Filament 3D joint manufacturing equipment
By employing hydrophilic layers and surface configurations on guide members, the manufacturing process achieves a uniform three-dimensional filament assembly with consistent adhesive strength, addressing issues of water film retention and filament movement.
Patent Information
- Application Number
- JP2023173551
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-05
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2043-10-05
AI Technical Summary
Existing methods for manufacturing three-dimensional filament assemblies face challenges in forming a uniform cooling water film on the chute surface, leading to irregular filament movement and reduced adhesive strength at fusion points, due to inconsistent water retention and surface tension issues.
The use of hydrophilic layers on guide members with specific surface configurations, including grooves and inclined surfaces, to enhance water film retention and stabilize molten filament movement, ensuring uniform assembly formation.
This approach allows for the creation of a more uniform three-dimensional filament assembly without compromising adhesive strength at fusion points, improving the consistency and quality of the manufacturing process.
Smart Images

Figure 0007578317000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus for manufacturing a three-dimensional filament assembly that can be used as a cushioning material for mattresses, pillows, and the like. [Background technology]
[0002] As a cushioning material that overcomes the drawbacks of metal springs and urethane foam, which are difficult to recycle, a three-dimensional filament bonded body (three-dimensional network structure) obtained by three-dimensionally fusing and bonding filaments made of thermoplastic elastomers has been attracting attention. This cushioning material has the advantages of being easy to recycle, not easily becoming stuffy, and being washable.
[0003] As a method for producing a three-dimensional filament bond, for example, Patent Document 1 describes a method in which a group of molten filaments (a linear aggregate of molten thermoplastic resin) consisting of a large number of molten filaments flowing vertically downward is dropped into cooling water, and molten filament loops are formed by the buoyancy of the water, while at the same time the molten filaments are brought into contact with each other due to the bending that occurs when the loops are formed, and the contact points are fused and bonded to produce a three-dimensional filament bond (a three-dimensional network structure).
[0004] Patent Document 1 also describes that in order to keep the thickness of the three-dimensional filament bond constant, a pair of chutes (guide members) are provided that are inclined from both ends of the molten filaments in the thickness direction toward the center of the molten filaments in the thickness direction, and that in order to spread cooling water over the entire surface of the chute, the chute surface is covered with a water-permeable sheet such as bleached cloth, and cooling water is supplied to the water-permeable sheet to form a cooling water layer over the entire surface of the chute. Spreading the cooling water has the effect of preventing the molten filaments from adhering to the chute surface.
[0005] However, the method of covering the chute surface with a water-permeable sheet has drawbacks such as wrinkles on the water-permeable sheet, adhesion of foreign matter (rust, etc.), wear and tear of the water-permeable sheet over a long period of production, etc. As a method to overcome these drawbacks, Patent Document 2 describes a method of roughening the chute surface by sandblasting, thereby forming a cooling water layer on the chute surface without using a water-permeable sheet.
[0006] Fig. 10(a) is a conceptual diagram showing the state when surface 531a of chute (guide member) 531 is roughened by sandblasting. As shown in the figure, unevenness is formed on surface 531a. Fig. 10(b) shows how cooling water supplied to surface 531a of chute 531 is retained or decelerated by the unevenness, forming a cooling water film W. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-218116 A [Patent Document 2] International Publication No. 2012 / 35736 Summary of the Invention [Problem to be solved by the invention]
[0008] However, in sandblasting, it is difficult to make the depth and width of the recesses constant over the entire area of the chute surface, and because the inclination angle of the recesses is small, the ability to retain or slow down the cooling water is low, and when there is little cooling water, it is difficult to form a uniform thin film of cooling water. Even locally, in areas with shallow recesses (areas that are relatively convex), the ability to retain or slow down the cooling water is reduced, so even if cooling water is supplied to the chute surface, it may flow down without forming a cooling water film due to the surface tension of the water. As a result, there was a problem that the molten filament temporarily adhered to the chute surface where the cooling water film was not formed, and the speed at which it moved over the chute surface became irregular, resulting in uneven filament 3D bonding.
[0009] In addition, if the amount of cooling water supplied is increased in order to reliably form a cooling water film on the chute surface, the molten filaments cool, causing a problem of a decrease in the adhesive strength at the fusion points between the molten filaments. In addition, if the chute surface is made rough overall in order to retain or slow down the cooling water in areas with shallow recesses, the molten filaments become less likely to slip on the chute surface, which creates a trade-off problem in that the molten filaments tend to temporarily adhere to each other.
