High strength austenitic stainless steel cold rolled annealed steel sheet and its manufacturing method

Optimized austenitic stainless steel with controlled alloying elements and formulae achieves high yield strength and formability, addressing the challenges of conventional materials by minimizing expensive elements and ensuring stability and cost-effectiveness.

JP7579887B2Active Publication Date: 2024-11-08POHANG IRON & STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2022570237
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-23
Filing Date
2021-06-22
Publication Date
2024-11-08
Estimated Expiration
2041-06-22

AI Technical Summary

Technical Problem

Conventional structural steel materials face challenges in achieving high yield strength and formability simultaneously, often requiring expensive alloying elements like nickel, which affects price competitiveness and stability due to fluctuating raw material prices.

Method used

Austenitic stainless steel with optimized alloy composition (C: 0.1-0.2%, N: 0.2-0.3%, Si: 0.8-1.5%, Mn: 7.0-8.5%, Cr: 15.0-17.0%, Ni: ≤0.5%, Cu: ≤1.0%, Nb: ≤0.2%) and specific formulae (14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn, 30≦551-462(C+N)-9.2Si-8.1Mn-13.7Cr-29(Ni+Cu)-68Nb≦80, 16≦1+45C-5Si+0.09Mn+2.2Ni-0.28Cr-0.67Cu+88.6N≦20) to ensure high yield strength and formability while minimizing expensive elements.

Benefits of technology

The solution maintains high yield strength (450 MPa after cold rolling annealing and 1,800 MPa after temper rolling) with excellent formability and price competitiveness by reducing nickel content, ensuring high productivity and preventing cracks during hot rolling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579887000001
    Figure 0007579887000001
  • Figure 0007579887000002
    Figure 0007579887000002
  • Figure 0007579887000003
    Figure 0007579887000003
Patent Text Reader

Abstract

To provide a high-strength austenitic stainless steel with excellent productivity and cost-saving effects, and a method for manufacturing the same. [Solution] The stainless steel of the present invention has excellent hot workability, high productivity, and a significant reduction in the content of the expensive element nickel (Ni), resulting in excellent cost savings. It also has a yield strength of 450 MPa or more and an elongation of 45% or more after cold rolling and annealing, and an ultra-high strength of 1800 MPa or more even after temper rolling.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention , high High strength austenitic stainless steel Cold rolled and annealed steel sheet And the present invention relates to a method for producing the same. [Background technology]

[0002] Structural steel, which constitutes the framework and exterior panels of automobiles and buildings and must protect humans and property from damage caused by external stress and impact, has traditionally required high strength properties to ensure the stability and reliability of the product. In addition, recent market trends in automobiles, buildings, and the like are driving the pursuit of complex and unique exterior shapes, and structural steel materials are required to have high strength properties as well as excellent formability. That is, to meet market demands, structural steels must have excellent formability in the annealed state, be easily deformed into various shapes, and have high strength properties after final processes such as forming and temper rolling.

[0003] However, conventional steel materials, even if they have excellent formability, tend to have poor strength properties after forming, and steel materials with excellent strength properties tend to have poor formability, making it difficult to reflect recent market trends. Even if they do meet these requirements, they often contain large amounts of expensive elements and are therefore not economical. Meanwhile, stainless steel has excellent corrosion resistance and does not require separate capital investment for corrosion resistance, making it suitable for the small-variety mass production required by the recent battery-centered, environmentally friendly automobile market. It is also suitable for use in buildings in environments where corrosion is relatively accelerated, such as seaside and urban areas. In particular, austenitic stainless steel has the advantage of being aesthetically pleasing, as it has excellent elongation and can be molded into complex and unique shapes to meet the diverse needs of customers.

[0004] However, compared to general structural carbon steels, austenitic stainless steels have poorer yield strength and use high amounts of expensive alloy elements, which creates economic problems. Nickel (Ni) in particular has the disadvantage that it is difficult to ensure stable supply prices due to the unstable supply and demand of raw materials caused by serious fluctuations in material prices, and the material itself is expensive, significantly reducing price competitiveness. Therefore, there was a need to develop a structural austenitic stainless steel that could ensure high yield strength in the final product while maintaining high formability, and that was cost-competitive by minimizing the content of expensive alloy elements such as nickel (Ni). Summary of the Invention [Problem to be solved by the invention]

[0005] Books invention Eyes The goal is to develop a high-strength austenitic stainless steel that can ensure high yield strength of 1800 MPa or more in the final product while maintaining high formability. Cold rolled and annealed steel sheet And to provide a method for producing the same. Another object of the present invention is to provide an austenitic stainless steel that can ensure excellent price competitiveness by minimizing the content of expensive alloy elements such as nickel (Ni). Cold rolled and annealed steel sheet And to provide a method for producing the same. The present invention Also Another objective is to develop an austenitic stainless steel that does not crack during hot rolling and has excellent yield and productivity even when expensive alloying elements are reduced. Cold rolled and annealed steel sheet And to provide a method for producing the same. The object of the present invention is not limited to the above object, and a person having ordinary knowledge in the technical field to which the present invention pertains will be able to clearly understand other objects not mentioned from the following description. [Means for solving the problem]

[0006] The high strength austenitic stainless steel of the present invention has been developed to achieve the above object. Cold rolled and annealed steel sheet is characterized in that it contains, by weight percentage, C: 0.1-0.2%, N: 0.2-0.3%, Si: 0.8-1.5%, Mn: 7.0-8.5%, Cr: 15.0-17.0%, Ni: 0.5% or less (0 is excluded), Cu: 1.0% or less (0 is excluded), Nb: 0-0.2%, and the balance being Fe and unavoidable impurities, and satisfies the following formula (1): Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn (In formula (1), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.)

