Manufacturing method of martensitic stainless steel strip and martensitic stainless steel strip

The method enhances martensitic stainless steel strips' fatigue and mechanical properties by controlling residual stress and retained austenite through quenching, tempering, and heat-retaining conveyance in a non-oxidizing gas atmosphere, resulting in improved tensile strength and uniform residual stress.

JP7581621B2Active Publication Date: 2024-11-13PROTERIAL LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020010550
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-27
Publication Date
2024-11-13
Estimated Expiration
2040-01-27

AI Technical Summary

Technical Problem

Existing martensitic stainless steel strips used in high-pressure compressor valves lack sufficient fatigue and mechanical properties, and existing manufacturing methods struggle to control residual stress uniformly and maintain productivity.

Method used

A manufacturing method involving quenching and tempering processes in a non-oxidizing gas atmosphere, with a heat-retaining conveyance step to control retained austenite content and residual stress, ensuring a martensitic structure with specific compositional ranges of C and Cr, and continuous processing to maintain productivity.

Benefits of technology

The method produces a martensitic stainless steel strip with enhanced fatigue properties and mechanical strength, achieving tensile strengths of 1600-2300 MPa and improved residual stress uniformity without reducing productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581621000001
    Figure 0007581621000001
  • Figure 0007581621000002
    Figure 0007581621000002
  • Figure 0007581621000003
    Figure 0007581621000003
Patent Text Reader

Abstract

To provide a martensitic stainless steel strip having fatigue characteristics and mechanical strength superior to those of conventional products, and a method capable of easily producing the martensitic stainless steel strip.SOLUTION: A martensitic stainless steel strip contains C: 0.3-1.2% and Cr: 10.0-18.0% by mass, and has a thickness of 1 mm or less. A method for producing the steel strip includes: a quenching step in which a steel strip is passed through a quenching furnace and heated to a quenching temperature and then cooled to a temperature of Ms point or lower; a thermal insulation conveying step in which the steel strip cooled to a temperature of Ms point or lower in the quenching step is conveyed to a tempering furnace while keeping it warm so that the temperature does not fall to a temperature of less than 80°C; and a tempering step in which the steel strip conveyed while keeping it warm so that the temperature does not fall to a temperature of less than 80°C in the thermal insulation conveying step is passed through the tempering furnace in a non-oxidizing gas atmosphere and heated to a tempering temperature. The martensitic stainless steel strip has a retained austenite amount of 10-25 vol.%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a martensitic stainless steel strip, and to a martensitic stainless steel strip. [Background technology]

[0002] Martensitic stainless steel strips have excellent corrosion resistance, hardness, and fatigue properties, and are used in a wide range of applications, such as for blades and for materials that are subjected to repeated stress, such as spring materials, valve materials, and cover materials. In particular, for applications as spring materials and valve materials, martensitic stainless steel strips with sufficiently high fatigue strength are required to suppress fatigue failure due to repeated stress.

[0003] In order to improve the fatigue strength of the martensitic stainless steel strip as described above, various proposals have been made in the past. For example, in the cited document 1, a spring steel strip having good durability, characterized by being composed of, in weight percent, C: 0.35-0.45%, Si: 0.10-0.50%, Mn: 0.10-0.50%, Cr: 10-15%, Mo: 1.0-1.5%, P: 0.05% or less, S: 0.005% or less, O: 0.002% or less, N: 0.02% or less, Al: 0.005% or less, Ti: 0.01% or less, and the balance being substantially Fe, is described in order to obtain a spring steel strip having a fatigue limit improved compared to the conventional ones.

[0004] Patent Document 2 also describes a flapper valve body made of martensitic stainless steel having compressive residual stress on the plate surface and having a solid solution nitrogen concentrated layer in the plate surface layer portion in order to improve the corrosion resistance and fatigue properties of the flapper valve body. Here, Patent Document 2 also describes that the residual stress on the surface of the martensitic stainless steel can be adjusted to compressive stress by heating to a temperature at which the stainless steel transforms into austenite single phase and then quenching in an atmosphere containing 20% ​​or more nitrogen and 10% or less (including 0%) oxygen (percentages are by volume).

