Evaluation method for polyarylene sulfide resin

By measuring zeta potential under controlled pH conditions, the method addresses the challenge of accurately quantifying PAS resin reactivity, improving the evaluation of its interface reactions.

JP7582088B2Active Publication Date: 2024-11-13DIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021102016
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-18
Publication Date
2024-11-13
Estimated Expiration
2041-06-18

AI Technical Summary

Technical Problem

Existing methods for evaluating polyarylene sulfide (PAS) resins fail to consider the functional groups at the molecular ends, which significantly affect reactivity, and lack accurate quantification of these groups due to high polymerization temperatures and pressures, leading to variations in interface reactivity.

Method used

A method involving the measurement of zeta potential using a streaming potential technique to evaluate PAS resins, focusing on the surface properties under controlled pH conditions to quantify reactivity accurately.

Benefits of technology

This approach reduces variation and enhances the accuracy of evaluating PAS resin reactivity, allowing for better control of its interface reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582088000007
    Figure 0007582088000007
  • Figure 0007582088000001
    Figure 0007582088000001
  • Figure 0007582088000002
    Figure 0007582088000002
Patent Text Reader

Abstract

To provide a method for evaluating polyarylenesulfide resin that can homogeneously quantify the surface characteristics of polyarylenesulfide resin, and thus has less variation and more homogeneous reactivity than a conventional evaluation method.SOLUTION: The present disclosure is a method for evaluating polyarylenesulfide resin having a preparation step of preparing polyarylenesulfide resin, and an evaluation step of evaluating a test piece formed from at least part of the polyarylenesulfide resin. In the method for evaluating polyarylenesulfide resin, the evaluation step has a test piece manufacturing step of solidifying melted polyarylenesulfide resin obtained by melting the polyarylenesulfide resin to obtain the test piece, and a zeta potential measuring step of measuring the zeta potential of the surface of the test piece with a flow potential method.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating a polyarylene sulfide resin. [Background technology]

[0002] Polyarylene sulfide resins (hereinafter also referred to as "PAS resins"), such as polyphenylene sulfide resins (hereinafter referred to as "PPS resins"), are widely used in electrical and electronic parts, automobile parts, water-related parts, fibers, and film applications, etc., because of their excellent heat resistance and chemical resistance. The PAS resins used in the above applications are maximized in their functions by combining various additives such as glass fibers, fillers, and elastomers. Therefore, control of the reactivity of the interface between the PAS resin and additives such as glass fibers, and the reactivity between the elastomer and the PAS resin, is an essential technique for the functional expression of the resulting PAS resin (parts). For example, Patent Document 1 discloses a technique for a PAS resin that is more reactive with epoxysilane than conventional PAS resins. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 06-256517 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the technology of the above Patent Document 1 does not consider at all the functional groups at the molecular end of the PAS resin, which is a factor that greatly contributes to the reactivity of the interface between the PAS resin and a different material. In addition, PAS resin has a unique circumstance that it is polymerized under high temperature and high pressure of 200°C or more. As a result, many side reactions proceed during the polymerization of PAS resin, and various functional groups are mixed at the molecular end in the PAS resin, which greatly contributes to the reactivity. Furthermore, the high heat resistance / chemical resistance of PAS resin limits the analytical prescription, and the amount of various functional groups has not yet been quantified. Therefore, although controlling and evaluating the interfacial reactivity between PAS resin and different materials by using the molecular end structure of PAS resin is a technology with very high barriers, it is a technology that is in demand in various technical fields as various applications are expected.

[0005] Therefore, an object of the present disclosure is to provide a method for evaluating PAS resins that has less variation and more accurate reactivity than conventional evaluation methods that use the degree of viscosity increase by quantifying the surface characteristics of PAS resins. [Means for solving the problem]

[0006] In view of the above problems, the present inventors conducted intensive research and repeated experiments, and as a result, discovered that the above problems can be solved by evaluating the characteristics of PAS resin using the zeta potential value measured by the streaming potential method, thereby completing the present invention.

[0007] [1] The present disclosure relates to a method for producing a polyarylene sulfide resin, and evaluating a test piece formed from at least a portion of the polyarylene sulfide resin, The evaluation step includes a test piece preparation step of melting the polyarylene sulfide resin and solidifying the molten polyarylene sulfide resin to obtain the test piece; a zeta potential measuring step of measuring the zeta potential of the surface of the test piece by a streaming potential method; The method for evaluating a polyarylene sulfide resin is characterized by having the following: [2] A more preferred embodiment of the present disclosure includes a polymerization step for obtaining a polyarylene sulfide resin, a purification step of purifying the polyarylene sulfide resin; and an evaluation step of evaluating a test piece formed from at least a part of the purified polyarylene sulfide resin obtained through the purification step. Evaluation method And, the evaluation step includes a test piece preparation step of obtaining the test piece by solidifying a molten PAS resin obtained by melting the polyarylene sulfide resin; The method for evaluating a polyarylene sulfide resin comprises a zeta potential measurement step of measuring the zeta potential of the surface of the test piece under conditions of pH 3 to 9 by a streaming potential method. Effect of the Invention

[0008] According to the present disclosure, by evaluating the surface characteristics of a PAS resin using the zeta potential, the reactivity of the PAS resin can be grasped with less variability and higher accuracy than with evaluation methods using the degree of viscosity increase. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of a method for measuring zeta potential by the streaming potential method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The following describes in detail an embodiment of the present invention (hereinafter referred to as the "present embodiment"); however, the present invention is not limited to the following description and can be implemented in various modified forms within the scope of its gist.