[0007] High-strength austenitic stainless steel Cold rolled and annealed steel sheet is characterized in that it satisfies the following formula (2). Formula (2): 30≦551-462(C+N)-9.2Si-8.1Mn-13.7Cr-29(Ni+Cu)-68Nb≦80 (In formula (2), C, N, Si, Mn, Cr, Ni, Cu, and Nb represent the content (wt%) of each element.) High-strength austenitic stainless steel Cold rolled and annealed steel sheet is characterized in that it satisfies the following formula (3). Formula (3): 16≦1+45C-5Si+0.09Mn+2.2Ni-0.28Cr-0.67Cu+88.6N≦20 (In formula (3), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.) High-strength austenitic stainless steel Cold rolled and annealed steel sheet is characterized in that it satisfies the following formula (4). JPEG0007579887000001.jpg23150 (In formula (4), C, N, Si, Mn, Cr, Ni, Cu and Nb mean the content (wt%) of each element.)

[0008] High-strength austenitic stainless steel Cold rolled and annealed steel sheetIt is preferable that the yield strength after cold rolling and annealing is 450 MPa or more, and the yield strength after temper rolling is 1,800 MPa or more. High-strength austenitic stainless steel Cold rolled and annealed steel sheet The elongation after cold rolling and annealing can be 45% or more, and the elongation after temper rolling can be 3% or more.

[0009] The high-strength austenitic stainless steel of the present invention Cold rolled and annealed steel sheet The manufacturing method of the present invention includes the steps of heating and hot rolling a slab consisting of, by weight%, C: more than 0.1 to 0.2%, N: 0.2 to 0.3%, Si: 0.8 to 1.5%, Mn: 7.0 to 8.5%, Cr: 15.0 to 17.0%, Ni: 0.5% or less (excluding 0), Cu: 1.0% or less (excluding 0), Nb: 0 to 0.2%, and the balance being Fe and unavoidable impurities, hot rolling annealing the hot rolled steel sheet, cold rolling the hot rolled and annealed steel sheet, and cold rolling annealing the cold rolled steel sheet, wherein the slab satisfies the following formula (1): Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn (In formula (1), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.)

[0010] In the above-mentioned manufacturing method, the slab is characterized in that it satisfies the following formula (2). Formula (2): 30≦551-462(C+N)-9.2Si-8.1Mn-13.7Cr-29(Ni+Cu)-68Nb≦80 (In formula (2), C, N, Si, Mn, Cr, Ni, Cu, and Nb represent the content (wt%) of each element.) In the above-mentioned manufacturing method, the slab is characterized in that it satisfies the following formula (3). Formula (3): 16≦1+45C-5Si+0.09Mn+2.2Ni-0.28Cr-0.67Cu+88.6N≦20 (In formula (3), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.) In the above-mentioned manufacturing method, the slab is characterized in that it satisfies the following formula (4). TIFF0007579887000002.tif14152 (In formula (4), C, N, Si, Mn, Cr, Ni, Cu and Nb mean the content (wt%) of each element.) Effect of the Invention

[0011] According to the present invention, the austenitic stainless steel of the present invention Cold rolled and annealed steel sheet satisfies the above alloy composition and content range, and at the same time satisfies formula (1), thereby ensuring high yield strength of 450 MPa or more after cold rolling and annealing, and 1,800 MPa after temper rolling, while maintaining high formability. Furthermore, the content of expensive alloy elements such as nickel (Ni) is reduced to 0.5 wt% or less, resulting in excellent price competitiveness, no cracks caused by hot rolling, and excellent yield and productivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] One aspect of the present invention relates to a high-strength austenitic stainless steel comprising, by weight%, 0.1-0.2% C, 0.2-0.3% N, 0.8-1.5% Si, 7.0-8.5% Mn, 15.0-17.0% Cr, 0.5% or less (excluding 0) Ni, 1.0% or less (excluding 0) Cu, 0-0.2% Nb, and the balance being Fe and unavoidable impurities, and which satisfies the following formula (1): Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn (In the above formula (1), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.)

[0013] Hereinafter, the high strength austenitic stainless steel and its manufacturing method according to the present invention will be described in detail. The drawings introduced below are provided as examples so that the concept of the present invention can be fully conveyed to those skilled in the art. Therefore, the present invention may be embodied in other forms without being limited to the drawings presented below, and the drawings presented below may be exaggerated to clarify the concept of the present invention. In this case, unless otherwise defined, the technical and scientific terms used have the meanings that are commonly understood by those having ordinary skill in the art to which the present invention belongs, and in the following description and the accompanying drawings, descriptions of known functions and configurations that may unnecessarily obscure the gist of the present invention will be omitted. Throughout the specification, when a part is said to "comprise" any element, this does not mean to exclude other elements, but means that it may further include other elements, unless specifically stated to the contrary.

