Exhaust gas purification catalysts and hydrocarbon adsorbents

Aluminophosphate molecular sieves with 12-membered rings and controlled crystallite diameters are used to address the HC purification performance decline in exhaust gas catalysts after hydrothermal endurance, ensuring effective HC removal at cold starts by mitigating silicon migration issues.

JP7580012B1Active Publication Date: 2024-11-08CATALER CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024546998
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-07-11
Filing Date
2024-05-22
Publication Date
2024-11-08
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Existing exhaust gas purification catalysts experience a significant reduction in hydrocarbon (HC) purification performance at cold starts after hydrothermal endurance due to the migration of silicon from zeolite, which affects the precious metals used as catalysts.

Method used

The use of aluminophosphate molecular sieves with 12-membered rings and crystallite diameters between 360 Å to 700 Å, which do not substantially contain silicon, as the HC adsorbent in the catalyst layer, to enhance HC purification performance after hydrothermal durability.

Benefits of technology

The aluminophosphate molecular sieves significantly improve HC purification performance at cold starts by minimizing the adverse effects of silicon migration, maintaining high efficiency even after exposure to high-temperature exhaust gas for extended periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580012000002
    Figure 0007580012000002
  • Figure 0007580012000003
    Figure 0007580012000003
  • Figure 0007580012000004
    Figure 0007580012000004
Patent Text Reader

Abstract

The present invention provides an exhaust gas purification catalyst having high HC purification performance during cold start after hydrothermal durability. The exhaust gas purification catalyst disclosed herein includes a substrate and an exhaust gas purification layer provided on the substrate. The exhaust gas purification layer contains a catalytic metal and a molecular sieve that is substantially free of Si as a hydrocarbon adsorbent. The molecular sieve that is substantially free of Si is an aluminophosphate molecular sieve having a 12-membered ring. The crystallite diameter of the aluminophosphate molecular sieve determined by X-ray diffraction measurement is 360 Å to 700 Å.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for exhaust gas purification. The present invention also relates to a hydrocarbon adsorbent suitable for a catalyst for exhaust gas purification. This application claims priority based on Japanese Patent Application No. 2023-113569 filed on July 11, 2023, the entire contents of which are incorporated herein by reference. [Background technology]

[0002] Exhaust gas emitted from internal combustion engines such as automobile engines contains harmful components such as hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NOx). In order to efficiently react and remove these harmful components from exhaust gas, exhaust gas purification catalysts have been used. A typical structure of an exhaust gas purification catalyst is one in which a catalyst layer containing catalytic metals such as Pt (platinum), Pd (palladium), and Rh (rhodium) is formed on a highly heat-resistant substrate such as ceramics.

[0003] In a state where the exhaust gas purification catalyst is not sufficiently heated immediately after starting the engine (so-called cold start), the temperature of the exhaust gas purification catalyst is low, so it is difficult to obtain sufficient catalytic activity for treating hydrocarbons (HC). For this reason, HC adsorption type exhaust gas purification catalysts have been developed in which a catalyst layer containing a catalytic metal is laminated on an HC adsorption layer containing an HC adsorbent (see, for example, Patent Documents 1 to 4). As described in Patent Documents 1 to 4, molecular sieves such as zeolite are known as HC adsorbents. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-256114 [Patent Document 2] JP 2009-167973 A [Patent Document 3] JP 2004-116331 A [Patent Document 4] Special Publication No. 2020-510519 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, with further tightening of exhaust gas regulations, catalysts for purifying exhaust gas are required to have higher performance in removing harmful components contained in exhaust gas. For example, higher exhaust gas purification performance during cold start is required. As a result of intensive studies by the present inventors, it was found that the above-mentioned conventional catalysts for purifying exhaust gas have a problem in that the HC purification performance during cold start is significantly reduced after being exposed to high-temperature exhaust gas containing water for a long period of time (hereinafter, this is referred to as "after hydrothermal durability").

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an exhaust gas purification catalyst that has high HC purification performance at the time of cold start after hydrothermal durability. [Means for solving the problem]

[0007] As a result of intensive research by the present inventors, it was found that the reason why the purification performance of the above-mentioned conventional exhaust gas purification catalyst using zeolite is significantly reduced after hydrothermal durability is that the Si contained in the zeolite (aluminosilicate salt) moves during hydrothermal durability and adversely affects the precious metal, which is the catalytic metal. And, it was found that by using a molecular sieve that does not substantially contain Si at a predetermined ratio or more as the HC adsorbent, the HC purification performance of the exhaust gas purification catalyst at cold start after hydrothermal durability is rapidly increased. As a result of further intensive research by the present inventors, it was found that, among the molecular sieves that do not substantially contain Si, the use of an aluminophosphate molecular sieve having a 12-membered ring and a crystallite diameter of 360 Å to 700 Å significantly increases the HC purification performance of the exhaust gas purification catalyst at cold start after hydrothermal durability.

[0008] That is, the catalyst for exhaust gas purification [1] disclosed herein comprises a substrate and an exhaust gas purification layer provided on the substrate. The exhaust gas purification layer contains a catalytic metal and a molecular sieve that is substantially free of Si as a hydrocarbon adsorbent. The molecular sieve that is substantially free of Si is an aluminophosphate molecular sieve having a 12-membered ring. The crystallite diameter of the aluminophosphate molecular sieve, as determined by X-ray diffraction measurement, is 360 Å to 700 Å. With this configuration, it is possible to provide a catalyst for exhaust gas purification that has high HC purification performance during cold start after hydrothermal durability.

[0009] The exhaust gas purifying catalyst [2] disclosed herein is the above exhaust gas purifying catalyst [1], wherein the aluminophosphate molecular sieve has a crystallite diameter of 360 Å to 400 Å. According to such a configuration, the exhaust gas purifying catalyst has excellent production efficiency.

[0010] The exhaust gas purification catalyst [3] disclosed herein is the above-mentioned exhaust gas purification catalyst [1], in which the crystallite diameter of the aluminophosphate molecular sieve is 450 Å to 600 Å. With such a configuration, the exhaust gas purification catalyst has an excellent balance between production efficiency and HC adsorption capacity.

[0011] The catalyst for exhaust gas purification [4] disclosed herein is any one of the catalysts for exhaust gas purification [1] to [3], in which the framework structure of the aluminophosphate molecular sieve is an AFI type. Such a configuration is advantageous in terms of the HC purification performance of the catalyst for exhaust gas purification.

[0012] The catalyst for exhaust gas purification [5] disclosed herein is any one of the catalysts for exhaust gas purification [1] to [4], in which the exhaust gas purification layer has an HC adsorption layer containing the molecular sieve substantially free of Si, and a catalyst layer containing the catalytic metal. Such a configuration is advantageous in terms of the HC purification performance of the catalyst for exhaust gas purification.

[0013] The exhaust gas purifying catalyst body [6] disclosed herein is the above-mentioned exhaust gas purifying catalyst [5], in which the HC adsorption layer and the catalyst layer are laminated, and the HC adsorption layer is located closer to the substrate than the catalyst layer. This configuration is particularly advantageous in terms of the above-mentioned HC purification performance of the exhaust gas purifying catalyst.

[0014] The exhaust gas purification catalyst body [7] disclosed herein is the above-mentioned exhaust gas purification catalyst [6], in which a first partial catalyst layer and a second partial catalyst layer are laminated in the catalyst layer. The first partial catalyst layer is located closer to the substrate than the second partial catalyst layer. The first partial catalyst layer and the second partial catalyst layer each contain the catalytic metal. The first partial catalyst layer contains an oxidation catalyst as the catalytic metal. The second partial catalyst layer contains a reduction catalyst as the catalytic metal. This configuration is extremely advantageous in terms of the above-mentioned HC purification performance of the exhaust gas purification catalyst.

[0015] From another aspect, the hydrocarbon adsorbent [8] disclosed herein includes an aluminophosphate molecular sieve. The aluminophosphate molecular sieve has a 12-membered ring. The aluminophosphate molecular sieve has a crystallite diameter of 360 Å to 700 Å as determined by X-ray diffraction measurement. With this configuration, the HC adsorption amount of the hydrocarbon adsorbent is high even after hydrothermal durability. Therefore, when an exhaust gas purification catalyst is configured using the hydrocarbon adsorbent disclosed herein, the HC purification performance at cold start after hydrothermal durability is high. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic diagram showing an exhaust gas purification system according to a first embodiment. [Diagram 2] FIG. 2 is a perspective view that typically illustrates the exhaust gas purifying catalyst of FIG. [Diagram 3] 2 is a partial cross-sectional view of the exhaust gas purifying catalyst of FIG. 1 cut in the cylinder axis direction. [Figure 4] FIG. 4(A) is a schematic diagram of an AFI type skeletal structure, and FIG. 4(B) is a conceptual schematic diagram of the AFI type skeletal structure at a grain boundary. [Diagram 5] FIG. 5(A) is a schematic diagram showing one primary particle of an ALPO molecular sieve having a large crystallite size, and FIG. 5(B) is a schematic diagram showing one crystallite in the primary particle. [Figure 6] FIG. 6(A) is a schematic diagram showing one primary particle of an ALPO molecular sieve having a small crystallite size, and FIG. 6(B) is a schematic diagram showing four crystallites in the primary particle. [Figure 7] 2 is a partial cross-sectional view showing the configuration of a modified example of the exhaust gas purifying catalyst of FIG. 1. [Figure 8] FIG. 5 is a partial cross-sectional view of an exhaust gas purifying catalyst according to a second embodiment, cut in the cylinder axis direction. [Figure 9] FIG. 11 is a partial cross-sectional view of an exhaust gas purifying catalyst according to a third embodiment, cut in the cylinder axis direction. [Figure 10] 2 is a graph showing the decane adsorption amount (mg / g) of the ALPO molecular sieves of each Example and each Comparative Example after hydrothermal durability. [Figure 11] 1 is a graph showing the HC50% purification temperature (° C.) of exhaust gas purification catalysts of each Example and each Comparative Example after hydrothermal durability. [Figure 12] 4 is a graph showing HC emissions (mg / km) in the cold range in vehicle tests of the exhaust gas purification catalysts of each of the Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [First embodiment] Hereinafter, a preferred embodiment of the present invention will be described with reference to the drawings. Matters other than those specifically mentioned in this specification and necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, the same reference numerals are used for members and parts that perform the same function, and duplicated explanations may be omitted or simplified. The dimensional relationships (length, width, thickness, etc.) in each drawing do not necessarily reflect the actual dimensional relationships. In addition, the expression "A to B" (A and B are arbitrary numbers) indicating a range in this specification includes the meaning of A or more and B or less, as well as "preferably larger than A" and "preferably smaller than B".