[0010] The present invention has been made in consideration of the above-mentioned problems, and aims to provide an apparatus for manufacturing a three-dimensional filament bonded body that is capable of forming a more uniform three-dimensional filament bonded body without reducing the adhesive strength at the fusion points between the molten filaments. [Means for solving the problem]
[0011] In order to achieve the above-mentioned object, a manufacturing apparatus for a three-dimensional bound filament body according to one embodiment of the present invention is a manufacturing apparatus for a bound body in which a large number of filaments are bound in three dimensions, and is characterized in that it comprises a molten filament supply unit that supplies a group of molten filaments consisting of a large number of straight molten filaments, a pair of guide members that are spaced apart in a first direction perpendicular to the supply direction of the group of molten filaments and have inclined surfaces that receive both ends of the group of molten filaments in the first direction and guide them toward the opposing sides, and a cooling water supply unit that supplies cooling water to the inclined surfaces of the guide members, and is characterized in that the pair of guide members have a hydrophilic layer on the surface of the inclined surfaces.
[0012] In this specification, "hydrophilic" refers to a contact angle with water of less than 90. The term "hydrophilic layer" refers to a layer that has water film retention properties in the water film retention evaluation method described below.
[0013] In the manufacturing apparatus having the above configuration, it is preferable that the hydrophilic layer is a plated layer made of at least one metal selected from the group consisting of chromium (Cr), tin (Sn), zinc (Zn), titanium (Ti), nickel (Ni), cadmium (Cd), aluminum (Al), gold (Au), silver (Ag), lead (Pb), and platinum (Pt).
[0014] In addition, in the manufacturing apparatus of the above configuration, the pair of guide members may have an inclined portion having the inclined surface, and a parallel portion connected to the downstream end of the inclined portion in the supply direction of the group of molten filaments and extending parallel to the supply direction of the group of molten filaments downstream in the supply direction, and the opposing side surfaces of the parallel portion may also have a hydrophilic layer on their surfaces.
[0015] In the manufacturing apparatus configured as described above, a number of grooves may be formed in the inclined surfaces of the pair of guide members in a direction intersecting a second direction perpendicular to the first direction.
[0016] It is preferable that the numerous grooves extend in parallel at predetermined intervals.
[0017] It is also preferable that the cross-sectional shape of the numerous grooves perpendicular to the extending direction is any one of a triangular shape, a rectangular shape, and a circular arc shape.
[0018] The intersecting angle between the plurality of grooves and the second direction may be 90°.
[0019] The numerous grooves may also include a first groove group having an intersecting angle with the second direction of 30° or more and 60° or less, and a second groove group having an intersecting angle with the second direction of 120° or more and 150° or less.
[0020] It is preferable that the grooves of the first groove group extend in parallel at a predetermined interval, and that the grooves of the second groove group also extend in parallel at a predetermined interval.
[0021] In this specification, unless otherwise specified, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit. Effect of the Invention
[0022] According to the manufacturing device of the present invention, it is possible to form a more uniform three-dimensional bound filament body without reducing the adhesive strength at the fusion points between the molten filaments. [Brief description of the drawings]
[0023] [Figure 1] 1 is a conceptual diagram of a manufacturing apparatus for a three-dimensional filament assembly according to a first embodiment. [Diagram 2] 2 is a cross-sectional view taken along line AA' of the manufacturing apparatus shown in FIG. [Diagram 3] FIG. 4 is a bottom view of the nozzle portion according to the first embodiment. [Figure 4] FIG. 2 is a perspective view of the chute according to the first embodiment. [Diagram 5] 5 is a cross-sectional view perpendicular to the left-right direction of the chute in FIG. 4. [Figure 6] FIG. 11 is a perspective view of a chute according to a second embodiment. [Figure 7]7 is a cross-sectional view perpendicular to the front-rear direction of the chute in FIG. 6. [Figure 8] FIG. 11 is a perspective view of a chute according to a third embodiment. [Figure 9] 9 is a cross-sectional view perpendicular to the front-rear direction of the chute of FIG. 8. [Figure 10] FIG. 1 is a schematic diagram of a conventional chute having a roughened surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the "front-rear direction" corresponds to the "first direction," the "left-right direction" corresponds to the "second direction," and the direction from top to bottom corresponds to the "supply direction" of the molten filament group. In addition, in the following embodiments, the same or corresponding configurations may be denoted by the same reference numerals, and the description may be omitted as appropriate.
[0025] (First embodiment) First, a first embodiment of the present invention will be described. Fig. 1 is a conceptual diagram of a manufacturing apparatus 1 for a three-dimensional bound filament body according to the first embodiment of the present invention. Fig. 2 is a cross-sectional view of the manufacturing apparatus 1 shown in Fig. 1 taken along line A-A'.
[0026] The manufacturing apparatus 1 for manufacturing a three-dimensional filament bond includes a molten filament supply unit 10 that discharges a molten filament group MF consisting of a large number of molten filaments with diameters of 0.5 mm to 3 mm vertically downward, a pair of chutes (guide members) 5a, 5b that receive both front-to-rear end portions of the molten filament group MF and guide them toward the center of the molten filament group MF in the front-to-rear direction, in other words, that shift the molten filament group MF in a direction that reduces its thickness in the front-to-rear direction, cooling water supply units 4a, 4b that supply cooling water to the upper portions of the chutes 5a, 5b, and a fusion bond forming unit 20 that entangles the molten filament group MF in a three-dimensional manner and simultaneously fusion-bonds the contact points, and then cools and solidifies the fusion bond forming unit 20 to form a three-dimensional filament bond.