[0014] The high-strength austenitic stainless steel of the present invention is characterized in that it contains, by weight percentage, 0.1-0.2% C, 0.2-0.3% N, 0.8-1.5% Si, 7.0-8.5% Mn, 15.0-17.0% Cr, 0.5% or less (0 is excluded), 1.0% or less Cu (0 is excluded), 0-0.2% Nb, and the balance being Fe and unavoidable impurities, and satisfies the following formula (1): Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn (In formula (1), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.)

[0015] In this way, the austenitic stainless steel according to the present invention satisfies the above-mentioned alloy composition and content ranges, and at the same time satisfies formula (1), thereby ensuring high yield strength of 450 MPa or more after cold rolling and annealing, and 1,800 MPa after temper rolling, while maintaining high formability. The content of expensive alloy elements such as nickel (Ni) is reduced to 0.5 wt.% or less, which has the advantages of being price competitive, not causing cracks due to hot rolling, and excellent yield and productivity. The reasons for limiting the numerical values ​​of the alloy component contents in one embodiment of the present invention will be described below. In the following, unless otherwise specified, the unit is weight percent.

[0016] In the high-strength austenitic stainless steel of the present invention, the carbon (C) content is preferably 0.1 to 0.2%, and more preferably 0.15 to 0.2%. C is an element effective in stabilizing the austenite phase, and is added to ensure the yield strength of austenitic stainless steel. If the C content is low, the sufficient yield strength required in the present invention cannot be ensured, and the lower limit is limited to 0.1%, and more preferably 0.15%. On the other hand, if the C content is excessive, it not only reduces cold workability due to the solid solution strengthening effect, but also induces grain boundary precipitation of chromium carbide during hot working, which leads to a decrease in hot workability, and may adversely affect the softness, toughness, corrosion resistance, etc. of the material, and the upper limit is preferably limited to 0.2%.

[0017] In the high-strength austenitic stainless steel of the present invention, the nitrogen (N) content is preferably 0.2 to 0.3%, and more preferably 0.2 to 0.25%. N is one of the most important elements in the present invention. N is a strong austenite stabilizing element and is an element that is effective in improving the corrosion resistance and yield strength of austenitic stainless steel. If the N content is low, sufficient yield strength required in the present invention cannot be ensured, so the lower limit is limited to 0.2%. On the other hand, if the N content is excessive, defects such as nitrogen pores occur during the production of the slab, and the cold workability is reduced due to the solid solution strengthening effect, so the upper limit is preferably limited to 0.3%, more preferably 0.25%.

[0018] In the high-strength austenitic stainless steel of the present invention, the silicon (Si) content is preferably 0.8 to 1.5%, and more preferably 0.8 to 1.2%. Silicon acts as a deoxidizer during the steelmaking process and is an effective element for improving corrosion resistance. Among substitutional elements, silicon is also an effective element for improving the yield strength of steel, and is added to improve the yield strength of the present invention. If the silicon content is low, sufficient corrosion resistance and yield strength required in the present invention cannot be ensured, so the lower limit is limited to 0.8%. On the other hand, if silicon is added in excess, it not only reduces hot workability by promoting the formation of delta ferrite (δ-ferrite) in the cast slab, but also has a risk of adversely affecting the softness and impact properties of the material, so the upper limit is preferably limited to 1.5%, and more preferably 1.2%.

[0019] In the high-strength austenitic stainless steel of the present invention, the manganese (Mn) content is preferably 7.0 to 8.5%, and more preferably 7 to 8%. Mn is an austenite phase stabilizing element added in place of nickel (Ni) in the present invention, and is preferably added in an amount of 7.0% or more in order to suppress the formation of processing-induced martensite and improve cold rolling properties. However, if the content is excessive, it may form excessive amounts of S-based inclusions (MnS), reduce the softness and toughness of the austenitic stainless steel, and generate Mn fumes during the steelmaking process, which may pose a manufacturing hazard. In addition, since the addition of an excessive amount of Mn rapidly reduces the corrosion resistance of the product, the upper limit should be limited to 8.5%, and more preferably 8%.

[0020] In the high-strength austenitic stainless steel of the present invention, the chromium (Cr) content is preferably 15.0 to 17.0%, and more preferably 15.5 to 16.5%. Cr is a ferrite stabilizing element, but it is effective in suppressing the formation of martensite phase, and is a basic element for ensuring the corrosion resistance required for stainless steel, and can be added at 15% or more. However, if the content is excessive, it forms a large amount of delta ferrite in the slab as a ferrite stabilizing element, which reduces hot workability and has an adverse effect on material properties, so the upper limit should be limited to 17.0%, and more preferably 16.5%.

[0021] In the high-strength austenitic stainless steel of the present invention, the content of nickel (Ni) is preferably more than 0% and 0.5% or less, more preferably 0.01 to 0.3%. Ni is a strong austenite phase stabilizing element and is essential for ensuring good hot workability and cold workability. However, Ni is an expensive element, and adding a large amount of Ni increases the cost of raw materials. Therefore, taking into consideration both the cost and efficiency of the steel material, the upper limit is preferably limited to 0.5%, more preferably 0.3%.

