Fe-based electroplated high strength steel sheet and its manufacturing method

By applying Fe-based electroplating before annealing and controlling the annealing atmosphere, the issues of hydrogen ingress and delayed fracture in high-strength cold-rolled steel sheets are mitigated, achieving superior chemical conversion and corrosion resistance.

JP7578118B2Active Publication Date: 2024-11-06JFE STEEL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022084829
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-24
Filing Date
2022-05-24
Publication Date
2024-11-06
Estimated Expiration
2042-05-24

AI Technical Summary

Technical Problem

Existing high-strength cold-rolled steel sheets with added silicon (Si) face issues with chemical conversion treatment properties, post-painting corrosion resistance, and increased likelihood of delayed fracture due to hydrogen ingress during electroplating, particularly when tensile strength exceeds 980 MPa.

Method used

Applying Fe-based electroplating before annealing to suppress hydrogen entry, controlling the dew point and hydrogen concentration during annealing to reduce diffusible hydrogen content, and ensuring crystal orientation unification between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet.

Benefits of technology

Results in an Fe-based electroplated high-strength steel sheet with excellent chemical conversion treatment properties, improved post-painting corrosion resistance, and enhanced delayed fracture resistance, maintaining mechanical properties even at high tensile strengths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578118000003
    Figure 0007578118000003
  • Figure 0007578118000004
    Figure 0007578118000004
  • Figure 0007578118000005
    Figure 0007578118000005
Patent Text Reader

Abstract

To provide an Fe-based electric plating high-strength steel sheet that has excellent chemical conversion properties and excellent corrosion resistance after coating and also has excellent resistance to delayed fracture.SOLUTION: An Fe-based electric plating high-strength steel sheet has: a Si-containing cold-rolled steel sheet that contains Si of 0.5 to 3.0 mass%; and an Fe-based electric plated layer that is deposited on at least one side of the Si-containing cold-rolled steel sheet with its amount of deposition being 1.0 to 20.0 g / m2 for each side. The content of in-steel diffusible hydrogen is 0.25 mass ppm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an Fe-based electroplated high-strength steel sheet having excellent chemical conversion treatability, corrosion resistance after painting, and excellent delayed fracture resistance, and a method for producing the same. [Background technology]

[0002] In recent years, there has been a strong demand for improving the fuel efficiency of automobiles from the viewpoint of protecting the global environment. In addition, there has been a strong demand for improving the safety of automobiles from the viewpoint of ensuring the safety of passengers in the event of a collision. In order to meet these demands, it is important to simultaneously achieve weight reduction and high strength in automobile bodies, and in cold-rolled steel sheets, which are the raw material for automobile parts, high strength and thinning have been actively promoted. In addition, since many automobile parts are manufactured by forming steel sheets, good formability is also required in addition to high strength.

[0003] Here, one method for increasing the strength of cold-rolled steel sheets without impairing their formability is solid-solution strengthening by adding Si. However, when a large amount of Si, particularly 0.5 mass% or more, is added to cold-rolled steel sheets, SiO 2 It is known that Si-containing oxides such as Si-Mn-based composite oxides and Si-Mn-based composite oxides are formed. The formed Si-containing oxides significantly reduce the chemical conversion treatability, and therefore, not only is the chemical conversion treatability poor, but in a hot and salty water test after electrodeposition coating, the coating peels off more easily than with ordinary steel sheets, and the corrosion resistance after coating is also poor.

[0004] It is also known that increasing the strength of cold-rolled steel sheets increases the likelihood of delayed fracture. This tendency is particularly pronounced in high-strength steels with tensile strengths of 980 MPa or more. Delayed fracture is a phenomenon in which, when high-strength steel is subjected to a static load stress (load stress below the tensile strength) and a certain amount of time has passed, a sudden brittle fracture occurs without any apparent plastic deformation. In the case of steel plates, it is known that this delayed fracture occurs due to the residual tensile stress when pressed into a specified shape and hydrogen embrittlement of the steel at the stress concentration area.

[0005] Furthermore, in addition to the above-mentioned strength and formability, improvements in the formation state of a chemical conversion coating (chemical conversion treatability) are also desired for cold-rolled steel sheets. For example, Patent Document 1 describes a method for producing a high-strength cold-rolled steel sheet containing 0.5 to 2.0 mass% Si, which is annealed, pickled, and then has a coating weight of 1 to 5 g / m 2 Patent Document 2 discloses a technique for improving chemical conversion treatability by electroplating a Zn-Fe alloy in the range of 1 to 50 mg / m. 2 A technique for improving chemical conversion treatability by plating has been disclosed. Patent Document 3 discloses a technique for improving chemical conversion treatability by plating an annealed steel sheet with an Fe-Ni alloy, and Patent Document 4 discloses a technique for improving chemical conversion treatability by plating an annealed steel sheet with an Fe-Ni alloy of 0.02 to 1.5 g / m 2 A technique for improving chemical conversion treatability by forming an Fe coating layer has been disclosed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-89946 A [Patent Document 2] JP 2008-190030 A [Patent Document 3] Japanese Patent Application Laid-Open No. 61-113787 [Patent Document 4] Japanese Patent Application Publication No. 5-320952 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the techniques for improving chemical conversion treatability described in Patent Documents 1 to 4 all involve electroplating in the latter stage, and therefore there is a problem in that hydrogen penetrates into the steel sheet during electroplating, and in high-strength steel sheets having a tensile strength of more than 980 MPa, the above-mentioned delayed fracture is likely to occur.

[0008] In view of the above circumstances, the present invention provides an Fe-based electroplated high-strength steel sheet having excellent chemical conversion treatability, corrosion resistance after painting, and excellent delayed fracture resistance, and a method for producing the same. [Means for solving the problem]

[0009] As a result of investigations aimed at solving the above problems, the inventors have found that in order to suppress hydrogen penetration into a steel sheet during electroplating, it is effective to perform electroplating before annealing the steel sheet. Since steel sheets are usually annealed at a high temperature range of about 700 to 900°C, the diffusible hydrogen that penetrates into the steel sheet during electroplating is released into the furnace, and the content of diffusible hydrogen in the steel can be reduced. During annealing, Si contained in the steel sheet may diffuse into the Fe plating layer and become concentrated on the surface. However, the inventors have found that by controlling the dew point in the annealing furnace, it is possible to adjust the crystal grain size of the Fe plating layer and simultaneously satisfy chemical conversion treatability, which has led to the completion of the present invention.

