New granulated spherical graphite, secondary battery containing the same as negative electrode active material, and method for producing the granulated spherical graphite

A novel method for producing granulated spherical graphite through pulverization, mixing, and dual heat treatments addresses inefficiencies in existing processes, achieving high-performance lithium ion batteries with improved discharge capacity and efficiency.

JP7577875B2Active Publication Date: 2024-11-05イージーマテリアルズ カンパニー リミテッド
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023572552
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-29
Filing Date
2021-10-13
Publication Date
2024-11-05
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

Existing methods for producing crystalline spherical graphite from flaky natural graphite are inefficient, resulting in low yield and high manufacturing costs, with over 70% of the material being discarded, and the produced graphite does not meet the requirements for high performance lithium ion secondary batteries.

Method used

A method involving pulverization, mixing with pitch, solvent addition, granulation and spheroidization, additional pitch coating, and dual heat treatments is employed to produce granulated spherical graphite with specific surface area and crystallinity, enabling mass production and use as a negative electrode active material.

Benefits of technology

The method produces granulated spherical graphite with excellent crystallinity and uniform particle size, enhancing the initial discharge capacity and efficiency of lithium ion batteries, making it suitable for mass production at lower costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577875000003
    Figure 0007577875000003
  • Figure 0007577875000004
    Figure 0007577875000004
  • Figure 0007577875000005
    Figure 0007577875000005
Patent Text Reader

Abstract

The present invention relates to a novel method for producing granulated spherical graphite, and more specifically, to a novel method for producing granulated spherical graphite, in which, when spherical graphite having a particle size of several tens of μm is produced by a mechanical process from scaly natural graphite, composite spherical graphite is produced from natural graphite that is discarded in the mechanical process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a new granulated spherical graphite, a battery containing the same as a negative electrode active material, and a method for producing the granulated spherical graphite. Specifically, the present invention relates to granulated spherical graphite having a particle size of several μm produced through a spheroidizing process from scaly natural graphite and pitch which is amorphous carbon, a battery which uses the granulated spherical graphite as a negative electrode active material, and a method for producing the granulated spherical graphite. [Background technology]

[0002] In recent years, with the development of portable information devices such as mobile phones due to the emergence of laptops and 5G communications, the demand for batteries has rapidly increased, and the applications of batteries have also expanded. In response to this situation, lithium-ion secondary batteries that satisfy the requirements for small size and weight reduction are required. To achieve high performance in such lithium secondary batteries, carbonaceous materials such as graphite are used as the negative electrode active material of the battery.

[0003] The graphite of the carbonaceous material used in the negative electrode active material for the secondary battery should be used in a spherical shape, and more preferably in a crystalline spherical shape, for the charge / discharge efficiency of the battery. There are various methods for producing the spherical graphite used in the negative electrode active material for the secondary battery.

[0004] Meanwhile, generally, the higher the crystallinity of graphite, the more regularly the crystallinity grows and the more scaly it appears. As a result, one method for obtaining crystalline spherical graphite, which is preferable as a negative electrode active material for secondary batteries, is to process scaly natural graphite collected from natural resources into a spherical shape through mechanical methods such as crushing, refining, grinding, and sorting. The yield of crystalline spherical graphite obtained from scaly natural graphite by such mechanical methods is about 30% or less, and the remaining 70% or more is discarded during the mechanical process.

[0005] Although flake natural graphite can be purchased inexpensively, the production efficiency of crystalline spherical graphite from flake natural graphite is low at about 30%, as mentioned above, and ultimately, the production of crystalline spherical graphite is costly.

[0006] Therefore, there is a need to develop a new manufacturing method that can increase the utility of discarded flake natural graphite, produce granulated spherical graphite with high efficiency, is relatively easy to produce, and can be mass-produced. Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention provides a method for producing granulated spherical graphite for use as a negative electrode active material, which is highly efficient, low-cost, easy to produce, and capable of mass production using discarded natural graphite.

[0008] Another object of the present invention is to provide a method for producing granulated spherical graphite for use as a negative electrode active material, which is excellent in initial discharge capacity and initial efficiency for batteries, and to provide granulated spherical graphite obtained by this production method.

[0009] Another object of the present invention is to provide a method for producing granulated spherical graphite having excellent crystallinity, and to provide granulated spherical graphite obtained by this production method.

[0010] It is still another object of the present invention to provide a method for producing a crystalline graphite having a specific surface area of ​​4.5 m2 after the crystallization of the granulated spherical graphite. 2 The object of the present invention is to provide a method for producing granulated spherical graphite having a uniform particle size of 0.1 / g or less and an excellent degree of crystallinity such that d002 (nm, graphite layer distance), which indicates the degree of crystallinity of the granulated spherical graphite particles after crystallization, is 0.338 or less, and to provide granulated spherical graphite obtained by this production method. [Means for solving the problem]

