Structure including metal wiring and method for manufacturing the same

The described method improves metal wiring adhesion to solder by using copper and solder with controlled mass content and a porous surface, addressing the complexity and adhesion issues in conventional methods.

JP7579209B2Active Publication Date: 2024-11-07ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021100224
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-22
Filing Date
2021-06-16
Publication Date
2024-11-07
Estimated Expiration
2041-06-16

AI Technical Summary

Technical Problem

Conventional methods for manufacturing metal wiring on circuit boards are complex and require photoresist materials, leading to weak adhesion between solder and metal wiring, causing separation under vibrations.

Method used

A structure and method involving copper and solder metal wiring with a specific mass content ratio, porous surface, and laser-irradiated coating to enhance adhesion, using a coating solution containing metal and metal oxide particles applied to a substrate, followed by laser firing and soldering.

Benefits of technology

The method produces metal wiring with excellent adhesion to solder, enhancing durability against vibrations and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579209000001
    Figure 0007579209000001
  • Figure 0007579209000002
    Figure 0007579209000002
  • Figure 0007579209000003
    Figure 0007579209000003
Patent Text Reader

Abstract

To provide a structure that has metal wiring excellent in adhesion with solder, and a method for manufacturing the same.SOLUTION: In one aspect, there is provided a structure that has a substrate, metal wiring arranged on the substrate, and a solder layer arranged on the metal wiring, wherein the metal wiring includes copper and solder and the content of the solder in the metal wiring is 2 mass% or more and 30 mass% or less. In one aspect, there is provided a method for manufacturing a structure including: an application step of applying a coating liquid including metal and / or metal oxide onto a substrate to obtain a coating film; a calcination step of calcining the coating film to form metal wiring; and soldering step of forming a solder layer on the metal wiring.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a structure including metal wiring and a method for manufacturing the same. [Background technology]

[0002] A circuit board has a structure in which conductive wiring is applied onto a substrate. The manufacturing method of a circuit board is generally as follows. First, a photoresist is applied onto a substrate to which a metal foil has been attached. Next, the photoresist is exposed to light and developed to obtain a negative shape of a desired circuit pattern. Next, the metal foil not covered by the photoresist is removed by chemical etching to form a pattern. This allows a high-performance conductive substrate to be manufactured.

[0003] However, the conventional methods have drawbacks such as the large number of steps, the complexity, and the need for a photoresist material.

[0004] In response to this, a direct wiring printing technique has been attracting attention, in which a dispersion (hereinafter also referred to as a "paste material") in which fine particles selected from the group consisting of metal fine particles and metal oxide fine particles are dispersed is used to directly print desired metal wiring on a substrate. This technique has a small number of steps, does not require the use of photoresist materials, and is therefore extremely productive.

[0005] One example of a direct printed wiring technique is a method in which a paste material is printed on a substrate by screen printing or inkjet printing, and then the paste material is thermally fired to obtain low-resistance metal wiring (see, for example, Patent Document 1).

[0006] Also, a method is known in which a paste material is applied to the entire surface of a substrate, and the paste material is selectively thermally fired by being irradiated with laser light in a pattern to obtain desired metal wiring (see, for example, Patent Documents 1 and 2).

[0007] Also, a method is known in which a dispersion liquid containing aggregate particles of cuprous oxide is applied to a polyethylene terephthalate (PET) substrate to a thickness of 10 to 20 μm, and then the coating is fired with a laser to produce copper wiring (see, for example, Patent Document 3). According to this method, areas other than the laser irradiated area are not heated, so that a low heat-resistant resin material such as PET can be used as the substrate.

[0008] After providing conductive wiring on a substrate by the above-mentioned method, when mounting components on a circuit board, the components are generally joined to the metal wiring by soldering. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2010 / 024385 [Patent Document 2] Japanese Patent Application Publication No. 5-37126 [Patent Document 3] Special Publication No. 2010-534932 Summary of the Invention [Problem to be solved by the invention]

[0010] However, since metal wiring is usually a smooth metal film (e.g., a copper film), when soldering is performed on the metal wiring, the adhesion between the solder and the metal wiring is weak, and a problem occurs in which the metal wiring and the solder peel off at their interface due to shocks such as bending and vibration when the circuit board is in use.

[0011] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a structure having metal wiring with excellent adhesion to solder, and a method for manufacturing the same. [Means for solving the problem]

[0012] The present disclosure encompasses the following aspects. [1] A substrate; A metal wiring disposed on the substrate; a solder layer disposed on the metal trace; A structure having the metal wiring includes copper and solder; A structure, wherein the solder content in the metal wiring is 2% by mass or more and 30% by mass or less. [2] 0.01 μm on the cross section of the thickness direction of the metal wiring 2 More than 1.8μm 2 The structure of claim 1, wherein there is at least one pore having a cross-sectional area less than [3] 1.8 μm in the cross section of the thickness direction of the metal wiring 2 3. The structure of claim 1 or 2, wherein no pores having a cross-sectional area greater than or equal to the diameter of the pores are present. [4] The structure according to any one of the above aspects 1 to 3, wherein the metal wiring further contains carbon. [5] The structure according to any one of the above aspects 1 to 4, which is a wiring material, an antenna for a housing of a portable information device, a mesh electrode, an electromagnetic wave shielding material, or a heat dissipation material. [6] A method for producing the structure according to any one of the above aspects 1 to 5, comprising the steps of: a coating step of applying a coating liquid containing a metal and / or a metal oxide onto a substrate to obtain a coating film; a firing step of firing the coating film to form metal wiring; and a soldering step of forming a solder layer on the metal wiring. [7] The method for producing a structure according to aspect 6, wherein the firing step includes irradiating the coating with a laser. [8] The method for producing the structure according to aspect 7, wherein in the firing step, the coating film is irradiated with the laser while a gas is flowing over the coating film. Effect of the Invention

[0013] According to one aspect of the present invention, it is possible to provide a structure having metal wiring with excellent adhesion to solder, and a method for manufacturing the same. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a schematic cross-sectional view showing a structure according to the present embodiment. [Diagram 2] 4 is a scanning electron microscope (SEM) image of holes on the surface of the metal wiring according to the embodiment. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a metal wiring manufacturing apparatus used for manufacturing the structure according to the present embodiment. [Figure 4] 5A to 5C are schematic diagrams illustrating overlapping laser irradiation in the method for manufacturing a metal wiring according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An exemplary embodiment of the present invention (hereinafter, abbreviated as "the present embodiment") will be described in detail below.

[0016] ≪Structure≫ One aspect of the present invention provides a structure having a substrate, a metal trace disposed on the substrate, and a solder layer disposed on the metal trace. In one aspect, the metal trace comprises copper and solder.