[0010] The present invention has been made based on the above findings, and the gist of the present invention is as follows. 1. A Si-containing cold-rolled steel sheet containing 0.5 to 3.0 mass% Si; The Si-containing cold-rolled steel sheet has a coating weight of 1.0 to 20.0 g / m 2 and an Fe-based electroplating layer, An Fe-based electroplated high-strength steel sheet, characterized in that the content of diffusible hydrogen in the steel is 0.25 mass ppm or less.

[0011] 2. The Fe-based electroplated high-strength steel sheet according to 1, characterized in that the Si-containing cold-rolled steel sheet has a tensile strength of 980 MPa or more.

[0012] 3. The Fe-based electroplated high-strength steel sheet according to 1 or 2 above, characterized in that the rate at which the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet are integrated at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet exceeds 50%.

[0013] 4. The Si-containing cold-rolled steel sheet has, in mass%, Si: 0.5-3.0%, C: 0.8% or less, Mn: 1.5-3.5%, P: 0.1% or less, S: 0.03% or less, and Al: 0.1% or less 4. The Fe-based electroplated high-strength steel sheet according to any one of the above items 1 to 3, characterized in that it has a composition containing the above and the remainder consisting of Fe and unavoidable impurities.

[0014] 5. The composition of the Si-containing cold-rolled steel sheet further comprises, in mass%, B: 0.005% or less, Ti: 0.2% or less, N: 0.010% or less, Cr: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Mo: 1.0% or less Nb: 0.20% or less, V: 0.5% or less, Sb: 0.200% or less, Ta: 0.1% or less, W: 0.5% or less, Zr: 0.1% or less, Sn: 0.20% or less, Ca: 0.005% or less, Mg: 0.005% or less, and REM: 0.005% or less 5. The Fe-based electroplated high-strength steel sheet according to 4 above, characterized in that it contains at least one selected from the group consisting of:

[0015] 6. The Fe-based electroplated high-strength steel sheet according to any one of the above items 1 to 5, characterized in that the Fe-based electroplated layer contains one or more elements selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co in a total amount of 10 mass% or less, with the remainder consisting of Fe and unavoidable impurities.

[0016] 7. A Si-containing cold-rolled steel sheet containing 0.5 to 3.0 mass% Si is electroplated with an Fe-based coating to obtain a coating weight of 1.0 to 20.0 g / m2 on one side. 2 obtaining a pre-annealed Fe-based electroplated steel sheet having an Fe-based electroplated layer formed on at least one side thereof; annealing the pre-annealed Fe-based electroplated steel sheet in an atmosphere having a dew point of −30° C. or less and a hydrogen concentration of 8 volume % or less to obtain an Fe-based electroplated steel sheet; A method for producing an Fe-based electroplated steel sheet, comprising:

[0017] 8. The method for producing an Fe-based electroplated steel sheet according to 7 above, characterized in that the atmosphere during the annealing has a dew point of -40°C or less and a hydrogen concentration of 5 volume % or less. Effect of the Invention

[0018] According to the present invention, there can be provided an Fe-based electroplated high-strength steel sheet having excellent chemical conversion treatability, corrosion resistance after painting, and excellent delayed fracture resistance, and a manufacturing method thereof. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1(a) is a perspective view showing an outline of an observation sample for measuring the number of crystal grain boundaries of an Fe-based electroplating layer in contact with a Si-containing cold-rolled steel sheet at the interface between the Fe-based plating layer and the Si-containing cold-rolled steel sheet, and FIG. 1(b) is a cross-sectional view taken along the line AA of FIG. 1(a). [Diagram 2](a) is an image in which the boundary line B is drawn at the interface between the Fe-based electroplated layer of the SIM image and the Si-containing cold-rolled steel sheet using a scanning electron microscope, (b) is an image in the binarized image, and is an image drawn along the boundary line B in the region surrounded by L1 and L2 of a determination region having a width of 40 pixels centered on the boundary line B, and (c) is an enlarged view of the portion surrounded by the square in (b). [Diagram 3] It is a figure showing the process of the composite cycle corrosion test in the example. [Figure 4] It is a figure schematically showing a specimen for evaluating delayed fracture used in the example.

Mode for Carrying Out the Invention

[0020] Hereinafter, embodiments of the present invention will be described. Note that the present invention is not limited to the following embodiments. In the following description, the unit of the content of each element of the steel component composition and the content of each element of the electroplated layer component composition is both "mass%", and is simply indicated by "% " unless otherwise specified.

[0021] <Fe-based electroplated high-strength steel sheet> The Fe-based electroplated high-strength steel sheet of the present invention includes a Si-containing cold-rolled steel sheet containing 0.5 to 3.0% by mass of Si, and a Fe-based electroplated layer formed on at least one side of the Si-containing cold-rolled steel sheet and having an adhesion amount per side of 1.0 to 20.0 g / m 2 and is provided with a Fe-based electroplated layer.

[0022] (Si-containing cold-rolled steel sheet) The Fe-based electroplated high-strength steel sheet of the present invention includes a Si-containing cold-rolled steel sheet containing 0.5 to 3.0% by mass of Si. Hereinafter, the steel components of the Si-containing cold-rolled steel sheet will be described.

