Hot-rolled steel sheet
A hot rolled steel sheet with a controlled chemical composition and metal structure, optimized through precise manufacturing processes, addresses the challenge of achieving high strength and fatigue properties in automobile parts by enhancing ductility and reducing surface roughness, thereby improving fatigue resistance.
Patent Information
- Application Number
- JP2023529703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-14
- Filing Date
- 2022-05-20
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2042-05-20
AI Technical Summary
Conventional high-strength steel plates used in automobile parts face challenges in achieving both high fatigue properties and ductility, particularly due to the deterioration of descaling properties caused by the addition of Si, which complicates the control of surface roughness and reduces fatigue strength.
A hot rolled steel sheet with a specific chemical composition and controlled metal structure, including a high ductile ferrite content, limited Si content, and precise control of Sn concentration and surface roughness, achieved through optimized slab heating, hot rolling, and cooling processes, to enhance both strength and fatigue properties.
The solution results in a hot rolled steel sheet with high tensile strength, excellent fatigue properties, and improved ductility, suitable for automobile parts, mechanical structural parts, and building parts, while maintaining smooth surface texture and reducing the need for precise descaling control.
Smart Images

Figure 0007578895000001 
Figure 0007578895000002 
Figure 0007578895000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet. Specifically, the present invention relates to a high-strength hot-rolled steel sheet having excellent fatigue properties and ductility. This application claims priority based on Japanese Patent Application No. 2021-098517, filed on June 14, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] Conventionally, high-strength steel sheets have been widely used in suspension parts and structural parts of automobile bodies to reduce the weight of the automobile body. However, it is difficult to sufficiently improve the fatigue properties of conventional high-strength steel sheets, which are particularly important properties for suspension parts of automobiles, and there is still room for improvement in reducing the plate thickness of parts even if the strength of the material is increased.
[0003] In general, solid solution strengthening and precipitation strengthening can provide a large increase in strength, and therefore these effects are applied to high-strength steel sheets. For example, Non-Patent Document 1 discloses that, as a result of investigating the effects of solid solution strengthening, precipitation strengthening, and fine grain strengthening on tensile strength and fatigue properties, the increase in fatigue strength relative to the increase in tensile strength is solid solution strengthening > precipitation strengthening > fine grain strengthening.
[0004] It is known that the addition of a solid solution strengthening element, particularly Si, improves fatigue properties. However, the addition of Si causes the formation of Fe at the iron-scale interface. 2 SiO 4 The formation of , reduces the descaling ability. Therefore, in order to ensure the fatigue properties of Si-added steel, it was necessary to precisely control the descaling conditions.
[0005] For example, Patent Documents 1 and 2 disclose techniques for improving the descaling ability by increasing the descaling temperature, thereby reducing the surface roughness Ra of the steel sheet after pickling to 1.2 μm or less, and improving the fatigue properties. Furthermore, Patent Document 3 discloses a technique for improving fatigue properties by controlling the scale thickness before the start of finish rolling to set the roughness Ra of the base steel / scale interface to 1.5 μm or less. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent No. 4404004 [Patent Document 2] Japanese Patent No. 4518029 [Patent Document 3] Japanese Patent No. 5471918 [Non-patent literature]
[0007] [Non-Patent Document 1] Abe, Takashi et al.: Iron and Steel, No. 10, 1984, 70th year, pp. 145-152 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been devised in view of the above circumstances, and has an object to provide a hot-rolled steel sheet having high strength, excellent fatigue properties and ductility. [Means for solving the problem]
[0009] In view of the above circumstances, the present inventors have conducted extensive research into the chemical composition and metal structure of hot-rolled steel sheets and the relationship between the chemical composition and metal structure and the mechanical properties thereof, and have obtained the following findings (a) to (h) and completed the present invention.
[0010] (a) In order to increase ductility, it is preferable to include highly ductile ferrite in the metal structure.
[0011] (b) However, since ferrite is a soft structure, simply using ferrite as the main component cannot ensure high strength and excellent fatigue properties.
[0012] (c) In order to combine excellent ductility with excellent fatigue properties in hot-rolled steel sheets, it is effective to solid-solution strengthen ferrite with Si. However, the inclusion of Si deteriorates the descaling property, so precise control of the descaling conditions is required to prevent deterioration of fatigue properties due to increased surface roughness. Precise control of the descaling conditions may require additional capital investment or reduce the yield.
[0013] (d) By using Sn as a substitute for Si and reducing the Si content, it is possible to obtain excellent fatigue properties without deteriorating the descaling ability. This is thought to be because Sn has the same cross slip suppression effect as Si, and by restricting the movement of dislocations during repeated deformation, it is possible to suppress the damage accumulated in the material during fatigue testing.
[0014] (e) In order to obtain both fatigue properties and ductility by adding Sn, it is effective to keep the standard deviation of the Sn concentration below a certain value and to keep the arithmetic mean roughness of the surface below a certain value.
[0015] (f) In order to keep the standard deviation of the Sn concentration at a certain value or less, it is effective to control the slab heating process and the subsequent hot rolling process. For example, it is effective to heat the slab, hold it in the temperature range of 700 to 850°C for 900 seconds or more, and then perform hot rolling in the temperature range of 850°C to 1100°C so that the sheet thickness is reduced by 90% or more in total.