[0027] (Melted filament supply section) The molten filament supply section 10 includes a pressure melting section (extruder) 11 and a filament discharge section (die) 12. The pressure melting section 11 includes a cylinder 11a, a screw 14 rotatably housed in the cylinder 11a, a screw motor 15 that drives the screw 14, a heater 16 that heats the cylinder 11a, a material input section (hopper) 13 for inputting thermoplastic resin into the cylinder 11a, and a plurality of temperature sensors (not shown). The thermoplastic resin supplied from the material input section 13 is heated and melted by the heater 16 and transported forward by the screw 14.
[0028] A cylinder outlet 11b is formed at the front end of the cylinder 11a for discharging the thermoplastic resin toward the filament discharge part 12. The heating temperature of the heater 16 is controlled based on a detection signal of a temperature sensor provided in the molten filament supply part 10, for example.
[0029] The filament discharge section 12 includes a nozzle section 17, a die heater 18, and a plurality of temperature sensors (not shown). Inside the filament discharge section 12, a guide passage 12a is formed to guide the molten thermoplastic resin discharged from the cylinder outlet 11b to the nozzle section 17.
[0030] The nozzle section 17 is a thick metal plate having a substantially rectangular parallelepiped shape in which a large number of nozzle holes 17a (shown in FIG. 3) are formed, and is provided in the lower part of the filament discharge section 12, which corresponds to the most downstream part of the guide channel 12a. The large number of nozzle holes 17a formed in the nozzle section 17 will be described later with reference to FIG. 3.
[0031] A plurality of die heaters 18 (six die heaters 18a to 18f in the example shown in FIG. 2) are provided in the left-right direction and heat the guide passage 12a of the filament discharge section 12. The heating temperature of the die heater 18 is controlled based on a detection signal of a temperature sensor (not shown) provided in the filament discharge section 12, for example.
[0032] Examples of thermoplastic resins that can be used as materials for the filament three-dimensional bonded body include polyolefin resins such as polyethylene and polypropylene, polyester resins such as polyethylene terephthalate, polyamide resins such as nylon 66, polyvinyl chloride resins, and polystyrene resins, as well as thermoplastic elastomers such as styrene-based elastomers, PVC-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, nitrile-based elastomers, polyamide-based elastomers, and fluorine-based elastomers.
[0033] The thermoplastic resin supplied from the material input section 13 is heated and melted in the cylinder 11a, and is extruded by the screw 14, and is supplied as molten thermoplastic resin from the cylinder outlet 11b to the guide channel 12a of the filament discharge section 12. Thereafter, the molten filaments are discharged downward from each of the multiple nozzle holes 17a of the nozzle section 17, and a molten filament group MF is formed.
[0034] (Fusion joint forming part) The fusion bond forming section 20 forms loops of the molten filaments by the buoyancy of the water, and at the same time, the molten filaments come into contact with each other by the bending caused by the loop formation, and the contact points are fusion bonded and then cooled and solidified to form a three-dimensional bond. The fusion bond forming section 20 has a cooling water tank 23, a pair of conveyors 24a, 24b, and a plurality of transport rollers 25a to 25h. The cooling water tank 23 is a water tank for storing cooling water. Inside the cooling water tank 23, a pair of conveyors 24a, 24b and a plurality of transport rollers 25a to 25h are arranged. The pair of conveyors 24a, 24b and the plurality of transport rollers 25a to 25h are driven by a drive motor (not shown).
[0035] (Nozzle part) 3 is a bottom view of the nozzle portion 17. A large number of nozzle holes 17a for discharging the molten filament group MF are formed in the nozzle portion 17. In the example of this embodiment, the cross-sectional shape of the nozzle holes 17a is a circle with an inner diameter of 1 mm, and the distance (pitch) between adjacent nozzle holes 17a is 10 mm. However, based on the specifications of the filament three-dimensional combined body to be manufactured, the shape, inner diameter, spacing between adjacent nozzle holes 17a, and arrangement pattern of each nozzle hole 17a can be appropriately adjusted.
[0036] (Shoot) Fig. 4 is a schematic perspective view of the pair of chutes 5a, 5b shown in Fig. 1. Fig. 5 is a cross-sectional view perpendicular to the left-right direction of the pair of chutes 5a, 5b. In the following description of the chutes 5a, 5b, only one of the chutes 5a and 5b will be described, and the description of the other may be omitted.
[0037] A pair of chutes 5a, 5b receive both front-to-rear end portions of the molten filament group MF supplied from the molten filament supply section 10, guide them toward the center of the molten filament group MF in the front-to-rear direction, and shift the molten filament group MF in a direction that reduces its front-to-rear thickness, thereby adjusting the front-to-rear thickness of the molten filament group MF and, ultimately, the front-to-rear thickness of the three-dimensional filament bond.