[0023] Si: 0.5 to 3.0% The Si-containing cold-rolled steel sheet contains 0.5 to 3.0% Si. Since Si has a large effect of increasing the strength of steel (solid solution strengthening ability) without significantly impairing workability, it is an effective element for achieving high strength of steel. Therefore, when Si is added as a means for achieving high strength, it is necessary to add 0.5% or more. If the Si content is less than 0.5%, the effect on chemical conversion treatability and resistance weld crack resistance is small. On the other hand, since Si is also an element that adversely affects chemical conversion treatability, post-painting corrosion resistance, and resistance weld crack resistance, the Si content is 3.0% or less. If the Si content exceeds 3.0%, the hot rolling property and cold rolling property are significantly reduced, which may adversely affect productivity or cause a decrease in the ductility of the steel sheet itself. From the same viewpoint, the Si content is preferably in the range of 0.7 to 2.5%.

[0024] The Si-containing cold-rolled steel sheet must contain Si in the above range, but other components are permissible as long as they are within the composition ranges of ordinary cold-rolled steel sheets, and are not particularly limited. However, when the cold rolled steel sheet of the present invention is applied to a high strength cold rolled steel sheet having a tensile strength TS of 590 MPa or more for use in automobile bodies and the like, it is preferable that the cold rolled steel sheet has the following composition.

[0025] C: 0.05 to 0.3% C forms martensite or the like as a steel structure, which makes it easier to improve workability. Therefore, it is preferable to contain 0.05% or more. However, since excessive addition of C reduces weldability, it is preferable to set the content to 0.3% or less. Therefore, the Si-containing cold-rolled steel sheet preferably contains C in a range of 0.5% to 0.3%.

[0026] Mn: 1.5-3.5% Mn is an element that strengthens steel through solid solution strengthening, improves hardenability, and promotes the formation of retained austenite, bainite, and martensite. Such effects are achieved by adding 1.5% or more. On the other hand, if the Mn content is 3.5% or less, the above effects can be obtained without increasing costs. Therefore, the Si-containing cold-rolled steel sheet preferably contains Mn in the range of 1.5 to 3.5%.

[0027] P: 0.1% or less (excluding 0%) P not only reduces weldability, but also segregates at grain boundaries to deteriorate ductility, bendability, and toughness. Furthermore, if added in large amounts, it promotes ferrite transformation and increases the grain size. Therefore, the Si-containing cold-rolled steel sheet preferably contains P in an amount of 0.1% or less.

[0028] S: 0.03% or less (excluding 0%) S reduces weldability and significantly reduces hot ductility, inducing hot cracking and significantly deteriorating surface properties. Furthermore, S not only contributes very little to strength, but also forms coarse sulfides as an impurity element, thereby reducing ductility, bendability, and stretch flangeability. These problems become significant when the S content exceeds 0.030%, so it is desirable to reduce the S content as much as possible. Therefore, the S content in the Si-containing cold-rolled steel sheet is preferably 0.03% or less.

[0029] Al: 0.01 to 0.1% Al is an element added as a deoxidizer in the steelmaking process, and is an effective element for separating nonmetallic inclusions that reduce stretch flangeability as slag, so it is preferable to contain 0.01% or more. On the other hand, if the Al content is 0.1% or less, the above effects can be obtained without increasing the raw material cost. Therefore, it is preferable that the Si-containing cold-rolled steel sheet contains Al in an amount of 0.01% or more and 0.1% or less.

[0030] Nb: 0.005 to 0.05% Nb forms carbides and nitrides, suppresses the growth of ferrite during the heating stage of annealing, refines the structure, and improves formability, particularly stretch flangeability. Such effects are achieved by adding 0.005% or more. On the other hand, if the content is 0.05% or less, the above effects can be obtained without increasing costs. Therefore, the Si-containing cold-rolled steel sheet preferably contains 0.005 to 0.05% Nb.

[0031] Ti: 0.005 to 0.05% Like Nb, Ti forms carbides and nitrides, suppresses the growth of ferrite during the heating stage of annealing, refines the structure, and improves formability, particularly stretch flangeability. Such effects are achieved by adding 0.005% or more. On the other hand, if the content is 0.05% or less, the above effects can be obtained without increasing costs. Therefore, the Si-containing cold-rolled steel sheet preferably contains 0.005 to 0.05% of Ti.

[0032] Cu: 0.05-0.5% When Cu is contained in an amount of 0.05% or more, the effect of promoting the formation of the residual γ phase is easily obtained. On the other hand, if the Cu content exceeds 0.5%, the cost increases. Therefore, when Cu is added to the Si-containing cold-rolled steel sheet, the Cu content is preferably 0.05 to 0.5%.

[0033] Ni: 0.05~0.5% When Ni is contained in an amount of 0.05% or more, the effect of promoting the formation of the residual γ phase is easily obtained. On the other hand, if the Ni content exceeds 0.5%, the cost increases. Therefore, when Ni is added to the Si-containing cold-rolled steel sheet, it is preferable that the Ni content be 0.05 to 0.5%.

[0034] Sb: 0.001 to 0.2% Sb can be added from the viewpoint of suppressing nitridation and oxidation of the steel sheet surface, or decarburization of the steel sheet surface in a region of several tens of microns caused by oxidation. Sb prevents a decrease in the amount of martensite formed on the steel sheet surface by suppressing nitridation and oxidation, thereby improving fatigue properties and surface quality. Such effects can be obtained at 0.001% or more. On the other hand, if it exceeds 0.2%, toughness deteriorates. Therefore, when Sb is added to the Si-containing cold-rolled steel sheet, it is preferable that the content be 0.001 to 0.2%.

[0035] The Si-containing cold rolled steel sheet contains Fe and unavoidable impurities as the balance other than the above-mentioned components, however, other components may be added within a range that does not impair the effects of the present invention. For example, Mo is an element that improves the hardenability of steel and promotes the formation of bainite and martensite, and therefore may be further added in the range of 0.005 to 0.3%. Ca and REM are elements that control the morphology of sulfide-based inclusions and improve the stretch flangeability of steel sheet, and therefore one or two selected from Ca: 0.001 to 0.1% and REM: 0.001 to 0.1% may be further added.

[0036] (Fe-based electroplating layer) The Fe-based electroplated high strength steel sheet of the present invention has a coating weight of 1.0 to 20.0 g / m per side formed on at least one side of the Si-containing cold rolled steel sheet. 2 The plated layer is an Fe-based electroplating layer.