[0005] Furthermore, in Patent Document 3, the applicant has proposed a manufacturing method for martensitic stainless steel strip, with the aim of suppressing shape defects without reducing productivity, which successively carries out the following steps: an unwinding process of unwinding a martensitic stainless steel strip having a thickness of 1 mm or less; a quenching process of passing the steel strip through a quenching furnace in a non-oxidizing gas atmosphere to heat it and then cool it; a tempering process of passing the quenched steel strip through a tempering furnace in a non-oxidizing gas atmosphere to temper it; and a coiling process of coiling the tempered steel strip, wherein the quenching furnace during the quenching process has at least a heating section and a holding section. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 4-48050 [Patent Document 2] Japanese Patent Application Publication No. 10-274161 [Patent Document 3] JP 2018-111881 A Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, compressors for air conditioners have become highly compressed, and valves used in compressors are also required to have improved fatigue and mechanical properties to accommodate the increased pressure. The invention of Patent Document 1 is an invention that can improve the fatigue limit of steel strips, but depending on the usage environment, the fatigue limit may be insufficient, and there is still room for further improvement. The invention described in Patent Document 2 is an invention that specifies the compressive residual stress due to the nitrogen-enriched layer formed on the plate surface, but it is difficult to uniformly form the nitrogen-enriched layer on the edge and outer periphery of the valve shape, and there is a possibility that the desired residual stress cannot be obtained. Furthermore, since the formation range of the nitrogen-enriched layer differs depending on the thickness of the material, the amount of gas and the composition of the gas must be changed every time the plate thickness changes, and there is a concern that productivity will decrease. Patent Document 3 is an excellent invention that can obtain a martensitic stainless steel strip with excellent flatness without decreasing productivity, but there is no description regarding the improvement of fatigue and mechanical properties, and there is still room for consideration. Therefore, the object of the present invention is to provide a martensitic stainless steel strip with superior fatigue properties and mechanical strength compared to conventional products, and a manufacturing method that can easily manufacture the martensitic stainless steel strip. [Means for solving the problem]

[0008] The present invention has been made in view of the above-mentioned problems. That is, one embodiment of the present invention is a method for producing a martensitic stainless steel strip, which comprises a quenching process in which a steel strip containing, by mass, 0.3 to 1.2% C and 10.0 to 18.0% Cr and having a thickness of 1 mm or less is passed through a quenching furnace in a non-oxidizing gas atmosphere to be heated to the quenching temperature and then cooled to a temperature below the Ms point, a heat-retaining and transporting process in which the steel strip cooled to a temperature below the Ms point in the quenching process is transported to a tempering furnace while maintaining the temperature so that it does not drop below 80°C, and a tempering process in which the steel strip transported in the heat-retaining and transporting process while maintaining the temperature so that it does not drop below 80°C is passed through a tempering furnace in a non-oxidizing gas atmosphere and heated to the tempering temperature.

[0009] Another aspect of the present invention is a martensitic stainless steel strip having a thickness of 1 mm or less and containing, by mass, 0.3 to 1.2% C and 10.0 to 18.0% Cr, and having a martensitic structure, wherein the amount of retained austenite in the martensitic stainless steel strip is 10 to 25 volume %, the tensile strength is 1600 MPa or more and 2300 MPa or less, and the proof stress ratio, which is the ratio of 0.2% proof stress to tensile strength, is 75% or less. Preferably, the ratio of compressive residual stress in the width direction to the compressive residual stress in the rolling direction of the martensitic stainless steel strip is 75% or more. Effect of the Invention