[0018] <Exhaust gas purification system> FIG. 1 is a schematic diagram of an exhaust gas purification system 1. The exhaust gas purification system 1 includes an internal combustion engine 2, an exhaust gas purification device 3, and an engine control unit (Engine Control Unit: ECU) 7. The exhaust gas purification system 1 is configured to purify harmful components, such as HC, CO, and NOx, contained in exhaust gas discharged from the internal combustion engine 2, using the exhaust gas purification device 3. Note that the arrows in FIG. 1 indicate the flow direction of exhaust gas. In the following description, the side closer to the internal combustion engine 2 along the flow of exhaust gas is referred to as the upstream side, and the side farther from the internal combustion engine 2 is referred to as the downstream side.

[0019] Here, the internal combustion engine 2 is mainly configured as a gasoline engine of a gasoline vehicle. However, the internal combustion engine 2 may be an engine other than gasoline, such as a diesel engine or an engine mounted on a hybrid vehicle. The internal combustion engine 2 has a combustion chamber (not shown). The combustion chamber is connected to a fuel tank (not shown). Gasoline is stored in the fuel tank here. However, the fuel stored in the fuel tank may be diesel fuel (light oil) or the like. In the combustion chamber, the fuel supplied from the fuel tank is mixed with oxygen and burned. This converts the combustion energy into mechanical energy. The combustion chamber is communicated with an exhaust port 2a. The exhaust port 2a is communicated with an exhaust gas purification device 3. The burned fuel gas becomes exhaust gas and is discharged to the exhaust gas purification device 3.

[0020] The exhaust gas purification device 3 includes an exhaust path 4 communicating with the internal combustion engine 2, a pressure sensor 8, a first catalyst 9, and a second catalyst 10. The exhaust path 4 is an exhaust gas flow path through which exhaust gas flows. The exhaust path 4 includes an exhaust manifold 5 and an exhaust pipe 6. An upstream end of the exhaust manifold 5 is connected to an exhaust port 2a of the internal combustion engine 2. A downstream end of the exhaust manifold 5 is connected to the exhaust pipe 6. In the middle of the exhaust pipe 6, the first catalyst 9 and the second catalyst 10 are arranged in this order from the upstream side. However, the arrangement of the first catalyst 9 and the second catalyst 10 may be arbitrarily variable. In addition, the number of the first catalyst 9 and the second catalyst 10 is not particularly limited, and a plurality of each may be provided. In addition, a third catalyst may be further arranged downstream of the second catalyst 10.

[0021] The first catalyst 9 may be the same as the conventional one, and is not particularly limited. The first catalyst 9 may be, for example, a diesel particulate filter (DPF) that removes PM contained in exhaust gas; a diesel oxidation catalyst (DOC) that purifies HC and CO contained in exhaust gas; a three-way catalyst that simultaneously purifies HC, CO, and NOx contained in exhaust gas; a NOx storage-reduction (NSR) catalyst that stores NOx during normal operation (under lean conditions) and purifies NOx using HC and CO as reducing agents when a large amount of fuel is injected (under rich conditions); etc. The first catalyst 9 may have, for example, a function of increasing the temperature of exhaust gas flowing into the second catalyst 10. Note that the first catalyst 9 is not an essential component, and may be omitted in other embodiments.

[0022] The second catalyst 10 has a function of purifying harmful components (e.g., HC) in exhaust gas. The second catalyst 10 is a three-way catalyst here. The second catalyst 10 is an example of a catalyst for purifying exhaust gas disclosed herein. In the following, the second catalyst 10 may be referred to as the "catalyst for purifying exhaust gas." The configuration of the second catalyst (catalyst for purifying exhaust gas) 10 will be described in detail later.

[0023] The ECU 7 controls the internal combustion engine 2 and the exhaust gas purification device 3. The ECU 7 is electrically connected to the internal combustion engine 2 and sensors (e.g., pressure sensor 8, temperature sensor, oxygen sensor, etc.) installed at various locations of the exhaust gas purification device 3. The configuration of the ECU 7 may be the same as that of a conventional device, and is not particularly limited. The ECU 7 is, for example, a processor or an integrated circuit. The ECU 7 has an input port (not shown) and an output port (not shown). The ECU 7 receives information, for example, on the operating state of the vehicle, and the amount, temperature, and pressure of exhaust gas discharged from the internal combustion engine 2. The ECU 7 receives information detected by a sensor (e.g., pressure measured by the pressure sensor 8) via the input port. The ECU 7 transmits a control signal via the output port based on, for example, the received information. The ECU 7 controls the operation of the internal combustion engine 2, for example, fuel injection control, ignition control, intake air amount adjustment control, etc. The ECU 7 controls the driving and stopping of the exhaust gas purification device 3 based on, for example, the operating state of the internal combustion engine 2, the amount of exhaust gas discharged from the internal combustion engine 2, and the like.

[0024] <Exhaust gas purification catalyst> FIG. 2 is a perspective view showing the catalyst 10 for purifying exhaust gas. The arrows in FIG. 2 indicate the flow of exhaust gas. In FIG. 2, the upstream side of the exhaust path 4 relatively close to the internal combustion engine 2 is shown on the left side, and the downstream side of the exhaust path relatively far from the internal combustion engine 2 is shown on the right side. Also, in FIG. 2, the symbol X indicates the cylinder axis direction of the catalyst 10 for purifying exhaust gas. The catalyst 10 for purifying exhaust gas is installed in the exhaust path 4 so that the cylinder axis direction X is along the flow direction of the exhaust gas. The cylinder axis direction X is the flow direction of the exhaust gas. Hereinafter, one direction X1 of the cylinder axis direction X may be referred to as the upstream side (also referred to as the exhaust gas inflow side or front side), and the other direction X2 may be referred to as the downstream side (also referred to as the exhaust gas outflow side or rear side). However, these are merely directions for convenience of explanation, and do not limit the installation form of the catalyst 10 for purifying exhaust gas in any way.

[0025] As illustrated in Fig. 3, the exhaust gas purifying catalyst 10 includes a substrate 11 having a straight flow structure and an exhaust gas purifying layer 40. An end of the exhaust gas purifying catalyst 10 in one direction X1 is an exhaust gas inlet 10a, and an end of the exhaust gas purifying catalyst 10 in the other direction X2 is an exhaust gas outlet 10b. The outer shape of the exhaust gas purifying catalyst 10 here is cylindrical. However, the outer shape of the exhaust gas purifying catalyst 10 is not particularly limited, and may be, for example, an elliptical cylindrical shape, a polygonal cylindrical shape, a pipe shape, a foam shape, a pellet shape, a fiber shape, or the like.

[0026] The substrate 11 constitutes the framework of the exhaust gas purification catalyst 10. The substrate 11 is not particularly limited, and various materials and shapes used in the conventional use of this type can be used. The substrate 11 may be, for example, a ceramic carrier made of ceramics such as cordierite, aluminum titanate, and silicon carbide, or a metal carrier made of stainless steel (SUS), Fe-Cr-Al alloy, Ni-Cr-Al alloy, and the like. As shown in FIG. 2, the substrate 11 has a honeycomb structure. The substrate 11 includes a plurality of cells (cavities) 12 regularly arranged in the cylindrical axis direction X, and partition walls (ribs) 14 separating the plurality of cells 12. Although not particularly limited, the volume of the substrate 11 (apparent volume including the volume of the cells 12) may be approximately 0.1 to 10 L, for example, 0.5 to 5 L. The average length (total length) L of the substrate 11 along the cylindrical axis direction X may be approximately 10 to 500 mm, for example, 50 to 300 mm.

[0027] The cells 12 are flow paths for exhaust gas. The cells 12 extend in the cylinder axis direction X. The cells 12 are through-holes that penetrate the substrate 11 in the cylinder axis direction X. The shape, size, number, etc. of the cells 12 may be designed, for example, in consideration of the flow rate and components of the exhaust gas flowing through the exhaust gas purification catalyst 10. The shape of the cross section of the cells 12 perpendicular to the cylinder axis direction X is not particularly limited. The cross-sectional shape of the cells 12 may be, for example, a quadrangle such as a square, parallelogram, rectangle, or trapezoid, or other polygonal shape (for example, a triangle, hexagon, or octagon), a corrugated shape, a circle, or any other geometric shape. The partition walls 14 face the cells 12 and separate the adjacent cells 12. Although not particularly limited, the average thickness of the partition walls 14 (the dimension in the direction perpendicular to the surface; the same applies below) may be approximately 0.1 to 10 mils (1 mil is approximately 25.4 μm), for example 0.2 to 5 mils, from the viewpoint of improving mechanical strength and reducing pressure loss. The partition walls 14 may be porous so that exhaust gas can pass through.

[0028] Fig. 3 is a partial cross-sectional view that shows a schematic view of a part of a cross section of the exhaust gas purification catalyst 10 cut along the cylinder axis direction X. As shown in Fig. 3, an exhaust gas purification layer 40 is provided on the substrate 11, and the exhaust gas purification layer 40 includes a hydrocarbon (HC) adsorption layer 20 and a catalyst layer 30. Thus, the HC adsorption layer 20 and the catalyst layer 30 are laminated on the substrate 11. In this manner, the exhaust gas purification layer 40 is composed of layers involved in purifying exhaust gas.

[0029] The HC adsorption layer 20 is disposed closer to the substrate 11 (i.e., on the lower layer side) than the catalyst layer 30. With this arrangement, when HCs adsorbed in the HC adsorption layer 20 are desorbed from the HC adsorption layer 20, the HCs can be efficiently removed by the catalyst layer 30.

[0030] The exhaust gas purification layer 40 contains a catalytic metal and a molecular sieve that is a hydrocarbon (HC) adsorbent and does not substantially contain Si. In this embodiment, the HC adsorption layer 20 of the exhaust gas purification layer 40 contains a molecular sieve that is a hydrocarbon (HC) adsorbent and does not substantially contain Si, and the catalytic layer 30 contains a catalytic metal.

[0031] In this specification, "the molecular sieve does not substantially contain Si" means that the ratio of Si atoms to all atoms constituting the molecular sieve is 6 atomic % or less (preferably 3 atomic % or less, more preferably 1 atomic % or less, and even more preferably 0 atomic %). Therefore, for example, it is acceptable for the molecular sieve to contain Si due to migration of Si, unavoidable impurities, etc. The ratio of Si atoms to all atoms constituting the molecular sieve can be determined by X-ray fluorescence analysis (XRF).