[0016] (g) In order to reduce the arithmetic mean roughness of the surface of hot-rolled steel sheets, it is effective to control the behavior of scale formation during hot rolling. For example, it is effective to set the maximum heating temperature of the slab in the slab heating process to less than 1200°C and the reduction rate of each stage in the hot rolling process to less than 30%. By combining the slab heating conditions and the hot rolling conditions, it is possible to create thin and smooth scale and reduce the arithmetic mean roughness of the surface.
[0017] (h) In order to ensure that ductile ferrite is sufficiently contained in the metal structure, it is effective to hold the material in a temperature range of 600 to 750° C. for 3 seconds or more during cooling after hot rolling.
[0018] The gist of the present invention made based on the above findings is as follows. (1) A hot-rolled steel sheet according to one aspect of the present invention has a chemical composition, in mass%, C: 0.040~0.250%, Si: 0.30% or less, Mn: 1.00-4.00%, Sol.Al: 0.001-1.000%, Sn: 0.300~1.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Ti+Nb+V: 0~0.500%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-1.00%, Ni: 0-2.00%, B: 0~0.0100%, Ca: 0 to 0.0200%, Mg: 0 to 0.0200%, REM: 0~0.1000%, Bi: 0 to 0.020%, One or more of Zr, Co, Zn and W: 0 to 1.00% in total; the balance being Fe and impurities, The metal structure is Ferrite is 20.0% or more and less than 90.0% by area%, The standard deviation of the Sn concentration is 0.50 mass% or less, The arithmetic mean roughness of the surface is less than 2.00 μm; The tensile strength is 590MPa or more. (2) The hot-rolled steel sheet according to the above (1) has a chemical composition, in mass%, Ti+Nb+V: 0.020~0.500%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01 to 1.00%, Ni: 0.02 to 2.00%, B: 0.0001 to 0.0100%, Ca: 0.0005~0.0200%, Mg: 0.0005~0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005 to 0.020% The resin may contain one or more selected from the group consisting of: Effect of the Invention
[0019] According to the above aspect of the present invention, it is possible to obtain a hot-rolled steel sheet having high strength, excellent fatigue properties and ductility. The hot-rolled steel sheet according to the above aspect of the present invention is suitable as an industrial material used for automobile parts, machine structural parts and building parts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The chemical composition and metal structure of the hot-rolled steel sheet according to this embodiment will be described in more detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention.
[0021] In the following, the numerical ranges described with "~" include the lower and upper limits. Numerical values indicated as "less than" or "more than" are not included in the numerical range. In the following description, percentages related to the chemical composition of the steel sheet are mass% unless otherwise specified.
[0022] 1.Chemical composition The hot-rolled steel sheet according to the present embodiment contains, by mass%, C: 0.040-0.250%, Si: 0.30% or less, Mn: 1.00-4.00%, sol.Al: 0.001-1.000%, Sn: 0.300-1.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, and the balance: Fe and impurities. Each element will be described in detail below.
[0023] (1-1) C: 0.040-0.250% C increases the fraction of hard structures and lowers the transformation point to increase the strength of ferrite and hard structures. If the C content is less than 0.040%, it is difficult to obtain the desired strength. Therefore, the C content is set to 0.040% or more. The C content is preferably 0.050% or more, more preferably 0.060% or more. On the other hand, if the C content exceeds 0.250%, the ferrite fraction decreases, and the ductility of the hot-rolled steel sheet decreases. Therefore, the C content is set to 0.250% or less. The C content is preferably 0.150% or less.
[0024] (1-2)Si: 0.30% or less Si is present at the iron-iron oxide interface. 2 SiO 4 This reduces the descaling ability by generating Si. If the conditions for descaling ability cannot be precisely controlled, the surface roughness of the steel sheet after pickling increases, which may result in a reduction in the fatigue strength of the hot-rolled steel sheet. In order to suppress the above-mentioned action, the Si content is set to 0.30% or less, preferably 0.25% or less, and more preferably 0.20% or less. The Si content may be 0%, but since Si has the effect of promoting the formation of ferrite to improve the ductility of the hot-rolled steel sheet, and the effect of suppressing cross slip and suppressing the accumulation of strain during repeated deformation, thereby improving fatigue strength, the Si content is preferably 0.05% or more.
[0025] (1-3) Mn: 1.00-4.00% Mn increases the fraction of hard structures and lowers the transformation point to increase the strength of ferrite and hard structures. If the Mn content is less than 1.00%, a tensile strength of 590 MPa or more cannot be obtained. Therefore, the Mn content is set to 1.00% or more. The Mn content is preferably 1.10% or more, and more preferably 1.20% or more. On the other hand, if the Mn content exceeds 4.00%, the fraction of hard structures becomes too high, making it difficult to obtain the desired ductility. Therefore, the Mn content is set to 4.00% or less. The Mn content is preferably 3.70% or less, and more preferably 3.50% or less.
[0026] (1-4) sol.Al: 0.001-1.000% Al has the effect of deoxidizing steel and improving its soundness (suppressing the occurrence of defects such as blowholes in steel), as well as promoting the formation of ferrite and increasing the ductility of hot-rolled steel sheets. If the sol.Al content is less than 0.001%, the above effects cannot be obtained. Therefore, the sol.Al content is set to 0.001% or more. The sol.Al content is preferably 0.010% or more, and more preferably 0.050% or more. On the other hand, if the sol.Al content exceeds 1.000%, the above effects are saturated and it is economically undesirable. Therefore, the sol.Al content is set to 1.000% or less. The sol.Al content is preferably 0.700% or less, more preferably 0.500% or less, and even more preferably 0.400% or less. Incidentally, sol. Al means acid-soluble Al, and indicates solute Al that is present in the steel in a solid solution state.