[0011] In order to achieve the above-mentioned object, the present invention provides a method for producing granulated spherical graphite, comprising the steps of: (a) a step of pulverizing flake-like natural graphite and pitch, respectively ("respective pulverization steps of natural graphite and pitch"); (b) a mixing step of the micronized natural graphite and the micronized pitch, respectively, of said step (a) ("the natural graphite and pitch mixing step"); (c) adding a solvent to the mixture of step (b) (the "solvent mixing step"); (d) spheronizing the mixture of step (c) to produce a spheronized first graphite composite (the "spheronization step"); (e) adding and mixing-coating additional pitch onto the first graphite composite material that has been granulated and spheroidized in step (d) (the "additional pitch adding and mixing-coating step"); (f) further mixing the mixture of step (e) to complete the mixing, thereby producing a secondary composite in which the outside of the spheroidized first graphite composite is coated with pitch ("completion of further mixing step"). (g) subjecting the secondary composite of step (f) to a first heat treatment (the "first heat treatment step"); and (h) after the primary heat treatment in step (g), cooling to room temperature and then subjecting the mixture to a secondary heat treatment;

[0012] The granulated spherical graphite produced by the method for producing granulated spherical graphite according to the present invention, which includes the steps (a) to (h), can be used to produce a negative electrode active material for a secondary battery. In relation to the present invention, the following is further disclosed: [1] (a) a step of pulverizing flake-like natural graphite and pitch, respectively ("respective pulverization steps of natural graphite and pitch"); (b) a mixing step of the micronized natural graphite and the micronized pitch, respectively, of said step (a) ("the natural graphite and pitch mixing step"); (c) adding a solvent to the mixture of step (b) (the "solvent mixing step"); (d) spheronizing the mixture of step (c) to produce a spheronized first graphite composite (the "spheronization step"); (e) adding and mixing-coating additional pitch onto the first graphite composite material that has been granulated and spheroidized in step (d) (the "additional pitch adding and mixing-coating step"); (f) further mixing the mixture of step (e) to complete the mixing, thereby producing a secondary composite in which the outside of the spheroidized first graphite composite is coated with pitch ("completion of further mixing step"). (g) subjecting the secondary composite of step (f) to a first heat treatment (the "first heat treatment step"); and (h) after the primary heat treatment in step (g), cooling to room temperature and then subjecting the mixture to a secondary heat treatment. [2] The method for producing granulated spherical graphite according to [1], wherein the "flake-like natural graphite" in step (a) has an average particle size of 5 μm to 500 μm, the pulverization of the natural graphite is carried out using a high-speed mechanical milling device under a pressure of 5 bar to 10 bar, and the average particle size of the pulverized natural graphite particles is 1 μm to 10 μm. [3] The method for producing granulated spherical graphite according to [1], wherein the pulverization of the pitch in step (a) is carried out using a high-speed mechanical milling device under a pressure of 5 bar to 10 bar, and the average particle size of the pulverized pitch is 0.5 μm to 10 μm. [4] The method for producing granulated spherical graphite according to [1], wherein the mixing weight percentage of the finely powdered natural graphite and the finely powdered pitch in step (b) is 99:1 to 50:50. [5] The method for producing granulated spherical graphite according to [1], wherein the solvent in the solvent mixing step (c) is one or more selected from the group consisting of mineral oils such as kerosene, heavy oil, light oil, and paraffin oil; hydrocarbon solvents such as toluene and decane; and mixtures thereof. [6] The method for producing granulated spherical graphite according to [1], characterized in that the amount of solvent used in the solvent mixing step (c) is 10 to 50 parts by weight per 100 parts by weight of the "mixture of finely powdered natural graphite and finely powdered pitch." [7] The method for producing granulated spherical graphite according to [1], characterized in that the granulation and spheronization in the step (d), the "granulation and spheronization step", is carried out at a rotational force of more than 4,000 m / min and up to 8,000 m / min for an operation time of 100 seconds to 600 seconds. [8] The method for producing granulated spherical graphite according to [1], wherein the amount of the finely divided pitch added in the step (e) of "additional pitch addition and mixed coating step" is more than 25% by weight based on the total weight of the finely divided natural graphite, the finely divided pitch, and the finely divided pitch added in the step (a). [9] The method for producing granulated spherical graphite according to [1], wherein the additional mixing in the step (f), which is the "step of completing additional mixing", is performed by mixing the spheroidized first graphite composites formed in the step (e) in a high-speed mixer at a speed of 1,000 rpm to 3,000 rpm for one minute or more.

[10] The method for producing granulated spherical graphite according to [1], characterized in that the heat treatment conditions in the step (g), the "primary heat treatment step", are at 1,000°C or higher for 30 minutes or more.

[11] The method for producing granulated spherical graphite described in [1], wherein the heat treatment conditions of the "secondary heat treatment step" which is step (h) are 2,000°C or higher for 30 minutes or more.

[12] Granulated spherical graphite, characterized by being produced by the production method according to any one of [1] to

[11] .

[13] A granulated spheroidal graphite produced using natural graphite and amorphous carbon pitch, characterized in that the ratio of crystalline carbon to natural graphite in the granulated spheroidal graphite is more than 15%.

[14] The specific surface area of ​​the granulated spherical graphite particles is 4.5m 2 / g or less, and d002 (nm, distance between graphite layers), which indicates the crystallinity of graphite particles, is 0.338 or less.