[0017] FIG. 1 is a schematic cross-sectional view showing a structure according to the present embodiment. Referring to FIG. 1, the structure 1 has a base material 11 and a metal wiring 13 arranged on a surface constituted by the base material 11. In a typical embodiment, the metal wiring 13 and an insulating region 14 are arranged adjacent to each other on the base material 11 in a cross-sectional view in the thickness direction to form a single layer 15. In one embodiment, the metal wiring 13 is a region of a coating film described later that is irradiated with laser light. In one embodiment, the insulating region 14 is a region of a coating film described later that is not irradiated with laser light. The insulating region may or may not be present. A solder layer 16 is arranged on the metal wiring 13. Solder 17 is also present in the metal wiring 13.

[0018] In the present disclosure, the presence and composition of elements in each member of the structure are confirmed by scanning electron microscope observation-energy dispersive X-ray analysis (SEM-EDX) or X-ray photoelectron spectroscopy. In one embodiment, element mapping is performed using SEM-EDX under the following conditions. Measurement equipment: Scanning electron microscope (e.g., SU8220 manufactured by Hitachi High-Technologies Corporation) Measurement conditions: Acceleration voltage 15 kV Measurement mode: Backscattered electrons Observation magnification: 10,000x Field of view size for observation and image analysis: [metal wiring thickness] × [length 10 μm in the direction perpendicular to the thickness direction] rectangle In the present disclosure, the thickness of each member of the structure is a value obtained by measuring an image obtained by cross-sectional observation under the above-mentioned conditions using a scanning electron microscope.

[0019] <Base material> The substrate 11 constitutes a surface for disposing the single layer 15, and the shape is not particularly limited. When the insulating region 14 is present, the material of the substrate 11 is preferably an insulating material in order to ensure electrical insulation between the metal wirings 13 separated by the insulating region 14. However, it is not necessary that the entire substrate 11 is made of an insulating material. It is sufficient that the portion constituting the surface on which the single layer 15 is disposed is made of an insulating material.

[0020] The surface of the base material on which the metal wiring is arranged may be a flat or curved surface, or may be a surface including steps. More specifically, the base material may be a substrate (e.g., a plate-like body, a film, or a sheet) or a three-dimensional object (e.g., a housing, etc.). The plate-like body is, for example, a support used in a circuit board such as a printed circuit board. The film or sheet is, for example, a base film that is a thin-film insulator used in a flexible printed circuit board.

[0021] Examples of the three-dimensional object include the housings of electrical devices such as mobile phone terminals, smartphones, smart glasses, televisions, personal computers, etc. Other examples of the three-dimensional object include dashboards, instrument panels, steering wheels, chassis, etc. in the automotive field.

[0022] Specific examples of the substrate include a substrate made of an inorganic material (hereinafter referred to as an "inorganic substrate") and a substrate made of a resin (hereinafter referred to as a "resin substrate").

[0023] The inorganic substrate is composed of, for example, glass, silicon, mica, sapphire, quartz, clay film, ceramic material, etc. The ceramic material is selected from, for example, alumina, silicon nitride, silicon carbide, zirconia, yttria, aluminum nitride, and a mixture of at least two of these. In addition, as the inorganic substrate, a substrate composed of glass, sapphire, quartz, etc., which has particularly high light transmittance, can be used.

[0024] Examples of the resin substrate include polypropylene (PP), polyimide (PI), polyester (polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), etc.), polyethersulfone (PES), polycarbonate (PC), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyacetal (POM), polyarylate (PAR), polyamide (PA) (PA6, PA66, etc.), polyamideimide (PAI), polyetherimide (PEI), polyphenylene ether (PPE), modified polyphenylene ether (m-PPE), polyphenylene sulfide (PPS), polyetherketone (PEK), polyetheretherketone (PEEK), polyphthalamide (PPA), polyethernitrile (PENt), polybenzimidazole (PBI), polycarbodiimide, polymethacrylamide, nitrile rubber, acrylic rubber, polyethylene tetrafluoride, epoxy resin, etc. It is composed of oil, phenolic resin, melamine resin, urea resin, polymethylmethacrylate resin (PMMA), polybutene, polypentene, ethylene-propylene copolymer, ethylene-butene-diene copolymer, polybutadiene, polyisoprene, ethylene-propylene-diene copolymer, butyl rubber, polymethylpentene (PMP), polystyrene (PS), styrene-butadiene copolymer, polyethylene (PE), polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), phenol novolac, benzocyclobutene, polyvinylphenol, polychloropyrene, polyoxymethylene, polysulfone (PSF), polyphenylsulfone resin (PPSU), cycloolefin polymer (COP), acrylonitrile-butadiene-styrene resin (ABS), acrylonitrile-styrene resin (AS), polytetrafluoroethylene resin (PTFE), polychlorotrifluoroethylene (PCTFE), and silicone resin (polysiloxane).

[0025] In addition to the above, a resin sheet containing cellulose nanofibers can also be used as the substrate.

[0026] In particular, at least one selected from the group consisting of PI, PET, and PEN is preferable because it has excellent adhesion to a single layer, is readily available in the market, and is available at low cost, which makes it advantageous from a business perspective.

[0027] Furthermore, at least one selected from the group consisting of PP, PA, ABS, PE, PC, POM, PBT, m-PPE, and PPS is preferable, particularly when used for a housing, because it has excellent adhesion to a single layer, excellent moldability and mechanical strength after molding, and heat resistance sufficient to withstand heat from laser light or the like irradiated when forming metal wiring.

[0028] The deflection temperature under load of the resin substrate is preferably 400° C. or less, or 280° C. or less, or 250° C. or less in terms of availability at low cost and commercial advantage, and is preferably 40° C. or more, or 50° C. or more, or 60° C. or more, or 80° C. or more, or 100° C. or more, or 150° C. or more in terms of handleability of the resin substrate. The deflection temperature under load is a value measured, for example, in accordance with JIS K7191.

[0029] The thickness of the substrate is preferably 1 μm to 100 mm, or 25 μm to 10 mm, or 25 μm to 250 μm, for example, when the substrate is a plate, film, or sheet. When the substrate has a thickness of 250 μm or less, the electronic device to be produced can be made lighter, more space-saving, and more flexible, which is preferable.

[0030] When the substrate is a three-dimensional object, its maximum dimension (i.e., the maximum length of one side) is preferably 1 μm to 1000 mm, or 200 μm to 100 mm, or 200 μm to 5 mm. When a substrate having a thickness within the above range is used, the mechanical strength and heat resistance after molding are good.

[0031] <Single layer> In this embodiment, the structure includes metal wiring 13, and typically has a single layer 15 including metal wiring 13 and insulating region 14. From the viewpoint of manufacturing using a simple process, it is preferable that both metal wiring 13 and insulating region 14 are present. On the other hand, from the viewpoint of improving insulation, it is preferable that insulating region 14 is not present.