[0022] In the high-strength austenitic stainless steel of the present invention, the copper (Cu) content is preferably more than 0% and not more than 1.0%, and more preferably 0.1 to 1%. Cu is an austenite phase stabilizing element, and is added in place of nickel (Ni) in the present invention. Cu is added as an element to improve corrosion resistance in a reducing environment. However, if the content is excessive, not only does it increase the cost of the material, but it also causes problems of liquefaction and low-temperature brittleness. In addition, the addition of excessive Cu causes problems of segregation at the slab edge and deterioration of hot workability. Therefore, in consideration of the cost-effectiveness and material properties of the steel material, the upper limit is limited to 1.0%.

[0023] The high-strength austenitic stainless steel of the present invention may optionally further contain 0.2% or less of niobium (Nb). Nb has a high affinity with carbon and nitrogen, so it forms precipitates during heat treatment, which contributes to grain refinement of the material and is effective in improving yield strength. However, if there is an excess of Nb as a ferrite stabilizing element, not only does it reduce the hot workability of the material, but it is also an expensive element, so adding it increases the cost of raw materials. For this reason, in consideration of the cost efficiency and material properties of the steel, the upper limit should be limited to 0.2%, and more preferably 0.15%.

[0024] Moreover, the high-strength austenitic stainless steel according to one example of the present invention may further contain one or more of the following unavoidable impurities: P: 0.035% or less and S: 0.01% or less.

[0025] Phosphorus (P) is an impurity that is inevitably contained in steel and is a major cause of grain boundary corrosion and impaired hot workability, so it is preferable to control the P content as low as possible. In the present invention, the upper limit of the P content is controlled to 0.035% or less.

[0026] Sulfur (S) is an impurity that is inevitably contained in steel and is an element that segregates at grain boundaries and is the main cause of impairing hot workability, so it is preferable to control the content as low as possible. In the present invention, the upper limit of the S content is controlled to 0.01% or less.

[0027] The remaining component of the present invention is iron (Fe). However, in normal manufacturing processes, unintended impurities may be inevitably mixed in from raw materials or the surrounding environment, and it is not possible to exclude them. Since these impurities are known to anyone skilled in normal manufacturing processes, not all of the contents are specifically mentioned in this specification.

[0028] Recently, improvement of yield strength of steel is considered as an important issue for weight reduction and stability of steel. In particular, sufficient elongation must be secured after annealing for manufacturing structural materials of various shapes including vehicle structural materials. Also, a very high level of yield strength is required for the final products used as structural materials after temper rolling and forming, so a high level of yield strength is required after temper rolling or forming. In addition, in order to ensure the price competitiveness of austenitic stainless steel, the content of expensive austenite stabilizing elements such as Ni must be reduced, and it is necessary to determine the amounts of Mn, N, and Cu added that can compensate for this. However, when Ni is reduced and Mn, N, and Cu are added in order to ensure price competitiveness, there is a risk that the work hardening will increase rapidly, reducing the elongation of the steel material, or that the hot deformation resistance will decrease, reducing productivity. Therefore, it is necessary to determine the amounts of each added element while taking into consideration the balance between them.

[0029] In order to secure a high-strength austenitic stainless steel that has excellent price competitiveness while reducing the content of expensive alloy elements such as nickel (Ni) to 0.5 weight % or less, does not generate cracks due to hot rolling, has excellent yield and productivity, and can maintain high formability, and has a high yield strength of 450 MPa or more after cold rolling annealing and 1,800 MPa or more after temper rolling, it is preferable to satisfy the above alloy composition and content and at the same time satisfy formula (1). Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn (In formula (1), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.)

[0030] In the present invention, in order to ensure high yield strength of austenitic stainless steel, the following formula (1) was derived in consideration of the improvement of yield strength due to the stress field of the steel material. The higher the value of formula (1), the more the interlattice stress field increases due to the difference in atomic size between alloy elements, and the limit of resistance to plastic deformation against external stress increases. Specifically, when the value of formula (1) is less than 14, there is a problem that it is difficult to ensure the yield strength required in the present invention. However, if the value of formula (1) is too high, the yield strength may be lowered after temper rolling. Preferably, the upper limit of formula (1) is 16.5 or less. Thus, when the value of formula (1) satisfies 14 to 16.5, a high-strength austenitic stainless steel having a high yield strength of 450 MPa or more after cold rolling annealing and 1,800 MPa or more after temper rolling can be ensured.

[0031] Moreover, it is preferable that the high-strength austenitic stainless steel according to one embodiment of the present invention satisfies the following formula (2). Formula (2): 30≦551-462(C+N)-9.2Si-8.1Mn-13.7Cr-29(Ni+Cu)-68Nb≦80 (In formula (2), C, N, Si, Mn, Cr, Ni, Cu, and Nb represent the contents (wt%) of each element.) The above formula (2) was derived in consideration of the phase transformation that occurs due to deformation of austenitic stainless steel, and when the value of formula (2) exceeds 80, the austenitic stainless steel exhibits rapid deformation-induced martensitic transformation behavior in response to deformation, which may cause plastic nonuniformity, resulting in a problem of inferior elongation of the austenitic stainless steel. On the other hand, when the value of formula (2) is less than 30, the austenitic stainless steel is unlikely to exhibit deformation-induced martensitic transformation behavior in response to deformation, and the martensitic phase required to ensure ultra-high strength after temper rolling cannot be secured.