[0011] [Evaluation method of polyarylene sulfide resin] The method for evaluating a PAS resin according to this embodiment includes a preparation step of preparing a PAS resin, and an evaluation step of evaluating a test piece made from at least a part of the PAS resin obtained in the preparation step. The evaluation step includes a test piece preparation step of melting the PAS resin obtained in the preparation step to prepare a molten PAS resin, and then solidifying the molten PAS resin to obtain the test piece, and a zeta potential measurement step of measuring the zeta potential of the surface of the test piece by a streaming potential method. In other words, the method for evaluating a PAS resin in this embodiment involves preparing a test piece as an evaluation sample from at least a portion of the prepared PAS resin for the purpose of evaluating the surface characteristics of the prepared PAS resin, and then measuring the zeta potential of the test piece using a streaming potential method to grasp the surface characteristics of the prepared PAS resin. This allows the surface characteristics of PAS resin to be quantified uniformly, making it possible to evaluate the reactivity of PAS resin with less variation and greater precision than conventional evaluation methods (e.g., the degree of viscosity increase using MFR, etc.). In the PAS resin evaluation method according to the present embodiment, the zeta potential measurement step preferably measures the zeta potential of the surface of the test piece under conditions of pH 3 to 9, more preferably pH 7.8 to 8.2. This not only reduces variation but also makes it easier to evaluate the properties of the PAS resin with higher accuracy. Furthermore, in a preferred embodiment of the method for evaluating a PAS resin according to the present embodiment, the method may further include a determination step of determining whether or not the zeta potential value of the surface of the test piece measured in the zeta potential measurement step under a range of predetermined pH conditions is within a specific range. The determination step will be described later, but for example, it is preferable to further include a determination step (2) of determining whether or not the zeta potential value of the surface of the test piece measured in the zeta potential measurement step under a range of pH 7.8 to 8.2 (e.g., pH=8.0) is within a range of -50 to -65 mV. This makes it possible to provide a PAS resin with excellent reactivity.

[0012] Each step of the method for evaluating a PAS resin according to this embodiment will be described below. "Preparation process" The preparation step in this embodiment is a step of preparing a PAS resin. The PAS resin prepared as the evaluation target in this embodiment is not particularly limited as long as it has a chemical structure in which a structure in which an aromatic ring and a sulfur atom are bonded is a repeating unit, and may be a PAS resin obtained by a known polymerization method, or a commercially available PAS resin. In addition, the known polymerization method is not particularly limited, and an example of the polymerization method is the polymerization method described in the section on the polymerization step below. (PAS resin) The chemical structure of the PAS resin used in the evaluation method of the present embodiment is specifically represented by the following general formula (1): [ka] (In the above general formula (1), R 1 and R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a nitro group, an amino group, a phenyl group, a methoxy group, or an ethoxy group.) and, if necessary, a structural portion represented by the following general formula (2): [ka] and a resin structure having as repeating units a trifunctional structural moiety represented by the general formula (2) in an amount of preferably 0.001 to 3 mol %, and particularly preferably 0.01 to 1 mol %, based on the total number of moles of the trifunctional structural moiety and other structural moieties.

[0013] Here, the structural portion represented by the general formula (1) is particularly R 1 and R 2 is preferably a hydrogen atom from the viewpoint of the mechanical strength of the PAS resin, and in that case, examples include those bonded at the para position represented by the following general formula (3) and those bonded at the meta position represented by the following general formula (4). [ka] Among these, a structure in which the bond between the sulfur atom and the aromatic ring in the repeating unit is at the para position represented by the general formula (3) is particularly preferred in terms of the heat resistance and crystallinity of the PAS resin.

[0014] The PAS resin may contain not only the structural moiety represented by the general formula (1) or (2) but also the structural moiety represented by the following general formulas (5) to (8): [ka] The structural moieties represented by the general formulae (1) and (2) may account for 30 mol % or less of the total of the structural moieties represented by the general formulae (1) and (2). In particular, in the present invention, it is preferred from the viewpoints of heat resistance and mechanical strength of the PAS resin that the structural moieties represented by the general formulae (5) to (8) account for 10 mol % or less. When the PAS resin contains the structural moieties represented by the general formulae (5) to (8), the bonding mode thereof may be either a random copolymer or a block copolymer.

[0015] The PAS resin may have naphthyl sulfide bonds or the like in its molecular structure, but the amount of such bonds is preferably 3 mol % or less, and particularly preferably 1 mol % or less, relative to the total number of moles including other structural portions. The physical properties of the PAS resin are not particularly limited as long as they do not impair the effects of the present invention, but are as follows. In the preparation step of the present embodiment, the PAS resin is preferably prepared by a polymerization step to obtain a PAS resin, and more preferably, the PAS resin is prepared by a polymerization step to obtain a PAS resin and a purification step to purify the PAS resin. In the present embodiment, an example of the polymerization step and the purification step will be described below.

[0016] (Polymerization process) In the present embodiment, the polymerization step for obtaining the PAS resin is not particularly limited, and a known polymerization method can be applied depending on the chemical structure of the PAS resin to be evaluated or the intended use of the PAS resin. In addition, as a preferred embodiment of the polymerization step in the present embodiment, specific polymerization conditions may be further applied under which the zeta potential value of the surface of a test piece, which is an evaluation sample formed from at least a part of the obtained PAS resin, is likely to be in the range of -50 to -65 mV at pH = 7.8 to 8.2 (e.g., pH = 8.0) or -30 to -45 mV at pH = 4.8 to 5.2 (e.g., pH = 5.0). Therefore, a general polymerization method applicable to this embodiment will be described below, and then specific polymerization conditions will be described in detail.

[0017] <Polymerization method> Representative examples of the polymerization method applicable to this embodiment include the following Production Method 1 to Production Method 4. (Production method 1): A method of polymerizing a dihalogenoaromatic compound in the presence of sulfur and sodium carbonate, and, if necessary, adding a polyhalogenoaromatic compound or other copolymerization components. (Production method 2): A method of polymerizing a dihalogenoaromatic compound in the presence of a sulfidizing agent or the like in a solvent (e.g., a polar solvent, an organic solvent, or a polar organic solvent) by adding, if necessary, a polyhalogenoaromatic compound or other copolymerization component (hereinafter, dihalogenoaromatic compounds). (Production method 3): Self-condensation of p-chlorothiophenol with other copolymerization components, if necessary (Production Method 4): A method of melt-polymerizing a diiodo aromatic compound and elemental sulfur under reduced pressure in the presence of a polymerization inhibitor which may have a functional group such as a carboxyl group or an amino group.