[0032] In this embodiment, an aluminophosphate (ALPO) molecular sieve having a 12-membered ring is used as the molecular sieve that does not substantially contain Si. The ALPO molecular sieve may be an aluminophosphate (AlPO4) having the same, similar, or different framework structure as zeolite. The ALPO molecular sieve does not substantially contain Si, but the SiO2 / Al2O3 ratio (molar ratio) of the ALPO molecular sieve is preferably less than 1, more preferably 0.5 or less, even more preferably 0.1 or less, and most preferably 0. The ALPO molecular sieve used here does not substantially contain Si, and is therefore different from aluminophosphate-based zeolites that have a high content of Al2O3 relative to SiO2 (even low-silica zeolites usually have a SiO2 / Al2O3 ratio of 1 or more). The SiO2 / Al2O3 ratio can be determined by X-ray fluorescence analysis (XRF).

[0033] The skeletal structure of the ALPO molecular sieve used is not particularly limited as long as it has a 12-membered ring. Examples of skeletal structures having 12-membered rings include AFI, AFR, AFS, AFY, ATO, ATS, BEA, CON, DFO, EZT, FAU, LTL, MOR, OSI, SAF, SBE, SBS, SBT, SFO, etc., as skeletal type codes defined by the International Zeolite Association (IZA). The skeletal structure is preferably AFI. The maximum number of rings of the ALPO molecular sieve having 12-membered rings is typically 12.

[0034] In addition, in this embodiment, the crystallite size of the ALPO having a 12-membered ring is 360 Å to 700 Å.

[0035] In the prior art, molecular sieves such as zeolite are used as HC adsorbents. Zeolite is a crystalline aluminosilicate that functions as a molecular sieve, and therefore contains Si and Al. According to findings obtained through studies by the present inventors, when a hydrothermal durability treatment is performed on a catalyst layer containing zeolite, Si contained in the zeolite moves and adversely affects the precious metal, which is the catalytic metal, thereby reducing the exhaust gas purification performance during cold start. This is believed to be because SiO2 contained in the zeolite is reduced to SiO in a high-temperature reducing atmosphere, causing interface movement and transpiration in the form of SiOx. It is also believed to be due to poisoning caused by the interaction between Si and the precious metal.

[0036] Therefore, in this embodiment, by using a molecular sieve that does not substantially contain Si as the HC adsorbent, the HC purification performance at the time of cold start is high even after hydrothermal durability.

[0037] It is also known that ALPO molecular sieves can be used as HC adsorbents. In this embodiment, an ALPO molecular sieve having a 12-membered ring is used. Since the skeletal structure of the ALPO molecular sieve has a 12-membered ring, it can efficiently adsorb HC, and the HC purification performance after hydrothermal durability is significantly improved.

[0038] Here, the AFI type skeleton structure, which is one of the skeleton structures of ALPO molecular sieves having 12-membered rings, is shown in FIG. 4(A). As shown in FIG. 4(A), the AFI type skeleton structure has a continuous structure in which 4-membered rings and 6-membered rings surround 12-membered rings. FIG. 4(B) is a conceptual schematic diagram of the AFI type skeleton structure at the grain boundary GB. As shown in FIG. 4(B), at the grain boundary GB, the structure in which 4-membered rings and 6-membered rings surround 12-membered rings cannot be maintained, and lattice defects occur. In particular, since the 12-membered rings that easily adsorb HC are large, lattice defects are likely to occur in the 12-membered rings at the grain boundary. The part where this lattice defect occurs cannot contribute to HC adsorption. Note that FIG. 4(B) is a conceptual diagram, and does not accurately show the ring structure of the part with lattice defects.

[0039] FIG. 5(A) is a schematic diagram showing one primary particle 500 of the ALPO molecular sieve having a large crystallite diameter. The primary particle 500 of the ALPO molecular sieve has a hexagonal prism shape, and FIG. 5(A) shows the hexagonal faces of the hexagonal prism. In FIG. 5(A), the squares inside the outline of the hexagon represent the crystallites 510.

[0040] FIG. 5(B) is a schematic diagram showing a crystallite 510 of the primary particle 500 of FIG. 5(A). FIG. 5(B) shows one crystallite 510. In FIG. 5(B), in the grain boundary 520, a region 512 where lattice defects occur is shown by dot hatching, and a region 514 without lattice defects is shown by a mesh pattern. This region 512 where lattice defects occur cannot contribute to HC adsorption. Note that, since these are schematic diagrams, the primary particle 500 and the crystallite 510 of the ALPO molecular sieve are drawn in a simplified manner.

[0041] On the other hand, Fig. 6(A) is a schematic diagram showing one primary particle 600 of the ALPO molecular sieve having a small crystallite diameter. In Fig. 6(A), the squares inside the hexagonal outline also show the crystallites 610. The size (i.e., crystallite diameter) of the crystallites 610 in Fig. 6(A) is smaller than the size of the crystallites 510 in Fig. 5(A).

[0042] FIG. 6(B) is a schematic diagram showing a crystallite 610 of the primary particle 600 of FIG. 6(A). FIG. 6(B) shows four crystallites 610, which are the same size as one crystallite 510 of FIG. 5(B). In FIG. 6(B) as well, in the grain boundary 620, a region 612 where lattice defects occur is shown by dot hatching, and a region 614 without lattice defects is shown by a mesh pattern. This region 612 where lattice defects occur cannot contribute to HC adsorption. Note that, since these are schematic diagrams, the primary particle 600 and the crystallite 610 of the ALPO molecular sieve are drawn in a simplified manner.

[0043] Here, when comparing Fig. 5(B) with Fig. 6(B), it is found that Fig. 6(B) has an extra cross-shaped crystal grain boundary 620 and an extra region 612 with lattice defects in the vicinity. Therefore, comparing Fig. 5(B) with Fig. 6(B) it is found that the smaller the crystallite diameter of the primary particles is, the larger the region that cannot contribute to HC adsorption per unit area is. In other words, it is found that the larger the crystallite diameter is, the smaller the region that cannot contribute to HC adsorption per unit area is.

[0044] Therefore, in this embodiment, by the crystallite diameter of the ALPO having a 12-membered ring being 360 Å or more, the region that cannot contribute to HC adsorption can be sufficiently reduced, and the HC purification performance after hydrothermal durability can be further significantly improved. On the other hand, ALPO having a crystallite diameter of more than 700 Å is difficult to manufacture. From the viewpoint of ease of manufacture, the crystallite diameter of the ALPO is preferably 600 Å or less, more preferably 550 Å or less, even more preferably 500 Å or less, and particularly preferably 400 Å or less. Therefore, when the crystallite diameter of the ALPO having a 12-membered ring is 360 Å to 400 Å, the exhaust gas purification catalyst 10 has excellent production efficiency. On the other hand, the larger the crystallite diameter of the ALPO, the higher the HC adsorption ability. From the viewpoint of HC adsorption ability, the crystallite diameter of the ALPO having a 12-membered ring is preferably 380 Å or more, more preferably 450 Å or more, even more preferably 480 Å or more, and particularly preferably 500 Å or more. From the viewpoint of the balance between production efficiency and HC adsorption capacity, the crystallite diameter of the ALPO having a 12-membered ring is preferably 360 Å to 650 Å, more preferably 380 Å to 600 Å, further preferably 450 Å to 600 Å, and particularly preferably 480 Å to 550 Å. Note that this crystallite diameter is a value determined by X-ray diffraction (XRD) measurement, and can be measured using a known XRD device according to a known method.

[0045] The ALPO molecular sieve having the above crystallite size and 12-membered ring can be produced as follows.

[0046] A well-known method for producing ALPO molecular sieves is to first mix an aluminum source, a phosphorus source, a template (in other words, a structure-directing agent (SDA)) and water to produce an aqueous gel, which is then subjected to a hydrothermal synthesis reaction. According to this method, ALPO molecular sieves of various structures can be produced by selecting the template and reaction conditions, and a method for producing an ALPO molecular sieve having a 12-membered ring is also known.

[0047] In the above-mentioned production method, the crystallite size of the ALPO molecular sieve can be controlled by adjusting the amount of water. In particular, in order to make the crystallite size of the ALPO molecular sieve 360 ​​Å or more, a larger amount of water than usual is used. By using a larger amount of water, the generation of nuclei is reduced, so that the crystallite size of the ALPO molecular sieve can be increased.

[0048] For example, when alumina (Al2O3) is used as the aluminum source, diphosphorus pentoxide as the phosphorus source, and triethylamine as the template, for example, 80 moles or more, preferably 100 moles or more of water is used per mole of Al2O3. If the amount of water used is too excessive, the amount of nuclei generated will be too small, and the ALPO molecular sieve may become amorphous. Therefore, the amount of water used is, for example, about 400 moles or less per mole of Al2O3. By carrying out the preparation of an aqueous gel and the hydrothermal synthesis reaction with such an amount of water used, an ALPO molecular sieve with a crystallite diameter of 360 Å to 700 Å can be easily obtained. Here, the crystallite diameter can be controlled to some extent within the above range by adjusting the preparation conditions of the aqueous gel (particularly, the stirring time) and the reaction conditions of the hydrothermal synthesis (particularly, the reaction time).

[0049] In this embodiment, the HC adsorption layer 20 may contain an HC adsorbent other than the above-mentioned ALPO molecular sieve (e.g., zeolite, molecular sieve such as ALPO having no 12-membered ring). In the HC adsorption layer 20, typically more than 50 mass%, preferably 80 mass% or more, more preferably 90 mass% or more, and even more preferably 100 mass% of the total HC adsorbent is an ALPO molecular sieve having the above-mentioned crystallite size and 12-membered ring.

[0050] The particle size of the HC adsorbent is not particularly limited. The average primary particle size of the HC adsorbent (particularly, the ALPO molecular sieve having the above crystallite size and 12-membered ring) is, for example, 0.5 μm to 60 μm, and may be 0.5 μm to 30 μm. Since the peel resistance of the exhaust gas purification layer 40 to the substrate 11 is particularly high, the average primary particle size of the HC adsorbent (particularly, the ALPO molecular sieve having the above crystallite size and 12-membered ring) is preferably 1 μm to 26 μm, more preferably 1 μm to 10 μm. The average particle size of the HC adsorbent can be obtained by acquiring a scanning electron microscope (SEM) image, determining the particle sizes of 100 or more arbitrarily selected HC adsorbent particles, and calculating the average value. When the HC adsorbent particles are ALPO molecular sieves, the particle size is measured by measuring the height dimension of the hexagonal columnar particles.