[0032] Moreover, it is preferable that the high-strength austenitic stainless steel according to one embodiment of the present invention satisfies the following formula (3). Formula (3): 16≦1+45C-5Si+0.09Mn+2.2Ni-0.28Cr-0.67Cu+88.6N≦20 (In formula (3), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.) The above formula (3) was derived in consideration of the potential slip behavior of the steel material with respect to the deformation of the austenitic stainless steel. When the value of formula (3) is less than 16, the austenitic stainless steel actively exhibits planar slip behavior with respect to the deformation, and the accumulation of potential due to external stress occurs seriously, resulting in plastic nonuniformity and high work hardening. This causes problems such as poor elongation of the austenitic stainless steel and difficulty in performing temper rolling. In addition, when hot deformation proceeds at high temperatures, hot rolling defects such as edge cracks are likely to occur, resulting in a decrease in productivity. On the other hand, when the value of formula (3) exceeds 20, frequent cross slip occurs, reducing the potential accumulation inside the steel material, and as deformation is applied, potential clusters and potential cells are formed, which reduces the strength of the material. The more temper rolling is performed, the greater the effect of the formation of such potential clusters and potential cells. Therefore, in the case of a steel material characterized by high temper rolling and ultra-high strength as in the present invention, the target strength cannot be ensured. More preferably, the upper limit of formula (3) is equal to or less than 19. When the value of formula (3) exceeds 19, the yield strength and tensile strength of the temper rolled material are close to each other, and there is a risk of the strength characteristics of the austenitic stainless steel decreasing.

[0033] Moreover, it is preferable that the high-strength austenitic stainless steel according to one embodiment of the present invention satisfies the following formula (4). TIFF0007579887000003.tif14152 (In formula (4), C, N, Si, Mn, Cr, Ni, Cu and Nb mean the content (wt%) of each element.) The above formula (4) was derived in consideration of the delta ferrite fraction, which has a large effect on hot workability, and when the value of formula (4) is less than 2, the delta ferrite fraction at high temperatures is significantly reduced, and the material is present in austenite single phase during hot working, and the growth of crystal grain boundaries and segregation of S and P at the grain boundaries occur, resulting in cracks in the material. The cracks thus generated reduce the material yield and reduce productivity. On the other hand, when the value of formula (4) is more than 10, the delta ferrite fraction, which is inferior in workability, becomes very large, and the boundaries of austenite-ferrite phase, which are vulnerable to deformation, increase, resulting in reduced hot workability and reduced productivity. More preferably, the lower limit of formula (4) is 3 or more. When the value of formula (4) is less than 3, the yield strength and tensile strength of the temper rolled material are close to each other, and there is a risk of the strength properties of the austenitic stainless steel being reduced.

[0034] As a result, the high-strength austenitic stainless steel of the present invention satisfies the above-mentioned alloy composition and content ranges, and at the same time satisfies all of formulas (1) to (4), thereby ensuring high yield strength, tensile strength and elongation while maintaining high formability, and ensuring excellent price competitiveness and productivity. Specifically, the high-strength austenitic stainless steel according to one embodiment of the present invention preferably has a yield strength of 450 MPa or more after cold rolling and annealing, and a yield strength of 1,800 MPa or more after temper rolling. In this case, the upper limit of the yield strength after cold rolling and annealing may be, for example, 1,000 MPa or less, and the upper limit of the yield strength after temper rolling may be 2,500 MPa or less, but is not limited thereto. Moreover, the high-strength austenitic stainless steel according to one embodiment of the present invention has an elongation percentage of 45% or more after cold rolling annealing and an elongation percentage of 3% or more after temper rolling. In this case, the upper limit of the elongation percentage after cold rolling annealing may be, for example, 70% or less, and the upper limit of the elongation percentage after temper rolling may be 10%, but is not limited thereto.

[0035] Next, a method for producing the above-mentioned high strength austenitic stainless steel will be described. Conventionally, a method for improving the yield strength of austenitic stainless steel has been to perform final annealing at a low temperature of 1000°C or less. Low-temperature annealing is a method that utilizes the energy stored in the steel during cold rolling without completing recrystallization. However, austenitic stainless steel to which low-temperature annealing is applied has the disadvantages of not only the risk of non-uniformity in the material, but also of insufficient pickling in the subsequent pickling process and an unattractive surface shape. Therefore, the present invention provides a high-ductility, high-strength austenitic stainless steel that has excellent yield strength and a high yield ratio even when cold-rolled and annealed at 1,000° C. or higher.