[0018] Among the above-mentioned Production Methods 1 to 4, the above-mentioned (Production Method 2) is preferred because it is versatile. During the reaction, an alkali metal salt of carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization. Among the above-mentioned (Production Method 2), a mixture containing dihalogeno aromatic compounds, a polar organic solvent, and a sulfidizing agent is charged into a reactor so that the ratio of (polar organic solvent) / (sulfidizing agent) is within the range of 0.02 / 1 to 0.9 / 1 (molar ratio), and the mixture is dehydrated by starting to increase the temperature in an open system under an inert gas atmosphere, and a solid is precipitated as the dehydration proceeds, and a low-water-containing solid in which each component is uniformly dispersed is obtained. The mixture is then cooled to a predetermined temperature, and if necessary, a polar organic solvent and / or a dihalogeno aromatic compound is further added to the low-water-containing solid, and the mixture is heated under an inert gas atmosphere. and a method in which a dihalogeno aromatic compound and, if necessary, a polyhalogeno aromatic compound or other copolymerization components are added in the presence of a solid alkali metal sulfide and an aprotic polar organic solvent, and an alkali metal hydrosulfide and an organic acid alkali metal salt are reacted while controlling the organic acid alkali metal salt in the range of 0.01 to 0.9 mol per mol of the sulfur source and the amount of water in the reaction system to 0.02 mol or less per mol of the aprotic polar organic solvent (see WO2010 / 058713 pamphlet).

[0019] The polymerization step of this embodiment will be described below by taking as an example a polymerization method using the above-mentioned Production Method 2, more specifically, a step of reacting at least one polyhalogeno aromatic compound and at least one sulfidizing agent in a polar solvent (e.g., a polar organic solvent) under appropriate polymerization conditions to obtain a reaction mixture (slurry) containing a PAS resin. This embodiment also includes a form in which the reaction mixture (slurry) is obtained by reacting the polyhalogeno aromatic compound and / or the organic solvent in the presence of a sulfidizing agent and an organic solvent while continuously or intermittently adding the polyhalogeno aromatic compound and / or the organic solvent.

[0020] -Raw materials- The polyhalogeno aromatic compound in this embodiment is a halogenated aromatic compound having two or more halogen atoms directly bonded to an aromatic ring, and among them, a halogenated aromatic compound having two halogen atoms is called a dihalogeno aromatic compound. Specific examples of the dihalogeno aromatic compound include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, 4,4'-dihalobenzophenone, 4,4'-dihalodiphenyl sulfone, 4,4'-dihalodiphenyl sulfoxide, 4,4'-dihalodiphenyl sulfide, and compounds having an alkyl group having 1 to 18 carbon atoms in the aromatic ring of each of the above compounds. The above dihalogeno aromatic compounds may be used alone or in combination of two or more. In addition, examples of polyhalogenoaromatic compounds other than dihalogenoaromatic compounds include 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, and 1,4,6-trihalonaphthalene. These compounds may be block copolymerized. Among the above specific examples, dihalogenated benzenes are preferred, and those containing 80 mol % or more of p-dichlorobenzene are particularly preferred. The above polyhalogenoaromatic compounds may be used alone or in combination of two or more. The halogen atoms contained in each of the above halogenoaromatic compounds are preferably chlorine atoms and / or bromine atoms.

[0021] In order to increase the viscosity of the PAS resin by forming a branched structure, a polyhalogenoaromatic compound having three or more halogen substituents in one molecule may be used as a branching agent as desired. Examples of such polyhalogenoaromatic compounds include 1,2,4-trichlorobenzene, 1,3,5-trichlorobenzene, and 1,4,6-trichloronaphthalene.

[0022] Further examples include polyhalogenoaromatic compounds having a functional group having active hydrogen, such as an amino group, a thiol group, or a hydroxyl group. Specific examples include dihaloanilines such as 2,6-dichloroaniline, 2,5-dichloroaniline, 2,4-dichloroaniline, and 2,3-dichloroaniline; trihaloanilines such as 2,3,4-trichloroaniline, 2,3,5-trichloroaniline, 2,4,6-trichloroaniline, and 3,4,5-trichloroaniline; dihaloaminodiphenyl ethers such as 2,2'-diamino-4,4'-dichlorodiphenyl ether and 2,4'-diamino-2',4-dichlorodiphenyl ether; and mixtures thereof in which the amino group is replaced with a thiol group or a hydroxyl group.

[0023] In addition, the hydrogen atom bonded to the carbon atom forming the aromatic ring in these active hydrogen-containing polyhalogenoaromatic compounds can be replaced with other inactive groups, for example, hydrocarbon groups such as alkyl groups, and the like. Among these various active hydrogen-containing polyhalogenoaromatic compounds, the active hydrogen-containing dihalogenoaromatic compounds are preferred, and dichloroaniline is particularly preferred.

[0024] Examples of polyhalogeno aromatic compounds having a nitro group include mono- or dihalonitrobenzenes such as 2,4-dinitrochlorobenzene and 2,5-dichloronitrobenzene; dihalonitrodiphenyl ethers such as 2-nitro-4,4'-dichlorodiphenyl ether; dihalonitrodiphenyl sulfones such as 3,3'-dinitro-4,4'-dichlorodiphenyl sulfone; mono- or dihalonitropyridines such as 2,5-dichloro-3-nitropyridine and 2-chloro-3,5-dinitropyridine; and various dihalonitronaphthalenes.