[0027] (1-5) Sn: 0.300-1.000% Sn is an element that plays an important role in this embodiment. Sn has the effect of increasing the strength of the hot-rolled steel sheet by solid solution strengthening ferrite. In addition, Sn has the effect of suppressing cross slip, thereby suppressing irreversible movement of dislocations during repeated deformation, and of improving the fatigue properties of the hot-rolled steel sheet by reducing accumulated strain during fatigue testing. In order to obtain these effects, the Sn content is set to 0.300% or more, preferably 0.350% or more, and more preferably 0.400% or more. On the other hand, Sn is an element that easily segregates, and if the Sn content exceeds 1.000%, the ductility of the hot-rolled steel sheet deteriorates. Therefore, the Sn content is set to 1.000% or less, preferably 0.950% or less, and more preferably 0.900% or less.
[0028] (1-6)P:0.100% or less P is an element that is generally contained as an impurity, but it also has the effect of increasing the strength of the hot-rolled steel sheet by solid solution strengthening. Therefore, P may be intentionally contained, but P is an element that easily segregates, and if the P content exceeds 0.100%, the ductility of the hot-rolled steel sheet decreases significantly due to grain boundary segregation. Therefore, the P content is set to 0.100% or less. The P content is preferably 0.030% or less. There is no need to specify a lower limit for the P content, but from the viewpoint of refining costs, it is preferable to set the lower limit to 0.001% or more.
[0029] (1-7)S: 0.0300% or less S is an element contained as an impurity, and forms sulfide-based inclusions in steel, reducing the ductility of the hot-rolled steel sheet. If the S content exceeds 0.0300%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the S content is set to 0.0300% or less. The S content is preferably 0.0050% or less. There is no need to specify a lower limit for the S content, but from the viewpoint of refining costs, it is preferable to set the lower limit to 0.0001% or more.
[0030] (1-8)N: 0.1000% or less N is an element contained in steel as an impurity, and has the effect of reducing the ductility of a hot-rolled steel sheet. If the N content exceeds 0.1000%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the N content is set to 0.1000% or less. The N content is preferably 0.0800% or less, more preferably 0.0700% or less, and even more preferably 0.0100% or less. The lower limit of the N content does not need to be particularly specified, but may be 0.0001% or more. When one or more of Ti, Nb, and V are added to make the metal structure finer, the N content is preferably 0.0010% or more, and more preferably 0.0020% or more, in order to promote the precipitation of carbonitrides.
[0031] (1-9)O: 0.0100% or less When O is contained in a large amount in steel, it forms coarse oxides that become the starting points of fracture, causing brittle fracture and hydrogen-induced cracking. Therefore, the O content is set to 0.0100% or less. The O content is preferably 0.0080% or less, and more preferably 0.0050% or less. In order to disperse a large number of fine oxides during deoxidation of molten steel, the O content may be set to 0.0005% or more, or 0.0010% or more.
[0032] The balance of the chemical composition of the hot-rolled steel sheet according to the present embodiment may be Fe and impurities. In the present embodiment, the term "impurities" refers to those mixed in from raw materials such as ore, scrap, or the manufacturing environment, and / or those that are permitted within a range that does not adversely affect the hot-rolled steel sheet according to the present embodiment. Examples of impurities include H, Na, Cl, Ga, Ge, As, Se, Tc, Ru, Rh, Pd, Ag, Cd, In, Sb, Te, Cs, Ta, Re, Os, Ir, Pt, Au, Pb, and Po. These impurities may be contained in a total content of 0.100% or less.
[0033] The hot-rolled steel sheet according to the present embodiment may contain optional elements such as Ti, Nb, V, Cu, Cr, Mo, Ni, B, Ca, Mg, REM, Bi, Zr, Co, Zn, and W instead of a portion of Fe. When the optional elements are not contained, the lower limit of the content is 0%. The optional elements will be described in detail below.
[0034] (1-10) One or more of Ti, Nb and V: 0.020 to 0.500% in total Ti, Nb and V are elements that finely precipitate in steel as carbides and nitrides, improving the strength of steel through precipitation strengthening. In order to obtain this effect more reliably, it is preferable that the total content of Ti, Nb and V is 0.020% or more. It is not necessary to contain all of Ti, Nb and V, and it is sufficient to contain at least one of them, and the total content of them is 0.020% or more. The total content of Ti, Nb and V is more preferably 0.030% or more, and even more preferably 0.040% or more. On the other hand, if the total content of Ti, Nb and V exceeds 0.500%, the ductility of the hot-rolled steel sheet deteriorates. Therefore, the total content of Ti, Nb and V is set to 0.500% or less, preferably 0.300% or less, more preferably 0.250% or less, and even more preferably 0.200% or less.
[0035] (1-11) Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-1.00%, Ni: 0.02-2.00% and B: 0.0001-0.0100% Cu, Cr, Mo, Ni and B all have the effect of increasing the hardenability of the hot-rolled steel sheet. Cu and Mo also have the effect of precipitating as carbides in the steel to increase the strength of the hot-rolled steel sheet. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing grain boundary cracking of the slab caused by Cu. Therefore, one or more of these elements may be contained.