[0051] The amount of the HC adsorbent in the exhaust gas purification catalyst 10 is not particularly limited, and can be appropriately designed in consideration of the size of the cells 12 of the substrate 11, the flow rate of the exhaust gas flowing through the exhaust gas purification catalyst 10, and the like. The amount of the HC adsorbent per 1 L of volume of the substrate 11 may be, for example, 1 g / L or more, 5 g / L or more, 10 g / L or more, 15 g / L or more, or 20 g / L or more, and may be, for example, 200 g / L or less, 150 g / L or less, 100 g / L or less, 80 g / L or less, 60 g / L or less, 50 g / L or less, or 40 g / L or less.

[0052] In this specification, "per 1 L of substrate volume" refers to 1 L of the total bulk volume including the net volume of the substrate and the volume of the cell passages. In the following explanation, the amount indicated as (g / L) indicates the amount contained in 1 L of substrate volume.

[0053] The HC adsorption layer 20 may contain components other than the HC adsorbent as optional components. Examples of the optional components of the HC adsorption layer 20 include binders such as alumina sol and silica sol, and various additives.

[0054] The HC adsorption layer 20 may contain, as other optional components, an oxygen absorbing / releasing material having oxygen absorbing / releasing ability (so-called OSC material) and a non-oxygen absorbing / releasing material not having oxygen absorbing / releasing ability (so-called non-OSC material). Examples of the OSC material and the non-OSC material are the same as the OSC material and the non-OSC material contained in the catalyst layer 30 described later.

[0055] There is no particular limitation on the contents of the OSC material and non-OSC material in the HC adsorption layer 20. The more the amount of HC adsorption material in the HC adsorption layer 20, the more HC can be adsorbed. For this reason, the contents of the OSC material and non-OSC material in the HC adsorption layer 20 are each preferably 40 mass % or less, and more preferably 20 mass % or less.

[0056] On the other hand, since the exhaust gas purifying catalyst 10 has the catalyst layer 30, the HC adsorption layer 20 usually does not contain a catalytic metal.

[0057] In one preferred embodiment, the HC adsorption layer 20 is composed only of an HC adsorbent and a binder component.

[0058] A part of the HC adsorption layer 20 may have a different composition from the other part of the HC adsorption layer 20. For example, an upstream side X1 part (front part) and a downstream side X2 part (rear part) in the axial direction X of the HC adsorption layer 20 may have different compositions. Specifically, for example, the upstream side X1 part (front part) and the downstream side X2 part (rear part) in the axial direction X of the HC adsorption layer 20 may contain ALPO molecular sieves having different skeletal structures.

[0059] The coating amount (i.e., the molding amount) of the HC adsorption layer 20 is not particularly limited. The coating amount is, for example, 3 to 200 g / L, and may be 10 to 100 g / L per 1 L of the volume of the portion of the substrate on which the HC adsorption layer 20 is formed along the cylinder axis direction X. By satisfying the above range, it is possible to achieve both an improvement in the purification performance of harmful components and a reduction in pressure loss at a high level. In addition, it is possible to improve durability and peeling resistance.

[0060] The thickness of the HC adsorption layer 20 is not particularly limited, and may be appropriately designed in consideration of durability, peel resistance, etc. The thickness of the HC adsorption layer 20 is, for example, 1 to 100 μm, and may be 5 to 100 μm.

[0061] There are no particular limitations on the coat width (average length) in the cylinder axis direction X of the HC adsorption layer 20. Since the larger the coat width, the better the HC purification performance, the coat width is, for example, 20% or more of the total length L of the substrate 11, preferably 50% or more, more preferably 80% or more, and even more preferably 90% or more, and may be the same length as the total length L of the substrate 11.

[0062] The catalyst layer 30 is a reaction field that purifies harmful components in exhaust gas. The catalyst layer 30 is a porous body having a large number of pores (voids). The exhaust gas that flows into the exhaust gas purification catalyst 10 comes into contact with the catalyst layer 30 while flowing through the flow paths (cells 12) of the exhaust gas purification catalyst 10. This purifies the harmful components in the exhaust gas. For example, HC and CO contained in the exhaust gas are oxidized by the catalyst layer 30 and converted (purified) into water, carbon dioxide, etc. For example, NOx contained in the exhaust gas is reduced by the catalyst layer 30 and converted (purified) into nitrogen.

[0063] The catalyst layer 30 includes at least a catalyst metal as an essential component. As the catalyst metal, various metal species that can function as an oxidation catalyst or reduction catalyst in purifying harmful components can be used. Typical examples of the catalyst metal include platinum group metals, i.e., rhodium (Rh), palladium (Pd), platinum (Pt), ruthenium (Ru), osmium (Os), and iridium (Ir). Other metal species may be used instead of or in addition to the platinum group metals. For example, metal species such as iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), silver (Ag), and gold (Au) may be used. Furthermore, an alloy of two or more of these metals may be used. As the catalyst metal, an oxidation catalyst with high oxidation activity (e.g., at least one of Pd and Pt) and a reduction catalyst with high reduction activity (e.g., Rh) are suitable, and it is particularly preferable to combine two or more of these. The oxidation catalyst and the reduction catalyst may be present in the same (single) catalyst layer or in separate catalyst layers.

[0064] From the viewpoint of increasing the contact area with the exhaust gas, it is preferable that the catalytic metal is used as fine particles having a sufficiently small particle size. The average particle size of the catalytic metal (specifically, the average particle size of 50 or more catalytic metal particles determined by observation with a transmission electron microscope (TEM)) is generally 1 to 15 nm, for example, 10 nm or less, and further 5 nm or less.

[0065] The amount of catalytic metal in the exhaust gas purification catalyst 10 is not particularly limited and can be appropriately determined depending on the type of catalytic metal, etc. The amount of catalytic metal per 1 L of the volume of the substrate 11 may be, for example, 0.01 g / L or more, 0.03 g / L or more, 0.05 g / L or more, 0.08 g / L or more, or 0.10 g / L or more, from the viewpoint of particularly high exhaust gas purification performance. From the viewpoint of the balance between exhaust gas purification performance and cost, it may be, for example, 15.00 g / L or less, 10.00 g / L or less, 5.00 g / L or less, 3.00 g / L or less, 1.50 g / L or less, 1.00 g / L or less, 0.80 g / L or less, or 0.50 g / L or less.

[0066] The catalytic metal is usually supported on a carrier, and therefore the catalytic layer 30 may further contain a carrier that supports the catalytic metal.

[0067] As the carrier for supporting the catalytic metal, a known material used as a carrier for catalytic metal of an exhaust gas purification catalyst can be used. The carrier is typically an inorganic porous body. Examples of the carrier include materials that do not have oxygen storage capacity (non-OSC materials) such as aluminum oxide (Al2O3, alumina), titanium oxide (TiO2, titania), zirconium oxide (ZrO2, zirconia), silicon oxide (SiO2, silica), etc.; materials that have oxygen storage capacity (OSC materials) such as ceria (CeO2) and composite oxides containing ceria; etc. The carrier may be either a non-OSC material or an OSC material, or may be both.

[0068] A small amount (e.g., 1% by mass to 10% by mass) of an oxide of a rare earth element such as Pr2O3, Nd2O3, La2O3, or Y2O3 may be added to the oxide used as the non-OSC material in order to improve heat resistance, etc. Since the non-OSC material is particularly excellent in heat resistance and durability, Al2O3 is preferable, and Al2O3 composited with La2O3 (La2O3-Al2O3 composite oxide; LA composite oxide) is more preferable.

[0069] Regarding the OSC material, an example of a composite oxide containing ceria is a composite oxide containing ceria and zirconia (ceria-zirconia composite oxide (so-called CZ composite oxide or ZC composite oxide)). When zirconium oxide is contained in the OSC material, thermal deterioration of cerium oxide can be suppressed, and therefore ceria-zirconia composite oxide is preferable as the OSC material.

[0070] The OSC material may contain oxides of rare earth elements for the purpose of improving properties (particularly heat resistance and oxygen absorption / release properties, etc.). Examples of rare earth elements include Sc, Y, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Preferred oxides of rare earth elements are Pr2O3, Nd2O3, La2O3, and Y2O3.

[0071] When the OSC material is a composite oxide containing cerium oxide, the content of cerium oxide in the composite oxide is preferably 15% by mass or more, more preferably 20% by mass or more, from the viewpoint of fully exerting its oxygen storage capacity. On the other hand, if the content of cerium oxide is too high, the basicity of the OSC material may be too high. Therefore, the content of cerium oxide is preferably 40% by mass or less, more preferably 30% by mass or less.

[0072] As an example, catalyst layer 30 includes an OSC material and a non-OSC material, and the catalytic metal is supported on both the OSC material and the non-OSC material.

[0073] The catalyst layer 30 may further contain the above-mentioned OSC material and / or the above-mentioned non-OSC material in a form that does not support a catalytic metal. The OSC material and non-OSC material used as the support and the OSC material and non-OSC material used as the non-support preferably do not contain Si.

[0074] The amount of the OSC material and the non-OSC material in the exhaust gas purification catalyst 10 is not particularly limited, and can be appropriately designed in consideration of the size of the cells 12 of the substrate 11, the flow rate of the exhaust gas flowing through the exhaust gas purification catalyst 10, and the like. The total amount of the OSC material and the non-OSC material (the total amount of the OSC material and the non-OSC material including both the carrier and the non-carrier) per 1 L of volume of the substrate 11 may be, for example, 50 g / L or more, 70 g / L or more, 80 g / L or more, 90 g / L or more, or 100 g / L or more, and may be, for example, 300 g / L or less, 250 g / L or less, 200 g / L or less, 180 g / L or less, or 160 g / L or less.

[0075] The catalyst layer 30 preferably contains an OSC material as a catalyst metal carrier or in a form that does not support a catalyst metal. In this case, even when the air-fuel ratio of the exhaust gas varies due to, for example, the running conditions of the vehicle, the catalyst layer 30 can exhibit stable and excellent purification performance.

[0076] The catalyst layer 30 may contain an alkaline earth element such as calcium (Ca) or barium (Ba). The alkaline earth element can suppress poisoning of the catalyst metal (particularly the oxidation catalyst). The alkaline earth element can also increase the dispersibility of the catalyst metal and suppress sintering caused by grain growth of the catalyst metal. When the catalyst layer 30 contains an alkaline earth element together with the OSC material, the amount of oxygen absorbed by the OSC material can be further improved in a lean atmosphere (oxygen-excess atmosphere) in which the fuel is leaner than the theoretical air-fuel ratio. The alkaline earth element can be contained in the form of an oxide, hydroxide, carbonate, nitrate, sulfate, phosphate, acetate, formate, oxalate, halide, or the like.