[0032] In the single layer 15, "single" means that the layer is not a multilayer structure and that the layer is continuous in cross section. Therefore, the single layer is distinguished from a state in which the space between patterned wiring layers is filled with solder paste to form a single layer, as seen in a printed circuit board, for example. Also, "single" does not mean that the entire layer is homogeneous. In other words, the single layer may have differences in conductivity, particle state (fired and unfired), etc., such as the relationship between the metal wiring 13 and the insulating region 14, and a boundary (i.e., an interface) may exist between the metal wiring 13 and the insulating region 14.

[0033] The thickness of a single layer may be, in one embodiment, 500 nm or more, or 700 nm or more, or 1000 nm or more, and may be 500 μm or less, or 300 μm or less, or 100 μm or less.

[0034] <Metal wiring> The metal wiring 13 exhibits electrical conductivity. In one embodiment, the metal wiring 13 is an irradiated region irradiated with laser light in a manufacturing method for obtaining a desired metal wiring by irradiating a laser light in a pattern and thermally sintering the same. In another embodiment, the metal wiring 13 is a sintered region including a sintered body obtained by sintering the insulating region 14 by light irradiation.

[0035] The shape of the metal wiring 13 in a plan view, i.e., the pattern, may be any shape such as a straight line, a curved line, a circle, a square, a bent shape, etc., and is not particularly limited. For example, when the metal wiring is formed by scanning a coating film with a laser beam, there are few restrictions on the shape.

[0036] In one embodiment, the metal wiring includes copper and solder. Copper is preferred because of its low cost and high migration resistance. The copper in the metal wiring may have a structure in which some or all of the copper-containing particles are fused to each other, for example.

[0037] [Solder] The solder of the present disclosure is a material containing one or more metals selected from the group consisting of tin, lead, bismuth, indium, and zinc, and having a melting point of 250° C. or less. In a preferred embodiment, the lead content in the solder is 0.1% by mass or less.

[0038] The solder preferably contains tin in an amount of 4% by mass to 99.5% by mass, or 10% by mass to 95% by mass, or 20% by mass to 60% by mass. When the solder contains more than 0.1% by mass of lead, the solder may contain preferably 1% to 95% by mass, or 10% to 80% by mass, or 20% to 60% by mass of lead. The solder preferably contains bismuth in an amount of 0 to 60% by mass, or 0.1 to 50% by mass, or 0.3 to 40% by mass. The solder preferably contains 0 mass % to 60 mass %, or 0.5 mass % to 20 mass %, or 1 mass % to 10 mass % of indium. The solder preferably contains 0% to 15% by mass, or 5% to 12% by mass, or 7% to 10% by mass of zinc.

[0039] When the lead content in the solder is 0.1% by mass or less, the amount of tin in the solder is preferably 30% by mass or more and 99% by mass or less, or 35% by mass or more and 98% by mass or less, or 40% by mass or more and 97% by mass or less.

[0040] In a preferred embodiment, the solder has the following composition: Tin: 40% to 95% by mass, Bismuth: 0% by mass to 60% by mass, Indium: 0% by mass to 60% by mass, and Zinc: 0% to 10% by mass.

[0041] The melting point of the solder is, in one embodiment, 250° C. or less, or 240° C. or less, or 220° C. or less, or 200° C. or less from the viewpoint of realizing good adhesion between the solder layer and the metal wiring, and, in one embodiment, 120° C. or more, or 140° C. or more, or 160° C. or more from the viewpoint of ensuring good mechanical strength of the solder layer. In the present disclosure, the melting point of the solder is a value determined as the endothermic peak temperature when measured using a differential scanning calorimeter under a nitrogen atmosphere under the temperature increase condition of 5° C. per minute.

[0042] The solder 17 may form a solder area having a certain size within the metal wiring 13. The solder area may contain only solder, or may contain components other than solder (specifically, one or more of copper, carbon, etc.). In the latter case, the ratio of components other than solder in the solder area is preferably 90 mass % or less, 80 mass % or less, or 70 mass % or less. The ratio may be, for example, 5 mass % or more, 10 mass % or more, or 15 mass % or more.

[0043] The shape of the solder region is not particularly limited, and may form a continuous phase or a dispersed phase (i.e., an island structure) inside the metal wiring 13. In the case of a dispersed phase, the dispersed size (area of ​​the dispersed phase in the cross section in the thickness direction of the metal wiring) is preferably 0.001 μm in one embodiment. 2 More than 1.8μm 2 Less than or equal to 0.001μm 2 More than 1.5μm 2 Less than or equal to 0.001μm 2 1.0μm or more 2 Less than or equal to 0.001μm 2 More than 0.5μm 2 The dispersion size may be less than 1 / 2 mm. The dispersion size is a value calculated from an image obtained by cross-sectional observation using a scanning electron microscope (SEM). In one embodiment, as described below, after a solder layer is disposed on a metal wiring, the constituent material of the solder layer penetrates into the metal wiring to form a solder region. Therefore, in one embodiment, the dispersion size of the dispersed phase in the solder region may be similar to the size of a hole that the metal wiring may have before the solder layer is formed, as described below.

[0044] The solder 17 may or may not be continuous with the solder layer 16 described below. When the solder 17 and the solder layer 16 are continuous, in an observation image of a cross section of the structure in the thickness direction using a scanning electron microscope (SEM) described below, the substrate side of the metal wiring at the maximum thickness part of the metal wiring is taken as the boundary, and the solder layer 16 is taken as the substrate side.

[0045] The solder content in the metal wiring is preferably 2 mass% or more, or 2.2 mass% or more, or 2.5 mass% or more, or 2.7 mass% or more, or 3 mass% or more from the viewpoint of improving adhesion between the solder layer and the metal wiring due to the anchor effect of the solder, and is preferably 30 mass% or less, or 28 mass% or less, or 25 mass% or less, or 22 mass% or less, or 20 mass% or less from the viewpoint of containing an appropriate amount of copper in the metal wiring to achieve good conductivity.

[0046] From the viewpoint of realizing good electrical conductivity of the metal wiring, the copper content in the metal wiring is preferably 70 mass% or more, or 72 mass% or more, or 75 mass% or more, or 78 mass% or more, or 80 mass% or more, and from the viewpoint of containing an appropriate amount of solder in the metal wiring to realize a good anchor effect, the copper content is preferably 98 mass% or less, or 97.8 mass% or less, or 97.5 mass% or less, or 97.3 mass% or less, or 97 mass% or less.

[0047] The metal wiring may contain a metal (e.g., silver) and a metal oxide (e.g., copper oxide, which is cuprous oxide, cupric oxide, and / or cuprous oxide) in addition to copper and solder. For example, the surface side portion of the metal wiring may have a structure in which copper-containing particles are fused to each other, and the substrate side portion may have a structure containing copper oxide. This is preferable because the copper oxide generates strong bonds between the copper particles and the copper oxide can further increase the adhesion between the copper particles and the substrate.