[0036] As described above, Cu has the effect of increasing the hardenability of the hot-rolled steel sheet and the effect of precipitating as carbides in the steel at low temperatures to increase the strength of the hot-rolled steel sheet. In order to obtain the above-mentioned effects more reliably, the Cu content is preferably 0.01% or more, and more preferably 0.05% or more. However, if the Cu content exceeds 2.00%, grain boundary cracking of the slab may occur. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably 1.50% or less, more preferably 1.00% or less.
[0037] As described above, Cr has the effect of improving the hardenability of the hot-rolled steel sheet. In order to obtain the above-mentioned effect more reliably, the Cr content is preferably 0.01% or more, and more preferably 0.05% or more. However, if the Cr content exceeds 2.00%, the chemical conversion treatability of the hot-rolled steel sheet is significantly reduced. Therefore, the Cr content is set to 2.00% or less.
[0038] As described above, Mo has the effect of increasing the hardenability of a hot-rolled steel sheet and the effect of precipitating in the steel as carbides to increase the strength of the hot-rolled steel sheet. In order to obtain the above-mentioned effects more reliably, the Mo content is preferably 0.01% or more, and more preferably 0.02% or more. However, even if the Mo content exceeds 1.00%, the above-mentioned effects are saturated and it is not economically preferable. Therefore, the Mo content is set to 1.00% or less. The Mo content is preferably 0.50% or less, and more preferably 0.20% or less.
[0039] As described above, Ni has the effect of increasing the hardenability of hot-rolled steel sheet. Furthermore, when Cu is contained, Ni has the effect of effectively suppressing grain boundary cracking of slabs caused by Cu. In order to obtain the above-mentioned effect more reliably, the Ni content is preferably 0.02% or more. Since Ni is an expensive element, it is economically undesirable to contain a large amount of Ni. Therefore, the Ni content is set to 2.00% or less.
[0040] As described above, B has the effect of improving the hardenability of the hot-rolled steel sheet. In order to obtain the effect of this effect more reliably, the B content is preferably 0.0001% or more, and more preferably 0.0002% or more. However, if the B content exceeds 0.0100%, the formability of the hot-rolled steel sheet is significantly reduced, so the B content is set to 0.0100% or less. The B content is preferably set to 0.0050% or less.
[0041] (1-12) Ca: 0.0005-0.0200%, Mg: 0.0005-0.0200%, REM: 0.0005-0.1000%, and Bi: 0.0005-0.020% Ca, Mg and REM all have the effect of adjusting the shape of inclusions in steel to a preferred shape, thereby increasing the ductility of the hot-rolled steel sheet. Bi also has the effect of refining the solidification structure, thereby increasing the ductility of the hot-rolled steel sheet. Therefore, one or more of these elements may be contained. In order to obtain the effect of the above action more reliably, it is preferable that any one or more of Ca, Mg, REM and Bi is 0.0005% or more. However, if the Ca content or Mg content exceeds 0.0200%, or if the REM content exceeds 0.1000%, inclusions are excessively generated in the steel, which may actually reduce the ductility of the hot-rolled steel sheet. Also, even if the Bi content exceeds 0.020%, the effect of the above action is saturated, which is not economically preferable. Therefore, the Ca content and Mg content are 0.0200% or less, the REM content is 0.1000% or less, and the Bi content is 0.020% or less. The Bi content is preferably 0.010% or less. Here, REM refers to a total of 17 elements consisting of Sc, Y and lanthanides, and the content of the above REM refers to the total content of these elements. In the case of lanthanides, they are added industrially in the form of misch metals.
[0042] (1-13) One or more of Zr, Co, Zn and W: 0 to 1.00% in total The inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if the total content of Zr, Co, Zn, and W is 1.00% or less. Therefore, one or more of Zr, Co, Zn, and W may be contained in a total content of 1.00% or less.
[0043] The chemical composition of the above-mentioned hot-rolled steel sheet may be measured by a general analytical method. For example, it may be measured by using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Sol. Al may be measured by ICP-AES using the filtrate after thermally decomposing the sample with acid. C and S may be measured by the combustion-infrared absorption method, N by the inert gas fusion-thermal conductivity method, and O by the inert gas fusion-non-dispersive infrared absorption method.
[0044] 2. Metal structure of hot-rolled steel sheets Next, the metal structure of the hot-rolled steel sheet according to this embodiment will be described. The hot-rolled steel sheet according to the present embodiment has a metal structure in which, in terms of area percentage, ferrite is 20.0% or more and less than 90.0%, and the standard deviation of the Sn concentration is 0.50 mass% or less, so that the hot-rolled steel sheet according to the present embodiment can obtain excellent fatigue strength and ductility.
[0045] In this embodiment, the structure fraction in the metal structure at a 1 / 4 depth from the surface of the sheet thickness (a region from 1 / 8 depth to 3 / 8 depth from the surface) and at the center position in the sheet width direction in a cross section parallel to the rolling direction is specified because the metal structure at this position shows a typical metal structure of a steel sheet.
[0046] (2-1) Area ratio of ferrite: 20.0% or more, less than 90.0% Ferrite is a structure that is formed when fcc transforms to bcc at a relatively high temperature. Ferrite has a high work hardening rate, and therefore acts to improve the strength-ductility balance of hot-rolled steel sheets. In order to obtain the desired strength and ductility through the above-mentioned action, the area ratio of ferrite is set to 20.0% or more. It is preferably 30.0% or more, and more preferably 40.0% or more. On the other hand, since ferrite has low strength, if the area ratio is excessive, the desired tensile strength cannot be obtained. Therefore, the ferrite area ratio is set to less than 90.0%, preferably less than 85.0%, and more preferably less than 80.0%.