[0038] The pair of chutes 5a, 5b are arranged facing each other at a predetermined distance in the front-rear direction (first direction). Specifically, the pair of chutes 5a, 5b are arranged symmetrically with respect to a virtual plane VP (shown in FIG. 5) including the front-rear direction and the left-right direction. The pair of chutes 5a, 5b have inclined portions 51a, 51b that face the opposing chute as they move toward the downstream side of the supply direction of the molten filament group MF, and parallel portions 52a, 52b that are connected to the downstream ends of the inclined portions 51a, 51b and extend downstream in the supply direction in parallel with the supply direction of the molten filament group MF. The inclined portions 51a, 51b and the parallel portions 52a, 52b are integrally formed. The material of the inclined portions 51a, 51b and the parallel portions 52a, 52b is not particularly limited as long as it has a predetermined heat resistance, rust resistance, processability, etc., and examples of the material include metals such as stainless steel, aluminum, and copper, and heat-resistant resins such as polycarbonate. Among these, metal materials such as stainless steel and copper are preferably used.
[0039] The inclined portions 51a, 51b receive both ends of the molten filament group MF in the front-rear direction and guide them toward the center of the molten filament group MF in the front-rear direction. The parallel portions 52a, 52b adjust the thickness of the molten filament group MF in the front-rear direction, and thus the thickness of the 3-dimensional bound filament body in the front-rear direction. The upper surfaces of the inclined portions 51a, 51b form inclined surfaces 53a, 53b.
[0040] As shown in Fig. 5, the pair of chutes 5a, 5b have a continuous hydrophilic layer HL on the surfaces of the inclined surfaces 53a, 53b and the opposing inner surfaces of the parallel parts 52a, 52b. The hydrophilic layer HL has a preferred contact angle with water of 30° or less, more preferably 10° or less. In the present invention, the hydrophilic layer HL is formed at least on the inclined surfaces 53a, 53b, and does not need to be formed up to the opposing inner surfaces of the parallel parts 52a, 52b. However, from the viewpoint of forming a more uniform filament three-dimensional bond TDF, it is preferable that the hydrophilic layer HL is formed at least up to the upper part exposed above the water surface of the stored water in the cooling water tank 23 (the middle part of the parallel part in the manufacturing apparatus shown in Figs. 1 and 2).
[0041] Both ends of the molten filament group MF consisting of a large number of linear molten filaments discharged from the nozzle portion 17 are received by the inclined surfaces 53a, 53b of the pair of chutes 5a, 5b and guided toward the center of the molten filament group MF in the front-rear direction. At this time, since a hydrophilic layer HL is formed on the surfaces of the inclined surfaces 53a, 53b of the pair of chutes 5a, 5b, the cooling water supplied from the cooling water supply units 4a, 4b described later flows evenly over the entire inclined surfaces 53a, 53b, and a cooling water film is stably formed on the surfaces of the inclined surfaces 53a, 53b. As a result, the molten filament group MF received by the pair of chutes 5a, 5b is smoothly guided toward the center of the front-rear direction, the thickness (front-rear dimension) is adjusted, and a precursor of a uniform filament three-dimensional bond is formed.
[0042] The hydrophilic layer HL provided on the inclined surfaces 53a and 53b may be a plating layer of at least one metal selected from the group consisting of chromium (Cr), tin (Sn), zinc (Zn), nickel (Ni), titanium (Ti), cadmium (Cd), aluminum (Al), gold (Au), silver (Ag), lead (Pb), and platinum (Pt). Among these, a plating layer of at least one metal selected from the group consisting of chromium (Cr), tin (Sn), zinc (Zn), and nickel (Ni) is preferred.
[0043] The plating method is not particularly limited, and may be any method such as hot-dip plating, electroplating, penetration plating, thermal spraying, chemical plating, etc. The thickness of the hydrophilic layer HL formed by these plating methods is not particularly limited, but is usually preferably in the range of 0.1 μm to 300 μm.
[0044] The hydrophilic layer HL of the present invention may be a composite plating layer in which hydrophilic particles are dispersed in the plating layer. Examples of the hydrophilic particles include PTFE (polytetrafluoroethylene) particles that have been hydrophilized by sodium treatment, hydrophilic silica, nanodiamond, SiC (silicon carbide), and BN (boron nitride) particles that are coated with a surfactant.
[0045] (Hydrophilic resin layer) The material constituting the hydrophilic layer in the present invention may be a resin material or an inorganic material as long as it has heat resistance, in addition to a metal plating material. Examples of hydrophilic resin materials include polyvinyl alcohol, polyacrylic acid, polystyrene sulfonic acid, polyacrylamide, polyethylene glycol, polysaccharides, and gelatin. The polysaccharides or gelatin may be derivatives thereof, and examples thereof are not particularly limited, and examples thereof include compounds into which any substituent has been introduced. Among them, from the viewpoint of imparting hydrophilicity, the substituents are preferably carboxyl groups, phosphonyl groups, phosphoryl groups, sulfo groups, boric acid groups, hydroxyl groups, and amino groups. Examples of hydrophilic inorganic materials include glass. As the glass material, plate-shaped glass may be provided on the inclined surfaces 53a and 53b, or a glass coating agent may be used to cover the resin or metal surfaces of the inclined surfaces 53a and 53b.