[0048] <Carbon> The metal wiring preferably contains carbon from the viewpoint of improving bending resistance. The amount of carbon in the metal wiring is preferably 0.5% by mass to 40% by mass, or 1% by mass to 35% by mass, or 5% by mass to 35% by mass. When carbon is present in the metal wiring, the carbon may be present in a state of being uniformly mixed with copper, in a sea part or an island part in a sea-island structure, or in other continuous structures. For example, carbon may be present in a solder region in the metal wiring. Carbon can be contained in the metal wiring by adding an organic substance to the coating liquid described later. In a typical embodiment, the organic substance in the coating liquid is baked by laser irradiation, and can be present in the metal wiring as inorganic carbon.

[0049] <Metal wiring holes> It is preferable that holes are present on the surface of the metal wiring before the solder layer is formed. The presence of the holes allows the solder to penetrate into the metal wiring when forming the solder layer 16 on the metal wiring 13 (also referred to simply as soldering in this disclosure), making it easy to form a metal wiring containing solder. In one embodiment, the surface of the metal wiring is provided with holes having a diameter of 0.001 μm. 2 1.0μm or more 2 From the viewpoint of allowing solder to easily penetrate into the metal wiring during soldering and maintaining the strength of the metal wiring, the opening area of ​​the hole is preferably 0.001 μm 2 1.0μm or more 2 Less than or equal to 0.001μm 2 More than 0.5μm 2 Less than or equal to 0.001μm 2 More than 0.1μm 2 The surface of the metal wiring is less than 0.001 μm. 2 1.0μm or more 2 The area ratio of holes having the following opening area is preferably 0.01 area % or more and 5 area % or less, or 0.01 area % or more and 3 area % or less, or 0.01 area % or more and 2 area % or less, or 0.05 area % or more and 2 area % or less, or 0.1 area % or more and 1 area % or less, in a 40 μm × 40 μm field of view of a metal wiring surface image obtained by magnifying 2000 times with a scanning electron microscope (SEM).

[0050] FIG. 2 is a scanning electron microscope (SEM) image of a hole on the surface of a metal wiring according to this embodiment. 2 1.0μm or more 2 The example shows that the area ratio of holes having the following opening areas is in the range of 0.01 area % to 5 area %. With such metal wiring, the solder easily penetrates into the holes during soldering, and the anchor effect realizes good adhesion between the solder layer and the metal wiring.

[0051] Before the solder layer is formed, the cross section of the metal wiring in the thickness direction is 0.01 μm. 2 More than 1.8μm 2 Preferably, there is at least one hole having a cross-sectional area of ​​less than 1.8 μm. 2 From the viewpoint of allowing solder to easily penetrate into the metal wiring during soldering and of being able to favorably maintain the strength of the metal wiring, the cross-sectional area of ​​the hole is preferably 0.01 μm or less. 2 More than 1.8μm 2 Less than or equal to 0.01 μm 2 More than 1.5μm 2 Less than or equal to 0.01μm 2 1.0μm or more 2 Less than or equal to 0.01μm 2 More than 0.5μm 2 Less than 0.01μm 2 More than 1.8μm 2 When holes having a cross-sectional area of ​​less than 1.8 μm exist, the solder easily penetrates into the metal wiring, and therefore good adhesion between the solder layer and the metal wiring can be achieved by the anchor effect. 2 The absence of holes having a cross-sectional area of ​​this magnitude makes it possible to suppress a decrease in strength and adhesion of the metal wiring caused by infiltrating solder.

[0052] When holes are present in the cross section of the metal wiring after the solder layer is formed, the bending resistance of the metal wiring is good, which is preferable. From the viewpoint of obtaining good bending resistance, the size of the holes is preferably 0.01 μm. 2 More than 1.8μm2 Less than or equal to 0.01 μm 2 More than 1.5μm 2 Less than or equal to 0.01μm 2 1.0μm or more 2 Less than or equal to 0.01μm 2 More than 0.5μm 2 The following is the result.

[0053] The confirmation of the presence of holes having the above opening area or cross-sectional area and the calculation of the above area ratio are carried out using a scanning electron microscope (SEM) under the following conditions. Measurement equipment: Scanning electron microscope (e.g., SU8220, manufactured by Hitachi High-Technologies Corporation) Measurement conditions: Accelerating voltage 5 kV Measurement mode: Secondary electrons (for surface observation), or backscattered electrons (for cross-sectional observation) Observation magnification: 2000x (for surface observation) or 10000x (for cross-sectional observation) Field of view size for observation and image analysis: 40 μm × 40 μm (for surface observation), or a rectangle of [metal wiring thickness] × [length perpendicular to the thickness direction 10 μm] (for cross-sectional observation)

[0054] The area and area ratio of the holes are values ​​obtained by image analysis using the analysis software ImageJ (open source, public domain image processing software) from the SEM image. Specifically, the image is binarized (in one embodiment, the threshold value is set to the default) and color-coded so that the holes can be identified, and the area ratio between the holes and the non-hole parts is obtained, and the above-mentioned area ratio is calculated.

[0055] The metal wiring having holes before forming the solder layer can be formed by baking the coating liquid by a heating method, a light irradiation method, or the like to form a pattern of the metal wiring. For example, the size and amount of holes can be adjusted by adjusting the baking temperature and / or baking time in the thermal baking process or the light baking process after the coating liquid is applied. More specifically, the size of the holes can be controlled by the scanning speed and spot diameter of the laser light during laser light irradiation. Increasing the laser light scanning speed tends to increase the size of the holes, and decreasing the laser light scanning speed tends to decrease the size of the holes. Increasing the spot diameter tends to increase the size of the holes, and decreasing the spot diameter tends to decrease the size of the holes. On the other hand, the above-mentioned area ratio of the holes can be controlled by the scanning speed of the laser light during laser light irradiation and the overlap ratio described below when the laser light is irradiated overlappingly as described below. Increasing the laser light scanning speed tends to increase the above-mentioned area ratio, and decreasing the laser light scanning speed tends to decrease the above-mentioned area ratio. When the overlap rate described below is decreased, the above area ratio tends to increase, and when the overlap rate is increased, the above area ratio tends to decrease.

[0056] The width of the metal wiring may be, in one embodiment, 50 μm or more, or 100 μm or more, or 150 μm or more, and in one embodiment, 30 mm or less, or 25 mm or less, or 20 mm or less.

[0057] The thickness of the metal wiring may be, in one embodiment, 500 nm or more, or 700 nm or more, or 1000 nm or more, and in one embodiment, 50 μm or less, or 40 μm or less, or 30 μm or less.

[0058] <Insulation area> The insulating region 14 exhibits electrical insulation. In one embodiment, the insulating region 14 is an unirradiated region that is not irradiated with laser light in a manufacturing method in which a desired metal wiring is obtained by irradiating a laser light in a pattern and thermally sintering the pattern. In one embodiment, the insulating region 14 is an unfired region that is not sintered by light irradiation.