[0047] In addition, the hot-rolled steel sheet according to the present embodiment includes a hard structure consisting of one or more of pearlite, bainite, martensite, tempered martensite, and retained austenite, with a total area ratio of more than 10.0% and not more than 80.0%, as a remaining structure other than ferrite. The area ratio of the remaining structure may be more than 15.0% or more than 20.0%. The area ratio of the remaining structure may be 70.0% or less, 60.0% or less.
[0048] The area ratio of ferrite is measured by the following method. A sample is taken from a hot-rolled steel sheet in a cross section parallel to the rolling direction, at a depth of 1 / 4 of the sheet thickness from the surface (a region from 1 / 8 depth from the surface to 3 / 8 depth from the surface) and in the center position in the sheet width direction. The cross section of the sample parallel to the rolling direction is mirror-finished and polished for 8 minutes at room temperature with colloidal silica that does not contain an alkaline solution to remove strain introduced into the surface layer of the sample.
[0049] At any position in the longitudinal direction of the sample cross section, a region 50 μm long, 1 / 4 of the plate thickness from the surface (the region from 1 / 8 of the plate thickness from the surface to 3 / 8 of the plate thickness from the surface), and at the center of the plate width direction is measured at measurement intervals of 0.1 μm using electron backscatter diffraction to obtain crystal orientation information. For the measurements, an EBSD device consisting of a thermal field emission scanning electron microscope (JEOL JSM-7001F) and an EBSD detector (TSL DVC5 detector) is used. The degree of vacuum inside the EBSD device was 9.6×10 -5 The irradiation current level is 13, and the electron beam irradiation level is 62.
[0050] Furthermore, a backscattered electron image is taken in the same field of view. First, crystal grains in which ferrite and cementite are precipitated in layers are identified from the backscattered electron image, and the crystal grains are determined to be pearlite. Then, for the crystal grains other than those determined to be pearlite, the obtained crystal orientation information is used to determine the areas with a Grain Average Misorientation value of 1.0° or less as ferrite using the "Grain Average Misorientation" function installed in the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device. The area ratio of the areas determined to be ferrite is obtained by calculating the area ratio of the ferrite.
[0051] The area ratio of the remaining structure excluding pearlite is obtained by subtracting the area ratios of pearlite and ferrite from 100%.
[0052] (2-2) Standard deviation of Sn concentration: 0.50 mass% or less The standard deviation of the Sn concentration at a 1 / 4 depth of the sheet thickness from the surface (a region from 1 / 8 depth to 3 / 8 depth from the surface) and at the center position in the sheet width direction of the hot-rolled steel sheet according to this embodiment is 0.50 mass% or less. This makes it possible to prevent early fracture of the Sn-enriched portion and improve the ductility of the hot-rolled steel sheet. The standard deviation of the Sn concentration is preferably 0.47 mass% or less, and more preferably 0.45 mass% or less. From the viewpoint of ensuring ductility, it is preferable that the lower limit of the standard deviation of the Sn concentration is as small as possible. However, due to restrictions imposed by the manufacturing process, the practical lower limit is 0.10 mass %.
[0053] The standard deviation of the Sn concentration is obtained by the following method. After mirror polishing a cross section (L cross section) parallel to the rolling direction of the hot-rolled steel sheet, the standard deviation of the Sn concentration is measured by measuring the 1 / 4 depth of the sheet thickness from the surface (the region from 1 / 8 depth of the sheet thickness from the surface to 3 / 8 depth of the sheet thickness from the surface) and the center position in the sheet width direction with an electron probe microanalyzer (EPMA). The measurement conditions are an acceleration voltage of 15 kV and a magnification of 5000 times, and a distribution image is measured in a range from 1 / 8 depth of the sheet thickness from the surface to 3 / 8 depth of the sheet thickness from the surface and in a range of 20 μm in the rolling direction of the sample. More specifically, the measurement interval is 0.1 μm, and the Sn concentration is measured at 40,000 or more points. Next, the standard deviation is calculated based on the Sn concentrations obtained from all measurement points to obtain the standard deviation of the Sn concentration.
[0054] 3.Surface texture In the hot-rolled steel sheet according to the present embodiment, it is important to control the arithmetic mean roughness of the surface. Since fatigue cracks usually initiate from the surface of the hot-rolled steel sheet, it is important to keep the arithmetic mean roughness of the surface at a certain value or less in order to realize the effect of improving fatigue properties by the solid solution strengthening elements. As a result of intensive studies by the present inventors, it was found that excellent fatigue properties can be obtained when the arithmetic mean roughness of the surface of the hot-rolled steel sheet is less than 2.00 μm.
[0055] By making the arithmetic mean roughness of the surface less than 2.00 μm, the occurrence of fatigue cracks when bending deformation is applied to the hot-rolled steel sheet is suppressed, and the fatigue properties are improved. Therefore, the arithmetic mean roughness is made less than 2.00 μm. The arithmetic mean roughness is preferably 1.80 μm or less, and more preferably 1.60 μm or less. From the viewpoint of ensuring fatigue strength, it is preferable that the lower limit of the arithmetic mean roughness is as small as possible. However, due to restrictions imposed by the manufacturing process, the practical lower limit is 0.50 μm.