[0046] The molecular weight of the hydrophilic resin to be used is not particularly limited, but is generally 1.0×10 4 ~1.0×10 7 is preferred, and 1.0×10 4 ~5.0×10 6 It is more preferable that the molecular weight is set to the lower limit or more, since defects due to repellency and the like can be reduced and the performance can be stabilized. On the other hand, it is preferable that the molecular weight is set to the upper limit or less, since the polymer is easily dissolved in a solvent during preparation and the manufacturing suitability can be improved.
[0047] (Cooling water supply section) The cooling water supply units 4a, 4b supply cooling water evenly and continuously to the inclined surfaces of the chutes 5a, 5b. The cooling water supply units 4a, 4b are provided above the upper ends of the chutes 5a, 5b, covering substantially the entire area of the chutes 5a, 5b in the front-rear direction (second direction). The cooling water supplied to the chutes 5a, 5b by the cooling water supply units 4a, 4b may be, for example, water supplied from outside the manufacturing apparatus 1, or a portion of the cooling water in the cooling water tank 23.
[0048] (Formation of 3D filament aggregates) The molten filament group MF discharged from the nozzle portion 17 has its thickness (front-rear dimension) adjusted by the chutes 5a and 5b, and then is deflected by the buoyancy of the cooling water in the cooling water tank 23, and each molten filament therein forms a random loop. The random loops are three-dimensionally entangled with adjacent random loops in a molten state, and the contact points are fused and bonded to form a three-dimensional filament bond.
[0049] Thereafter, the combined body is transported by a pair of conveyors 24a, 24b and a plurality of transport rollers 25a to 25h while being cooled by cooling water in the cooling water tank 23, and is discharged as a three-dimensional combined filament body TDF to the outside of the cooling water tank 21. In this manner, a three-dimensional combined filament body TDF is manufactured.
[0050] Second embodiment Next, a manufacturing apparatus according to a second embodiment of the present invention will be described. The manufacturing apparatus according to the second embodiment has basically the same configuration as the manufacturing apparatus according to the first embodiment, except for the configuration of the pair of chutes. In the following description, the emphasis will be placed on the differences from the first embodiment, and the description of the commonalities with the first embodiment may be omitted.
[0051] FIG. 6 is a perspective view of a pair of chutes 6a, 6b used in the second embodiment. In the pair of chutes 6a, 6b shown in FIG. 6, a number of grooves GL are formed in parallel at a predetermined interval on the inclined surfaces 63a, 63b of the inclined portions 61a, 61b in a direction perpendicular to the left-right direction (second direction) (θa=90°). The number of grooves GL are formed continuously from the lower ends of the inclined surfaces 63a, 63b to the opposing surfaces of the parallel portions 62a, 62b. Note that the number of grooves GL only needs to be formed on at least the inclined surfaces 63a, 63b, and does not need to be formed on the opposing surfaces of the parallel portions 62a, 62b. However, from the viewpoint of forming a more uniform filament three-dimensional combined body TDF, it is desirable that the number of grooves GL is formed at least up to the upper portion exposed above the water surface of the stored water in the cooling water tank 23 (the middle portion of the parallel portion in the manufacturing apparatus shown in FIG. 1 and FIG. 2).
[0052] 7 is a partial cross-sectional view of the inclined portions 61a and 61b that are perpendicular to the inclined surfaces 63a and 63b and parallel to the left-right direction. A hydrophilic layer HL is provided on the surfaces of the inclined surfaces 63a and 63b, including the inner peripheral surfaces of the numerous grooves GL. The material and forming method of the hydrophilic layer HL are the same as those exemplified in the first embodiment.
[0053] The cooling water supplied from the cooling water supply units 4a and 4b to the inclined surfaces 63a and 63b of the inclined parts 61a and 61b of the chutes 5a and 5b enters into a number of grooves GL formed on the upper surfaces of the inclined surfaces 63a and 63b. The flow rate of the cooling water that enters into the number of grooves GL slows down significantly and becomes trapped (stagnant or decelerated) water. Further cooling water is supplied from the cooling water supply units 4a and 4b, and the cooling water flowing down the inclined surfaces is held back by the surface tension of the trapped water in the number of grooves GL to form a film between two adjacent grooves GL, which are connected to form a more uniform thin film of cooling water over the entire inclined surface. As a result, the molten filament group MF received by the pair of chutes 6a and 6b is guided more smoothly toward the center in the front-rear direction, the thickness (front-rear dimension) is adjusted, and a uniform filament three-dimensional combined body TDF is formed.