[0059] In one embodiment, the insulating region contains a metal oxide, more specifically, copper oxide (cuprous oxide and / or cupric oxide in one embodiment). The copper oxide has, for example, a particulate shape. The average primary particle size of the particles containing copper oxide is preferably 1 nm or more and 100 nm or less, more preferably 1 nm or more and 50 nm or less, and even more preferably 1 nm or more and 20 nm or less. The smaller the particle size, the better the electrical insulation of the insulating region, and therefore, it is preferable. The average primary particle size is a value measured by a scanning electron microscope.

[0060] The insulating region may contain metal particles, such as copper particles, in addition to the metal oxide, i.e., the coating liquid described below may contain copper.

[0061] <Solder layer> A solder layer 16 is disposed on the metal wiring 13. The solder layer may be composed of the same solder as exemplified in the above section [Solder]. Thus, the solder layer contains at least one selected from the group consisting of tin, lead, bismuth, indium, and zinc, and in one embodiment, the lead content is 0.1 mass % or less from the viewpoint of safety. The solder layer may be disposed on the entire surface or a part of the surface of the metal wiring 13. Furthermore, when an insulating region exists, the solder layer may be formed on the insulating region in addition to on the metal wiring. The solder layer and the solder in the metal wiring may be continuous or discontinuous.

[0062] The thickness of the solder layer is preferably 50 μm or more, or 70 μm or more, or 100 μm or more, and preferably 3 mm or less, or 2.5 mm or less, or 2 mm or less.

[0063] <Manufacturing method of structure> One aspect of the present invention provides a method for producing a structure, the method comprising the steps of: a coating step of applying a coating liquid containing a metal and / or a metal oxide onto a substrate to obtain a coating film; a firing step of firing the coating film to form metal wiring; a soldering step of forming a solder layer on the metal wiring; Includes.

[0064] Hereinafter, a method using a coating liquid containing cuprous oxide particles will be described as an example, but the present invention is not limited thereto.

[0065] <Coating process> In this step, the coating liquid is applied onto the substrate to obtain a coating film. The coating liquid can be prepared by dispersing a metal and / or metal oxide in a dispersion medium. From the viewpoint of obtaining low-resistance metal wiring, copper particles are preferred as the metal. From the viewpoint of the stability of the coating liquid, copper oxide particles are preferred as the metal oxide, and cuprous oxide particles are particularly preferred as the copper oxide particles. In a preferred embodiment, the coating liquid contains copper oxide particles and a dispersant. The dispersant is preferably a phosphorus-containing organic compound, but other dispersants may be used as long as they do not adversely affect the electrical insulation of the insulating region.

[0066] As the dispersion medium, alcohols (monohydric alcohols and polyhydric alcohols (eg, glycol)), ethers of alcohols (eg, glycol), esters of alcohols (eg, glycol), and the like can be used. Specific examples of the solvent include propylene glycol monomethyl ether acetate, 3-methoxy-3-methyl-butyl acetate, ethoxyethyl propionate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol tertiary butyl ether, dipropylene glycol monomethyl ether, ethylene glycol butyl ether, ethylene glycol ethyl ether, ethylene glycol methyl ether, ethylene glycol, 1,2-propylene glycol, 1,3-butylene glycol, 2-pentanediol, 2-methylpentane-2,4-diol, 2,5-hexanediol, 2,4-heptanediol, 2-ethylhexane-1,3-diol, diethylene glycol, hexanediol, octanediol, triethylene glycol, tri-1,2-propylene glycol, glycerol, and ethylene glycol monohexyl. ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, ethylene glycol monobutyl acetate, diethylene glycol monoethyl ether acetate, methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, 2-butanol, t-butanol, n-pentanol, i-pentanol, 2-methylbutanol, 2-pentanol, t-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, 1-hexanol, 2-hexanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, 2-octanol, n-nonyl alcohol, 2,6 dimethyl-4-heptanol, n-decanol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, diacetone alcohol, and the like.These may be used alone or in combination, and are selected according to the coating method, taking into consideration volatility, coating equipment, solvent resistance of the substrate to be coated, and the like.

[0067] In one embodiment, the total content of metal and / or metal oxide particles in the coating liquid may be 5% by mass or more and 70% by mass or less, the content of the dispersant, if any, may be 0.025% by mass or more and 35% by mass or less, and the content of the dispersion medium may be 30% by mass or more and 95% by mass or less.

[0068] Methods for forming metal wiring include 1) a method in which a pattern of a coating liquid is formed as a coating film using a specific printing method, and then the coating film is baked, and 2) a method in which a coating liquid is coated over the entire surface of a substrate to form a coating film, and then the coating film is laser-drawn to form a specific pattern, thereby producing a desired pattern. Baking methods include methods using an incinerator, plasma baking, light baking, etc.

[0069] The coating film (i.e., a thin film made of a coating liquid) can be formed by applying the coating liquid onto a substrate and, if necessary, removing the dispersion medium by drying. The method for forming the coating film is not particularly limited, and coating methods such as die coating, spin coating, slit coating, bar coating, knife coating, spray coating, and dip coating can be used. It is desirable to apply the coating liquid to a uniform thickness on the substrate using these methods.

[0070] The coating liquid may be dried as desired. The method of the present embodiment preferably includes a drying step for removing the dispersion medium from the coating liquid. The drying step is preferably carried out at 60° C. to 120° C. for 30 minutes to 5 hours.

[0071] <Firing process> In this step, firing is performed to sinter and reduce the metal and / or metal oxide particles in the coating film to form low-resistance metal wiring. The firing method includes a heating method and a light irradiation method, but the light irradiation method is preferred in that a part of the coating film is selectively fired to obtain a metal wiring of a desired pattern.

[0072] As the light irradiation method, for example, a flash light method using a discharge tube such as xenon as a light source or a laser light method can be applied. With these methods, the coating film formed on the substrate can be heated to a high temperature in a short time by exposing it to high-intensity light for a short time, and baked. Since the baking time is short, damage to the substrate is small, and the method can be applied to resin film substrates with low heat resistance.

[0073] The flash light method is a method in which, for example, a xenon lamp (discharge tube) is used to instantly discharge the charge stored in a capacitor. In this method, a large amount of pulsed light (e.g., xenon lamp light) is generated and irradiated onto the coating film formed on the substrate, thereby instantly heating the coating film to a high temperature. The amount of exposure can be adjusted by the light intensity, light emission time, light irradiation interval and number of times. By selectively irradiating a portion of the coating film with light from a light source through a mask, it is possible to form metal wiring in a desired pattern.

[0074] When a laser light source is used as the light emitting light source, the desired irradiation effect can be obtained, as with the flash light method. In addition to the adjustment items described above for the flash light method, the laser light source also has a degree of freedom in wavelength selection. Therefore, it is possible to select the wavelength taking into account the light absorption wavelength of the coating film and / or substrate. A preferred example of firing using a laser beam method will be further described below.