[15] A secondary battery using the granulated spherical graphite according to

[12] as a negative electrode active material.

[16] A secondary battery using the granulated spherical graphite according to

[13] or

[14] as a negative electrode active material. Effect of the Invention

[0013] The novel method for producing granulated spherical graphite according to the present invention has the advantages of being low cost, highly efficient, and easy to produce, allowing for mass production.

[0014] In addition, the novel method for producing granulated spherical graphite according to the present invention can produce granulated spherical graphite that can be used as a negative electrode active material having excellent crystallinity and a uniform particle size. Due to these characteristics, when the granulated spherical graphite produced by the method for producing granulated spherical graphite according to the present invention is used as a negative electrode active material of a battery, it has the advantage that the initial discharge capacity and initial efficiency of the battery are excellent. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is an SEM of a granulated spherical graphite aggregate produced by Example 1 of the method for producing granulated spherical graphite according to the present invention. [Diagram 2] FIG. 2 is an SEM image of the granulated spherical graphite aggregates produced in Example 2 of the present invention. [Diagram 3] FIG. 3 is an SEM image of the granulated spherical graphite aggregates produced in Comparative Example 2 of the present invention.

[0016] (Best Mode for Carrying Out the Invention) Please note that in the following description, only the parts necessary for understanding the embodiments of the present invention will be described, and the description of other parts will be omitted to the extent that it does not deviate from the gist of the present invention.

[0017] The terms and words used in the following specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted according to the meaning and concept that corresponds to the technical idea of ​​the present invention in accordance with the principle that the inventor can appropriately define the concept of the term in order to describe his / her invention in the best possible way. Therefore, the embodiment described in this specification and the configuration shown in the drawings are only the most preferred embodiment of the present invention and do not represent the entire technical idea of ​​the present invention, so it should be understood that there are various equivalents and modifications that can replace them at the time of this application.

[0018] The present invention provides a method for producing granulated spherical graphite which is capable of mass production at low cost due to high efficiency and which produces granulated spherical graphite with excellent crystallinity and uniform particle size.

[0019] A method for producing granulated spherical graphite according to one embodiment of the present invention includes the steps of: (a) a step of pulverizing flake-like natural graphite and pitch, respectively ("respective pulverization steps of natural graphite and pitch"); (b) a mixing step of the micronized natural graphite and the micronized pitch, respectively, of said step (a) ("the natural graphite and pitch mixing step"); (c) adding a solvent to the mixture of step (b) (the "solvent mixing step"); (d) spheronizing the mixture of step (c) to produce a spheronized first graphite composite (the "spheronization step"); (e) adding and mixing-coating additional pitch onto the first graphite composite material that has been granulated and spheroidized in step (d) (the "additional pitch adding and mixing-coating step"); (f) further mixing the mixture of step (e) to complete the mixing, thereby producing a secondary composite in which the outside of the spheroidized first graphite composite is coated with pitch ("completion of further mixing step"). (g) subjecting the secondary composite of step (f) to a first heat treatment (the "first heat treatment step"); and (h) after the primary heat treatment in step (g), cooling to room temperature and then subjecting the mixture to a secondary heat treatment;

[0020] The steps (a) to (h) will be described in detail below.

[0021] In the method for producing granulated spherical graphite according to the present invention, the "flake-like natural graphite" in step (a) may have an average particle size of 5 μm to 500 μm, preferably 5 μm to 100 μm. If the average particle size exceeds 500 μm, the overall production time increases, which is economically undesirable.

[0022] In the method for producing granulated spherical graphite according to the present invention, the pulverization of natural graphite in step (a) is carried out using a high-speed mechanical milling device such as a hammer mill, a jet mill, a bead mill, or a mixture thereof, and preferably a jet mill is used. In this case, the operating pressure of the hammer mill, jet mill, and bead mill is set to a pressure required for the mill used, and the pressure when pulverizing using a jet mill is 5 bar to 10 bar, and preferably 7 bar to 10 bar.

[0023] Furthermore, natural graphite particles having an average particle size of 1 μm to 10 μm, preferably 1 μm to 5 μm, are produced from the above-mentioned scaly natural graphite through a pulverization process using a jet mill, etc. The natural graphite particles having an average particle size of 1 μm to 10 μm produced in this manner are called "pulverized natural graphite."

[0024] The pitch in step (a) is a petroleum-based pitch, a coal-based pitch, or a polymer resin, and is preferably a petroleum-based pitch.

[0025] The pitch is pulverized by a high-speed mechanical milling device such as a hammer mill, a jet mill, a bead mill, or a mixture thereof, preferably a jet mill. In this case, the operating pressure of the hammer mill, jet mill, and bead mill is required for each mill, and the pressure when pulverizing using a jet mill is 5 bar to 10 bar, preferably 6 bar to 10 bar.

[0026] Furthermore, pitch particles having an average particle size of 0.5 μm to 10 μm, preferably 0.5 μm to 5 μm, are produced from the above-mentioned pitch through a pulverization process using a jet mill, etc. Such pitch particles having an average particle size of 0.5 μm to 10 μm are called "pulverized pitch."