[0010] According to the present invention, it is possible to obtain a martensitic stainless steel strip having superior fatigue properties and mechanical properties to conventional products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. However, the present invention is not limited to the embodiments described here, and appropriate combinations and improvements can be made without departing from the technical idea of ​​the invention. The present invention is applicable to those having a martensitic stainless steel composition. Although the composition range is not limited, for example, the composition of the steel strip of the present invention preferably contains, in mass%, C: 0.3 to 1.2%, and Cr: 10.0 to 18.0%. Furthermore, the chemical composition of the steel strip of the present invention is preferably martensitic stainless steel, which is C: 0.3 to 1.2% (more preferably 0.3 to 1.0%, and even more preferably 0.3 to 0.8%), Si: 1% or less, Mn: 2% or less, Mo: 3.0% or less (more preferably 2.5% or less, and even more preferably 2.0% or less), Ni: 1.0% or less (including 0%), Cr: 10.0 to 18.0% (more preferably 11.0% to 16.0%, and even more preferably 12.0% to 15.0%), the balance being Fe and unavoidable impurities.

[0012] First, the manufacturing method of the martensitic stainless steel strip of the present invention will be described. The present invention is a manufacturing method of the martensitic stainless steel strip, which includes a quenching step in which a steel strip with a thickness of 1 mm or less is passed through a quenching furnace in a non-oxidizing gas atmosphere, heated, and then cooled; a warming conveying step in which the steel strip after the quenching step is conveyed to a tempering furnace while being kept at a temperature not lowered below 80°C (in other words, while being kept at a temperature range of 80°C or higher and below the Ms point or below the tempering temperature); and a tempering step in which the steel strip conveyed in the warming conveying step is passed through a tempering furnace in a non-oxidizing gas atmosphere and tempered. The above-mentioned quenching step, warming conveying step, and tempering step may be performed consecutively, and other steps such as a preheating step may be added as long as they do not impair the effects of the present invention. The manufacturing method of the embodiment of the present invention will be described below.

[0013] (Quenching process) In this embodiment, the prepared steel strip is passed through a quenching furnace in a non-oxidizing gas atmosphere to heat it, and then a quenching process is performed to cool the steel strip. Before being transported to this quenching furnace, the rolled steel strip wound in a coil shape may be loaded onto an unwinder, and an unwinding process may be performed to transport the steel strip to the quenching furnace. The set heating temperature in this quenching furnace is preferably 850 to 1200°C. If it is less than 850°C, the solid solution of carbides tends to be insufficient. On the other hand, if it is more than 1200°C, the amount of solid solution of carbides tends to increase, and the hardness during tempering tends to decrease. The temperature of the quenching furnace may be set to a constant temperature from the inlet to the outlet of the furnace, and at least one of a temperature increasing section and a temperature decreasing section may be provided before and after a holding section where quenching is performed at a constant temperature.

[0014] In order to further improve production efficiency, the present invention may provide a preheating step between the unwinding step and the quenching step. In the preheating step, an existing heating device can be used, but it is preferable to use an induction heating device that allows for rapid heating of the steel strip. The preheating temperature in the preheating step is preferably set to 600° C. or higher to ensure effective preheating, but is preferably set to less than 800° C. to more reliably suppress deformation due to a rapid temperature rise.

[0015] The steel strip heated in the quenching furnace is then quenched. As the quenching method, a salt bath, molten metal, oil, water, polymer aqueous solution, saline solution, or gas can be used. Preferably, a spray cooling method in which water is sprayed, or a gas cooling method in which a non-oxidizing gas is used is used. When gas cooling is selected as the quenching method, the non-oxidizing gas is preferably hydrogen, helium, nitrogen, argon, or a mixed gas of hydrogen. In this quenching step, the temperature of the steel strip is cooled to the Ms point or below, but in order to obtain the effect of the heat-retaining transport step described below, the temperature of the steel strip is adjusted so that it does not drop below 80°C. In addition, the quenching step may be a two-stage quenching step in which quenching and slow cooling are combined to avoid pearlite nose. For example, after a primary cooling step in which the steel strip is cooled to a temperature above the Ms point but below 350°C by spray cooling, a secondary cooling step is preferably performed in which the steel strip is restrained by a water-cooled platen so as to sandwich the steel strip and cooled to the Ms point or below while correcting the shape.