[0077] The catalyst layer 30 may also contain a NOx adsorbent having NOx storage capacity, a stabilizer, etc. Examples of the stabilizer include rare earth elements such as yttrium (Y), lanthanum (La), and neodymium (Nd). The rare earth elements may be present in the catalyst layer 30 in the form of oxides.

[0078] Other optional components of the catalyst layer 30 include binders such as alumina sol and silica sol, various additives, etc. The binder is preferably one that does not contain Si, and therefore alumina sol is preferred.

[0079] The catalyst layer 30 may contain an HC adsorbent. However, since the exhaust gas purifying catalyst 10 according to this embodiment has the HC adsorption layer 20, it is preferable that the catalyst layer 30 does not contain an HC adsorbent.

[0080] Although not particularly limited, the coating amount (molding amount) of the catalyst layer 30 may be approximately 30 g / L or more, typically 50 g / L or more, preferably 70 g / L or more, for example 100 g / L or more, per 1 L of the volume of the exhaust gas purification catalyst 10 (volume of the substrate 11), and may be approximately 500 g / L or less, typically 400 g / L or less, for example 300 g / L or less. By satisfying the above range, it is possible to achieve both improvement in purification performance and reduction in pressure loss at a high level. In this specification, the "coating amount" refers to the mass of solids contained per unit volume of the exhaust gas purification catalyst 10.

[0081] The length and thickness of the catalyst layer 30 can be appropriately designed in consideration of, for example, the size of the cells 12 of the substrate 11 and the flow rate of exhaust gas flowing through the exhaust gas purification catalyst 10. The catalyst layer 30 may be provided continuously or intermittently on the partition walls 14 of the substrate 11. The catalyst layer 30 may be provided, for example, from the exhaust gas inlet 10a along the cylinder axis direction X, or from the exhaust gas outlet 10b along the cylinder axis direction X.

[0082] Although not particularly limited, the entire coating width (average length) of the catalyst layer 30 in the cylinder axis direction X is approximately 20% or more, preferably 50% or more, typically 80% or more, for example 90% or more of the total length L of the substrate 11, and may be the same length as the total length L of the substrate 11. Although not particularly limited, the coating thickness (average thickness) of the catalyst layer 30 is approximately 1 to 300 μm, typically 5 to 200 μm, for example 10 to 100 μm. This makes it possible to achieve both improved purification performance and reduced pressure loss at a high level.

[0083] A part of the catalyst layer 30 may have a different composition from the other part of the catalyst layer 30. For example, the upstream side X1 part (front part) and the downstream side X2 part (rear part) in the cylindrical axis direction X of the catalyst layer 30 may have different compositions. Specifically, for example, the upstream side X1 part (front part) and the downstream side X2 part (rear part) in the cylindrical axis direction X of the catalyst layer 30 may contain different catalytic metals.

[0084] The exhaust gas purifying catalyst 10 illustrated in FIG. 3 has only the exhaust gas purifying layer 40. However, the exhaust gas purifying catalyst 10 may further have layers other than these. For example, the exhaust gas purifying catalyst 10 may have another layer (which may also be called an underlayer) between the substrate 11 and the exhaust gas purifying layer 40, or may have another layer on the exhaust gas purifying layer 40. In addition, the exhaust gas purifying layer 40 may further have layers other than the HC adsorption layer 20 and the catalyst layer 30 that are involved in purifying the exhaust gas.

[0085] The catalyst layer 30 of the exhaust gas purification catalyst 10 illustrated in Fig. 3 has a single-layer structure. However, the catalyst layer 30 may have a multi-layer structure in which each layer contains a catalytic metal. Hereinafter, an example of the exhaust gas purification catalyst in which the catalyst layer 30 has a multi-layer structure will be described.

[0086] <Modification of exhaust gas purification catalyst 10> 7 is a partial cross-sectional view showing a schematic view of a part of a cross section of an exhaust gas purifying catalyst 10', which is a modified example of the exhaust gas purifying catalyst 10, cut along the cylinder axis direction X. The exhaust gas purifying catalyst 10' includes a substrate 11 and an exhaust gas purifying layer 40' provided on the substrate 11. The exhaust gas purifying layer 40' includes an HC adsorption layer 20 and a catalyst layer 30' having a multi-layer structure. The HC adsorption layer 20 and the catalyst layer 30' are laminated such that the HC adsorption layer 20 is closer to the substrate 11 than the catalyst layer 30'. The catalyst layer 30' has a multi-layer structure, which can further improve the exhaust gas purification performance.

[0087] The substrate 11 and the HC adsorption layer 20 are the same as described above. The catalyst layer 30' has a multi-layer structure, unlike the example shown in FIG. 3. Specifically, the catalyst layer 30' has a laminated structure in which a first partial catalyst layer (lower layer) 31 and a second partial catalyst layer (upper layer) 32 are laminated in the thickness direction. Therefore, the lower layer 31 is disposed on the substrate 11 side. In the illustrated example, the lower layer 31 is provided so as to contact the surface of the HC adsorption layer 20, and the upper layer 32 is provided so as to contact the upper surface of the lower layer 31. In the illustrated example, the catalyst layer 30' has a two-layer structure, but the catalyst layer 30' may have a laminated structure of three or more layers. For example, the catalyst layer 30' may have an intermediate layer between the lower layer 31 and the upper layer 32, and the catalyst layer 30' may have another layer on the upper layer 32.

[0088] The lower layer 31 and the upper layer 32 each contain a catalytic metal. Here, the lower layer 31 and the upper layer 32 may contain the same catalytic metal or different catalytic metals, and preferably contain different catalytic metals.

[0089] Specifically, for example, the lower layer 31 contains an oxidation catalyst (e.g., at least one of Pd and Pt) as a catalytic metal, and the upper layer 32 contains a reduction catalyst (e.g., Rh) as a catalytic metal. In this case, the exhaust gas purification catalyst 10' is particularly excellent in exhaust gas purification performance. From the viewpoint of higher exhaust gas purification performance, it is advantageous that the catalytic metal of the lower layer 31 is Pt and the catalytic metal of the upper layer 32 is Rh. In this case, it is particularly advantageous for purification of paraffin. Alternatively, from the viewpoint of higher exhaust gas purification performance, it is advantageous that the catalytic metal of the lower layer 31 is Pd and the catalytic metal of the upper layer 32 is Rh. In this case, it is particularly advantageous for purification of olefin.

[0090] When the lower layer 31 contains Pt, preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 100% by mass of the catalytic metal contained in the lower layer 31 is Pt. When the lower layer 31 contains Pd, preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 100% by mass of the catalytic metal contained in the lower layer 31 is Pd. When the upper layer 32 contains Rh, preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 100% by mass of the catalytic metal contained in the upper layer 32 is Rh.

[0091] The lower layer 31 and the upper layer 32 may contain the same optional components as the catalyst layer 30 described above.

[0092] <Method for manufacturing exhaust gas purification catalyst 10> The exhaust gas purifying catalyst 10 can be manufactured, for example, by the following method. First, the substrate 11, a slurry for forming the HC adsorption layer 20, and a slurry for forming the catalyst layer 30 are prepared.

[0093] The slurry for forming the HC adsorption layer can be prepared, for example, by mixing the ALPO molecular sieve having the above-mentioned crystallite size and 12-membered ring with other optional components (for example, non-OSC material, OSC material, binder, various additives, etc.) in a dispersion medium. The slurry for forming the catalyst layer can be prepared, for example, by mixing a catalyst metal source (for example, a solution containing a catalyst metal as ions) with other optional components (for example, non-OSC material, OSC material, binder, various additives, etc.) in a dispersion medium. As the dispersion medium, for example, water, a mixture of water and a water-soluble organic solvent, etc. can be used. The properties of these slurries (for example, viscosity, solid content, etc.) can be appropriately determined depending on the size of the substrate 11 used, the shape of the cell 12 (partition wall 14), the required properties of the HC adsorption layer 20 and the catalyst layer 30, etc.

[0094] Next, the HC adsorption layer 20 is formed on the substrate 11 using the slurry for forming the HC adsorption layer. The HC adsorption layer 20 can be formed by a conventionally known method (for example, an impregnation method, a washcoat method, etc.). Specifically, for example, the slurry for forming the HC adsorption layer is made to flow into the cells 12 from the end of the substrate 11 and is supplied to a predetermined length along the cylindrical axis direction X. The slurry may be made to flow from either the inlet 10a or the outlet 10b. At this time, excess slurry may be sucked from the end on the opposite side. Also, excess slurry may be discharged from the cells 12 by blowing air from the end on the opposite side, etc.

[0095] Next, the substrate 11 to which the slurry has been supplied is fired at a predetermined temperature for a predetermined time. The firing method may be the same as that of the conventional method. Also, before firing, drying may be performed to remove the dispersion medium. In this way, the HC adsorption layer 20 can be formed on the substrate 11.

[0096] Next, the catalyst layer 30 is formed using the catalyst layer forming slurry. The catalyst layer 30 can be formed by a conventionally known method (for example, an impregnation method, a washcoat method, etc.). For example, in the same manner as above, the catalyst layer forming slurry is made to flow into the cells 12 from the end of the substrate 11 and is supplied to a predetermined length along the cylindrical axis direction X, and the catalyst layer forming slurry is applied onto the HC adsorption layer 20 formed on the substrate 11.

[0097] Next, this is calcined at a predetermined temperature for a predetermined time. The calcination method may be the same as that of the conventional method. Also, before the calcination, drying may be performed to remove the dispersion medium. In this way, the catalyst layer 30 can be formed on the HC adsorption layer 20 formed on the substrate 11. In this manner, the exhaust gas purification catalyst 10 can be obtained.

[0098] Second Embodiment The second embodiment differs from the first embodiment in the structure of the exhaust gas purification layer of the exhaust gas purification catalyst, and therefore this point will be mainly described, and a description of the points that are the same as those in the first embodiment will basically be omitted.

[0099] Fig. 8 is a partial cross-sectional view of the exhaust gas purification catalyst 110 according to the second embodiment, cut in the cylinder axis direction. As shown in Fig. 8, the exhaust gas purification catalyst 110 according to the second embodiment includes a substrate 11 and an exhaust gas purification layer 140. The substrate 11 is the same as that of the first embodiment. The exhaust gas purification layer 140 contains a catalytic metal and a molecular sieve that is substantially free of Si as an HC adsorbent. The molecular sieve that is substantially free of Si is an ALPO molecular sieve having a 12-membered ring. The crystallite diameter of the ALPO molecular sieve, as determined by X-ray diffraction measurement, is 360 Å to 700 Å.