[0037] By forming the Fe-based electroplating layer, the external oxidation of Si and Mn during annealing is delayed, and even if the cold-rolled steel sheet contains Si, it is possible to obtain a cold-rolled steel sheet having good chemical conversion treatability. In the present invention, 1.0 g / m 2 In order to obtain the effect of improving the chemical conversion treatability, the Fe-based electroplating layer should have a coating weight of 1.0 g / m2 or more per side. 2 From the same viewpoint, the coating weight of the Fe-based electroplating layer is preferably 3.0 g / m 2More preferably, 5.0 g / m 2 The upper limit of the coating weight of the Fe-based electroplating layer per side is not particularly limited, but from the viewpoint of cost, the coating weight of the Fe-based electroplating layer per side is set to 20 g / m or more. 2 The following applies. In the Fe-based electroplated high strength steel sheet of the present invention, it is preferable that an Fe-based electroplated layer is formed on both sides of the Si-containing cold rolled steel sheet. 2 By adjusting the content to the above level, chemical conversion treatability becomes particularly good.

[0038] The adhesion weight of the Fe-based electroplating layer is measured as follows. A sample of 10×15 mm size is taken from the annealed Si-containing cold-rolled steel sheet and embedded in resin to obtain a cross-section-embedded sample. Three arbitrary points of the cross-section-embedded sample are observed using a scanning electron microscope (SEM) at an accelerating voltage of 15 kV and a magnification of 2000 to 10000 times depending on the thickness of the Fe-based electroplating layer, and the average thickness value of the three fields of view is multiplied by the specific gravity of iron to convert it into the adhesion weight per side of the Fe-based electroplating layer.

[0039] Here, the type of the Fe-based electroplating layer is not particularly limited and can be appropriately selected depending on the required performance. For example, as the Fe-based electroplating layer, in addition to pure Fe, alloy plating layers such as Fe-B alloy, Fe-C alloy, Fe-P alloy, Fe-N alloy, Fe-O alloy, Fe-Ni alloy, Fe-Mn alloy, Fe-Mo alloy, Fe-W alloy, etc. can be appropriately used. The composition of the Fe-based electroplating layer is not particularly limited. For example, it is preferable that the composition contains one or more elements selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co in a total amount of 10 mass% or less, with the remainder being Fe and unavoidable impurities. By limiting the total amount of elements other than Fe to 10 mass% or less, it is possible to prevent a decrease in electrolysis efficiency and form an Fe-based electroplating layer at low cost.

[0040] In addition, it is preferable that the Si-containing cold-rolled steel sheet according to the present invention does not have a plating layer other than the Fe-based electroplating formed on the surface. By not having a plating layer other than the Fe-based electroplating on the surface of the Si-containing cold-rolled steel sheet, it is possible to provide at low cost parts that do not require excessive galvanized steel sheet for rust prevention or parts that are used in environments where the corrosive environment is mild and excessive rust prevention is not required.

[0041] (Diffusible hydrogen in steel) The Fe-based electroplated high-strength steel sheet of the present invention is characterized in that the content of diffusible hydrogen in the steel is 0.25 mass ppm or less. By setting the content of diffusible hydrogen in the steel to 0.25 mass ppm or less, the delayed fracture resistance can be improved.

[0042] If the content of diffusible hydrogen in the steel exceeds 0.25 ppm by mass, this leads to deterioration of bendability and delayed fracture resistance. If the content of diffusible hydrogen in the steel is 0.25 ppm by mass or less, the delayed fracture resistance can be significantly improved, and the content of diffusible hydrogen in the steel is preferably 0.10 ppm by mass or less. If the content of diffusible hydrogen in the steel is 0.10 ppm by mass or less, in addition to the delayed fracture resistance, mechanical properties such as bendability can also be significantly improved.

[0043] The delayed fracture is more pronounced in high-strength steel plates having a tensile strength of 980 MPa or more, and therefore the content of diffusible hydrogen in steel of 0.25 mass ppm or less is preferably applied to high-strength steel plates having a tensile strength of 980 MPa or more. However, since hydrogen in steel also affects mechanical properties such as bendability, which are important when the tensile strength is 590 MPa or more, the technology of the present invention can also be applied to high-strength steel plate with a tensile strength of 590 MPa or more.

[0044] Here, the method for reducing the content of diffusible hydrogen in the steel to 0.25 mass ppm or less is not particularly limited. For example, the content of diffusible hydrogen in the steel can be reduced to 0.25 mass ppm or less by performing an annealing treatment described later after forming the Fe-based electroplating.

[0045] By performing an annealing treatment after the formation of the Fe-based electroplating, hydrogen that has entered the electroplating is released into the annealing furnace in a high-temperature environment, making it possible to improve chemical conversion treatability without deteriorating delayed fracture resistance. When the electroplating is performed, the steel sheet side serves as the cathode, and Fe ions in the plating bath are reduced and electrodeposited as metallic Fe on the steel sheet surface mainly through the following reaction. Fe 2+ +2e - →Fe At the same time, since the plating bath is acidic, a hydrogen generating reaction occurs at a certain rate, as shown in the following reaction: 2H + +2e - →2H→H 2 A certain proportion of hydrogen generated on the steel sheet penetrates into the steel sheet as diffusible hydrogen, and the remainder becomes hydrogen gas. The hydrogen that penetrates remains in the steel and leads to deterioration of mechanical properties such as bendability, and is a factor in deteriorating delayed fracture resistance, which is particularly important for high-strength steel sheets of 980 MPa or more.

[0046] The content of diffusible hydrogen in steel can be measured by, for example, temperature rise analysis using gas chromatography etc. In general, hydrogen released at a temperature of 250° C. or less is called diffusible hydrogen.