[0027] In the method for producing granulated spherical graphite according to the present invention, the mixing weight percentage of the "powdered natural graphite" and the "powdered pitch" in the "mixing step of natural graphite and pitch" of step (b) is 99:1 to 50:50, and preferably 99:1 to 70:30. If it is outside this range, the crystallization of the completed granulated spherical graphite may be low, and the particles of the granulated spherical graphite may be broken during a process such as pressing during the process of producing the negative active material, resulting in an unstable process of producing the negative active material.

[0028] The mixing time of the mixing step is the time until the "finely divided natural graphite" and the "finely divided pitch" are completely mixed, and can be determined depending on the amount used. The preferred mixing time is 1 hour or more.

[0029] The "solvent mixing step" of step (c) is a step of adding a solvent to the mixture of "micronized natural graphite" and "micronized pitch" from step (b) and further mixing them.

[0030] The solvent can be any solvent capable of dissolving pitch, and is preferably one or more selected from the group consisting of mineral oils such as kerosene, heavy oil, light oil, and paraffin oil; hydrocarbon solvents such as toluene and decane; and mixtures thereof, and is more preferably coal-based oils such as kerosene, light oil, heavy oil, and paraffin oil.

[0031] The amount of the solvent used in the "solvent mixing step" of step (c) is 10 to 50 parts by weight, preferably 20 to 40 parts by weight, and more preferably 20 to 30 parts by weight, per 100 parts by weight of the "mixture of finely powdered natural graphite and finely powdered pitch."

[0032] If the amount of the solvent used is less than 10 parts by weight, the mixing of the finely powdered natural graphite and the finely powdered pitch becomes poor, resulting in partial inspheroidization and a large amount of fine natural graphite that is not granulated, thereby decreasing the efficiency of producing granulated spherical graphite. If the amount of the liquid pitch used is more than 50 parts by weight, the average particle size of the produced granulated spherical graphite becomes large, which may cause a problem in the production yield of granulated spherical graphite particles having an appropriate particle diameter that can be used as a negative electrode active material for secondary batteries, etc.

[0033] The mixing in step (c) is carried out using a mixer such as a screw mixer, and the mixing time is the time required for the mixture of "finely powdered natural graphite and finely powdered pitch" to be completely mixed into the solvent, and can be determined depending on the amount used. The preferred mixing time is 1 hour or more.

[0034] In the method for producing granulated spheroidal graphite according to the present invention, the "spheroidizing step" of step (d) is a step for producing a "first composite of finely powdered natural graphite and finely powdered pitch", which is a first graphite composite, by granulating the mixture of step (c) using a spheroidizing device.

[0035] The granulation and spheronization device is a rotatable device known in the art, and is preferably a spheronization device having a rotor with blades that applies friction and shear stress to the reduced pressure treated mixture when rotating. It is believed that the spheronization of the fine graphite occurs due to the friction and shear stress applied to the reduced pressure treated mixture.

[0036] The granulation and spheroidizing device operates at a rotational force of more than 4,000 m / min to 8,000 m / min, preferably at a rotational force of 4,500 m / min to 6,000 m / min. The operation time at the rotational force is 100 seconds to 600 seconds, preferably 150 seconds to 400 seconds. If the rotational force is smaller than the above range, a lot of fine powder is generated during the production of the "first composite of finely powdered natural graphite and finely powdered pitch", and the specific surface area of ​​the whole particles of the finally produced granulated spheroidal graphite becomes large (see Comparative Example 2). Also, even if the rotational force exceeds the above range, it becomes difficult to finally produce granulated spheroidal graphite having an appropriate level of specific surface area. This reduces the production efficiency of granulated spheroidal graphite for the negative electrode active material of secondary batteries, which can show excellent effects in terms of initial discharge capacity, etc.

[0037] In addition, if the granulation and spheroidization time is shorter than the above-mentioned operating time range, the efficiency of granulation and spheroidization of graphite becomes low, whereas if the operating time is longer than the above-mentioned operating time range, the granulated graphite particles become large, making it difficult to produce granulated spherical graphite for use as a negative electrode active material for secondary batteries that can exhibit excellent effects in terms of initial discharge capacity, etc.

[0038] In the method for producing granulated spheroidal graphite according to the present invention, the step (e) of "additional pitch addition and mixing / coating step" is a step of adding, mixing, and coating the outside of the spheroidized first graphite composite, i.e., the "first composite of finely divided natural graphite and finely divided pitch", produced in the granulation / spheroidization step (d).

[0039] The amount of the finely powdered pitch added is an amount corresponding to a total pitch ratio of more than 25% by weight, i.e., the combined ratio of the finely powdered pitch and the finely powdered pitch added, out of the total weight parts of the finely powdered natural graphite, the finely powdered pitch, and the finely powdered pitch added in step (a). Preferably, it is more than 25% by weight to 60% by weight. If the amount of the added pitch is added in an amount of 25% by weight or less, the amount of pitch involved in bonding between the finely powdered natural graphite is insufficient, and as a result, the crystallization of the spheroidized first graphite composite, i.e., the "first composite of the finely powdered natural graphite and the finely powdered pitch", is not sufficiently performed, and the particle hardness of the granulated spheroidal graphite after the complete production is weakened (see Comparative Example 3).

