 5 to 50% by mass, the content of the (meth)acrylic acid ester component derived from a styrene-(meth)acrylic acid ester copolymer in the base resin is 20 to 40% by mass, The physical blowing agent comprises a hydrofluoroolefin, A method for producing an extruded thermoplastic resin foam board, wherein the ratio of the amount of said hydrofluoroolefin added to the total amount of said physical foaming agents added (100 mol %) is 50 mol % or more.
2. The method for producing an extruded thermoplastic resin foam board as described in claim 1, characterized in that the amount of the hydrofluoroolefin added is 0.5 mol or more and 1.5 mol or less per 1 kg of the base resin.
3. The method for producing an extruded thermoplastic resin foam board according to claim 1 or 2, characterized in that the hydrofluoroolefin contains 1,3,3,3-tetrafluoropropene and 1-chloro-3,3,3-trifluoropropene, and the molar ratio of 1,3,3,3-tetrafluoropropene to 1-chloro-3,3,3-trifluoropropene is 20:80 to 80:20.
Citation Information
Patent Citations
Method for producing styrenic resin foam
JP2008133424A
Styrene resin-extruded / foamed plate
JP2009215504A
Heat insulation plate of extruded thermoplastic resin foam
JP2011219631A
Thermoplastic resin extrusion foamed heat insulating plate
JP2013082805A
Thermoplastic resin foam body
JP2019189666A