[0036] Specifically, a method for producing a high-strength austenitic stainless steel according to one embodiment of the present invention includes the steps of heating and hot rolling a slab consisting of, by weight%, C: more than 0.1 to 0.2%, N: 0.2 to 0.3%, Si: 0.8 to 1.5%, Mn: 7.0 to 8.5%, Cr: 15.0 to 17.0%, Ni: 0.5% or less (excluding 0), Cu: 1.0% or less (excluding 0), Nb: 0 to 0.2%, and the balance being Fe and unavoidable impurities, hot-rolling annealing the hot-rolled steel sheet, cold-rolling the hot-rolled and annealed steel sheet, and cold-rolling annealing the cold-rolled steel sheet, and the slab can satisfy the following formula (1). Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn (In the above formula (1), C, N, Si, Mn, Cr, Ni, and Cu represent the content (wt%) of each element.) In this way, the manufacturing method according to the present invention uses a slab that satisfies the above-mentioned alloy composition and content ranges and also satisfies formula (1), thereby making it possible to produce a high-strength austenitic stainless steel having a high yield strength of 1,800 MPa or more in the final product while maintaining high formability. The present invention has the advantage that the content of expensive alloy elements such as nickel (Ni) is reduced to 0.5 wt% or less, which provides excellent price competitiveness, does not cause cracks due to hot rolling, and has excellent yield and productivity.

[0037] A method for producing a high-strength austenitic stainless steel according to an embodiment of the present invention will now be described in more detail. First, a step of heating and hot rolling a slab consisting of, by weight percent, C: more than 0.1 to 0.2%, N: 0.2 to 0.3%, Si: 0.8 to 1.5%, Mn: 7.0 to 8.5%, Cr: 15.0 to 17.0%, Ni: 0.5% or less (excluding 0), Cu: 1.0% or less (excluding 0), Nb: 0 to 0.2%, and the balance being Fe and inevitable impurities, can be performed. In this case, the reasons for limiting the numerical values ​​of the contents of each alloy component and the reason why formula (1) must be satisfied are the same as those explained above, so a duplicated explanation will be omitted. As explained above, the slab according to one example of the present invention can satisfy formulas (2), (3), and (4), and the reasons why these must be satisfied are the same as those explained above, so a duplicated explanation will be omitted. In this case, the temperature conditions for heating the slab may be at the normal rolling temperature level, and for example, the slab can be heated at a temperature of 1,100 to 1,300° C. for 1 to 3 hours, and then hot-rolled.

[0038] Next, the hot-rolled steel sheet is subjected to hot-roll annealing, which can also be performed by a conventional method, for example, the hot-rolled steel sheet is subjected to hot-roll annealing at a temperature range of 1000 to 1150° C. for 10 seconds to 10 minutes. Thereafter, the hot-rolled and annealed steel sheet is cold-rolled to produce a thin steel sheet. In this case, a cooling step may be performed before the rolling process, and the cooling is performed by water quenching. The cold rolling may be performed at a normal level, for example, at a rolling reduction of 50% or more, but is not necessarily limited thereto.

[0039] Next, the cold rolled steel sheet is subjected to cold rolling annealing. Specifically, the cold rolling annealing is performed at a temperature of 1000°C or more for 10 seconds to 10 minutes. In a conventional method for improving the yield strength of austenitic stainless steel, low-temperature annealing at 1000°C or less results in uneven material properties or unpickled steel in the subsequent pickling process, resulting in an unattractive surface shape. However, in the present invention, even when cold rolling annealing is performed at a temperature of 1000°C or more, an austenitic stainless steel having a yield strength of 450 MPa or more and an elongation of 45% or more can be obtained. By controlling the alloy components in this way and proceeding with a process that places no burden on production and distribution, it is possible to ensure high strength under general cold rolling annealing conditions rather than low-temperature annealing, thereby further improving price competitiveness. Furthermore, the method for producing a high-strength austenitic stainless steel according to an embodiment of the present invention may further include a step of temper rolling the cold-rolled and annealed steel sheet, and a higher level of high strength properties may be ensured through temper rolling.

[0040] Conventional skin pass rolling utilizes the phenomenon that high work hardening occurs as the austenite phase transforms into work-induced martensite during cold deformation, or utilizes the potential accumulation of the steel material, and excellent strength can be obtained when phase transformation and potential accumulation are appropriately utilized. Meanwhile, in the case of the austenitic stainless steel satisfying the above-mentioned alloy components and relational expressions of the present invention, the yield strength after skin pass rolling becomes 1800 MPa or more by appropriately controlling the phase transformation and potential behavior. At this time, the skin pass rolling is performed at a reduction ratio of 60 to 85%, but is not limited thereto. The high strength austenitic stainless steel according to the present invention can be used, for example, for general forming products, and can be manufactured and used in products such as slabs, blooms, billets, coils, strips, plates, sheets, bars, rods, wires, shape steels, pipes, or tubes.

[0041] Hereinafter, the high strength austenitic stainless steel and its manufacturing method according to the present invention will be described in more detail with reference to the following examples. However, the following examples are merely a reference for describing the present invention in detail, and the present invention is not limited thereto, and may be embodied in various forms. In addition, unless otherwise defined, all technical and scientific terms have the same meaning as commonly understood by those skilled in the art to which the present invention belongs. The terms used in the description in this application are merely for the purpose of effectively describing specific examples and are not intended to limit the present invention. In addition, the unit of additives not specifically described in the specification is weight %.