[0025] In this embodiment, since it is necessary that the PAS resin is dissolved in the organic solvent, the organic solvent used must be capable of dissolving the PAS resin under certain conditions. The condition for dissolving the PAS resin may be at room temperature or under heating, but with currently known solvents, heating to a certain temperature is required to dissolve PAS resins with a certain molecular weight or more. Examples of organic solvents capable of dissolving the PAS resin include N-methyl-2-pyrrolidone, formamide, acetamide, N-methylformamide, N,N-dimethylacetamide, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, tetramethylurea, N-dimethylpropyleneurea, amide urea of ​​1,3-dimethyl-2-imidazolidinoic acid, and lactams; sulfolanes such as sulfolane and dimethylsulfolane; nitriles such as benzonitrile; ketones such as methylphenyl ketone; and other solvents such as polyethylene dialkyl ether, 1-chloronaphthalene, and diphenyl sulfide.

[0026] The sulfidizing agent used in this embodiment includes alkali metal sulfides and alkali metal hydrosulfides (hereinafter, both are collectively referred to as alkali metal sulfides). The alkali metal sulfides include lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, cesium sulfide, and mixtures thereof. Such alkali metal sulfides can be used as hydrates, aqueous mixtures, or anhydrides. In addition, alkali metal sulfides can also be derived by the reaction of alkali metal hydrosulfides with alkali metal hydroxides. The alkali metal hydrosulfide includes sodium hydrosulfide, potassium hydrosulfide, lithium hydrosulfide, rubidium hydrosulfide, cesium hydrosulfide, and mixtures of two or more of these. In addition, a small amount of an alkali metal hydroxide may be added to react with the alkali metal hydrosulfide and alkali metal thiosulfate that are usually present in trace amounts in the alkali metal sulfide. The polymerization reaction of PAS resins can be carried out in the presence of these organic polar solvents by reacting the above alkali metal sulfides and alkali metal hydroxides, which are so-called sulfidizing agents, with a polyhalogeno aromatic compound.

[0027] - Polymerization conditions and recovery - The polymerization temperature of the PAS resin in this embodiment is preferably in the range of 200 to 330° C. The pressure during polymerization of the PAS resin should be in a range that substantially keeps the polymerization solvent and the polyhalogenoaromatic compound, which is the polymerization monomer, in the liquid phase, and is generally preferably selected in the range of 0.1 to 20 MPa, more preferably in the range of 0.1 to 2 MPa. The polymerization reaction time varies depending on the temperature and pressure, but is generally preferably in the range of 10 minutes to 72 hours, more preferably in the range of 1 hour to 48 hours. Furthermore, in this embodiment, the reaction mixture (slurry) containing the PAS resin obtained by the polymerization step is "desolvated" by an appropriate means in the purification step described below (a suitable method can be selected from among reduced pressure distillation, centrifugation, screw decanter method, reduced pressure filtration, and pressure filtration) to separate and remove the organic solvent, and then a crude polyarylene sulfide resin (a PAS resin that has not been subjected to a purification step) can be recovered.

[0028] The polymerization step in this embodiment is preferably a step of obtaining a reaction mixture (slurry) containing a PAS resin obtained by reacting at least one polyhalogeno aromatic compound with at least one alkali metal sulfide as a sulfidizing agent in an organic solvent. Therefore, the polymerization step is sufficient as long as the organic solvent, the polyhalogeno aromatic compound, and the alkali metal sulfides added as raw materials are contacted and the polymerization reaction proceeds, and it is not necessary to mix the entire amount of at least one selected from the group consisting of the organic solvent, the polyhalogeno aromatic compound, and the alkali metal sulfides required for the polymerization reaction from the charging stage. In other words, in order to charge the raw materials required for the polymerization reaction, the organic solvent, the polyhalogeno aromatic compound, and the alkali metal sulfides may be continuously or intermittently added to react until the polymerization reaction is completed.

[0029] In the polymerization step of this embodiment, a dehydration treatment may be carried out before polymerization, if necessary, in order to adjust the amount of water in the reaction system. Specifically, it is preferable to carry out a dehydration treatment on the raw materials, that is, the organic solvent, the polyhalogeno aromatic compound, and the alkali metal sulfide or alkali metal hydrosulfide, preferably in an inert gas atmosphere at a temperature range of from room temperature (25° C.) to 230° C., and then proceed with the polymerization step. The amount of water in the reaction system refers to the amount of water added to the reaction system as an aqueous solution and a hydrate when the raw materials are charged, minus the amount of water removed from the reaction system. In addition, the order in which the organic solvent, the polyhalogeno aromatic compound, and the alkali metal sulfides are mixed into a reactor such as an autoclave is not particularly limited. For example, the polymerization step in this embodiment is preferably in the following mode (A) or mode (B). Mode (A): After the alkali metal sulfide, the organic solvent, and the polyhalogeno-aromatic compound are contacted, the alkali metal sulfide, the organic solvent, and the polyhalogeno-aromatic compound are heated to a temperature above room temperature (25°C), preferably near the polymerization temperature (170°C to 300°C). Mode (B): The alkali metal sulfides are contacted with the organic solvent, and the alkali metal sulfides and the organic solvent are heated to room temperature (25°C) or higher, preferably to near the polymerization temperature (170°C to 300°C), and then the alkali metal sulfides are contacted with the polyhalogenoaromatic compound. In addition, in the polymerization steps using the above modes (A) and (B), the conditions described in the above section "Polymerization conditions and recovery" may be applied.