[0040] Such granulated spherical graphite, which has a low particle hardness, is easily broken under conditions such as pressure when it is manufactured into a negative electrode active material, which is disadvantageous in the manufacturing process of the negative electrode active material.

[0041] The mixing time in step (e) is the time required for the "finely powdered pitch to be added" to be completely mixed with the "first composite of finely powdered natural graphite and finely powdered pitch", which is the spheroidized first graphite composite, and can be determined depending on the amount used. The preferred mixing time is 1 hour or more.

[0042] The pitch added in step (e) is coated on the outside of the spheroidized first graphite composite produced in step (d), i.e., the "first composite of finely divided natural graphite and finely divided pitch", and the final granulated spheroidal graphite having a certain particle size and graphite crystallization is obtained by the subsequent primary and secondary heat treatments.

[0043] In the method for producing granulated spherical graphite according to the present invention, the step (f) "completion of additional mixing" is a step of mixing the first composite of finely powdered natural graphite and finely powdered pitch, which is the first spheroidized graphite composite formed in the step (e) "addition of additional pitch and mixing coating step", in a high-speed mixer such as Mechanofusion, to complete mixing of the mixture. The high-speed mixer operates at a speed of about 1,000 rpm to 3,000 rpm, and the mixing time can be determined depending on the mixing speed and the amount used, and is preferably 1 minute or more.

[0044] The completion step of the additional mixing in step (f) is for the purpose of successfully coating the outside of the spheroidized first graphite composite in step (e) with pitch. Through step (f), a "secondary composite in which the outside of the spheroidized first graphite composite is coated with pitch" is produced, which is a "secondary composite in which the outside of the first composite made of finely divided natural graphite and finely divided pitch is coated with pitch".

[0045] In the method for producing granulated spherical graphite according to the present invention, the "primary heat treatment step" of the step (g) is a step of primarily heat treating the "secondary composite in which the outside of the spheroidized primary graphite composite is coated with pitch" of the step (f).

[0046] The heat treatment temperature is 1,000° C. or more, preferably 1,000° C. to 1,500° C., and the heat treatment temperature is maintained for 30 minutes or more, preferably 1 hour or more. The primary heat treatment in step (g) is performed in a nitrogen atmosphere.

[0047] The primary heat treatment in step (g) is for carbonizing the pitch and / or solvent used in the "secondary composite in which pitch is coated on the outside of the spheroidized graphite composite" to form amorphous carbon, and also for removing external impurities of the secondary composite due to the additional pitch coating to improve the surface properties of the second composite of spheroidized graphite.

[0048] By the step (g), "primary heat-treated granulated spheroidal graphite" can be obtained.

[0049] In the method for producing granulated spheroidal graphite according to the present invention, the "secondary heat treatment step" of step (h) is a step of subjecting the "primarily heat-treated granulated spheroidal graphite" of step (g) to a secondary heat treatment. The granulated spheroidal graphite subjected to the primary heat treatment is cooled to room temperature and then subjected to a secondary heat treatment. The secondary heat treatment temperature is 2,000°C or higher. The secondary heat treatment is performed in an inert gas atmosphere such as argon gas, and the secondary heat treatment temperature is maintained for 30 minutes or more, preferably 1 hour or more.

[0050] The secondary heat treatment in step (h) is a step of crystallizing amorphous carbon such as carbonized pitch and natural graphite in the primary heat-treated granulated spheroidal graphite formed in the primary heat treatment in step (g), and such crystallization improves the crystallization of the granulated spheroidal graphite. Such excellent crystallization of the granulated spheroidal graphite is advantageous in the manufacturing process of the negative electrode active material.

[0051] Therefore, the degree of crystallinity of granulated spherical graphite that does not undergo step (h) is low (see Comparative Example 1). As a result, the granulated spherical graphite produced has disadvantages such as an increased irreversible capacity during initial charge / discharge, low initial efficiency, and poor charge / discharge life characteristics, and is therefore unfavorable for use in producing a negative electrode active material.

[0052] As described above, the granulated spherical graphite having undergone the secondary heat treatment in step (h) can be used as an anode active material for a secondary battery exhibiting excellent electrical properties such as initial discharge capacity and initial efficiency.

[0053] As described above, the method for producing granulated spherical graphite according to the present invention, which includes steps (a) to (h), comprises the steps of primarily producing a composite of pulverized flake-like natural graphite and pulverized pitch, coating the exterior of the composite with pitch to produce a secondary composite (steps (a) to (f)), primarily heating the secondary composite to amorphous carbonize the secondary composite (step (g)), and further subjecting the amorphous secondary composite to secondary heat treatment to crystallize it to produce granulated spherical graphite.

[0054] The granulated spherical graphite produced by the production method of the present invention including steps (a) to (h) has a crystalline carbon content of more than 15% compared to natural graphite.