[0075] [Light curing by laser irradiation] By selectively irradiating the coating film with a laser only at the places where metal wiring is to be formed, only the parts irradiated with the laser are fired, and metal wiring is formed. In one embodiment, the firing reduces metal oxide particles to generate metal particles, and the generated metal particles are sintered (fused) together to form a single body, thereby forming metal wiring.

[0076] The emission wavelength of the laser light preferably has a central wavelength in the range of 355 nm to 550 nm. By irradiating the laser light with a wavelength in this range, the metal in the coating film can be effectively sintered. From the viewpoint of enhancing the sinterability of the metal, the laser light preferably has a central wavelength in the range of 355 nm to 400 nm, more preferably 355 nm.

[0077] The laser light may be not only a fundamental wave but also a harmonic wave extracted as necessary. The laser light may be a CW wave (continuous wave) or a pulse wave. The pulse wave can instantaneously progress the baking while preventing the diffusion of heat by irradiating a light beam with a high peak value. The width of one pulse of the pulse wave is preferably 1 to 100 nanoseconds, or 2 to 50 nanoseconds, or 3 to 30 nanoseconds, from the viewpoint of suppressing ablation of the coating film during light irradiation.

[0078] From the viewpoint of suppressing scattering of laser light due to smoke generated during laser irradiation, it is preferable to irradiate the coating film with the laser while gas is flowing over the coating film. The gas to be used in this case is not particularly limited, but may include air, nitrogen, argon, helium, etc., and it is preferable to use nitrogen from the viewpoint of inertness and low cost.

[0079] In one embodiment, the term "gas flowing on the coating film" means that a flow with a flow rate of 0.01 m / s or more and 1.0 m / s or less occurs at the laser irradiated portion of the coating film. The gas flow rate is more preferably 0.05 m / s or more and 0.8 m / s or less, or 0.1 m / s or more and 0.6 m / s or less. The gas flow does not need to occur at the same flow rate over the entire coating film surface, and it is sufficient that the gas flow occurs at a certain point on the coating film irradiated with the laser light. The gas flow rate is a value measured by installing a measuring part of an anemometer at a position 10 mm away from the laser light irradiation point on the coating film surface in the vertical direction to the coating film. The means for causing the gas flow is not particularly limited as long as it can cause the gas to flow on the coating film surface. A blower of a type that blows air by motor drive may be used, or the gas may be directly flowed from a high-pressure gas cylinder through a pipe, or a device that flows gas compressed by a compressor or the like may be used.

[0080] (Metal wiring manufacturing equipment) The firing by the laser light method can be carried out, for example, by using a metal wiring manufacturing apparatus as described below. FIG. 3 is a schematic diagram showing an example of a metal wiring manufacturing apparatus used for manufacturing the structure according to this embodiment, and the metal wiring manufacturing apparatus 10 may have a structure holding unit 101, a light beam oscillator 102 that oscillates laser light, a gas supply unit 103, a light beam scanning unit 104, a speed control unit 105, and a computer 106. In one embodiment, the structure holding unit 101 is a sample chamber. The sample chamber may have a window, and the window may have optical transparency that allows the light beam to reach the coating film 12 through the window. The sample chamber may have a gas inlet, and may be configured such that, for example, gas from the gas supply unit 103 (which may be, for example, the above-mentioned blower, compressor, etc.) is introduced into the sample chamber through the gas inlet. Alternatively, the metal wiring manufacturing apparatus may not have a sample chamber. In this case, the gas may be directly flowed to the coating film 12 on the substrate 11.

[0081] Light beam scanning unit The light beam scanning unit 104 scans the light beam L emitted from the light beam oscillator 102. FIG. 3 shows an example in which the light beam scanning unit 104 is a galvanometer scanner. The galvanometer scanner as the light beam scanning unit 104 has an X-axis galvanometer mirror 104a, an X-axis galvanometer motor 104b, a Y-axis galvanometer mirror 104c, and a Y-axis galvanometer motor 104d. The galvanometer scanner may have an fθ lens (not shown), a Z-axis adjustment drive lens (not shown), and the like. The X-axis galvanometer motor 104b and the Y-axis galvanometer motor 104d are electrically connected to a speed control unit 105 (e.g., a scanner control unit).

[0082] The galvano scanner is configured to be able to control the rotation angle and rotation speed of the X-axis galvano motor 104b and the Y-axis galvano motor 104d in accordance with a control signal from a speed control unit 105. The speed control unit 105 is controlled by a computer . The light beam L is scanned by the light beam scanning unit 104 and irradiated onto the surface of the coating film 12 formed on the substrate 11 .

[0083] In the above, a galvano scanner is exemplified as the light beam scanning unit 104, but a light beam scanning unit other than a galvano scanner can also be used. For example, instead of the galvano scanner, the light beam scanning unit 104 may use an XY stage as a mounting table that can move the substrate 11 on which the coating film 12 is formed in both the X-axis direction and the Y-axis direction, and move the substrate 11 instead of moving the irradiation point P of the laser light L.

[0084] The light beam scanning unit 104 (galvanometer scanner) shown in FIG. 3 uses an X-axis galvanometer mirror 104a and a Y-axis galvanometer mirror 104c for movement in the X-axis and Y-axis directions, respectively. However, it is also possible to use a galvanometer mirror for either the X-axis or the Y-axis, for example, to use a galvanometer mirror for movement only in the X-axis direction and a motor of a mounting table (not shown) on which the substrate 11 is placed, for movement in the Y-axis direction.

[0085] Speed ​​Control Unit The scanning speed control in the metal wiring manufacturing apparatus 10 can be performed, for example, as follows. First, scanning data (coordinate data) indicating the desired shape, position, and size of the metal wiring pattern is input to the speed control unit 105. The scanner control unit as the speed control unit 105 calculates the length (L) (unit: mm) of the scanning line from the length along the X-axis direction of the pattern based on the scanning data. Next, based on the calculated scanning line length (L), the scanner control unit calculates the speed (V) (unit: mm / sec) at which the laser light is scanned (hereinafter referred to as scanning speed) so as to obtain a predetermined scanning period (F) (unit: Hz) (e.g., 15 Hz) using the following formula. Scanning speed (V) = Scanning period (F) x Scan line length (L)

[0086] Next, the scanner control unit causes the galvano scanner serving as the light beam scanning unit 104 to move the irradiation point P of the laser light L in the X-axis direction according to the scanning speed calculated in this manner, and executes one scan. Thereafter, the scanner control unit causes the galvano scanner to move the irradiation point P of the laser light L in the Y-axis direction. As described above, the scanning speed (V) of the laser light L can be set based on the length (L) of the scan line so that the scanning period (F) is the same at any position within the coating film 12.

[0087] Output adjustment mechanism The metal wiring manufacturing apparatus may include an output adjustment mechanism for adjusting the output of the light beam. This makes it possible to suppress ablation and / or carbonization during irradiation of the light beam. One example of the output adjustment mechanism is an attenuator disposed on the path of the light beam. The attenuator is electrically connected to a computer and can change the output value to an arbitrary value in response to a control signal from the computer. Alternatively, the output adjustment mechanism may be configured so that the output value can be changed by manual operation.