[0030] <Specific polymerization conditions> When the PAS resin used in the preparation step of this embodiment is prepared by a polymerization step, it is preferable that the zeta potential value of the surface of a test piece, which is an evaluation sample formed from at least a part of the PAS resin obtained by the polymerization step (or the polymerization step and the purification step described below), is in the range of -50 to -65 mV at pH 7.8 to 8.2 (for example, pH = 8.0). A PAS resin having a zeta potential value of the surface of a test piece in the range of -50 to -65 mV at pH 7.8 to 8.2 (for example, pH = 8.0) is excellent in reactivity, and therefore can exhibit fluidity with little variation and excellent mechanical properties in a PAS resin composition further blended with other reactive materials and a molded product thereof. Specific polymerization conditions required for the zeta potential value of the surface of the test piece to tend to be in the range of -50 to -65 mV at pH 7.8 to 8.2 (for example, pH = 8.0) include the following conditions (a) to (c). (a) The total amount of the organic solvent used from the time the raw materials are charged until the end of the polymerization reaction is preferably in a ratio of 1 to 6 mol per 1 mol of the alkali metal sulfide as the sulfur source. (b) The amount of the organic solvent initially charged is preferably 0.01 to 0.50 mol per 1 mol of the alkali metal sulfide as the sulfur source. (c) It is preferable to add an acid or a hydrogen salt to the PAS resin (or the reaction mixture (slurry)) after the polymerization reaction in the polymerization step. More preferably, an acid or a hydrogen salt is added to the PAS resin (or the reaction mixture (slurry)) after the polymerization reaction in the polymerization step to adjust the pH of the reaction mixture to 7 to 11.

[0031] As the organic solvent under the above conditions (a) and (b), an aliphatic cyclic compound is preferable, N-methyl-2-pyrrolidone (NMP), N-cyclohexylpyrrolidone, N-methylcaprolactam, ε-caprolactam, sulfolane or dimethylsulfolane is more preferable, and N-methyl-2-pyrrolidone (NMP) is particularly preferable.

[0032] Examples of the acid under the condition (c) above include organic acids such as saturated fatty acids such as carbonic acid, oxalic acid, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, and monochloroacetic acid; unsaturated fatty acids such as acrylic acid, crotonic acid, and oleic acid; aromatic carboxylic acids such as benzoic acid, phthalic acid, and salicylic acid; dicarboxylic acids such as oxalic acid, maleic acid, and fumaric acid; and sulfonic acids such as methanesulfonic acid and paratoluenesulfonic acid; and inorganic acids such as hydrochloric acid, sulfuric acid, sulfurous acid, nitric acid, nitrous acid, and phosphoric acid. Examples of hydrogen salts in the above condition (c) include sodium hydrogen sulfate, disodium hydrogen phosphate, sodium hydrogen carbonate, etc. In practical use, organic acids that are less corrosive to metal members are preferred.

[0033] In the polymerization process of this embodiment, when the above condition (a) is adopted, the concentration of the PAS resin during polymerization increases, and the reaction in which the ring-opened product of the aliphatic cyclic compound is attached to the terminal of the PAS resin becomes more likely to proceed, and therefore a specific zeta potential value can be exhibited. In the polymerization process of this embodiment, when the above condition (b) is adopted, the concentration of the PAS resin during polymerization increases, and the reaction in which the ring-opened product of the aliphatic cyclic compound is attached to the terminal of the PAS resin becomes more likely to proceed, and therefore a specific zeta potential value can be exhibited. In the polymerization step of this embodiment, when the above condition (c) is adopted, acidic components are encapsulated in the PAS resin, and the acidic components seep out during the purification step, causing some of the terminal functional groups of the PAS resin to undergo ion exchange and become protonated, which can result in a specific zeta potential value.

[0034] In this embodiment, in order to set the zeta potential value of the surface of the test piece in the range of -50 to -65 mV at pH 7.8 to 8.2 (e.g., pH = 8.0), it is preferable to add an acid to the PAS resin in the polymerization step or the purification step described below. Therefore, by satisfying the polymerization conditions (a) to (c) above, particularly (c), the zeta potential value is more likely to fall within the predetermined range. In another aspect of this embodiment, the above conditions (a) to (c) can be applied as specific polymerization conditions required for the test piece surface to have a zeta potential value in the range of −30 to −45 mV at pH 4.8 to 5.2 (e.g., pH = 5.0).

[0035] A preferred aspect of the polymerization step of this embodiment is a step of obtaining a reaction mixture (slurry) containing a PAS resin obtained by reacting at least one polyhalogeno aromatic compound with at least one alkali metal sulfide as a sulfidizing agent in an organic solvent, in which the total amount of the organic solvent used until the end of the reaction is 1 to 6 mol per mol of the total amount of the alkali metal sulfides. This polymerization step is more preferably combined with the above aspect (A) or the above aspect (B).

[0036] Another preferred embodiment of the polymerization step of the present embodiment is a step of contacting at least one alkali metal sulfide with an organic solvent and at least one polyhalogeno-aromatic compound, and then heating the alkali metal sulfide, the organic solvent and the polyhalogeno-aromatic compound to room temperature (25° C.) or higher, preferably to a temperature close to the polymerization temperature (170° C. to 300° C.), thereby obtaining a reaction mixture (slurry) containing a PAS resin obtained by reacting the polyhalogeno-aromatic compound with the alkali metal sulfides in the organic solvent, The amount of the organic solvent when the alkali metal sulfides, the organic solvent, and the polyhalogeno-aromatic compound are brought into contact with each other is preferably in the range of 0.01 to 0.50 mol per 1 mol of the alkali metal sulfides.

[0037] Furthermore, another aspect of the preferred polymerization step of this embodiment is a step of obtaining a reaction mixture (slurry) containing a PAS resin obtained by reacting at least one type of polyhalogeno-aromatic compound with at least one type of alkali metal sulfide, which is a sulfidizing agent, in an organic solvent, in which the alkali metal sulfides are brought into contact with the organic solvent, and the alkali metal sulfides and the organic solvent are heated to room temperature (25°C) or higher, preferably to near the polymerization temperature (170°C to 300°C), and then the alkali metal sulfides are brought into contact with the polyhalogeno-aromatic compound to react with each other, and an acid or a hydrogen salt is added to the reaction mixture (slurry) to adjust the pH of the reaction mixture (slurry) to 7 to 11.