[0056] The arithmetic mean roughness of the surface of a hot-rolled steel sheet is measured by pickling to remove scale, and then measuring the profile of five random lines along the rolling direction and the direction perpendicular to the rolling direction on the surface of the hot-rolled steel sheet. The measurement is performed in accordance with JIS B 0601:2013, and a roughness curve is obtained by applying a low-pass filter with a cutoff value λs and a high-pass filter with a cutoff value λc to the measured cross-sectional curve, and the measured value of the arithmetic mean roughness is obtained. The arithmetic mean roughness is obtained by calculating the average of the obtained measurements. In addition, when the hot-rolled steel sheet has a plating layer on the surface, the above-mentioned measurement may be carried out after removing the plating layer by chemical polishing.
[0057] 4. Mechanical properties (4-1) Tensile properties Among the mechanical properties of hot-rolled steel sheets, the tensile properties (tensile strength, total elongation) are evaluated in accordance with JIS Z 2241:2011. The test piece used is No. 5 test piece of JIS Z 2241:2011. The tensile test piece is taken from the 1 / 4 part from the end in the sheet width direction, with the direction perpendicular to the rolling direction as the longitudinal direction.
[0058] The hot-rolled steel sheet according to this embodiment has a tensile (maximum) strength of 590 MPa or more. If the tensile strength is less than 590 MPa, the applicable parts are limited, and the contribution to reducing the weight of the vehicle body is small. The upper limit does not need to be particularly set, but may be 1200 MPa from the viewpoint of suppressing die wear.
[0059] In addition, the total elongation of the hot-rolled steel sheet is preferably 14.0% or more, and the product of tensile strength and total elongation (TS × El) is preferably 14000 MPa·% or more. The total elongation is more preferably 16.0% or more, and even more preferably 18.0% or more. In addition, the product of tensile strength and total elongation is more preferably 16000 MPa·% or more, and even more preferably 18000 MPa·% or more. By making the total elongation 14.0% or more and the product of tensile strength and total elongation 14000 MPa·% or more, there are no limitations on the parts to which the steel sheet can be applied, and the steel sheet can make a significant contribution to reducing the weight of the vehicle body.
[0060] (4-2) Fatigue properties Regarding the fatigue strength of a hot-rolled steel sheet, the value "FS / (0.3×TS)+150" calculated from the 200,000 cycles strength FS and the tensile strength TS is 1.00 or more, or FS is 450 MPa or more. If either of these is satisfied, the hot-rolled steel sheet can be judged to have excellent fatigue strength. The value of "FS / (0.3 x TS) + 150" is preferably 1.05 or more, and more preferably 1.10 or more.
[0061] Fatigue strength is evaluated by taking a test piece as specified in JIS Z 2275-1978 from a position 1 / 4 of the way across the width of the hot-rolled steel sheet, with the longitudinal direction perpendicular to the rolling direction (C direction), and conducting a plane bending fatigue test in accordance with JIS Z 2275-1978. The 200,000 cycles time strength FS is obtained by determining the time strength at which the number of cycles to fracture is 200,000.
[0062] 5. Plate thickness The thickness of the hot-rolled steel sheet according to the present embodiment is not particularly limited, but may be 1.2 to 8.0 mm. If the thickness of the hot-rolled steel sheet is less than 1.2 mm, it may be difficult to ensure the rolling completion temperature and the rolling load may become excessive, making hot rolling difficult. Therefore, the thickness of the hot-rolled steel sheet according to the present embodiment may be 1.2 mm or more. It is preferably 1.4 mm or more. On the other hand, if the thickness exceeds 8.0 mm, it may be difficult to ensure the rolling reduction required to reduce the standard deviation of the Sn concentration, and it may be difficult to obtain the above-mentioned metal structure. Therefore, the thickness may be 8.0 mm or less. It is preferably 6.0 mm or less.
[0063] 6.Other (6-1) Plating layer The hot-rolled steel sheet according to the present embodiment having the above-mentioned chemical composition and metal structure may be provided with a plating layer on the surface for the purpose of improving corrosion resistance, etc., to form a surface-treated steel sheet. The plating layer may be an electroplating layer or a hot-dip plating layer. Examples of the electroplating layer include electrogalvanizing and electrogalvanizing Zn-Ni alloy plating. Examples of the hot-dip plating layer include hot-dip galvanizing, alloyed hot-dip galvanizing, hot-dip aluminum plating, hot-dip Zn-Al alloy plating, hot-dip Zn-Al-Mg alloy plating, and hot-dip Zn-Al-Mg-Si alloy plating. The coating weight is not particularly limited and may be the same as in the past. In addition, it is also possible to further improve the corrosion resistance by performing an appropriate chemical conversion treatment (for example, application of a silicate-based chromium-free chemical conversion treatment liquid and drying) after plating.
[0064] 7.Manufacturing conditions A suitable method for producing the hot-rolled steel sheet according to this embodiment having the above-mentioned chemical composition and metal structure is as follows.
[0065] In order to obtain the hot-rolled steel sheet according to this embodiment, it is effective to carry out slab heating and hot rolling under prescribed conditions, and then to adopt a cooling history that ensures a residence time in a prescribed temperature range.