[0042] [Examples 1 to 3 and Comparative Examples 1 to 19] The alloy compositions (wt %) and the values ​​of formulas (1) to (4) for each of the experimental steels used in Examples 1 to 3 and Comparative Examples 1 to 19 are shown in Table 1 below. Slabs were manufactured by melting ingots with the alloy compositions shown in Table 1 below, and were heated at 1,250°C for 2 hours, followed by hot rolling, and then hot rolling annealing at 1,100°C for 90 seconds. Thereafter, cold rolling was performed at a rolling reduction of 70%, and cold rolling annealing was performed at 1,100°C for 10 seconds to obtain cold rolled and annealed materials. The test pieces that had been subjected to the above-mentioned cold rolling and annealing were subjected to temper rolling at a rolling reduction of 70% to obtain temper rolled materials.

[0043] [Table 1]

[0044] [Physical property evaluation] The physical properties of the test pieces manufactured in Examples 1 to 3 and Comparative Examples 1 to 19 were measured. Specifically, the room temperature tensile test was performed according to the ASTM standard, and the yield strength (YS, Yield Strength, MPa), tensile strength (TS, Tensile Strength, MPa), and elongation (EL, Elongation, %) measured thereby, as well as the occurrence of cracks during hot rolling of the cold rolled annealed material, are shown in Table 2 below.

[0045] [Table 2]

[0046] Referring to Table 2, in the case of Examples 1 to 3, the alloy compositions proposed by the present invention satisfy the specified numerical ranges for the values ​​of formulas (1), (2), (3) and (4), thereby achieving a yield strength of 450 MPa or more and an elongation of 45% or more after cold rolling and annealing. With such high yield strength and elongation, it was confirmed that the austenitic stainless steel of the present invention can be used as a structural material for complex shapes and has high utility value. In addition, in Examples 1 to 3, the temper rolled materials obtained by temper rolling the cold-rolled annealed test pieces at a rolling reduction of 70% exhibited high strength properties of 1800 MPa or more. Such high yield strength after deformation means that the stability of the final product, the structural steel material, can be further improved. In addition, in Examples 1 to 3, sufficient hot workability is ensured, and cracks due to hot rolling are not generated, thereby improving yield and productivity. In addition, since the nickel (Ni) content is significantly low, costs can be reduced, and excellent price competitiveness can be ensured.

[0047] On the other hand, Comparative Examples 1 and 2 are commercially produced standard austenitic stainless steels, and are steel types that do not satisfy the range of component contents specified by the present invention. Comparative Examples 1 and 2 do not satisfy formula (1), exhibit low yield strengths of 300 MPa or less, and have values ​​of formula (2) that are lower than the specified range of the present invention, resulting in a problem that the yield strength after temper rolling is somewhat low. In addition, the commercial austenitic stainless steels have a problem of poor price competitiveness due to the addition of excessive nickel (Ni). Comparative Example 3 also does not satisfy formula (1), exhibiting a low yield strength of about 400 MPa, and also has the problem of being poor in price competitiveness due to the excessive addition of nickel (Ni).

[0048] In Comparative Example 4, the value of formula (3) is lower than the range specified by the present invention, and there is a problem that the plastic non-uniformity occurs severely during deformation, resulting in poor elongation. In addition, although formula (4) is satisfied and the amount of delta ferrite is appropriate during hot working, there is a problem that cracks are observed during hot working due to the low value of formula (3) and the high carbon (C) content, resulting in poor productivity. In Comparative Example 5, the value of formula (2) is high, and excessive martensite phase is formed during deformation, resulting in poor elongation. In Comparative Example 6, the value of formula (3) is low, and severe plastic non-uniformity is generated during deformation, resulting in poor elongation. Comparative Examples 7 to 9 had high values ​​of formula (1) and showed excellent yield strength after cold rolling and annealing, but the values ​​of formula (2) were much lower than 30 and the values ​​of formula (3) were much higher than 20, so there was a problem that a high level of yield strength of 1800 MPa or more could not be ensured after temper rolling. Furthermore, Comparative Examples 7 to 9 had low values ​​of formula (4) and high carbon (C) contents, so there was a problem that the hot workability was poor and a large number of cracks were generated by hot rolling.

[0049] In Comparative Examples 10 and 11, the values ​​of formula (1) are low, so there is a problem that it is difficult to ensure sufficient yield strength after annealing. The values ​​of formula (2) are much higher than 80, and the values ​​of formula (3) are much lower than 16, so there is a problem that the elongation of the cold-rolled annealed material is inferior. In Comparative Example 12, the manganese (Mn) content was excessive, and an excessive amount of S-based inclusions (MnS) was formed, which not only reduced the softness and toughness properties, but also generated Mn fumes during the steelmaking process, which was dangerous in production. In Comparative Example 13, the nickel (Ni) content was added at 1.1 wt %, and thus both the strength and elongation were excellent, but there was a problem in that the cost reduction effect was somewhat reduced.