[0038] (purification process) In this embodiment, if necessary, it is preferable to further carry out a purification step after the polymerization step. The purification step of this embodiment can be a step of purifying the PAS resin obtained by the polymerization step. This can further modify or homogenize the surface properties of the PAS resin. In the purification step of this embodiment, a known purification process can be applied depending on the chemical structure of the PAS resin to be evaluated. When the PAS resin used in the preparation step of this embodiment is prepared by a polymerization step, it is preferable that the zeta potential value of the surface of a test piece, which is an evaluation sample formed from at least a part of the PAS resin obtained by the polymerization step and the purification step, is in the range of -50 to -65 mV at pH 7.8 to 8.2 (e.g., pH = 8.0). When the zeta potential value of the surface of the test piece is in the range of -50 to -65 mV at pH 7.8 to 8.2 (e.g., pH = 8.0), a PAS resin having good reactivity can be provided. A preferred aspect of the purification step in this embodiment is to further apply specific purification conditions under which the zeta potential value of the surface of the test piece is likely to be in the range of -50 to -65 mV at pH 7.8 to 8.2 (eg, pH=8.0). In another preferred embodiment of the purification step in this embodiment, specific purification conditions may be further applied under which the zeta potential value of the surface of the test piece is likely to be in the range of -30 to -45 mV at pH = 4.8 to 5.2 (eg, pH = 5.0).

[0039] The purification process applicable to this embodiment will be described below, followed by a detailed description of the specific purification conditions. In this embodiment, the purification treatment of the PAS resin (reaction mixture (slurry) containing the PAS resin) obtained by the polymerization step is not particularly limited, but examples thereof include the following purification treatments 1 to 5. Purification process 1: After the polymerization reaction is completed, the reaction mixture (slurry) is either left as is or after the addition of an acid or base, and the solvent is then distilled off under reduced pressure or normal pressure, and the solid (crude PAS resin) obtained after the solvent distillation is washed once or twice or more times with a washing solution such as (hot) water, the reaction solvent (or an organic solvent having a similar solubility to the low molecular weight polymer), acetone, methyl ethyl ketone, or alcohols, and then neutralized, washed with (hot) water, filtered, and dried. Purification process 2: After the polymerization reaction is completed, a solvent such as (hot) water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, aliphatic hydrocarbons, etc. (a solvent that is soluble in the organic solvent used in the polymerization and is a poor solvent for at least the PAS resin) is added as a precipitating agent to the reaction mixture (slurry) to precipitate a solid (crude PAS resin) containing the PAS resin and inorganic salts, etc., which is then filtered, washed, and dried. Purification process 3: After the polymerization reaction is completed, a reaction solvent (or an organic solvent having a solubility equivalent to that of the low molecular weight polymer) is added to the reaction mixture (slurry) and stirred, and then the mixture is filtered to remove the low molecular weight polymer. The solid (crude PAS resin) is washed once or twice or more with a washing solution such as (hot) water, acetone, methyl ethyl ketone, or alcohols, and then neutralized, washed with (hot) water, filtered, and dried. Purification process 4: After the polymerization reaction is completed, hot water is added to the reaction mixture (slurry) as a washing solution, and the reaction mixture is washed with hot water. The solid matter obtained by filtration (crude PAS resin) is treated with acid by adding acid during the hot water washing if necessary, and then dried. Purification process 5: After the polymerization reaction is completed, the reaction mixture (slurry) is filtered to obtain a solid (crude PAS resin). If necessary, the solid is washed once or twice or more times with the reaction solvent as a washing solution, and then further washed with (hot) water, filtered and dried. In the purification processes exemplified above as purification process 1 to purification process 5, the drying of the PAS resin may be carried out in a vacuum, or in air or in an inert gas atmosphere such as nitrogen.

[0040] In the present embodiment, the purification step is preferably a step of adding a washing solution to the reaction mixture (slurry) containing the PAS resin obtained in the polymerization step or the crude PAS resin, which is the solid content of the reaction mixture (slurry), and carrying out a washing treatment, a filtration treatment, and a drying treatment. Moreover, the washing treatment of adding the washing solution, the filtration treatment, and the drying treatment can each be optionally carried out at least once or a plurality of times. In this specification, the term "crude PAS resin" refers to a solid content obtained by performing solid-liquid separation one or more times on the reaction mixture (slurry) containing the PAS resin obtained in the polymerization step.

[0041] The above washing treatment is not particularly limited, and acid washing, (hot) water washing, and solution washing with the above washing solution or reaction solvent can be carried out once or a plurality of times. The cleaning solution that can be used in the cleaning process in this embodiment is not particularly limited, and examples thereof include water, hot water, acid solution, N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, dimethylsulfoxide, dimethylsulfone, acetone, methyl ethyl ketone, diethyl ketone, acetophenone, dimethyl ether, dipropyl ether, tetrahydrofuran, chloroform, methylene chloride, trichloroethylene, ethylene dichloride, dichloroethane, tetrachloroethane, chlorobenzene, methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, benzene, toluene, xylene, etc. The above cleaning solutions may be used alone or in combination of two or more. The temperature of the above-mentioned cleaning solution is preferably 140 to 260° C. In the method of cleaning with a cleaning solution at 140 to 260° C., the crude PAS resin is preferably washed while pressurizing the cleaning solution (for example, in a pressure range of 0.1 to 5 MPa). The drying treatment is not particularly limited, and is preferably performed at a drying temperature of 120 to 270° C. The atmosphere for the drying treatment may be under reduced pressure, under a nitrogen or inert gas inert gas atmosphere, under an oxidizing atmosphere such as oxygen or air, or under a mixed gas atmosphere of air and nitrogen. The drying time is preferably 0.5 to 53 hours. The filtration treatment is not particularly limited as long as it is a method capable of performing solid-liquid separation, and examples of the filtration treatment include a method of performing solid-liquid separation using a filter, a centrifuge, or the like.

[0042] <Specific purification conditions> In the purification step of this embodiment, specific purification conditions required for the test piece surface to have a zeta potential value in the range of -50 to -65 mV at pH 7.8 to 8.2 (e.g., pH = 8.0) include the following conditions (d) to (f). In the (d) purification step, the crude PAS resin is preferably treated with an acid solution in a predetermined amount or more, more preferably in an amount of about twice the total weight of the PAS resin or more. (e) The acid solution used in the acid treatment in (d) above preferably has a pH of 6 or less. (f) In the purification step, washing with hot water at 140 to 260° C. is preferably performed in an amount of 1.5 to 10 times the total weight of the PAS resin.