[0100] In the second embodiment, the exhaust gas purification layer 140 has an upstream side X1 portion (front portion) 140A and a downstream side X2 portion (rear portion) 140B in the cylinder axis direction X. The front portion 140A is configured as an HC adsorption layer containing the above-mentioned ALPO molecular sieve, and the rear portion 140B is configured as a catalyst layer containing a catalytic metal.

[0101] The composition of the HC adsorption layer constituting the front portion 140A may be the same as the HC adsorption layer 20 of the exhaust gas purifying catalyst 10 according to the first embodiment. The composition of the catalyst layer constituting the rear portion 140B may be the same as the catalyst layer 30 of the exhaust gas purifying catalyst 10 according to the first embodiment.

[0102] The amounts of the catalytic metal, the ALPO molecular sieve, the OSC material, and the non-OSC material in the exhaust gas purifying catalyst 110 are not particularly limited, and may be the same as those in the exhaust gas purifying catalyst 10 according to the first embodiment.

[0103] The ratio of the coat widths (average lengths) in the cylinder axis direction X of the front portion 140A and the rear portion 140B is not particularly limited, but is, for example, 5:95 to 90:10, preferably 10:90 to 80:20, and more preferably 20:80 to 70:30.

[0104] The front portion 140A and the rear portion 140B each have a single-layer structure, but may have a multi-layer structure. For example, the rear portion 140B may have a multi-layer structure including an upper layer on the surface layer side and a lower layer on the substrate side, and the upper layer and the lower layer may contain different types of catalytic metals.

[0105] Specifically, for example, the rear portion 140B has a multi-layer structure including an upper layer on the surface layer side and a lower layer on the substrate side, the upper layer containing a reduction catalyst (e.g., Rh) as a catalytic metal, and the lower layer containing an oxidation catalyst (e.g., at least one of Pd and Pt) as a catalytic metal. In this case, the exhaust gas purification catalyst 110 is particularly excellent in exhaust gas purification performance.

[0106] It is also possible to configure the front portion 140A as a catalyst layer and the rear portion 140B as a HC adsorption layer in the exhaust gas purification layer 140. However, as described above, when the front portion 140A is configured as a HC adsorption layer and the rear portion 140B is configured as a catalyst layer, the HC adsorbed by the front portion 140A can be purified by the rear portion 140B when desorbed from the front portion 140A, which is particularly advantageous in terms of HC purification efficiency.

[0107] In the illustrated example, the front portion 140A and the rear portion 140B are in contact with each other, but they may be separated from each other. Also, for manufacturing reasons, the X2 side end of the front portion 140A and the X1 side end of the rear portion 140B may partially overlap each other.

[0108] Although not particularly limited, the coating amount (molding amount) of the exhaust gas purification layer 140 may be approximately 30 g / L or more, typically 50 g / L or more, preferably 70 g / L or more, for example 100 g / L or more, per 1 L of the volume of the exhaust gas purification catalyst 110 (volume of the substrate 11), and may be approximately 500 g / L or less, typically 400 g / L or less, for example 300 g / L or less. By satisfying the above range, it is possible to achieve both improvement in purification performance and reduction in pressure loss at a high level. In this specification, the "coating amount" refers to the mass of solid content contained per unit volume of the exhaust gas purification catalyst 10.

[0109] Although not particularly limited, the entire coating width (average length) of the exhaust gas purification layer 140 in the cylinder axis direction X is approximately 20% or more, preferably 50% or more, typically 80% or more, for example 90% or more of the total length L of the substrate 11, and may be the same length as the total length L of the substrate 11. Although not particularly limited, the coating thickness (average thickness) of the exhaust gas purification layer 140 is approximately 1 to 300 μm, typically 5 to 200 μm, for example 10 to 100 μm. This makes it possible to achieve both improved purification performance and reduced pressure loss at a high level.

[0110] The exhaust gas purifying catalyst 110 of the second embodiment can be manufactured, for example, by the following method: First, similarly to the first embodiment, the substrate 11, a slurry for forming an HC adsorption layer, and a slurry for forming a catalyst layer are prepared.

[0111] A slurry for forming an HC adsorption layer is poured into a predetermined position from the exhaust gas inlet end of the substrate 11 and dried. A slurry for forming a catalyst layer is poured into a predetermined position from the exhaust gas outlet end of the substrate 11 and dried. Then, firing is performed to form an exhaust gas purification layer 140 on the substrate 11, the exhaust gas purification layer 140 including a front portion composed of an HC adsorption layer and a rear portion composed of a catalyst layer. In this way, a catalyst 110 for purifying exhaust gas can be obtained.

[0112] Third Embodiment The third embodiment differs from the first embodiment in the structure of the exhaust gas purification layer of the exhaust gas purification catalyst, and therefore this point will be mainly described, and a description of the points that are the same as those in the first embodiment will basically be omitted.

[0113] FIG. 9 is a partial cross-sectional view of the exhaust gas purification catalyst 210 according to the third embodiment, cut in the cylinder axis direction. As shown in FIG. 9, the exhaust gas purification catalyst 210 according to the third embodiment includes a substrate 11 and an exhaust gas purification layer 240. The substrate 11 is the same as that of the first embodiment. The exhaust gas purification layer 240 contains a catalytic metal and a molecular sieve that does not substantially contain Si as an HC adsorbent. The molecular sieve that does not substantially contain Si is an ALPO molecular sieve having a 12-membered ring. The crystallite diameter of the ALPO molecular sieve, as determined by X-ray diffraction measurement, is 360 Å to 700 Å. In the third embodiment, the ALPO molecular sieve and the catalytic metal are mixed and contained in one layer.

[0114] In the exhaust gas purification layer 240, the catalytic metal may be supported on the above-mentioned ALPO molecular sieve or on a carrier. Therefore, the exhaust gas purification layer 240 may further contain a carrier that supports the catalytic metal. The catalytic metal may be supported on either the above-mentioned ALPO molecular sieve or the carrier, or may be supported on both. Examples of the carrier include the above-mentioned OSC material and the above-mentioned non-OSC material.

[0115] As one example, the exhaust gas purification layer 240 includes a catalytic metal, the above-mentioned ALPO molecular sieve, an OSC material, and a non-OSC material, and the catalytic metal is supported by all of the above-mentioned ALPO molecular sieve, the OSC material, and the non-OSC material. As another example, the exhaust gas purification layer 240 includes a catalytic metal, the above-mentioned ALPO molecular sieve, an OSC material, and a non-OSC material, and the catalytic metal is supported by the non-OSC material. As yet another example, the exhaust gas purification layer 240 includes a catalytic metal, the above-mentioned ALPO molecular sieve, an OSC material, and a non-OSC material, and the catalytic metal is supported by the OSC material and the non-OSC material.

[0116] The exhaust gas purification layer 240 may contain, as optional components, alkaline earth elements, NOx adsorbents, stabilizers, binders, various additives, NH3 adsorbents, etc. The binder is preferably one that does not contain Si, and therefore alumina sol is preferable.

[0117] The amounts of the catalytic metal, the ALPO molecular sieve, the OSC material, and the non-OSC material in the exhaust gas purifying catalyst 210 are not particularly limited, and may be the same as those in the exhaust gas purifying catalyst 10 according to the first embodiment.

[0118] Although not particularly limited, the coating amount (molding amount) of the exhaust gas purification layer 240 may be approximately 30 g / L or more, typically 50 g / L or more, preferably 70 g / L or more, for example 100 g / L or more, per 1 L of the volume of the exhaust gas purification catalyst 10 (volume of the substrate 11), and may be approximately 500 g / L or less, typically 400 g / L or less, for example 300 g / L or less. By satisfying the above range, it is possible to achieve both improvement in purification performance and reduction in pressure loss at a high level. In this specification, the "coating amount" refers to the mass of solids contained per unit volume of the exhaust gas purification catalyst 10.

[0119] Although not particularly limited, the entire coating width (average length) of the exhaust gas purification layer 240 in the cylinder axis direction X is approximately 20% or more, preferably 50% or more, typically 80% or more, for example 90% or more of the total length L of the substrate 11, and may be the same length as the total length L of the substrate 11. Although not particularly limited, the coating thickness (average thickness) of the exhaust gas purification layer 240 is approximately 1 to 300 μm, typically 5 to 200 μm, for example 10 to 100 μm. This makes it possible to achieve both improved purification performance and reduced pressure loss at a high level.

[0120] A part of the exhaust gas purification layer 240 may have a different composition from the other part of the exhaust gas purification layer 240. For example, an upstream side X1 part (front part) and a downstream side X2 part (rear part) in the axial direction X of the exhaust gas purification layer 240 may have different compositions. Specifically, for example, the upstream side X1 part (front part) and the downstream side X2 part (rear part) in the axial direction X of the exhaust gas purification layer 240 may contain different types of catalytic metals or different types of the above-mentioned ALPO molecular sieves.

[0121] In the illustrated example, the exhaust gas purification layer 240 has a single-layer structure, but may have a multi-layer structure. For example, the exhaust gas purification layer 240 may have a multi-layer structure including an upper layer on the surface layer side and a lower layer on the substrate side, and each of the upper layer and the lower layer may contain the above-mentioned ALPO molecular sieve and catalytic metal. In this case, the upper layer and the lower layer may contain different types of catalytic metals and different types of the above-mentioned ALPO molecular sieves.

[0122] Specifically, for example, the exhaust gas purification layer 240 has a multi-layer structure including an upper layer on the surface layer side and a lower layer on the substrate side, the upper layer containing the above-mentioned ALPO molecular sieve and a reduction catalyst (e.g., Rh) as a catalytic metal, and the lower layer containing the above-mentioned ALPO molecular sieve and an oxidation catalyst (e.g., at least one of Pd and Pt) as a catalytic metal. In this case, the exhaust gas purification catalyst 210 is particularly excellent in exhaust gas purification performance.

[0123] The exhaust gas purification catalyst 210 of the third embodiment can be manufactured, for example, by the following method. First, the substrate 11 and a slurry for forming the exhaust gas purification layer 240 are prepared. The slurry for forming the exhaust gas purification layer can be prepared, for example, by mixing a catalytic metal source (for example, a solution containing catalytic metal ions), the above-mentioned ALPO molecular sieve, and other optional components (for example, non-OSC material, OSC material, binder, various additives, etc.) in a dispersion medium.