[0054] In addition, since air bubbles may not be removed from the grooves GL immediately after the manufacturing apparatus 1 is started, water vapor may be supplied toward the inclined surfaces 63a, 63b of the chutes 6a, 6b before the manufacturing apparatus 1 is started to expel air bubbles from the numerous grooves GL.
[0055] There is no particular limitation on the size or shape of the groove GL, and it may be appropriately determined so that a uniform thin film of cooling water is formed on the inclined surfaces 63a, 63b of the chutes 6a, 6b. In general, the width (length in the left-right direction) of the groove GL is preferably in the range of 0.1 mm to 1.0 mm. The depth of the groove GL is preferably in the range of 0.1 mm to 3 mm. The interval between adjacent grooves GL is preferably in the range of 1 mm to 7 mm. There is no limitation on the shape of the cross section of the groove GL (cross section when cut on a plane perpendicular to the direction in which the groove GL extends), and it may be a polygon such as a triangle or a circular arc shape in addition to a rectangle. However, in the rectangle, the upper side is the opening surface of the groove GL. In this embodiment, the size and shape of the cross section are the same in all grooves GL.
[0056] Third embodiment Next, a manufacturing apparatus according to a third embodiment of the present invention will be described. The manufacturing apparatus according to the third embodiment has basically the same configuration as the manufacturing apparatus according to the second embodiment, except for the shape of the groove formed in the chute. In the following description, the emphasis will be placed on the differences from the second embodiment, and the description of the commonalities with the second embodiment may be omitted.
[0057] FIG. 8 is a perspective view of a pair of chutes 7a, 7b according to the third embodiment. The pair of chutes 7a, 7b shown in FIG. 8 has a first groove group G1 and a second groove group G2 that intersect with each other on the inclined surfaces 73a, 73b of the inclined portions 71a, 71b and the opposing surfaces of the parallel portions 72a, 72b. The first groove group G1 is composed of a number of first grooves GL1 that are parallel to each other at a predetermined interval and intersect with the left-right direction (second direction) at a predetermined angle θ1. The second groove group G2 is composed of a number of second grooves GL2 that are parallel to each other at a predetermined interval and intersect with the left-right direction (second direction) at a predetermined angle θ2. It is preferable that the intersecting angle θ1 of the first groove group G1 with respect to the left-right direction is in the range of 30° to 60°, and the intersecting angle θ2 of the second groove group G2 is in the range of 120° to 150°.
[0058] The first groove group G1 and the second groove group G2 are formed continuously from the lower ends of the inclined surfaces 73a, 73b to the mutually facing surfaces of the parallel parts 72a, 72b. Note that the first groove group G1 and the second groove group G2 only need to be formed on at least the inclined surfaces 73a, 73b, and do not need to be formed up to the mutually facing surfaces of the parallel parts 72a, 72b. However, from the viewpoint of forming a more uniform filament three-dimensional combined body TDF, it is desirable that the first groove group G1 and the second groove group G2 are formed at least up to the upper part exposed above the water surface of the stored water in the cooling water tank 23 (the middle part of the parallel part in the manufacturing device shown in FIG. 1 and FIG. 2).
[0059] 9 is a partial cross-sectional view of the inclined portions 71a and 71b that are perpendicular to the inclined surfaces 73a and 73b and parallel to the left-right direction. A hydrophilic layer HL is provided on the surfaces of the inclined surfaces 73a and 73b, including the inner peripheral surfaces of the grooves GL1 and GL2 of the first groove group G1 and the second groove group G2. The material and forming method of the hydrophilic layer HL are the same as those exemplified in the first embodiment.
[0060] The sizes and shapes of the grooves GL1, GL2 constituting the first groove group G1 and the second groove group G2 are the same as those exemplified in the second embodiment.
[0061] With the chutes 7a, 7b configured in this manner, as with the chutes 6a, 6b of the second embodiment, a portion of the cooling water supplied to the inclined surfaces 73a, 73b of the chutes 7a, 7b is reliably trapped (retained or slowed down) in the grooves GL1, GL2 of the first groove group G1 and the second groove group G2, and the supplied cooling water is further held back by the surface tension of the trapped water in the grooves GL1, GL2 of the first groove group G1 and the second groove group G2, forming a film between two adjacent grooves, which then connect to form a more uniform thin film of cooling water over the entire inclined surfaces 73a, 73b. In addition, in the chutes 7a and 7b of this embodiment, even if the angle of the inclined surfaces 73a and 73b of the chutes 7a and 7b is increased in the vertical direction to improve the sliding down of the molten filaments, the cooling water in the grooves GL1 and GL2 of the first groove group G1 and the second groove group G2 is prevented from stagnating or flowing down rapidly, and a uniform thin film of cooling water is formed and maintained on the inclined surfaces 73a and 73b. This prevents the molten filament group MF from adhering to the inclined surfaces 73a and 73b, and the molten filament group MF received by the chutes 7a and 7b is smoothly guided toward the center in the front-rear direction, the thickness (front-rear dimension) is adjusted, and a uniform filament three-dimensional combined body TDF is formed.