[0088] Pulse suppression mechanism When the light oscillator is configured to emit pulsed light, the metal wiring manufacturing apparatus may include a pulse suppression mechanism that suppresses the initial pulse of the pulsed light. The pulse suppression mechanism prevents ablation and / or carbonization by preventing an excessively large pulse of light at the start of emission from being irradiated onto the coating film. The pulse suppression mechanism may have, for example, a first pulse suppression function (FPS function), that is, a function of predicting excess output of the initial pulse in advance and reducing the excess output.

[0089] Spot adjustment mechanism The metal wiring manufacturing apparatus may have a spot adjustment mechanism that adjusts the spot diameter at the focal position of the light beam. The spot adjustment mechanism prevents ablation and / or carbonization by controlling the condensing density of the light beam to adjust the spot diameter. One example of the spot adjustment mechanism is a device that expands or reduces the diameter of the light beam incident on the galvano scanner, and for example, a beam expander can be used. By changing the diameter of the light beam, the spot diameter at the focal point focused by the focusing lens can be changed. By expanding the diameter of the light beam, the spot diameter becomes smaller, and by reducing the diameter of the light beam, the spot diameter becomes larger.

[0090] [Overlapping laser irradiation] The laser light may be repeatedly applied to a desired area on the coating film. FIG. 4 is a schematic diagram illustrating overlapping irradiation of the laser light in the manufacturing method of the metal wiring according to one embodiment of the present invention. Referring to FIG. 4, after irradiating the laser light as a first scanning line R1 having a scanning line width S1, the laser light is irradiated as a second scanning line R2 so as to overlap the first scanning line R1 in the scanning line width direction. According to such overlap, the amount of heat stored in the overlapping area is increased, so that the degree of sintering of the coating film can be increased and a hard metal wiring can be formed. As a result, for example, even when the metal wiring is formed on a flexible substrate and bent, the metal wiring can follow the flexible substrate without cracking. Furthermore, the high degree of sintering of the coating film allows the formation of a metal wiring with a low resistance value.

[0091] The ratio S2 / S1 (also referred to as overlap ratio S in the present disclosure) of the overlap width S2 to the scan line width S1 (e.g., 320 μm) of the first scan line R1 is preferably 5% or more, or 10% or more, or 15% or more, or 20% or more from the viewpoint of smoothly progressing the sintering of the metal and / or metal oxide, and is preferably 99.5% or less, or 99% or less, or 95% or less, or 90% or less, or 85% or less from the viewpoint of performing sintering while moving the laser at an industrially practical speed. The scanning direction of the second scan line may be the same as or different from that of the first scan line.

[0092] <Soldering process> In this process, a solder layer is formed on the metal wiring by soldering. As the solder material, those exemplified in the section "Structure" can be used. The soldering process is not particularly limited as long as it is a conventionally known method, but a soldering iron is heated according to the type of solder to be used. The heated soldering iron is placed on the metal wiring, and the solder is pressed and melted to form a solder layer. The soldering process forms a solder layer and allows the solder to penetrate into the metal wiring, particularly into the inside of the holes in the metal wiring.

[0093] <Application Examples> The structure according to the present embodiment can be suitably applied to, for example, wiring materials for electronic circuit boards and the like (printed circuit boards, RFID, replacement for wire harnesses in automobiles, etc.), antennas (antennas for portable information device housings) formed on the housings of portable information devices (smartphones, etc.), mesh electrodes (electrode films for capacitive touch panels), electromagnetic wave shielding materials, and heat dissipation materials. EXAMPLES

[0094] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples.

[0095] <Example 1> [Production of coating solution] 80 g of copper(II) acetate monohydrate (Wako Pure Chemical Industries, Ltd.) was dissolved in a mixed solvent consisting of 800 g of ion-exchanged water and 400 g of 1,2-propylene glycol (Wako Pure Chemical Industries, Ltd.), 20 g of hydrazine hydrate (Wako Pure Chemical Industries, Ltd.) was added, and the mixture was stirred under a nitrogen atmosphere and then separated into a supernatant and a precipitate by centrifugation.

[0096] 0.4 g of DISPERBYK-145 (trade name, manufactured by BYK-Chemie) (BYK-145) as a phosphorus-containing organic compound and 6.6 g of ethanol (manufactured by Wako Pure Chemical Industries, Ltd.) as a dispersion medium were added to 2.8 g of the obtained precipitate, and the mixture was dispersed using a homogenizer under a nitrogen atmosphere, and then centrifuged to recover the precipitate. The precipitate was diluted with ethanol and dispersed using a homogenizer. By repeating the above-mentioned centrifugation (concentration) and dispersion (dilution), a coating solution containing cuprous oxide particles containing cuprous oxide (copper(I) oxide) was obtained. The final composition was 2.8 g of precipitate, 0.4 g of BYK-145, 6.6 g of ethanol, and 0.01 g of hydrazine hydrate. The average primary particle diameter of the cuprous oxide was measured by the cumulant method using FPAR-1000 manufactured by Otsuka Electronics Co., Ltd., and was found to be 8 nm.

[0097] [Sample preparation] (Formation of coating film) The surface of a polyimide substrate measuring 70 mm x 70 mm x 0.1 mm in width x depth x thickness was subjected to UV ozone treatment for 3 minutes, after which 1 ml of the coating solution was dropped onto the substrate and spin-coated (500 rpm x 300 seconds), dried at room temperature for 10 minutes, and then dried at 90°C for 2 hours to obtain a sample in which a coating film with a thickness of 3.5 μm was formed on the substrate.

[0098] (Laser firing) Laser irradiation was performed using a metal wiring manufacturing device with the configuration shown in Figure 3. Nitrogen gas was fed into the sample case at 1.0 L / min. The top surface of the sample case was made of glass, with a structure that allowed the laser light to pass through. Using a galvano scanner, the sample in the sample case was irradiated with laser light (center wavelength 355 nm, frequency 300 kHz, pulse width 10 ns, output 395 mW, spot diameter 110 μm) while moving the focal position at a maximum speed of 5 mm / sec. At this time, the laser light was moved 5 mm in the scanning direction (first irradiation), and then moved 10 μm in a direction perpendicular to the scanning direction and moved again in the scanning direction at a maximum speed of 5 mm / sec (second irradiation). By repeating this operation, the laser light was scanned while moving 10 μm at a time in the direction perpendicular to the scanning direction, and a metal wiring containing copper with the desired dimensions of 5 mm in length and 1 mm in width was obtained. The overlap rate was calculated using the following method and was 91.1%. Specifically, the surface of the obtained metal wiring was observed with an optical microscope (20x magnification), and the scanning lines of the laser light were confirmed to be spaced 21μm apart. In addition, the width of the laser light irradiation track in the non-overlapping portion at the end of the scanning of the metal wiring was 235μm. The overlap rate calculated by the following formula was 91.1%. (Overlap rate) = (235 μm - 21 μm) ÷ 235 μm

[0099] (Soldering) The solder used was Eco Solder LEO (Senju Metal Industry Co., Ltd.) (element composition: tin 42% by mass, bismuth 58% by mass, melting point: 140° C.) The soldering iron was heated to 160° C. to form a solder layer on the metal wiring. The thicknesses of the metal wiring and the solder layer were 1.5 μm and 1000 μm, respectively.