[0043] In the purification step of this embodiment, when the above conditions (d), (e), and (f) are adopted, ion exchange occurs and the terminal functional groups of the PAS resin can be protonated. The acid used in the acid solution is not particularly limited as long as it can prepare an acid solution having a pH of 6 or less, and the acid in the above condition (c) can be used.

[0044] In this embodiment, an acid may be added to the PAS resin in the polymerization step or the purification step for the purpose of adjusting the zeta potential value of the surface of the test piece to within a range of -50 to -65 mV at pH 7.8 to 8.2 (e.g., pH = 8.0). More specifically, a preferred purification step in this embodiment includes adding an acid solution to the PAS resin (including the reaction mixture (slurry)) obtained in the polymerization step or a crude PAS resin which is a solid fraction obtained by solid-liquid separation of the reaction mixture (slurry) containing the PAS resin obtained in the polymerization step, thereby performing an acid treatment. In another preferred aspect of the purification step of this embodiment, during the step of adding a washing solution to the PAS resin (including the reaction mixture (slurry)) obtained in the polymerization step or to a crude PAS resin which is the solid content of the reaction mixture (slurry) containing the PAS resin obtained in the polymerization step, and washing, filtering and drying, an acid treatment is performed one or more times by adding an acid solution to the crude PAS resin. In another aspect of this embodiment, the above conditions (d) to (f) can be applied as a specific purification step required for the test piece surface to have a tendency for its zeta potential value to be in the range of -30 to -45 mV at pH 4.8 to 5.2 (e.g., pH = 5.0), in the same manner as in the measurement system at pH 7.8 to 8.2 (e.g., pH = 8.0).

[0045] "Evaluation process" The evaluation step in this embodiment is a step of evaluating a test piece prepared from at least a part of the PAS resin obtained in the preparation step, and includes a test piece preparation step and a zeta potential measurement step. In other words, the evaluation step in this embodiment is a step of preparing a test piece (=evaluation sample) from at least a part of the PAS resin (including polymerized and purified PAS resin) obtained in the preparation step, and measuring the zeta potential of the test piece under a predetermined condition to evaluate the surface properties of the test piece and grasp the properties of the PAS resin. Therefore, in the evaluation step in this embodiment, the chemical properties of the PAS resin, the raw material of the test piece, are quantified by the zeta potential value of the surface of the test piece, which is the evaluation sample formed from the PAS resin. As a result, it is not necessary to evaluate the entire amount of the PAS resin prepared in the preparation step, and it is sufficient to evaluate the PAS resin obtained in the preparation step. In addition, it is preferable that the test piece obtained in the test piece preparation step is formed from an amorphous PAS resin. The evaluation process in this embodiment makes it possible to identify PAS resins having a zeta potential value within a predetermined range, thereby enabling the surface characteristics of the PAS resin to be quantified with high accuracy.

[0046] The test piece preparation process and the zeta potential measurement process will be described in detail below. (Test piece preparation process) The test piece preparation step in this embodiment is a step of preparing a molten PAS resin by melting the PAS resin obtained in the preparation step, and then solidifying the molten PAS resin to prepare a test piece. In other words, the test piece preparation step in this embodiment is a step of taking at least a part of the PAS resin (including the polymerized and purified PAS resin) obtained in the preparation step, melting it once, and then solidifying the molten PAS resin to prepare a test piece having a predetermined shape and surface characteristics. From the viewpoint of performing an evaluation more in line with the molten state, the test piece in this embodiment is preferably in an amorphous state.

[0047] In this specification, the term "amorphous state" refers to a state in which no crystalline phase exists in the PAS resin constituting the test piece, and more specifically, refers to a state in which the following condition (i) is satisfied: (i) In DSC measurement of the PAS resin film test piece, when the temperature is increased at 20°C / min from 40°C to 350°C, no exothermic peak due to crystallization is observed between 100°C and 200°C.

[0048] In addition, in the evaluation method of this embodiment, the chemical properties of the PAS resin, the raw material of the test piece, are quantified by the zeta potential value of the surface of the test piece made from the PAS resin. The reason for evaluating the reactivity of the PAS resin from the chemical properties of the surface in this way is due to the extremely high chemical resistance of the PAS resin. As for the PPS resin, which is a particularly preferred embodiment of the PAS resin, a solvent that dissolves the PPS resin at 200°C or less has not yet been found, so there is currently no way to directly measure the properties (physical properties, chemical properties, etc.) of the PAS resin itself, especially the molecular terminals in the PAS resin that greatly contribute to reactivity. Therefore, in this disclosure, the properties of the PAS resin, which is the constituent material of the test piece, are grasped by using a specific test piece as a standard.

[0049] <Melting> In the present embodiment, the method of preparing the molten PAS resin by melting the PAS resin obtained in the preparation step includes a method of heating and melting the refined PAS resin using a heating means. The heating means is not particularly limited as long as it can heat and melt the PAS resin obtained in the preparation step, and known heating means can be used, such as a hot plate, an oil bath, a constant temperature oven with hot and cold air circulation, a microwave or (far) infrared heater, a roll heated for temperature control, a heat pipe roll, a metal belt, or a hot press. Furthermore, when the PAS resin is heated using the heating means, the heating time is not particularly limited as long as the PAS resin is melted, and is, for example, about 30 seconds to 10 minutes. In this embodiment, the temperature at which the PAS resin obtained in the preparation step is melted may be equal to or higher than the melting point of the PAS resin, and is preferably 300° C. or higher and 400° C. or lower. Since the oxidation crosslinking reaction of the PAS resin proceeds at temperatures of 200° C. or higher, the PAS resin may be thermally melted in a non-oxidizing inert gas atmosphere.