[0047] Annealing after the formation of an Fe-based electroplated layer is effective in dehydrogenating the steel sheet and does not deteriorate the delayed fracture resistance. However, even if an Fe-based electroplated layer is present, external oxidation of Si and Mn occurs in the outermost layer, and sufficient chemical conversion treatability may not be obtained. Therefore, in the present invention, it is preferable that the ratio of the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet integrated at the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet is more than 50%. Si and Mn of the Si-containing cold-rolled steel sheet diffuse through the grain boundaries of the Fe electroplating layer to form oxides on the surface. Therefore, if the integration of the crystal grains does not progress sufficiently and an ultrafine structure of the Fe plating layer remains after electroplating, the diffusion of Si and Mn is promoted, and sufficient chemical conversion treatability may not be obtained. Therefore, in the present invention, by making the ratio of the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet integrated to more than 50%, the effect of suppressing external oxidation of Si and Mn during annealing by providing the Fe-based electroplating layer becomes significant, and more excellent chemical conversion treatability can be achieved. The upper limit of the ratio of the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet integrated is not particularly limited and may be 100%.

[0048] Here, the ratio of the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet that are integrated at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet can be measured as follows. First, a sample of 10×10 mm size is taken from an Fe-based electroplated high-strength steel sheet. Three arbitrary locations of the sample are processed with a focused ion beam (FIB) device to form three 45° cross sections with a width of 30 μm in the direction perpendicular to the rolling and a length of 50 μm in the 45° direction relative to the T cross section direction, which are angled at 45° with respect to the T cross section direction (a cross section parallel to the rolling perpendicular direction of the steel sheet and perpendicular to the steel sheet surface) as shown in FIG. 1, to prepare samples for observation. Next, the center of the 45° cross section of the observation sample is observed at a magnification of 5000 times using a scanning ion microscope (SIM), and a SIM image of 1024 pixels wide x 943 pixels high and 8 bits is taken. From the SIM images taken at each of the 45° cross sections created at three locations, the percentage of the integrated crystal orientations between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is calculated based on the following formula (1), and the average value of the three locations is calculated. Note that the value is rounded up to the nearest whole number. Formula (1): Percentage of integrated crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet = (length of the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet where the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet are integrated) ÷ (length of the interface in the observation field) × 100 (%)

[0049] Whether or not the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet are integrated is determined by image processing. Using FIG. 2, the method for evaluating the rate at which the crystal orientations are integrated will be described. First, as shown in FIG. 2(a), a scanning electron microscope is used to draw a boundary line B at the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet in the SIM image described above. Next, an image is created by image processing the SIM image, separate from the image in which the boundary line was drawn. Specifically, a Sobel filter is used to emphasize the grain boundaries of the captured 8-bit SIM image with a width of 1024 pixels and a height of 943 pixels. Next, a smoothing process is performed on the image in which the grain boundaries have been emphasized using a Gaussian filter (radius (R): 10 pixels). Next, a binarization process (threshold: 17) is performed on the image after the smoothing process. Next, the boundary line B of the image in which the interface was drawn is transferred to the binarized image. After that, as shown in FIG. 2(b), a 40-pixel-wide judgment region (L in FIG. 2(b)) is created in the binarized image, with the boundary line B at the center. 1 and L 2Draw along the boundary line B on the binarized image of the area surrounded by (). The total length of the boundary line B where there is no interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet (the black-and-white boundary on the binarized image) within the determination area is regarded as the length of the part where the crystal orientations are integrated. Here, the total length of the boundary line where there is no interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet within the determination area is obtained as follows. First, search the entire determination area for a location where the determination area can be divided into a substantially rectangular shape by two normal lines of the boundary line B so that only one of black and white colors is included. Next, sum up the maximum distances between the intersections of the boundary line and the two normal lines at that location for the entire determination area, and take this as the total length of the boundary line where there is no interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet within the determination area. Note that the length of the part where the crystal orientations are integrated may be obtained by subtracting the length of the part where the crystal orientations are not integrated from the length of the interface in the observation field of view. For the purpose of explanation, Fig. 2(c) shows an enlarged view of the part surrounded by the square in Fig. 2(b). First, as shown in Fig. 2(c), search the entire determination area for a location where the determination area can be divided into a substantially rectangular shape by two normal lines of the boundary line B (in Fig. 2(c), l 1 and l 2 , and also l 3 and l 4 ) so that both black and white colors are included. Next, sum up the maximum distances between the intersections of the boundary line and the two normal lines at that location for the entire determination area, and take this as the total length of the boundary line where there is an interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet within the determination area. By subtracting this length, i.e., the length of the part where the crystal orientations are not integrated, from the length of the interface in the observation field of view, the length of the part where the crystal orientations are integrated can be obtained.

[0050] <Method for manufacturing Fe-based electroplated high-strength steel sheet> Next, the method for manufacturing an Fe-based electroplated high-strength steel sheet will be described. The method for manufacturing the Fe-based electroplated steel sheet of the present invention is to apply Fe-based electroplating to a Si-containing cold-rolled steel sheet containing 0.5 to 3.0% by mass of Si, with an adhesion amount per side of 1.0 to 20.0 g / m 2obtaining a pre-annealed Fe-based electroplated steel sheet having an Fe-based electroplated layer formed on at least one side thereof; and annealing the unannealed Fe-based electroplated steel sheet in an atmosphere having a dew point of −30° C. or lower and a hydrogen concentration of 8 volume % or lower to obtain an Fe-based electroplated steel sheet.

[0051] (Manufacturing of silicon-containing cold-rolled steel sheets) In the step of obtaining the pre-annealed Fe-based electroplated steel sheet, first, a Si-containing cold-rolled steel sheet containing 0.5 to 3.0 mass% of Si is produced. The Si-containing cold-rolled steel sheet can be produced according to a normal method for producing a cold-rolled steel sheet. As an example, the high-strength pre-annealed cold-rolled steel sheet is obtained by hot-rolling a steel slab having the above-mentioned composition to obtain a hot-rolled sheet, which is then pickled and then cold-rolled. This allows the production of a Si-containing cold-rolled steel sheet.