[0016] (Insulation transport process) In the present embodiment, a heat-retaining and conveying process is then carried out in which the steel strip after the quenching process is conveyed to a tempering furnace while being kept at a temperature so that the temperature does not fall below 80°C. By providing this process, the amount of residual austenite in the steel strip and the compressive residual stress in the surface layer of the steel strip can be increased, and the effect of improving fatigue strength can be obtained. If the temperature during the heat-retaining and conveying process is less than 80°C, it is difficult to obtain a desired amount of residual austenite. In addition, although the steel strip in the heat-retaining and conveying process is cooled to a temperature below the Ms point by the above-mentioned quenching process, it is possible that the temperature may rise above the Ms point due to subsequent reheating or the like. However, it should be avoided that the temperature exceeds the tempering temperature set in the next tempering process. Including such a case, if the temperature during heat-retaining becomes too high (e.g., above 300°C), the quenching hardness tends to decrease. As a method of keeping the steel strip warm in this heat-insulating transport step, for example, a metal cover with a heat insulating material or a tunnel furnace or the like may be installed between the quenching furnace and the tempering furnace as a heat-insulating equipment, and the steel strip may be transported so as to pass through the above-mentioned cover or furnace. The heat insulating material may be an existing inorganic fiber-based or plastic-based heat insulating material. Although an existing equipment may be used for the tunnel furnace, it is preferable to use a gas atmosphere furnace in order to obtain a higher surface oxidation prevention effect and an effect of more stabilizing the steel strip temperature during transport. Ideally, it is most preferable that the above-mentioned heat-insulating equipment is directly connected to the outlet of the quenching equipment and the inlet of the tempering furnace after quenching, but as long as the temperature of the steel strip does not become less than 80°C before it is passed through the tempering furnace, a gap may be provided between the quenching equipment and the tempering furnace and the heat-insulating equipment. In this embodiment, a continuous furnace is applied to the quenching furnace and the tempering furnace described later, but the present invention can also be implemented when the quenching furnace and the tempering furnace are batch furnaces.

[0017] (Tempering process) In this embodiment, the steel strip after the warming and conveying process is tempered in a tempering furnace in a non-oxidizing gas atmosphere to adjust the steel strip to a desired hardness. The temperature of this tempering furnace can be set to a desired temperature depending on the application. For example, if a higher hardness characteristic is required, it can be set to 200 to 300 ° C. In addition, in order to improve the shape workability such as press working, it can be set to 300 ° C. to 400 ° C. If the sheet passing speed in the tempering process is too fast, there is a possibility that the above-mentioned temperature range will not be reached. Therefore, when the time required for the steel strip to pass through the tempering furnace is M [min] and the sheet thickness of the steel strip is t [mm], it is preferable to set M / t to 5 to 9. It is preferable to perform the above-mentioned quenching process, warming conveying process, and tempering process continuously, since it is possible to obtain a steel strip having excellent mechanical properties and fatigue strength without reducing productivity.

[0018] The steel strip after the tempering process may be subjected to a polishing process to remove surface scale from the steel strip. As the polishing method, a mechanical polishing such as grindstone polishing, belt polishing, brush polishing, buff polishing, etc. may be selected. Among them, the application of buff polishing is preferable because it is possible to remove surface scale without causing significant damage to the surface of the steel strip.

[0019] Next, the martensitic stainless steel strip of this embodiment will be described. One of the features of the martensitic stainless steel strip of this embodiment is that the amount of retained austenite is 10 to 25% by volume. The amount of retained austenite in the steel strip after quenching has generally been reduced in order to improve mechanical properties. In the present invention, by making the amount of retained austenite in the steel strip after quenching and tempering 10% by volume or more, it is possible to suppress crack progression in the steel strip and significantly increase fatigue strength properties without significantly deteriorating the mechanical properties of the steel strip. On the other hand, if the amount of retained austenite is too large, the mechanical properties tend to be significantly degraded, so the upper limit of the amount of retained austenite is set to 25% by volume. The lower limit of the amount of retained austenite is preferably 12% by volume, and the upper limit of the amount of retained austenite is preferably 20% by volume. In the method of measuring the amount of retained austenite in this embodiment, an X-ray diffractometer is used, and the amount of retained austenite (volume %) is derived from the obtained diffracted X-ray intensity distribution.