[0124] Next, the slurry for forming the exhaust gas purification layer is applied to the substrate 11 by a conventionally known method, dried as necessary, and then fired. In this manner, the exhaust gas purification layer 240 is formed on the substrate 11, and the exhaust gas purification catalyst 210 can be obtained.

[0125] <Applications of exhaust gas purification catalysts 10, 110, 210> The exhaust gas purification catalysts 10, 110, and 210 can be suitably used for purifying exhaust gas discharged from internal combustion engines such as vehicles like automobiles and trucks, motorcycles and bicycles with engines, marine products such as ships, tankers, water bikes, personal watercraft, and outboard motors; gardening products such as lawn mowers, chain saws, and trimmers; leisure products such as golf carts and four-wheel buggies; power generation facilities such as cogeneration systems; garbage incinerators; and the like. Among them, they can be suitably used for vehicles such as automobiles, and in particular, for vehicles equipped with gasoline engines.

[0126] ≪Hydrocarbon Adsorbent≫ From another aspect, the hydrocarbon (HC) adsorbent disclosed herein contains the above-mentioned ALPO molecular sieve. That is, the HC adsorbent disclosed herein contains the ALPO molecular sieve. The ALPO molecular sieve has a 12-membered ring. The crystallite size of the ALPO molecular sieve determined by X-ray diffraction measurement is 360 Å to 700 Å. According to such a configuration, the HC adsorption amount remains high even after hydrothermal durability. Therefore, when an exhaust gas purification catalyst is configured using the HC adsorbent disclosed herein, the HC purification performance at cold start after hydrothermal durability is improved.

[0127] Hereinafter, test examples related to the present invention will be described, but the present invention is not intended to be limited to those shown in the following test examples.

[0128] <Preparation of HC Adsorbent> 〔Example 1-1〕 100 moles of water was mixed with 1 mole of Al2O3 and stirred for 30 minutes. 1 mole of P2O5 was added to 1 mole of Al2O3, and 1.55 moles of triethylamine (TEA) was further added. This was stirred for 30 minutes. As a result, an aqueous gel was obtained. The obtained aqueous gel was transferred to an autoclave and subjected to hydrothermal synthesis at 210°C for 36 hours. Then, centrifugation was performed, and the precipitate was filtered and washed. The precipitate was dried overnight in a dryer set at 80°C. Then, the precipitate was baked in an electric furnace at 150°C for 1 hour, and then further baked at 600°C for 6 hours to obtain an ALPO molecular sieve, which is an HC adsorbent of Example 1-1.

[0129] [Examples 1-2, 1-3, and Comparative Examples 1-1, 1-2] The ALPO molecular sieve, which is the HC adsorbent of each Example and Comparative Example, was obtained in the same manner as in Example 1-1, except that the amount of water used per mole of Al2O3 was changed to the amount shown in Table 1. The ALPO molecular sieve in Comparative Example 1-1 was produced under conventional general conditions.

[0130] [Examples 1-4] An ALPO molecular sieve, which is an HC adsorbent of Example 1-4, was obtained in the same manner as in Example 1-1, except that 200 moles of water were mixed with 1 mole of Al2O3 and the reaction time of the hydrothermal synthesis was changed from 36 hours to 42 hours.

[0131] [Examples 1 to 5] The ALPO molecular sieve, which is the HC adsorbent of Example 1-5, was obtained in the same manner as in Example 1-1, except that 200 moles of water were mixed with 1 mole of Al2O3, and the stirring time after adding P2O5 and triethylamine was changed from 30 minutes to 3 hours.

[0132] <Crystallite size measurement> The crystallite diameter of the ALPO molecular sieve of each Example and Comparative Example was measured using an XRD device "RINT TTR III" (manufactured by Rigaku Corporation). The measurement conditions are described below. The integrated powder X-ray analysis software PDXL2 (ver 2.8.1.1) attached to the device was used to calculate the crystallite diameter. Specifically, the crystallite diameter of the ALPO of each Example and Comparative Example was calculated from the analysis item "crystallite size" of the software. The analysis method was the Halder-Wangner method, and no correction was made. The measurement results of the crystallite diameter are shown in Table 1. Operation axis: 2θ / θ Source: CuKα Measurement method: Continuous Voltage: 40kV Current: 250mA Starting angle: 2θ=5° End angle: 2θ=85° Sampling width: 0.02° Scan speed: 8.00° / min Divergence slit: 1° Divergence vertical limit slit: 10mm Scattering slit: 8mm Receiving slit: 13mm

[0133] <Measurement of average primary particle size> Using a commercially available SEM device, SEM images of the ALPO molecular sieves of each Example and Comparative Example were measured. The particle diameters of 100 or more randomly selected primary particles of the ALPO molecular sieve were measured, and the average was calculated to obtain the average particle diameter. The particle diameter was determined by the height dimension of the hexagonal columnar ALPO particles. The results are shown in Table 1.

[0134] <Evaluation of HC adsorption amount after hydrothermal durability> As a hydrothermal durability treatment, rich gas and lean gas were alternately passed through the ALPO molecular sieves of each of the examples and comparative examples prepared above for 10 hours at 900°C, with switching every 10 minutes. The rich gas had a composition of CO: 5%, water: 10%, and N2: balance, and the lean gas had a composition of O2: 2.5%, water: 10%, and N2: balance.

[0135] 1.0 g of the ALPO molecular sieve of each Example and Comparative Example that had been subjected to the hydrothermal durability treatment was weighed out and transferred to a tablet molding machine with a diameter of 35 mm. This was compressed for 1 minute at a pressure of 26 MPa using a hydraulic hand press (TP-40 manufactured by HERZOG) to prepare a disk-shaped sample. This disk-shaped sample was roughly crushed in a mortar, and the crushed material was passed through a sieve with a mesh size of 1 mm and a sieve with a mesh size of 0.5 mm in sequence. As a result, pellet samples with a size of 0.5 mm to 1 mm were obtained.

[0136] A pellet sample of 0.5 g in dry weight was placed in the adsorption apparatus. Pretreatment was performed by increasing the temperature to 500°C at a rate of 25°C / min to remove HCs and water remaining in the pores of the ALPO molecular sieve. Next, the adsorption apparatus was cooled to 100°C, and 3000 ppmC decane (C 10 H 22 A mixed gas containing 100% N2 and 3% water was passed through the adsorption device at a flow rate of 5 L / min for 15 minutes. After that, the gas was switched to 100% N2 and passed for 5 minutes. After that, the temperature was increased to 550°C at a rate of 20°C / min while still passing N2. This caused the decane adsorbed on the ALPO to be desorbed. The amount of decane adsorbed on the ALPO molecular sieve (mg / g) was calculated by integrating the amount of desorbed decane. The results are shown in Figure 10.

[0137] [Table 1]

[0138] From the results of Table 1 and Figure 10, it can be seen that when the crystallite diameter of the ALPO molecular sieve is 360 Å or more, the amount of HC adsorption increases rapidly. The HC purification performance during cold start is highly dependent on the HC adsorption ability of the HC adsorbent, since the catalyst metal is not heated to its activation temperature. Therefore, the results of Figure 10 indicate that when the crystallite diameter of the ALPO molecular sieve is 360 Å or more, the HC purification performance during cold start after hydrothermal durability is particularly high.

[0139] <Production of exhaust gas purification catalyst> Example 2-1 A honeycomb substrate (made of cordierite, diameter 105.7 mm, total length 74.7 mm) was prepared. The ALPO molecular sieve prepared in Example 1-1 above, a binder, and ion-exchanged water were mixed to prepare an ALPO-containing slurry. This ALPO-containing slurry was poured into the substrate, and unnecessary portions were blown off with a blower to perform coating. This was fired in an electric furnace to form a lower layer containing the ALPO molecular sieve on the substrate. The coating amount of the lower layer was 50 g / L for the ALPO molecular sieve and 8.1 g / L for the binder. The coating width of the lower layer was 100% of the total length of the substrate.

[0140] Platinum nitrate, CeO2-ZrO2 composite powder (i.e., OSC material), Al2O3 powder, barium sulfate, binder, and ion-exchanged water were mixed to prepare a Pt-containing slurry. This Pt-containing slurry was poured onto the substrate, and the unnecessary parts were blown away with a blower to coat the substrate. This was then fired in an electric furnace to form an intermediate layer containing a Pt catalyst on the lower layer. The coating amount of the intermediate layer was 0.85 g / L for Pt, 26 g / L for OSC material, 26 g / L for Al2O3 powder, 8 g / L for barium sulfate, and 1.2 g / L for binder. The coating width of the intermediate layer was 100% of the total length of the substrate.

[0141] Rh-containing slurry was prepared by mixing rhodium nitrate, CeO2-ZrO2 composite powder (i.e., OSC material), Al2O3 powder, binder, and ion-exchanged water. This Rh-containing slurry was poured into the substrate on which the intermediate layer was formed, and unnecessary parts were blown off with a blower to perform coating. This was fired in an electric furnace to form an upper layer containing a Rh catalyst on the intermediate layer. The coating amount of the upper layer was 0.14 g / L of Rh, 40 g / L of OSC material, 70 g / L of Al2O3 powder, and 0.7 g / L of binder. The coating width of the upper layer was 100% of the entire length of the substrate. In this way, the exhaust gas purification catalyst of Example 2-1 was obtained.

[0142] Comparative Example 2-1 The exhaust gas purification catalyst of Comparative Example 2-1 was prepared in the same manner as in Example 2-1, except that the lower layer containing the ALPO molecular sieve was not formed. Therefore, the exhaust gas purification catalyst of Comparative Example 2-1 had a two-layer structure having a lower layer containing a Pt catalyst and an upper layer containing a Rh catalyst.

[0143] Comparative Example 2-2 The catalyst for exhaust gas purification of Comparative Example 2-2 was prepared in the same manner as in Example 2-1, except that BEA type zeolite was used instead of the ALPO molecular sieve prepared in Example 1-1. Therefore, the zeolite used in the catalyst for exhaust gas purification of Comparative Example 2-2 contained Si.

[0144] Comparative Example 2-3 The catalyst for exhaust gas purification of Comparative Example 2-3 was prepared in the same manner as in Example 2-1, except that the ALPO molecular sieve prepared in Comparative Example 1-1 was used instead of the ALPO molecular sieve prepared in Example 1-1. The catalyst for exhaust gas purification of Comparative Example 2-3 contained the ALPO molecular sieve having a general crystallite size.