[0055] The average particle size (D50) of the granulated spherical graphite produced by the method for producing granulated spherical graphite according to the present invention, which includes steps (a) to (h), is 15 to 50 μm, and preferably 15 to 30 μm. The granulated spherical graphite particles produced by the method for producing granulated spherical graphite according to the present invention have a specific surface area of ​​4.5 m 2 / g or less, the particle size is uniform, and d002 (nm, distance between graphite layers), which indicates the crystallinity of the granulated spherical graphite particles, is 0.338 or less. The crystallinity of the granulated spherical graphite particles is excellent, and the granulated spherical graphite particles maintain their granularity against the strong pressure applied during the production of the negative electrode active material, thereby exhibiting excellent initial discharge capacity (%) and initial efficiency (%) of the battery.

[0056] SEM images of the granulated spherical graphite aggregates produced by the method for producing granulated spherical graphite according to the present invention including steps (a) to (h) are shown in Figures 1 and 2. As can be seen from the SEM images in Figures 1 and 2, the granulated spherical graphite produced by the method for producing granulated spherical graphite according to the present invention exhibits a spherical morphology. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0057] The present invention will be described in more detail with reference to the following examples. However, the following examples are intended to illustrate and specifically explain the present invention, and the scope of the present invention is not limited thereto.

[0058] Incidentally, the contents not described here can be easily inferred by those skilled in the art, so the explanation thereof will be omitted.

[0059] <Production of Granulated Spherical Graphite> <Example 1> A flake-like natural graphite raw material having an average particle size of 100 μm was pulverized in a jet mill set at a pulverization pressure of 7 bar to 9 bar to produce finely pulverized natural graphite having an average particle size of 3 μm. In addition, pitch having an average particle size of 5 mm was pulverized in a jet mill set at a pulverization pressure of 6 bar to 8 bar to produce finely pulverized pitch having an average particle size of 2 μm ("Step (a)").

[0060] 10 kg of the finely powdered pitch and 90 kg of finely powdered natural graphite were placed in a screw mixer and mixed for 1 hour ("Step (b)"). After that, 10 kg of kerosene and 10 kg of paraffin oil were added and mixed for an additional hour ("Step (c)"). 6 kg of the mixed product was placed in a granulator and spheronized at a linear speed of 4,500 m / min for 150 seconds ("Step (d)").

[0061] 6 kg of the "spheroidized graphite composite" after the granulation and spheroidization process was placed in a screw mixer, and 25 kg of finely powdered pitch was added and mixed for 1 hour ("Step (e)"). After the additional mixing of the "spheroidized graphite composite" and the "finely powdered pitch" was completed, the mixture was placed in a Mechanofusion high-speed mixer and mixed again at 1,500 rpm for a further 10 minutes ("Step (f)").

[0062] After the remixing was completed, the "secondary composite in which the outside of the spheroidized graphite composite was coated with pitch" was placed in an electric furnace and subjected to a primary heat treatment at 1,000°C in a nitrogen atmosphere, and the time for maintaining the heat treatment temperature at 1,000°C was one hour ("Step (g)"). The granulated spheroidal graphite that had been subjected to the primary heat treatment at 1,000°C was cooled to room temperature and then placed in an electric furnace and subjected to a secondary heat treatment at 2,400°C in an argon gas atmosphere. The time for maintaining the heat treatment temperature at 2,400°C was one hour ("Step (h)"), and finally, granulated spheroidal graphite was obtained.

[0063] The granulated spherical graphite produced through steps (a) to (h) has an average particle size (D50, μm), a specific surface area (m 2The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0064] <Example 2> The final granulated spherical graphite was produced in the same manner as in Example 1, except that "15 kg of kerosene and 15 kg of paraffin oil were used as the solvent in step (c) of Example 1."

[0065] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0066] <Example 3> The final granulated spherical graphite was produced in the same manner as in Example 1, except that "20 kg of pulverized pitch in step (b) and 80 kg of pulverized natural graphite were used" and "15 kg of pulverized pitch in step (e) was added."

[0067] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0068] <Example 4> The final granulated spherical graphite was produced in the same manner as in Example 1, except that the granulation and spheroidization process in step (d) of Example 1 was carried out at a linear speed of 4,800 m / min for 150 seconds.

[0069] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0070] <Example 5> The final granulated spherical graphite was produced in the same manner as in Example 1, except that the granulation and spheroidization process in step (d) of Example 1 was carried out at a linear speed of 4,500 m / min for 300 seconds.

[0071] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0072] <Comparative Example 1> The final granulated spherical graphite was produced in the same manner as in Example 1, except that the "secondary heat treatment" in step (h) of Example 1 was not performed.

[0073] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0074] <Comparative Example 2> The final granulated spherical graphite was produced in the same manner as in Example 1, except that the granulation and spheroidization process in step (d) of Example 1 was carried out at a linear speed of 4,000 m / min for 150 seconds.

[0075] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0076] <Comparative Example 3> The final granulated spherical graphite was produced in the same manner as in Example 1, except that "15 kg of pulverized pitch in step (e) was added."

[0077] The average particle size (D50, μm) and specific surface area (m 2 The initial discharge capacity (mAh / g) and the graphite interlayer distance (d002, nm) were measured through XRD analysis, and a coin cell was manufactured using the granulated spherical graphite as the negative electrode active material, and the initial discharge capacity (mAh / g) and initial efficiency (%) of the battery were measured (see Tables 1 and 2).