[0020] The steel strip of this embodiment has a tensile strength of 1600 MPa or more and 2300 MPa or less in order to further improve the durability of the product. A more preferable lower limit of the tensile strength is 1700 MPa, and a more preferable upper limit of the tensile strength is 2200 MPa. An even more preferable upper limit of the tensile strength is 2000 MPa. The steel strip of this embodiment also has a yield strength ratio, which is the ratio of 0.2% yield strength to tensile strength, of 75% or less while satisfying the above tensile strength range. By setting the yield strength ratio at this level, it is possible to impart appropriate toughness to the steel strip and further improve the fatigue strength. There is no particular limit to the lower limit of the yield strength ratio, but since a yield strength ratio that is too low tends to cause a decrease in mechanical properties such as hardness, it can be set to, for example, 50% or more.

[0021] In the steel strip of this embodiment, the ratio of the compressive residual stress in the width direction to the compressive residual stress in the rolling direction of the martensitic stainless steel strip is preferably 75% or more. As a result, the steel strip of the present invention has small anisotropy of the compressive residual stress, making it possible to suppress the variation in characteristics depending on the cutting direction. This effect is particularly effective for a flapper valve having a rotationally symmetrical shape with a plurality of radially arranged leads. Preferably, the ratio of the compressive residual stress in the width direction to the compressive residual stress in the rolling direction is 77% or more. Although there is no particular limitation on the value of the compressive residual stress, in order to more reliably obtain the effect of improving fatigue strength, it is preferable that the lower limit of the compressive residual stress is 300 MPa. A more preferable lower limit of the compressive residual stress is 330 MPa, and an even more preferable lower limit of the compressive residual stress is 360 MPa. In this embodiment, the residual stress on the surface of the steel strip can be measured by an X-ray residual stress measuring device. In this embodiment, 2θ-sin 2 Residual stress is measured using the Ψ method. The direction perpendicular to the rolling direction is the direction perpendicular to the rolling direction, and corresponds to the width direction of a long steel strip when the length direction is the rolling direction.

[0022] The steel strip of this embodiment can be applied to a martensitic stainless steel strip having a thickness of 1 mm or less. As the thickness becomes thinner, there is a tendency for shape defects to occur more easily due to heating during quenching, so it is preferable to apply it to a martensitic stainless steel strip having a thickness of 0.5 mm or less. There is no particular need to set a lower limit for the thickness, but since it is difficult to manufacture a steel sheet produced by rolling if the thickness is too thin, it can be set to about 0.01 mm. A more preferable lower limit for the thickness is 0.05 mm, and an even more preferable lower limit for the thickness is 0.1 mm. . EXAMPLES

[0023] First, a martensitic stainless steel strip with a width of about 300 mm and a thickness of 0.15 mm was prepared. The composition is shown in Table 1. The prepared steel strip was wound in a coil shape, set on an unwinder 1, and unwound from the unwinder. The unwound steel strip was passed through a quenching furnace with an argon gas atmosphere and a temperature adjusted to 850°C to 1200°C. Next, a primary cooling was performed in which pure water was sprayed onto the steel strip from a coolant spraying device installed on the exit side of the quenching furnace to rapidly cool it, and then the steel strip was cooled to 290°C to 350°C, and a quenching process was performed in which the steel strip was pressed against a water-cooled platen to cool it to the Ms point (about 270°C) or lower by secondary cooling. The steel strip after the quenching process was subjected to a heat-retaining and conveying process in which it was passed through a rock wool tube as an example of the present invention, and the comparative example was not subjected to the heat-retaining and conveying process. Table 2 shows the temperatures of the steel strips of the present invention and the comparative example just before they were conveyed to the tempering furnace. The steel strip of the example of the present invention after the warming and conveying process and the steel strip of the comparative example after the quenching process were passed through a tempering furnace in an argon gas atmosphere and tempered at a temperature adjusted to about 350° C. Finally, the tempered steel strip was mechanically polished by buffing and wound up by a winding machine to produce the martensitic stainless steel strip of the example of the present invention.