[0052] (Fe-based electroplating treatment) In the step of obtaining the Fe-based electroplated steel sheet, the surface of the obtained Si-containing cold-rolled steel sheet is subjected to an Fe-based electroplating treatment to produce the Fe-based electroplated steel sheet. The method of the Fe-based electroplating is not particularly limited.

[0053] For example, as an Fe-based electroplating bath, a sulfuric acid bath, a hydrochloric acid bath, or a mixture of the two can be used. The Fe ion content in the Fe-based electroplating bath before the start of current application is 2+ The Fe ion content in the Fe-based electroplating bath is preferably 1.0 mol / L or more. 2+ If the concentration is 1.0 mol / L or more, a sufficient amount of Fe can be attached. The Fe-based electroplating bath may contain Fe ions, as well as alloying elements such as B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co, and may also contain conductivity enhancers such as sodium sulfate and potassium sulfate as additives or impurities. The above-mentioned metal elements may be contained as metal ions, and nonmetallic elements may be contained as parts of boric acid, phosphoric acid, nitric acid, organic acids, etc. The iron sulfate plating solution may also contain conductivity enhancers such as sodium sulfate and potassium sulfate, chelating agents, and pH buffers. Other conditions for the Fe-based electroplating bath are not particularly limited. The bath temperature is preferably 30° C. or higher in consideration of the ability to maintain a constant temperature. The pH of the Fe-based electroplating bath is not particularly limited, but is preferably 3.0 or lower in consideration of the electrical conductivity of the Fe-based electroplating bath. The current density is not particularly limited, but is usually 10 to 150 A / dm 2 The sheet passing speed during plating may be from 5 mpm to 150 mpm. If the sheet passing speed is less than 5 mpm, the productivity is poor, while if the sheet passing speed is 150 mpm or more, it is difficult to stably control the coating weight.

[0054] As a treatment before the Fe-based electroplating, a degreasing treatment and water washing for cleaning the surface of the Si-containing cold-rolled steel sheet, and further, an acid pickling treatment and water washing for activating the surface of the Si-containing cold-rolled steel sheet may be performed. Following these pretreatments, the Fe-based electroplating treatment is performed. The method of the degreasing treatment and the water washing is not particularly limited, and a conventional method can be used. For the pickling treatment, various acids such as sulfuric acid, hydrochloric acid, nitric acid, and mixtures thereof can be used. Among these, it is preferable to use sulfuric acid, hydrochloric acid, or mixtures thereof. In addition, the concentration of the acid used in the pickling treatment is not particularly specified, but considering the ability to remove the oxide film and the prevention of roughness (surface defects) due to excessive pickling, it is preferable that the concentration is about 1 to 20 mass %. In addition, the pickling treatment liquid may contain an antifoaming agent, a pickling promoter, a pickling inhibitor, etc.

[0055] (Annealing) In the method for producing an Fe-based electroplated steel sheet of the present invention, the pre-annealed Fe-based electroplated steel sheet is annealed in an atmosphere having a dew point of -30°C or lower and a hydrogen concentration of 8% by volume or lower. Annealing can remove distortion of the Fe-based electroplated steel sheet before annealing that occurs during the rolling process, recrystallize the structure, and increase the strength of the steel sheet. In addition, annealing can reduce the content of diffusible hydrogen in the steel.

[0056] In the method for producing an Fe-based electroplated steel sheet of the present invention, the dew point of the annealing atmosphere in the annealing is set to a low dew point of −30° C. or less, which is a condition that does not require additional equipment such as a humidification equipment. The present inventors have found through their own investigations that there is a correlation between the degree of integration of the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet and the dew point of the annealing atmosphere in the annealing step after the formation of the Fe-based electroplated layer. That is, when annealing the pre-annealed Fe-based electroplated steel sheet after the formation of the Fe-based electroplated layer, the lower the dew point of the annealing atmosphere, the higher the degree of integration of the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet obtained after annealing, and conversely, the higher the dew point of the annealing atmosphere, the lower the degree of integration of the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet. The reason why a correlation is found between the degree of integration of the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet and the dew point is not clear, but it can be assumed as follows. When the dew point is controlled to a certain level or higher, elements that diffuse from the steel sheet to the Fe-based electroplating layer during annealing form oxides inside the Fe-based electroplating layer, and these oxides inhibit the crystal growth of the Fe-plated grains and cause them to become finer. On the other hand, when the Fe-based electroplating layer is formed and annealed in an atmosphere with a low dew point, the oxides are not easily formed, and the crystal grain size of the Fe-based electroplating layer becomes coarser. Therefore, when annealing is performed at a low dew point, it can be considered that the crystal orientation of the Fe-based electroplating layer is integrated with the crystal orientation of the Si-containing cold-rolled steel sheet at a high rate. When the dew point of the annealing atmosphere in the annealing is set to -30°C or lower, the degree of integration of the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet increases. As a result, the diffusion paths of Si and Mn are reduced, and external oxidation of Si and Mn during annealing can be efficiently suppressed. In addition, it is more preferable that the dew point of the annealing atmosphere is -40°C or less, since it is possible to promote integration of the crystal orientation. There is no particular lower limit for the dew point of the annealing atmosphere, but since it is difficult to industrially achieve a dew point of less than -80°C, it is preferable to set it to -80°C or higher. The dew point of the annealing atmosphere is more preferably -55°C or higher.

[0057] The hydrogen concentration in the atmosphere during the annealing is required to be 8.0% by volume or less. Although hydrogen can suppress the oxidation of Fe on the surface of the Fe-based electroplated steel sheet before annealing during annealing and can play a role in activating the steel sheet surface, if the concentration is too high, hydrogen may penetrate into the steel sheet and deteriorate the delayed fracture resistance. Therefore, from the viewpoint of suppressing hydrogen penetration into the steel, the hydrogen concentration in the atmosphere during the annealing is required to be 8.0% by volume or less, and is preferably 5.0% by volume or less. Furthermore, if the hydrogen concentration in the atmosphere during the annealing is 1.0% by volume or more, the oxidation of the steel sheet can be suppressed by oxidizing Fe on the steel sheet surface. Therefore, the hydrogen concentration in the annealing is preferably 1.0% by volume or more, and more preferably 2.0% by volume or more. The balance of the annealing atmosphere other than hydrogen is preferably nitrogen.