[0145] [Hydrothermal durability treatment] Rich gas and lean gas were alternately passed through the exhaust gas purification catalysts of Example 2-1 and Comparative Examples 2-1 to 2-3 for 10 hours at 900° C. while switching every 10 minutes. The rich gas had a composition of CO: 5%, water: 10%, and N2 (balance), and the lean gas had a composition of O2: 2.5%, water: 10%, and N2 (balance).

[0146] [Evaluation of catalytic activity against HC] The catalysts for exhaust gas purification of Example 2-1 and Comparative Examples 2-1 to 2-3, which had been subjected to the hydrothermal durability treatment, were heated from 100°C to 500°C at a rate of 20°C / min while passing pretreatment gas A, and held at 500°C for 5 minutes. Then, the temperature was lowered to 100°C while passing inert gas (N2 gas). After the temperature was stabilized, the catalysts were heated to 550°C at a rate of 50°C / min while passing reaction gas A, and the temperature at which the purification rate of HC in the reaction gas reached 50% (HC50% purification temperature: T50) was determined. The following gases were used as pretreatment gas A and reaction gas A. A graph of the HC50% purification temperature of Example 2-1 and Comparative Examples 2-1 to 2-3 is shown in FIG. 11. Pretreatment gas A A / F ratio: 14.6; C3H6:2400ppmC, C3H8:600ppmC, CO:0.5%, NO: 800ppm, H2O: 10%, CO2: 10%, O2: 0.6%, N2: balance Reactive gas A A / F ratio: 14.5; C3H6: 1500ppmC,C 10 H 22 :1500ppmC, H2O:3%, CO2: 10%, O2: 0.3%, N2: balance

[0147] From the results of FIG. 11, it can be seen that the use of ALPO molecular sieve having 12-membered ring as HC adsorbent improves HC purification performance after hydrothermal durability. It can also be seen that the exhaust gas purification catalyst of Example 2-1, in which the crystallite size of ALPO molecular sieve is intentionally enlarged, has a lower HC50% purification temperature and higher HC purification performance than the exhaust gas purification catalyst of Comparative Example 2-3, in which ALPO molecular sieve with a general crystallite size is used. On the other hand, when zeolite was used as HC adsorbent, the HC purification performance after hydrothermal durability was poor. This is because Si contained in zeolite migrated to the catalyst layer during hydrothermal durability and poisoned the catalyst metal.

[0148] <Evaluation of HC purification performance through vehicle testing> Example 3-1 [First catalyst] A honeycomb substrate (made of cordierite, diameter 117 mm, total length 100 mm) was prepared. Palladium nitrate, CeO2-ZrO2 composite powder (i.e., OSC material), Al2O3 powder, barium sulfate, binder, and ion-exchanged water were mixed to prepare a Pd-containing slurry. This Pd-containing slurry was poured into the substrate, and unnecessary parts were blown off with a blower to coat the substrate. This was fired in an electric furnace to form a lower layer containing a Pd catalyst on the substrate. The coating amount of the lower layer was 2.0 g / L of Pd, 45 g / L of OSC material, 72 g / L of Al2O3 powder, 6 g / L of barium sulfate, and 2.4 g / L of binder. The coating width of the lower layer was 100% of the total length of the substrate.

[0149] Rh-containing slurry was prepared by mixing rhodium nitrate, CeO2-ZrO2 composite powder (i.e., OSC material), Al2O3 powder, binder, and ion-exchanged water. This Rh-containing slurry was poured onto the substrate on which the lower layer had been formed, and unnecessary parts were blown away with a blower to perform coating. This was fired in an electric furnace to form an upper layer containing a Rh catalyst on the lower layer. The coating amount of the upper layer was 0.14 g / L of Rh, 40 g / L of OSC material, 70 g / L of Al2O3 powder, and 0.7 g / L of binder. The coating width of the upper layer was 100% of the total length of the substrate. In this way, the first catalyst was obtained.

[0150] [Second catalyst] A honeycomb substrate (made of cordierite, diameter 105.7 mm, total length 74.7 mm) was prepared. The ALPO molecular sieve prepared in Example 1-1 above, a binder, and ion-exchanged water were mixed to prepare an ALPO-containing slurry. This ALPO-containing slurry was poured into the substrate, and unnecessary portions were blown off with a blower to perform coating. This was fired in an electric furnace to form a lower layer containing the ALPO molecular sieve on the substrate. The coating amount of the lower layer was 50 g / L for ALPO and 8.1 g / L for the binder.

[0151] A Pt-containing slurry was prepared by mixing platinum nitrate, CeO2-ZrO2 composite powder (i.e., OSC material), Al2O3 powder, barium sulfate, binder, and ion-exchanged water. This Pt-containing slurry was poured onto the substrate, and the unnecessary parts were blown away with a blower to coat the substrate. This was then fired in an electric furnace to form an intermediate layer containing a Pt catalyst on the lower layer. The coating amount of the intermediate layer was 0.85g / L for Pt, 26g / L for OSC material, 26g / L for Al2O3 powder, 8g / L for barium sulfate, and 1.2g / L for binder.

[0152] Rh-containing slurry was prepared by mixing rhodium nitrate, CeO2-ZrO2 composite powder (i.e., OSC material), Al2O3 powder, binder, and ion-exchanged water. This Rh-containing slurry was poured onto the substrate on which the intermediate layer was formed, and unnecessary parts were blown away with a blower to coat the substrate. This was then fired in an electric furnace to form an upper layer containing the Rh catalyst on the intermediate layer. The coating amount of the upper layer was 0.21 g / L for Rh, 50 g / L for OSC material, 35 g / L for Al2O3 powder, and 1.6 g / L for binder. In this way, the second catalyst was obtained.

[0153] [Vehicle testing] The first and second catalysts were installed as a catalyst system in a vehicle equipped with a gasoline engine. The first catalyst was housed in a housing and installed at the start-up catalyst position, and the second catalyst was housed in a housing and installed at the underfloor catalyst position. A THC meter was installed downstream of the second catalyst. The vehicle was driven on a chassis dynamometer according to the WLTC mode, and the THC emitted in the LOW phase (WLTC mode 0s to 600s region) was integrated to determine the amount of HC emissions (mg / km) in the cold region. The results are shown in Figure 12.

[0154] Comparative Example 3-1 A second catalyst was prepared in the same manner as in Example 3-1, except that the lower layer containing the ALPO molecular sieve was not formed. A vehicle test was carried out in the same manner as in Example 3-1, except that this second catalyst was used. The results are shown in FIG.

[0155] Comparative Example 3-2 A second catalyst was prepared in the same manner as in Example 3-1, except that BEA-type zeolite was used instead of the ALPO molecular sieve prepared in Example 1-1. A vehicle test was performed in the same manner as in Example 3-1, except that this second catalyst was used. The results are shown in FIG.

[0156] Comparative Example 3-3 A second catalyst was prepared in the same manner as in Example 3-1, except that the ALPO molecular sieve prepared in Comparative Example 1-1 was used instead of the ALPO molecular sieve prepared in Example 1-1. A vehicle test was carried out in the same manner as in Example 3-1, except that this second catalyst was used. The results are shown in FIG.

[0157] As shown in FIG. 12, Example 3-1 using ALPO molecular sieve with a crystallite diameter of 360 Å or more had the smallest HC emission amount, and therefore the highest HC purification performance. When Comparative Example 3-1 using BEA-type zeolite is used as a reference, the reduction in the emission amount in Comparative Example 3-1 using BEA-type zeolite was 4 mg / km. On the other hand, the reduction in the emission amount in Example 3-1 was 5 mg / km. Thus, in Example 3-1, the emission amount was reduced by 25% compared to Comparative Example 3-1 using BEA-type zeolite. In addition, in the vehicle test, the effect of improving the HC purification performance by increasing the crystallite diameter of the ALPO molecular sieve was significantly observed.

[0158] Although several embodiments of the present invention have been described above, the above embodiments are merely examples. The present invention can be implemented in various other forms. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modified form, and it is also possible to add another modified form to the above-mentioned embodiment. Furthermore, if a technical feature is not described as essential, it is also possible to delete it as appropriate.

Claims

1. A substrate; An exhaust gas purification layer provided on the substrate; An exhaust gas purifying catalyst comprising: The exhaust gas purification layer contains a catalytic metal and a molecular sieve that is substantially free of Si as a hydrocarbon adsorbent, The molecular sieve substantially free of Si is an aluminophosphate molecular sieve having a 12-membered ring; The crystallite diameter of the aluminophosphate molecular sieve, as determined by X-ray diffraction measurement, is 360 Å to 700 Å; Catalyst for purifying exhaust gas.

2. 2. The exhaust gas purifying catalyst according to claim 1, wherein the crystallite diameter of the aluminophosphate molecular sieve is 360 Å to 400 Å.

3. 2. The exhaust gas purifying catalyst according to claim 1, wherein the crystallite diameter of the aluminophosphate molecular sieve is 450 Å to 600 Å.

4. 2. The exhaust gas purifying catalyst according to claim 1, wherein the aluminophosphate molecular sieve has an AFI type framework structure.

5. 2. The exhaust gas purifying catalyst according to claim 1, wherein the exhaust gas purifying layer comprises an HC adsorption layer containing the molecular sieve substantially free of Si, and a catalyst layer containing the catalytic metal.

6. 6. The exhaust gas purifying catalyst according to claim 5, wherein the HC adsorption layer and the catalyst layer are laminated, and the HC adsorption layer is located closer to the substrate than the catalyst layer.

7. In the catalyst layer, a first partial catalyst layer and a second partial catalyst layer are laminated, the first partial catalytic layer is located closer to the substrate than the second partial catalytic layer, the first partial catalytic layer and the second partial catalytic layer each contain the catalytic metal, the first partial catalyst layer contains an oxidation catalyst as the catalytic metal, The exhaust gas purifying catalyst according to claim 6 , wherein the second partial catalyst layer contains a reduction catalyst as the catalytic metal.

8. A hydrocarbon adsorbent comprising an aluminophosphate molecular sieve, The aluminophosphate molecular sieve has a 12-membered ring, The aluminophosphate molecular sieve has a crystallite diameter of 360 Å to 700 Å as determined by X-ray diffraction measurement.

Citation Information

Patent Citations

  • Catalyst for catalytically reducing nox

    JP1993261289A

  • Hydrocarbon adsorbent for exhaust gas and exhaust emission control catalyst using the same

    JP2004116331A

  • Combined scr and pna for cold emission control

    JP2018501949A

  • Exhaust gas purification catalyst

    JP2019063733A

  • Exhaust gas purification catalyst

    JP7446541B1