[0100] [Evaluation of solder content in metal wiring] The solder content was determined based on the distribution of tin obtained by scanning electron microscope observation-energy dispersive X-ray analysis (SEM-EDX) in the cross section of the metal wiring in the thickness direction. In the cross section image obtained by magnifying 10,000 times, mapping observation was performed in a rectangular area of ​​[metal wiring thickness] x [length 10 μm in the direction perpendicular to the thickness direction]. The measurement conditions for SEM-EDX are as follows: Measurement equipment: Hitachi High-Technologies Corporation Scanning Electron Microscope SU8220 Measurement conditions: Acceleration voltage 15 kV Quantitative analysis was performed by mapping for copper, carbon, oxygen, tin, and bismuth. The total mass percentage of tin and bismuth determined that the solder content was 7 mass%. The mapping image of tin was binarized using the analysis software ImageJ, and a tin defect with a cross-sectional area of ​​0.001 μm was detected in the metal wiring. 2 ~0.15μm 2 A solder dispersion phase was confirmed. Furthermore, there were some areas where the solder layer and the solder region in the metal wiring were continuous and some areas where they were not. In addition, a spectrum analysis was performed on the metal wiring by selecting it with SEM-EDX, and it was found that the metal wiring contained copper and carbon. The measurement conditions of SEM-EDX were the same as those described in [Evaluation of solder content in metal wiring].

[0101] [Evaluation of holes in metal wiring, and thickness of metal wiring and solder layer] The area of ​​the hole in the cross section of the metal wiring in the thickness direction was measured by SEM image analysis, and the cross-sectional area was 0.01 μm 2 ~0.15μm 2 The presence of holes was confirmed. The SEM observation conditions were as follows. Measurement equipment: Hitachi High-Technologies Corporation Scanning Electron Microscope SU8220 Measurement conditions: Accelerating voltage 5 kV Measurement mode: Backscattered electron observation

[0102] The area of ​​the holes was determined by image analysis using the analysis software ImageJ. The area for image analysis was a rectangle of [metal wiring thickness] × [length 40 μm in the direction perpendicular to the thickness direction] in the cross-sectional direction. Next, the image of the field of view set above was binarized so that the holes could be identified. The threshold value for binarization was set to the default.

[0103] [Adhesion evaluation] The adhesion was evaluated by a tape peeling test in accordance with JIS K 5600. Cellotape (registered trademark) CT-18 (Nichiban Co., Ltd.) was used as the tape, and the test was deemed to pass if the solder layer did not peel off. As a result of the tape peeling test, no peeling of the solder layer was observed, and the adhesion test was passed.

[0104] <Comparative Example 1> Metal wiring was formed, soldered and evaluated in the same manner as in Example 1, except that the scanning speed of the focal position of the laser light was 100 mm / sec, the output was 920 mW, the spot diameter was 250 μm, and the overlap rate was 88.5%.

[0105] [Evaluation of solder content in metal wiring] When evaluated in the same manner as in Example 1, the solder content was found to be 1.8 mass %. In addition, a solder paste having a cross-sectional area of ​​0.001 μm 2 ~0.02μm 2 A solder dispersion phase was confirmed.

[0106] [Evaluation of holes in metal wiring] When evaluated in the same manner as in Example 1, the cross section of the metal wiring had a cross-sectional area of ​​0.01 to 1.9 μm 2 The presence of holes was confirmed.

[0107] [Adhesion evaluation] When evaluated in the same manner as in Example 1, peeling of the solder layer occurred, and the adhesion test was unsuccessful.

[0108] From the results of Example 1 and Comparative Example 1, it was found that when an appropriate amount of solder is contained in the metal wiring as in the Example, the adhesion between the solder layer and the metal wiring is high. [Industrial Applicability]

[0109] According to one aspect of the present invention, a metal wiring having high adhesion between a solder layer and the metal wiring can be provided. The metal wiring obtained by one aspect of the present invention can be suitably used for producing wiring materials for electronic circuit boards, mesh electrodes, electromagnetic shielding materials, and heat dissipation materials. [Explanation of symbols]

[0110] 1 structure 10 Metal wiring manufacturing equipment 11 Base material 12 Coating 13 Metal wiring 14 Insulation Area 15 Single Layer 16 Solder Layer 17 Solder 101 Structure holding part 102 Light Oscillator 103 Gas Supply Section 104 Light beam scanning unit 104a X-axis galvanometer mirror 104b X-axis galvanometer motor 104c Y-axis galvanometer mirror 104d Y-axis galvanometer motor 105 Speed ​​control section 106 Computer L Laser light R1 1st scan line R2 Second scan line S1 Scan line width S2 overlap width

Claims

1. A substrate; A metal wiring disposed on the substrate; a solder layer disposed on the metal trace; A structure having the metal wiring includes copper and solder; A structure, wherein the content of solder in the metal wiring is 2% by mass or more and 30% by mass or less.

2. The cross section of the metal wiring in the thickness direction is 2 More than 1.8 μm 2 13. The structure of claim 1, wherein there is at least one hole having a cross-sectional area less than 1 mm.

3. The cross section of the metal wiring in the thickness direction is 2 3. The structure of claim 1 or 2, wherein no holes have a cross-sectional area greater than or equal to 100 mm.

4. The structure according to any one of claims 1 to 3, wherein the metal wiring further contains carbon.

5. The structure according to any one of claims 1 to 4, which is a wiring material, an antenna for a portable information device housing, a mesh electrode, an electromagnetic wave shielding material, or a heat dissipation material.

6. A method for producing the structure according to any one of claims 1 to 5, comprising the steps of: A coating step of applying a coating liquid containing a metal and / or a metal oxide onto a substrate to obtain a coating film; a firing step of firing the coating film to form metal wiring; and a soldering step of forming a solder layer on the metal wiring.

7. The method for producing a structure according to claim 6 , wherein the firing step comprises irradiating the coating with a laser.

8. The method for producing a structure according to claim 7 , wherein in the firing step, the coating film is irradiated with the laser while a gas is flowing over the coating film.

Citation Information

Patent Citations

  • Printed wiring board

    JP1983170868U

  • Wiring substrate and information memory medium using metallic oxide

    JP1993037126A

  • Circuit board and manufacture thereof

    JP1999261182A

  • Method for forming an electrically conductive copper pattern layer by laser irradiation

    JP2010534932A

  • Manufacturing method of solder adhesive metal paste conductive film

    JP2019121568A