[0058] In addition, in the annealing, the holding time in the temperature range of 650°C to 900°C is preferably 30 seconds to 600 seconds. By holding the time in this temperature range for 30 seconds or more, the natural oxide film of Fe formed on the surface of the Fe-based electroplated layer before annealing can be suitably removed, and as described below, the chemical conversion treatability can be improved when a chemical conversion coating is provided on the surface of the Fe-based electroplated steel sheet. Therefore, the holding time in this temperature range is preferably 30 seconds or more. There is no particular upper limit for the holding time in this temperature range, but from the viewpoint of productivity, the holding time in this temperature range is preferably 600 seconds or less.

[0059] The maximum temperature of the Fe-based electroplated steel sheet before annealing is not particularly limited, but is preferably 650°C or more and 900°C or less. By setting the maximum temperature of the Fe-based electroplated steel sheet before annealing to 650°C or more, the recrystallization of the steel sheet structure proceeds favorably, and the desired strength can be obtained. Furthermore, if the maximum temperature of the Fe-based electroplated steel sheet is 900°C or less, the diffusion rate of Si and Mn in the steel can be prevented from increasing too much, and the diffusion of Si and Mn to the steel sheet surface can be prevented, so that the chemical conversion treatability can be improved. Furthermore, if the maximum temperature is 900°C or less, damage to the furnace body of the heat treatment furnace can be prevented, and costs can be reduced. Therefore, the maximum temperature of the Fe-based electroplated steel sheet before annealing is preferably 900°C or less. The above maximum temperature is based on the temperature measured on the surface of the Fe-based electroplated steel sheet before annealing.

[0060] Other conditions for the step of obtaining the pre-annealed Fe-based electroplated steel sheet and the step of obtaining the Fe-based electroplated steel sheet are similar to those described in the Fe-based electroplated high-strength steel sheet of the present invention. EXAMPLES

[0061] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.

[0062] <Sample 1-79> (1) Steel plates A to O having a thickness of 1.4 mm were obtained by melting steel having the chemical compositions shown in Table 1 and subjecting the resulting cast pieces to hot rolling, pickling, and cold rolling. (2) Each of the obtained steel sheets was subjected to an alkaline degreasing treatment, and then Fe-based electroplating and annealing were carried out under the conditions shown in Table 2 to produce samples of Fe-based electroplated steel sheets. The Fe-based electroplating bath used was a solution containing 1.5 mol / L Fe2+ and 0.35 mol / L sodium sulfate, with the pH adjusted to 2.0 with sulfuric acid, and an iridium oxide electrode was used as the anode. 2) was controlled by changing the current flow time. The ratio (%) of the integration of these crystal orientations at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet was determined by processing three arbitrary locations of each sample with a focused ion beam to prepare an observation sample, taking an SIM image of the observation sample using a scanning ion microscope, and determining the ratio of the integration of the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet from the SIM images taken based on formula (1), and calculating the average value of the three locations. Formula (1): Percentage of integrated crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet at the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet = (length of the interface between the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet where the crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet are integrated) ÷ (length of the interface in the observation field) × 100 (%) Table 2 shows the deposition weight of the Fe-based electroplated layer and the ratio of the crystal orientation of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet that are integrated for each sample. Annealing was performed at a temperature of 800° C. in a nitrogen atmosphere having a dew point and containing hydrogen at the content shown in Table 2. Table 2 also shows which of the Fe-based electroplating and the annealing was performed first.

[0063] <Evaluation> The following evaluations were carried out on each sample of Fe-based electroplated steel sheet obtained as described above. The evaluation results are shown in Table 2.

[0064] (1) Chemical conversion treatment Test pieces taken from the Fe-based electroplated steel sheets of each sample were treated with Nihon Parkerizing Co., Ltd.'s degreaser FC-E2011, surface conditioner PL-Z, and chemical conversion coating agent Palbond PB-SX35 under the following standard conditions until the chemical conversion coating had a coating weight of 2.0 to 3.0 g / m. 2 Chemical conversion treatment was carried out so that the (Conversion treatment conditions) Degreasing process: Processing temperature 43°C, processing time 120 seconds Spray degreasing, surface conditioning process: pH 9.5, processing temperature room temperature, processing time 20 seconds Chemical conversion treatment process: Chemical conversion treatment solution temperature 35℃, treatment time 90 seconds (Chemical conversion treatment evaluation) The surface of each test piece (n=1) that had been subjected to the chemical conversion treatment was observed with a SEM at a magnification of 1000 times, and evaluated according to the following criteria. ◎: The grain size of the chemical crystals is 5μm or less and no unprecipitated areas are observed. ○: The grain size of the chemical crystals is 5μm or more, but no unprecipitated areas are observed. ×: The grain size of the formed crystals is 5 μm or more and unprecipitated areas are observed.

[0065] (2) Corrosion resistance The surfaces of the test pieces that had been subjected to chemical conversion treatment under the same conditions as in the evaluation of chemical conversion treatability (1) above were electrocoated with an electrodeposition paint: GT-100 manufactured by Kansai Paint Co., Ltd. to a film thickness of 15 μm, and then subjected to the following corrosion test. (Salt water immersion test conditions) A cross-cut scratch 45 mm long was made with a cutter on the surface of the above test piece (n=1) that had been subjected to chemical conversion treatment and electrocoating, and the test piece was then immersed in a 5 mass% NaCl solution (60°C) for 360 hours, and then washed with water and dried. (Corrosion resistance evaluation) A tape peeling test was performed in which adhesive tape was applied to the cut flaw and then peeled off. The maximum total peel width of the cut flaw, including both the left and right sides, was measured and evaluated according to the following criteria. ◎: Maximum peel width is 3.0mm or less ○: Maximum peel width is 5.0mm or less ×: Maximum peel width exceeds 5.0 mm

[0066] (3) Delayed fracture resistance (3-1) Hydrogen content in steel For each sample of Fe-based electroplated steel sheet, the test pieces after annealing were stored in liquid nitrogen in order to suppress an increase in the temperature of the test pieces and the escape of hydrogen from the steel. The test piece was then heated to 250°C at a heating rate of 100°C / s in an Ar atmosphere, and the amount of released hydrogen gas was measured by gas chromatography.