[0050] In Comparative Example 14, the copper (Cu) content is excessive, which causes a large amount of delta ferrite to be formed in the slab, resulting in a decrease in hot workability and an adverse effect on material properties. As a result, cracks are observed during hot working, resulting in poor productivity. In Comparative Example 15, the value of formula (1) is slightly higher than the specific range of the present invention, in Comparative Example 16, the value of formula (2) is lower than the specific range of the present invention, and in Comparative Example 17, the value of formula (3) is higher than the specific range of the present invention, so there is a problem in that a high level of yield strength of 1800 MPa or more cannot be ensured after temper rolling. In Comparative Example 18, the value of formula (4) is lower than the specific range of the present invention, so that there is a problem that the hot workability is poor and a large amount of cracks are generated by hot rolling. In Comparative Example 19, the value of formula (4) exceeds the specific range of the present invention, so that there is a problem that the hot workability is poor due to an excessive amount of delta ferrite (δ-ferrite).

[0051] The present invention has been described above based on the specific matters and limited examples, but this is provided to assist in a more general understanding of the present invention. The present invention is not limited to the above examples, and various modifications and variations are possible from such descriptions by those having ordinary knowledge in the field to which the present invention pertains. Therefore, the concept of the present invention should not be limited to the described embodiments, and all modifications equivalent to or equivalent to the scope of the claims, as well as the claims set forth below, fall within the scope of the concept of the present invention. [Industrial Applicability]

[0052] The present invention can be used in a variety of industrial fields, such as the automotive and construction fields.

Claims

1. In mass%, C: 0.1 to 0.2%, N: 0.2 to 0.3%, Si: 0.8 to 1.5%, Mn: 7.0 to 8.5%, Cr: 15.0 to 17.0%, Ni: 0.5% or less (0 is excluded), Cu: 1.0% or less (0 is excluded), Nb: 0 to 0.2%, and the balance being Fe and unavoidable impurities, A high-strength austenitic stainless cold-rolled annealed steel sheet characterized by satisfying the following formulas (1) to (4): Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn≦15.16 Formula (2): 30≦551-462(C+N)-9.2Si-8.1Mn-13.7Cr-29(Ni+Cu)-68Nb≦80 Formula (3): 16≦1+45C-5Si+0.09Mn+2.2Ni-0.28Cr-0.67Cu+88.6N≦20 (In the formulas (1) to (4), C, N, Si, Mn, Cr, Ni, Cu, and Nb mean the content (mass%) of each element.)

2. The high-strength austenitic stainless cold-rolled annealed steel sheet according to claim 1, characterized in that the high-strength austenitic stainless cold-rolled annealed steel sheet has a yield strength of 450 MPa or more after cold-rolling annealing at a temperature of 1000°C or more for 10 seconds to 10 minutes, and has a yield strength of 1,800 MPa or more after temper rolling at a reduction ratio of 60 to 85%.

3. The high-strength austenitic stainless cold-rolled annealed steel sheet according to claim 1, characterized in that the high-strength austenitic stainless cold-rolled annealed steel sheet has an elongation of 45% or more after cold-rolling annealing at a temperature of 1000°C or more for 10 seconds to 10 minutes, and an elongation of 3% or more after temper rolling at a reduction ratio of 60 to 85%.

4. A method for producing the high strength austenitic stainless cold rolled annealed steel sheet according to any one of claims 1 to 3, A step of heating and hot rolling a slab consisting of, in mass%, C: more than 0.1 to 0.2%, N: 0.2 to 0.3%, Si: 0.8 to 1.5%, Mn: 7.0 to 8.5%, Cr: 15.0 to 17.0%, Ni: 0.5% or less (excluding 0), Cu: 1.0% or less (excluding 0), Nb: 0 to 0.2%, and the balance being Fe and unavoidable impurities; hot-rolling annealing the hot-rolled steel sheet; cold rolling the hot-rolled and annealed steel sheet; cold rolling annealing the cold rolled steel sheet; and subjecting the cold-rolled and annealed steel sheet to temper rolling. The method for producing a high-strength austenitic stainless cold-rolled annealed steel sheet is characterized in that the slab satisfies the following formulas (1) to (4): Formula (1): 14≦23(C+N)+1.3Si+0.24(Cr+Ni+Cu)+0.1Mn≦15.16 Formula (2): 30≦551-462(C+N)-9.2Si-8.1Mn-13.7Cr-29(Ni+Cu)-68Nb≦80 Formula (3): 16≦1+45C-5Si+0.09Mn+2.2Ni-0.28Cr-0.67Cu+88.6N≦20 (In the formulas (1) to (4), C, N, Si, Mn, Cr, Ni, Cu, and Nb mean the content (mass%) of each element.)

5. 5. The method of claim 4, wherein the hot-rolled annealing step comprises hot-rolling annealing the hot-rolled steel sheet at a temperature range of 1,000 to 1,150° C. for 10 seconds to 10 minutes.

6. 5. The method of claim 4, wherein the cold rolling is performed at a temperature of 1000° C. or more for 10 seconds to 10 minutes.

7. The method for producing a high strength austenitic stainless cold rolled annealed steel sheet according to claim 4, wherein the temper rolling is performed at a rolling reduction of 60 to 85%.

Citation Information

Patent Citations

  • Two-phase stainless steel wire for heat-resistant bolt, and heat-resistant bolt component using said two-phase stainless steel wire

    JP2018119174A