[0066] In a preferred method for producing a hot-rolled steel sheet according to this embodiment, the following steps (1) to (6) are carried out in sequence. Note that the temperature of the slab and the temperature of the steel sheet in this embodiment refer to the surface temperature of the slab and the surface temperature of the steel sheet. (1) The slab is held in the temperature range of 700 to 850°C for 900 seconds or more. The maximum heating temperature of the slab is less than 1200°C. (2) The reduction ratio at each stage of hot rolling shall be less than 30%. (3) In hot rolling, the total thickness reduction in the temperature range of 850 to 1100°C shall be 90% or more. (4) The hot rolling is completed so that the rolling completion temperature Tf is 850°C or higher and lower than 1010°C. (5) The material is allowed to remain in the temperature range of 600 to 750°C for 3 seconds or more. (6) Coiling is performed at a temperature of 400°C or less.
[0067] By adopting the above manufacturing method, it is possible to stably manufacture a hot-rolled steel sheet having a metal structure excellent in fatigue properties and ductility. That is, by appropriately controlling the slab heating conditions and hot rolling conditions, it is possible to reduce Sn segregation and smooth the iron-scale interface, and in combination with the cooling conditions after hot rolling described below, it is possible to stably manufacture a hot-rolled steel sheet having a desired metal structure.
[0068] (7-1) Slab, slab temperature and holding time when subjected to hot rolling The slab to be subjected to hot rolling may be a slab obtained by continuous casting or a slab obtained by casting and blooming, and if necessary, a slab that has been subjected to hot working or cold working may be used. The slab to be subjected to hot rolling is held in a temperature range of 700 to 850°C for 900 seconds or more when the slab is heated. After this holding, the slab is further heated and held. At this time, the maximum heating temperature of the slab is preferably less than 1200°C. When holding in the temperature range of 700 to 850°C, the steel sheet temperature may be varied within this temperature range or may be constant. When heating a slab to a temperature range of 1100°C or higher, the slab is usually placed in a heating furnace, and the set temperature of the heating furnace is set to a temperature range of 1100°C or higher to heat the slab. When the slab is heated in this manner, it is not possible to ensure a sufficient holding time in the temperature range of 700 to 850°C. For example, by adjusting the temperature of the slab to 700°C or higher and then lowering the set temperature of the heating furnace, a sufficient holding time in the temperature range of 700 to 850°C can be ensured.
[0069] During austenite transformation in the temperature range of 700 to 850°C, Sn is distributed between ferrite and austenite. Therefore, by extending the transformation time, Sn can diffuse into the ferrite region. This can significantly reduce the standard deviation of the Sn concentration unevenly distributed in the slab.
[0070] In addition, by setting the maximum heating temperature of the slab to less than 1200°C, the thickness of the scale formed on the slab surface can be reduced, scale fracture during rolling can be suppressed, and the iron-scale interface can be made smooth. There is no need to set a lower limit for the maximum heating temperature of the slab, but since it is difficult to ensure the final rolling temperature described below if the temperature is less than 1100°C, it may be set to 1100°C. After holding in the temperature range of 700 to 850°C, the holding time in the temperature range of less than 1200°C is not particularly limited.
[0071] In the hot rolling, a reverse mill or a tandem mill is preferably used as a multi-pass rolling mill. In particular, from the viewpoint of industrial productivity and the stress load on the steel sheet during rolling, it is more preferable to use a tandem mill for at least the final two stages of hot rolling.
[0072] (7-2) Reduction rate at each stage of hot rolling: less than 30% The reduction ratio in each stage of hot rolling is preferably less than 30%. That is, the reduction ratio in all rolling passes of hot rolling is preferably less than 30%. The hot rolling here includes rough rolling and finish rolling. That is, in this embodiment, the reduction ratio in each stage of rough rolling is also less than 30%, and the reduction ratio in each stage of finish rolling is also less than 30%.
[0073] Usually, in hot rolling, particularly rough rolling, the slab is rolled at least once with a reduction of 35 to 40%. In the initial stage of rough rolling (1st to 3rd passes), the slab temperature is high and the deformation resistance is low, so rolling is performed with a high reduction (e.g., 35 to 40%). By performing rolling with a high reduction in the initial stage of rough rolling, it is possible to produce a hot-rolled steel sheet of the desired thickness with fewer passes, including finish rolling. However, the present inventors have found that by setting the reduction rate at each stage of hot rolling to less than 30%, the scale is prevented from being crushed during hot rolling, the iron-scale interface becomes smooth, and as a result, the arithmetic mean roughness of the surface of the hot-rolled steel sheet can be reduced. Therefore, it is preferable that the reduction rate at each stage of hot rolling is less than 30%, more preferably less than 28%, and even more preferably less than 25%. There is no need to set a lower limit, but if the reduction rate at each stage is too low, the number of rolling passes increases, the temperature of the steel sheet decreases, and it becomes difficult to ensure the final rolling temperature described below. Therefore, the maximum reduction rate at each stage of hot rolling may be 15% or more.
[0074] (7-3) Reduction rate of hot rolling: Total thickness reduction of 90% or more in the temperature range of 850 to 1100°C By performing hot rolling so as to reduce the sheet thickness by 90% or more in total in the temperature range of 850 to 1100°C, mainly recrystallized austenite grains are refined and the accumulation of strain energy in the unrecrystallized austenite grains is promoted. In addition, the recrystallization of austenite is promoted and the atomic diffusion of Sn is promoted, so that the standard deviation of the Sn concentration can be reduced. Therefore, it is preferable to perform hot rolling so as to reduce the sheet thickness by 90% or more in total in the temperature range of 850 to 1100°C.