[0067] (3-2) Evaluation of delayed fracture properties Each sample of Fe-based electroplated steel sheet was tightened with a bolt so that a specified stress was generated at the bent tip (see Fig. 4). As shown in Fig. 3, the temperature was 10°C and the salt deposition amount was 10,000 mg / m 2 The occurrence of cracks was confirmed when a cycle of dry and wet conditions (relative humidity of 30% and 90% was repeated for 2 hours each, with salt water applied twice a week for 8 hours per cycle) was carried out over a period of 40 days under the above conditions. Evaluation was based on the following criteria. ○: No cracks for 40 days ×: Cracks occurred

[0068] (4) Tensile strength (TS) JIS No. 5 tensile test pieces (JIS Z 2201) were taken from each sample of Fe-based electroplated steel sheet in the direction perpendicular to the rolling direction, and tensile tests were conducted at a tension speed (crosshead speed) of 10 mm / min. The tensile strength TS was calculated by dividing the maximum load in the tensile test by the initial cross-sectional area of ​​the parallel part of the test piece. The thickness of the plated steel sheet used to calculate the cross-sectional area of ​​the parallel part was the thickness including the plating.

[0069] [Table 1]

[0070] [Table 2]

[0071] From the results in Table 2, it can be seen that all of the samples of the present invention have good chemical conversion treatability and corrosion resistance, and by annealing after Fe electroplating, the amount of hydrogen in the steel is small and the delayed fracture resistance is also excellent. In addition, in all of the samples of the present invention, the proportion of the crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet that are integrated at the interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet was 50% or more. [Industrial Applicability]

[0072] According to the present invention, there can be provided an Fe-based electroplated high-strength steel sheet having excellent chemical conversion treatability, corrosion resistance after painting, and excellent delayed fracture resistance, and a manufacturing method thereof.

Claims

1. In mass percent, Si: 0.5-3.0%, C: 0.8% or less, Mn: 1.5-3.5%, P: 0.1% or less, S: 0.03% or less, and Al: 0.1% or less and a Si-containing cold-rolled steel sheet having a composition consisting of Fe and unavoidable impurities and having a tensile strength of 980 MPa or more; The Si-containing cold-rolled steel sheet has a coating weight of 1.0 to 20.0 g / m 2 and an Fe-based electroplating layer, wherein no plating layer other than the Fe-based electroplating is formed on the surface of the Si-containing cold-rolled steel sheet, The content of diffusible hydrogen in the steel is 0.21 mass ppm or less, A Fe-based electroplated high-strength steel sheet, characterized in that a ratio of crystal orientations of the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet that are integrated at an interface between the Fe-based electroplated layer and the Si-containing cold-rolled steel sheet is more than 50%.

2. The composition of the Si-containing cold-rolled steel sheet further comprises, in mass%, B: 0.005% or less, Ti: 0.2% or less, N: 0.010% or less, Cr: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Mo: 1.0% or less, Nb: 0.20% or less, V: 0.5% or less, Sb: 0.200% or less, Ta: 0.1% or less, W: 0.5% or less, Zr: 0.1% or less, Sn: 0.20% or less, Ca: 0.005% or less, Mg: 0.005% or less; and REM: 0.005% or less The Fe-based electroplated high-strength steel sheet according to claim 1, further comprising at least one selected from the group consisting of:

3. 3. The Fe-based electroplated high-strength steel sheet according to claim 1, wherein the Fe-based electroplated layer has a composition containing one or more elements selected from the group consisting of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V, and Co in a total amount of 10 mass% or less, with the balance being Fe and unavoidable impurities.

4. In mass percent, Si: 0.5-3.0%, C: 0.8% or less, Mn: 1.5-3.5%, P: 0.1% or less, S: 0.03% or less, and Al: 0.1% or less and the balance being Fe and unavoidable impurities. The Si-containing cold-rolled steel sheet has a tensile strength of 980 MPa or more, and is subjected to Fe-based electroplating to obtain a coating weight of 1.0 to 20.0 g / m on one side. 2 a step of obtaining a pre-annealed Fe-based electroplated steel sheet, the pre-annealed Fe-based electroplated layer being formed on at least one side of the steel sheet, and no plating layer other than the Fe-based electroplating being formed on the surface of the Si-containing cold-rolled steel sheet; annealing the pre-annealed Fe-based electroplated steel sheet in an atmosphere having a dew point of −30° C. or less and a hydrogen concentration of 8 vol.% or less to obtain a Fe-based electroplated steel sheet; Including, a rate at which crystal orientations of the Fe-based electroplating layer and the Si-containing cold-rolled steel sheet are integrated at an interface between the formed Fe-based electroplating layer and the Si-containing cold-rolled steel sheet exceeds 50%.

5. 5. The method for producing an Fe-based electroplated steel sheet according to claim 4, wherein the atmosphere during the annealing has a dew point of −40° C. or less and a hydrogen concentration of 5 volume % or less.

Citation Information

Patent Citations

  • Cold rolled steel sheet having excellent phosphating property

    JP1986113787A

  • High strength cold rolled steel sheet excellent in corrosion resistance after coating

    JP1993320952A

  • Method and apparatus for producing high-strength cold-rolled steel sheet excellent in chemical conversion

    JP2008190030A

  • Nitrided slide member, steel material for slide member and method for manufacturing slide member

    JP2010270348A

  • High-tensile strength steel sheet having superior bending property and low-temperature toughness, and method for manufacturing the same

    JP2012036499A