[0062] (Other variations) Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these embodiments. Addition, omission, substitution and other modifications of the configuration are possible without departing from the spirit of the present invention. The present invention is not limited by the above description, but is limited only by the scope of the attached claims.
[0063] For example, in the above-described embodiment, the inclined and parallel portions of the chute are both flat, but when viewed from the left and right, the inclined and parallel portions of the chute may be arc-shaped, convex upward or downward. Also, the connection between the inclined and parallel portions may be arc-shaped.
[0064] In addition, within the scope of the invention, the components in the above-described embodiments may be replaced with well-known components, and the above-described modified examples may be combined as appropriate. EXAMPLES
[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0066] Example 1 In a microcrack bath (HEEF bath) containing chromium oxide (CrO3), a lead alloy (PbO2) was placed as the anode and a stainless steel (SUS304) chute (without grooves) was placed as the cathode. The surface of the stainless steel chute was subjected to a microcrack chrome plating process, forming a hydrophilic plating layer (microcrack chrome layer) 250 μm thick on the surface of the stainless steel chute. The produced shoots were evaluated for water film retention and observed for fusion of the molten filaments to the shoots. The results of the evaluation and observation are shown in Table 1.
[0067] Example 2 A shoot was prepared in the same manner as in Example 1, except that the material of the shoot was aluminum (Al), and the water film retention of the prepared shoot was evaluated and the fusion of the molten filament to the shoot was observed. The results of the evaluation and observation are shown in Table 1.
[0068] Example 3 A shoot was prepared in the same manner as in Example 1, except that the material of the shoot was changed to copper (Cu), and the water film retention of the prepared shoot was evaluated and the fusion of the molten filament to the shoot was observed. The results of the evaluation and observation are shown in Table 1.
[0069] Example 4 A chute was prepared in the same manner as in Example 1, except that the material of the chute was changed to polycarbonate, and the water film retention of the prepared chute was evaluated and the fusion of the molten filament to the chute was observed. The results of the evaluation and observation are shown in Table 1.
[0070] Example 5 A stainless steel (SUS304) chute was placed in a PTFE composite plating bath (HEEF bath) in which PTFE particles (polytetrafluoroethylene particles) with a mass average particle size of 0.5 μm were dispersed in an electroless nickel-phosphorus plating bath, and a plating layer (composite layer containing PTFE in a nickel matrix) 30 μm thick was formed on the surface of the chute. The composition of the resulting nickel-PTFE composite plating layer was 84w% nickel, 8w% phosphorus, and 8wt% PTFE. The obtained shoot was immersed in a solution in which 1 mass % of metallic sodium was dissolved in liquid ammonia to make the surfaces of the PTFE particles hydrophilic, thereby forming a hydrophilic plating layer on the surface of the shoot. The water film retention of the shoots was evaluated and the adhesion of the molten filaments to the shoots was observed. The results of the evaluation and observation are shown in Table 1.
[0071] Comparative Example 1 A chute was prepared in the same manner as in Example 1, except that no hydrophilic plating layer was provided on the surface of the chute. The water film retention of the prepared chute was evaluated, and the fusion of the molten filament to the chute was observed. The results of the evaluation and observation are shown in Table 1.
[0072] Comparative Example 2 A shoot was prepared in the same manner as in Example 2, except that no hydrophilic plating layer was provided on the surface of the shoot, and the water film retention of the prepared shoot was evaluated and the fusion of the molten filament to the shoot was observed. The results of the evaluation and observation are shown in Table 1.
[0073] Comparative Example 3 A chute was prepared in the same manner as in Example 3, except that no hydrophilic plating layer was provided on the surface of the chute. The water film retention of the prepared chute was evaluated, and the fusion of the molten filament to the chute was observed. The results of the evaluation and observation are shown in Table 1.
[0074] (Evaluation of water film retention) · Cut a square test piece, each side 2 cm long, from the chute. The cut test piece is immersed in water for 5 minutes. After immersion, in an environment with a temperature of 25°C, humidity of 70%, and a wind speed of 1m / sec or less, the test piece is tilted at an angle of 20 to 30 degrees from the horizontal, and while maintaining that angle, moved vertically upward at an upward speed of 5mm / sec to 10mm / sec, and then gently removed from the water into the air. 10 seconds after taking the test piece out into the air, visually observe the condition of the water film on the top surface of the test piece and evaluate the water film retention according to the following criteria. Water film retention: Water film coverage on the top surface of the test piece is 80% or more No water film retention: Water film coverage on the top surface of the test piece is less than 80%
[0075] (Observation of fusion of molten filament to the chute) The chutes produced in the examples and comparative examples were attached to the production apparatus shown in FIG. 1 to produce a three-dimensional filament bond, and it was visually observed whether the molten filaments were fused to the chutes.