[0075] In addition, the thickness reduction in the temperature range of 850 to 1100°C is the thickness at the entrance of the rolling process before the first rolling in this temperature range. 0 The exit thickness after the final rolling stage in this temperature range is t 1 Then, {(t 0 -t 1 ) / t 0}×100(%).
[0076] (7-4) Rolling completion temperature Tf: 850℃ or higher, less than 1010℃ The rolling completion temperature (rolling temperature in the final stage of hot rolling) Tf is preferably 850° C. or higher and lower than 1010° C. By setting the rolling completion temperature to 850° C. or higher and lower than 1010° C., the number of ferrite nucleation sites in austenite can be controlled within an appropriate range, and a desired ferrite fraction can be obtained.
[0077] (7-5) Residence time in the temperature range of 600 to 750°C: 3 seconds or more After the hot rolling is completed, the steel sheet is allowed to dwell in the temperature range of 600 to 750°C for 3 seconds or more, so that ferrite can be sufficiently generated. This allows the strength and ductility of the hot-rolled steel sheet to be compatible. The dwell time here refers to the time during which the steel sheet temperature is between 600°C and 750°C, and the steel sheet may be cooled during the dwell time. There is no need to set an upper limit for the dwell time, but it has been confirmed through experiments that there is no problem even if the dwell time is 30 seconds. In order to satisfy the above dwell time, it is not desirable to perform water cooling in the entire temperature range of 600 to 750°C.
[0078] (7-6) Winding temperature: 400℃ or less The coiling temperature is set to 400° C. or less. By setting the coiling temperature to 400° C. or less, the ferrite fraction can be controlled within a desired range, and high strength can be obtained. EXAMPLES
[0079] Next, the effect of one embodiment of the present invention will be described in more detail with reference to an example, but the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0080] Steels having the chemical compositions shown in Tables 1 and 2 were melted and continuously cast into slabs with thicknesses of 240 to 300 mm. The resulting slabs were used to obtain hot-rolled steel sheets shown in Table 4 under the manufacturing conditions shown in Table 3.
[0081] The area ratio of the metal structure, the standard deviation of the Sn concentration, the arithmetic mean roughness of the surface, the tensile strength TS, the total elongation El, and the 200,000 cycles strength FS of the obtained hot-rolled steel sheets were measured by the above-mentioned methods. The measurement results are shown in Table 4.
[0082] Method for evaluating the properties of hot-rolled steel sheets (1) Tensile strength properties If the tensile strength TS was 590 MPa or more, the total elongation El was 14.0% or more, and the tensile strength TS × total elongation El was 14,000 MPa·% or more, the hot-rolled steel sheet was deemed to have high strength and excellent ductility and passed the test. If any one of the conditions was not met, the hot-rolled steel sheet was deemed to have neither high strength nor excellent ductility and failed the test.
[0083] (2) Fatigue properties If the value "FS / (0.3×TS)+150" calculated from the 200,000 cycles strength FS and the tensile strength TS was 1.00 or more, or if FS was 450MPa or more, the hot-rolled steel sheet was deemed to have excellent fatigue strength and passed the test. On the other hand, if the value "FS / (0.3×TS)+150" calculated from the 200,000 cycles strength FS and the tensile strength TS was less than 1.00 and FS was less than 450MPa, the hot-rolled steel sheet was deemed to have poor fatigue strength and failed the test.
[0084] [Table 1]
[0085] [Table 2]
[0086] [Table 3]
[0087] [Table 4]
[0088] From Table 4, it can be seen that the hot-rolled steel sheets according to the examples of the present invention have high strength, as well as excellent ductility and fatigue properties. On the other hand, it can be seen that the hot-rolled steel sheets according to the comparative examples do not have one or more of the above properties. In addition, since the maximum rolling reduction rate in rough rolling of the hot-rolled steel sheet of Production No. 5 was 31%, the arithmetic mean roughness of the surface of the hot-rolled steel sheet increased.
Claims
1. The chemical composition, in mass%, is C: 0.040-0.250%, Si: 0.30% or less, Mn: 1.00-4.00%, sol. Al: 0.001 to 1.000%, Sn: 0.300-1.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Ti+Nb+V: 0 to 0.500%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-1.00%, Ni: 0-2.00%, B: 0 to 0.0100%, Ca: 0-0.0200%, Mg: 0 to 0.0200%, REM: 0-0.1000%, Bi: 0 to 0.020%, One or more of Zr, Co, Zn and W: 0 to 1.00% in total; The balance is Fe and impurities, The metal structure is Ferrite is 20.0% or more and less than 90.0% by area percent; The standard deviation of the Sn concentration is 0.50 mass% or less, The arithmetic mean roughness of the surface is less than 2.00 μm; A hot-rolled steel sheet having a tensile strength of 590 MPa or more.
2. The chemical composition, in mass%, Ti+Nb+V: 0.020-0.500%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-1.00%, Ni: 0.02-2.00%, B: 0.0001 to 0.0100%, Ca: 0.0005-0.0200%, Mg: 0.0005-0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005-0.020% The hot-rolled steel sheet according to claim 1, further comprising one or more selected from the group consisting of:
Citation Information
Patent Citations
Muting circuit
JP1979071918A
Hot rolled steel containing cu and sn
JP1994256904A
Hot rolled plate of sn-and ti-b-containing high strength steel excellent in surface characteristic and its production
JP1995118800A
Sn-containing low carbon hot rolled steel plate good in surface property and its production
JP1995138702A
Hot rolled steel sheet and manufacturing method therefor
JP2017031454A