[0024] [Table 1]

[0025] Next, the amount of retained austenite, residual stress, tensile strength, and 0.2% yield strength were measured for the samples of the invention and comparative examples. The amount of retained austenite was measured using a rotating anode type automatic X-ray diffractometer. Residual stress was measured using an AUTOMATE-II residual stress measuring device manufactured by Rigaku Corporation. Tensile strength and 0.2% yield strength were measured according to the method specified in JIS-Z2241, and JIS No. 13 B test pieces were used as test pieces. The results of the retained austenite and tensile tests are shown in Table 2, and the measurement results of the compressive residual stress are shown in Table 3.

[0026] [Table 2]

[0027] [Table 3]

[0028] As shown in Table 2, it was confirmed that samples No. 1 and No. 2, which underwent the warming transport process, had an increased amount of retained austenite compared to sample No. 11, which is a comparative example. It was also confirmed that the tensile strength was at the same level as the comparative example, but the yield strength ratio was lower than the comparative example. From these results, it can be seen that the examples of the present invention are advantageous in terms of improving fatigue strength while maintaining mechanical strength equivalent to that of conventional products. The compressive residual stress also showed a larger value than in the comparative example, and the compressive residual stress ratio was also higher. This means that there is less variation in compressive residual stress in the rolling direction and width direction. For example, when the material is applied to products such as flapper valve materials, improved productivity can be expected.

Claims

1. a quenching process in which a steel strip having a thickness of 1 mm or less and containing, by mass%, 0.3 to 1.2% C, 1% or less Si, 2% or less Mn, 3.0% or less Mo, 1.0% or less Ni, 12.0 to 15.0% Cr, the balance being Fe and unavoidable impurities, is passed through a quenching furnace in a non-oxidizing gas atmosphere, heated to a quenching temperature, and then cooled to a temperature not higher than the Ms point; a heat-retaining and transporting step of transporting the steel strip cooled to a temperature equal to or lower than the Ms point in the quenching step to a tempering furnace while maintaining the temperature so that the temperature does not fall below 80°C; A tempering process is performed in which the steel strip transported while being kept warm so that the temperature does not drop below 80°C in the warming transport process is passed through a tempering furnace in a non-oxidizing gas atmosphere and heated to a tempering temperature. The amount of retained austenite is 10 to 25 volume percent, The tensile strength is 1600 MPa or more and 2300 MPa or less, A method for producing a martensitic stainless steel strip, which produces a martensitic stainless steel strip having a proof stress ratio, which is the ratio of 0.2% proof stress to tensile strength, of 75% or less.

2. A martensitic stainless steel strip having a martensitic structure and a thickness of 1 mm or less, the martensitic stainless steel strip being, by mass%, 0.3 to 1.2% C, 1% or less Si, 2% or less Mn, 3.0% or less Mo, 1.0% or less Ni, 12.0 to 15.0% Cr, the balance being Fe and unavoidable impurities; The amount of retained austenite in the martensitic stainless steel strip is 10 to 25 volume %. the law of nature, The tensile strength is 1600 MPa or more and 2300 MPa or less, The yield strength ratio, which is the ratio of 0.2% yield strength to tensile strength, is 75% or less, The compressive residual stress in the width direction of the martensitic stainless steel strip relative to the compressive residual stress in the rolling direction is A martensitic stainless steel strip having a compression residual stress ratio of 75% or more.

Citation Information

Patent Citations

  • Spring steel strip

    JP1992048050A

  • High strength austenitic stainless steel plate for flapper valve, excellent in fatigue characteristic, and its production

    JP1998140294A

  • Flapper valve plug of compressor for air conditioner and its manufacture

    JP1998274161A

  • Annealed martensitic stainless steel excellent in strength, toughness, and spring characteristic

    JP2000129400A

  • Rolling apparatus

    JP2003213380A