[0078] The process conditions of Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1 below. The particle size (D50, μm) and specific surface area (m 2 / g) and d002 (nm, graphite interlayer distance).

[0079] The average particle size was measured using a Particle Size Analyser manufactured by Anton Paar, and the specific surface area was measured using a BET device manufactured by Micromertics.

[0080] The graphite interlayer distance d002 is the stacking distance of each carbon hexagonal mesh plane measured through XRD analysis, and is calculated as follows: d002=λ / 2(sinθ) λ: wavelength value of the X-rays target Cu (1.5406A) θ: The typical graphite 002 is 26.554 2θ

[0081] <Coin cell manufacturing> The granulated spherical graphite negative active material, SBR, and CMC were mixed with ultrapure water in a ratio of 98:1:1 to prepare a slurry. The slurry was uniformly applied to a copper foil, dried in an oven at 80°C for about 2 hours, roll-pressed, and further dried in a vacuum oven at 110°C for about 12 hours to prepare a negative plate.

[0082] A CR2032 coin-type half cell was manufactured by a commonly known manufacturing process using the manufactured negative electrode plate, lithium foil as a counter electrode, a porous polyethylene membrane separator, and a liquid electrolyte in which LiPF6 was dissolved at a concentration of 1.0 M in a solvent in which ethylene carbonate and diethyl carbonate (DEC) were mixed at a volume ratio of 3:7.

[0083] <Initial discharge capacity and efficiency measurement of coin cells> A constant current was applied at 25°C at a rate of 0.1 C until the battery voltage reached 0.01 V (vs. Li), and when the battery voltage reached 0.01 V, a constant voltage was applied to charge the battery until the current reached a rate of 0.01 C. During discharge, the battery was discharged at a constant current of 0.1 C until the voltage reached 1.5 V (vs. Li).

[0084] Table 1 below shows and compares the amounts of graphite, pitch, and solvent fuel inputs, the conditions of the granulation process, the amount of pitch input for the surface treatment process, and the heat treatment temperature in Examples 1 to 5 and Comparative Examples 1 to 3.

[0085] [Table 1]

[0086] The above Table 1 shows the conditions of each step in the above Examples 1 to 5, which relate to the method for producing granulated spherical graphite according to the present invention, including steps (a) to (h).

[0087] Specifically, in Examples 1 to 5 of the present invention, the content of pitch and pitch for the surface treatment process is 25% or more of the total amount of graphite, pitch, and pitch for the surface treatment process, whereas in Comparative Example 3, it is less than 25%.

[0088] In addition, in Comparative Example 1, only the primary heat treatment was performed and the secondary heat treatment was omitted, and in Comparative Example 2, the linear velocity in the granulation process in step (d) was 4,000 m / min, which does not satisfy the linear velocity condition of the present invention of 4,500 m / min or more.

[0089] Table 2 below shows the particle size (D50, μm) and specific surface area (m2) of the granulated spherical graphite of Examples 1 to 5 and Comparative Examples 1 to 3, which were produced under the process conditions of Table 1. 2 The physical properties of the graphite layers (i.e., d002 (nm, distance between graphite layers) and the initial discharge capacity (%) and initial efficiency (%) of a battery using the granulated spherical graphite as a negative electrode active material are shown.

[0090] [Table 2]

[0091] From Table 2, it can be seen that Examples 1 to 5 relating to the method for producing granulated spherical graphite according to the present invention have similar or higher initial discharge capacity and exceptionally excellent initial efficiency compared to Comparative Examples 1 to 3. Such high initial efficiency has the advantage that the consumption of lithium ions provided at the positive electrode during initial charging can be reduced, making it possible to design a high-capacity cell.

[0092] Also, unlike Examples 1 to 5 in Table 2, Comparative Examples 1 to 3 have the following shortcomings.

[0093] First, the granulated spheroidal graphite of Comparative Example 1, which was subjected to only the primary heat treatment, had a d002 indicating crystallization of 0.341 nm, which was larger than the granulated spheroidal graphite of Examples 1 to 5 and Comparative Examples 1 and 2, which were subjected to the primary and secondary heat treatments, meaning that the degree of crystallization of the granulated spheroidal graphite of Comparative Example 1 was low. As a result, when a battery is manufactured using the granulated spheroidal graphite of Comparative Example 1 as a negative electrode active material, there are disadvantages in that the irreversible capacity increases during initial charge / discharge, the initial efficiency decreases, and the charge / discharge life characteristics are poor.

[0094] Next, in Comparative Example 2, the linear velocity of granulation and spheroidization of the pulverized graphite and pulverized pitch is 4,000 m / min, which is lower than 4,500 m / min in Examples 1 to 5. As a result, as the degree of granulation and spheroidization decreases, the form of the granulated spheroidal graphite, which is the negative active material, is destroyed by pressure during the manufacturing process as in Comparative Example 1, resulting in a decrease in the efficiency of the negative active material and a decrease in the initial efficiency of the battery.