[0076] [Table 1]
[0077] As is clear from Table 1, in the chutes of Examples 1 to 5 in which a hydrophilic layer was provided on the surface including the inclined surface, 80% or more of the surface was covered with a water film. In addition, when used in an actual manufacturing device, no adhesion of molten filaments to the inclined surface was observed in the chutes of Examples 1 to 4. In addition, although slight adhesion of molten filaments to the inclined surface was observed in the chute of Example 5, this did not pose a problem in practical use.
[0078] In contrast, the chutes of Comparative Examples 1 to 3, which did not have a hydrophilic layer on the surface, had poor water film retention. Furthermore, when the chutes of Comparative Examples 1 to 3 were used in an actual production device, adhesion of molten filaments to the inclined surface of the chute was observed. [Industrial Applicability]
[0079] According to the manufacturing device of the present invention, it is possible to form a more uniform three-dimensional bound filament body without reducing the adhesive strength at the fusion points between the molten filaments. [Explanation of symbols]
[0080] 1 Manufacturing equipment 4a,4b Cooling water supply section 5a, 5b Chute (guide member) 6a, 6b Chute (guide member) 7a, 7b Chute (guide member) 10 Molten filament supply section 51a,51b Slope part 52a,52b Parallel part 53a,53b Slope 61a,61b Slope part 62a,62b Parallel part 63a,63b Slope 71a,71b Slope part 72a,72b Parallel part 73a,73b Slope GL,GL1,GL2 Groove G1 First groove group G2 2nd groove group HL hydrophilic layer MF fused filament group TDF filament 3D assembly
Claims
1. An apparatus for manufacturing a composite in which a large number of filaments are bonded in three dimensions, comprising: a molten filament supply unit that supplies a molten filament group consisting of a plurality of straight molten filaments; a pair of guide members each having an inclined surface that is spaced apart from and opposed to a first direction perpendicular to a supply direction of the molten filaments and receives both ends of the molten filaments in the first direction and guides them toward the opposite ends; a cooling water supply unit for supplying cooling water to the inclined surface of the guide member; Equipped with the pair of guide members each have a hydrophilic layer on the inclined surface thereof, the hydrophilic layer having a contact angle with water of less than 90°; The hydrophilic layer is a microcrack chromium layer or a composite plating layer containing PTFE (polytetrafluoroethylene) particles in a nickel matrix, and the surface of the PTFE particles is hydrophilized.
2. the pair of guide members each having an inclined portion having the inclined surface, and a parallel portion connected to a downstream end of the inclined portion in the supply direction of the group of molten filaments and extending parallel to the supply direction of the group of molten filaments and downstream in the supply direction, The parallel portion has a hydrophilic layer on its surface on each of its opposing sides.
2. An apparatus for producing a three-dimensional filament assembly according to claim 1.
3. An apparatus for manufacturing a composite in which a large number of filaments are bonded in three dimensions, comprising: a molten filament supply unit that supplies a molten filament group consisting of a plurality of straight molten filaments; a pair of guide members each having an inclined surface that is spaced apart from and opposed to a first direction perpendicular to a supply direction of the molten filaments and receives both ends of the molten filaments in the first direction and guides them toward the opposite ends; a cooling water supply unit for supplying cooling water to the inclined surface of the guide member; Equipped with A number of grooves are formed on the inclined surfaces of the pair of guide members in a direction intersecting a second direction perpendicular to the first direction, 4. The apparatus for manufacturing a three-dimensional filament assembly, wherein the pair of guide members have a hydrophilic layer on the inclined surface thereof, the hydrophilic layer having a contact angle with water of less than 90°.
4. 4. The apparatus for manufacturing a three-dimensional filament assembly according to claim 3, wherein said numerous grooves extend in parallel at predetermined intervals.
5. 5. The apparatus for manufacturing a three-dimensional filament assembly according to claim 3, wherein the cross-sectional shape of said numerous grooves perpendicular to the extending direction thereof is any one of a triangular shape, a rectangular shape, and a circular arc shape.
6. 5. The apparatus for manufacturing a three-dimensional filament assembly according to claim 3, wherein the intersecting angle of the numerous grooves with the second direction is 90 degrees.
7. The plurality of grooves are a first groove group having an intersection angle with the second direction of 30° or more and 60° or less; a second groove group having an intersection angle with the second direction of 120° or more and 150° or less; 5. The apparatus for producing a three-dimensional filament assembly according to claim 3, further comprising:
8. 8. The apparatus for manufacturing a three-dimensional filament assembly according to claim 7, wherein the grooves of said first groove group extend in parallel at a predetermined interval, and the grooves of said second groove group also extend in parallel at a predetermined interval.
Citation Information
Patent Citations
Mat consisting of filament loop aggregate and production and apparatus thereof
JP1989207462A
Production of spherical three-dimensional reticulated aggregate
JP1996099093A
Apparatus for forming net structure loop, machine and method for producing net structure, and the resultant net structure
JP2004218116A
Three-dimensional network structure, method for producing three-dimensional network structure and apparatus for producing three-dimensional network structure
JP2012127046A
Device for manufacturing filament three-dimensional conjugate
JP2018028161A