[0095] In addition, in Comparative Example 3, the amount of pitch used in the granulated spherical graphite is 25% or less, which is less than the amount of pitch used in Examples 1 to 5, which is more than 25%. Such a small amount of pitch reduces the role of a binder that spheroidizes the finely powdered graphite, and the specific surface area of ​​the finally produced granulated spherical graphite increases, which means that the granulated spherical graphite becomes powdered (see FIG. 3 of Comparative Example 2, in which the specific surface area is similar to that of Comparative Example 3), and when used as a negative electrode active material, the efficiency of the negative electrode active material decreases, resulting in disadvantages such as poor initial efficiency of the battery. [Industrial Applicability]

[0096] As described above, the method for producing the novel granulated spherical graphite according to the present invention in Examples 1 to 5 is used as a negative electrode active material for batteries, and exhibits excellent initial efficiency and initial discharge capacity, thereby having the effect of being usable as an excellent negative electrode active material for batteries, and thus having industrial applicability.

Claims

1. (a) a step of pulverizing flake natural graphite and pitch, respectively ("respective pulverization steps of natural graphite and pitch"); (b) a mixing step of the finely divided natural graphite and the finely divided pitch of step (a) ("the natural graphite and pitch mixing step"); (c) further mixing a solvent into the mixture of step (b) (the "solvent mixing step"); (d) spheronizing the mixture of step (c) to produce a spheronized first graphite composite material (the "spheronization step"); (e) adding and mixing-coating additional finely divided pitch onto the first graphite composite material after the granulation and spheroidization of the step (d) ("additional pitch adding and mixing-coating step"); (f) further mixing the mixture of step (e) to complete the mixing, thereby producing a secondary composite in which the outside of the spheroidized first graphite composite is coated with pitch ("additional mixing completion step"). (g) subjecting the secondary composite of step (f) to a first heat treatment (the "first heat treatment step"); and (h) a step of cooling to room temperature after the primary heat treatment of step (g) and then further performing a secondary heat treatment ("secondary heat treatment step"); The amount of the finely divided pitch added in the step (e) of "additional pitch addition and mixed coating step" is more than 25% by weight of the combined amount of the finely divided pitch in the step (a) and the finely divided pitch in the step (e) based on the total weight parts of the finely divided natural graphite, the finely divided pitch, and the finely divided pitch added in the step (a); The granulation conditions in the step (d) "granulation and spheronization step" are a linear velocity of 4,500 m / min to 8,000 m / min and a processing time of 100 seconds to 600 seconds, The heat treatment conditions of the step (g) of "first heat treatment step" are 1,000° C. or more for 30 minutes or more, The method for producing granulated spherical graphite, wherein the heat treatment conditions in the step (h), the "second heat treatment step", are 2,000° C. or higher for 30 minutes or more.

2. The method for producing granulated spherical graphite according to claim 1, wherein the average particle size of the "flake-like natural graphite" in step (a) is 5 μm to 500 μm, the pulverization of the natural graphite is performed using a high-speed mechanical milling device under a pressure of 5 bar to 10 bar, and the average particle size of the pulverized natural graphite particles is 1 μm to 10 μm.

3. 2. The method for producing granulated spherical graphite according to claim 1, wherein the pulverization of the pitch in step (a) is carried out using a high-speed mechanical milling machine under a pressure of 5 bar to 10 bar, and the average particle size of the pulverized pitch is 0.5 μm to 10 μm.

4. 2. The method for producing granulated spherical graphite according to claim 1, wherein the mixing weight percentage of the finely powdered natural graphite and the finely powdered pitch in step (b) is 99:1 to 50:

50.

5. 2. The method for producing granulated spherical graphite according to claim 1, wherein the solvent in the solvent mixing step (c) is one or more selected from the group consisting of mineral oils such as kerosene, heavy oil, light oil, or paraffin oil; hydrocarbon solvents such as toluene or decane; and mixtures thereof.

6. The method for producing granulated spherical graphite according to claim 1, wherein the amount of the solvent used in the solvent mixing step (c) is 10 to 50 parts by weight per 100 parts by weight of the "mixture of finely divided natural graphite and finely divided pitch".

7. 2. The method for producing granulated spherical graphite according to claim 1, wherein the additional mixing in the "completion step of additional mixing" (f) is performed by mixing the spheroidized first graphite composites formed in (e) in a high-speed mixer at a speed of 1,000 rpm to 3,000 rpm for 1 minute or more.

Citation Information

Patent Citations

  • COMPOSITE GRAPHITE PARTICLE, ITS PRODUCTION METHOD, Li ION SECONDARY BATTERY CATHODE MATERIAL, Li ION SECONDARY BATTERY CATHODE AND Li ION SECONDARY BATTERY

    JP2004210634A

  • Spherical carbonaceous material and method forpreparation thereof

    KR1020030087986A

  • Artificial graphite for lithium ion secondary battery and method for producing the same

    KR1020180078044A

  • Globular Carbon type Anode Active Material, Method for preparing the same, Anode Comprising the same, and Lithium Secondary Battery Comprising the same

    KR1020210040810A

  • The method for fabrication of spherical carbonaceous material

    KR102254549B1