[0050] In the test piece preparation step of this embodiment, the PAS resin obtained in the preparation step may be heated and melted through a sheet body in order to easily obtain a test piece of a predetermined size. As a more detailed method of heat melting, it is preferable to place the PAS resin obtained in the preparation step (e.g., powdered PAS resin) on a sheet body, and then heat the sheet body using a heating means to melt the PAS resin and prepare a molten PAS resin. As another method of heat melting, it is preferable to place the PAS resin obtained in the preparation step (e.g., solid or powdered purified PAS resin) between a pair of sheets so as to sandwich the PAS resin, and then heat the pair of sheets or one of the pair of sheets using a heating means to melt the PAS resin and prepare a molten PAS resin.

[0051] By using the sheet body, the test piece where the molten PAS resin has solidified can be easily collected. In particular, it is preferable that the sheet body has releasability. This allows the test piece to be easily collected without the solidified PAS resin adhering to it, which reduces the loss of appearance characteristics (thickness, etc.) and suppresses breakage of the test piece. The material of the sheet must have a higher melting point than PAS resin, and examples of such materials include metal materials (martensitic stainless steel such as SUS404C), fluorine-based resins, polyimide, and ceramics. Examples of the fluororesin include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), tetrafluoroethylene-ethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), polyvinylidene fluoride (PVDF), and ethylene-chlorotrifluoroethylene copolymer (ECTFE). The fluororesin may contain an inorganic filler such as glass fiber, if necessary. In the test piece preparation step of this embodiment, when a sheet body is used to prepare the test piece, a suitable sheet body preferably has a higher melting point than the PAS resin and has a hydrophobic surface.

[0052] <Solidification> In the present embodiment, the method for solidifying the molten PAS resin includes a method for solidifying the molten PAS resin by cooling. The cooling may be natural cooling or rapid cooling, with rapid cooling being preferred. A known cooling means may be used as the cooling method. Examples of the cooling means include a roll capable of adjusting the surface temperature (cooling roll), an air knife, immersion in water (water tank, etc.), and direct or indirect contact with a metal material at 35° C. or lower. As described above, the test piece of the present embodiment is preferably made of an amorphous PAS resin. A method for producing such an amorphous PAS resin is preferably to rapidly cool a molten PAS resin to solidify it. Rapid cooling makes it possible to produce an amorphous PAS resin that does not contain a crystalline phase, which is preferable from the viewpoint that it makes it easier to evaluate the PAS resin uniformly even by surface measurement and that it is easy to use as an indicator of reactivity in the molten state. In the test piece preparation step according to the present embodiment, the PAS resin obtained in the preparation step is preferably melted at 300° C. or higher and then cooled at a rate of 10° C. / sec or higher, and more preferably, the PAS resin obtained in the preparation step is melted at 280° C. or higher and 400° C. or lower and then cooled at a rate of 10° C. / sec. or higher and 100° C. / sec or lower. The cooling rate is preferably maintained in a temperature range from 400° C. to at least the Tg of the PAS resin. This makes it possible to solidify the PAS resin in an amorphous state, which makes it easier to evaluate the PAS resin uniformly even when measuring its surface, and has the effect of making it easier to use as an indicator of reactivity in the molten state. In this embodiment, it is preferable to cool the PAS resin from a molten state to a temperature not higher than the Tg of the PAS resin, preferably not higher than 90° C., at a cooling rate of 10° C. / sec to 100° C. / sec. In the test piece preparation step of this embodiment, the molten PAS resin may be solidified through a sheet body in order to easily obtain a test piece of a predetermined size. As a more detailed method for solidifying the molten PAS resin, it is preferable to use a cooling means to cool the sheet body on which the molten PAS resin is placed, thereby solidifying the molten PAS resin and recovering the test piece. As another method for solidifying the molten PAS resin, it is preferable to cool at least one of a pair of sheets placed so as to sandwich the molten PAS resin, thereby solidifying the molten PAS resin between the pair of sheets, thereby recovering the test piece. This allows the test piece to be easily recovered without the solidified PAS resin adhering to it, reducing the loss of appearance characteristics (such as thickness) and suppressing breakage of the test piece. A preferred test piece preparation process in this embodiment is a process in which the PAS resin obtained in the preparation process is placed on a sheet body, the sheet body is heated using a heating means to melt the PAS resin and produce molten PAS resin, and then the sheet body on which the molten PAS resin is placed is cooled using a cooling means to solidify the molten PAS resin to produce a test piece.

[0053] <Test piece> The test piece in this embodiment is an example of a measurement subject for zeta potential measurement, and it is necessary to set a certain appearance standard (certain shape or size, etc.) for each zeta potential measurement so as not to affect the measurement value itself as much as possible. Therefore, in the test piece preparation process of this embodiment, a test piece having a certain shape, size and thickness is prepared as the measurement subject for convenience of zeta potential measurement. The test piece in this embodiment is not considered to be particularly limited as long as it does not affect the measurement value itself as much as possible for each zeta potential measurement. The test piece in this embodiment is preferably a rectangular plate (including a film) with a thickness of 0.05 to 0.15 cm (4.5 to 5.5 cm (length) x 2.5 to 3.5 cm (width)). In this specification, for the convenience of measuring the zeta potential, a film-like PAS resin measuring 4.5 to 5.5 cm (length) × 2.5 to 3.5 cm (width) × 0.05 to 0.15 cm (thickness) is used as the test piece. However, it goes without saying that there are no particular limitations on the shape, size, thickness, etc. of the test piece as long as they do not affect the measured zeta potential value itself as much as possible. In addition, the test piece preparation step in this embodiment is preferably a step of preparing a test piece that is a flat plate (including a film) measuring 4.5 to 5.5 cm (length) x 2.5 to 3.5 cm (width) x 0.05 to 0.15 cm (thickness) and is made of an amorphous PAS resin. In other words, when the test piece of this embodiment is subjected to DSC measurement by increasing the temperature from 40°C to 350°C at a rate of 20°C / min, it is preferable that no exothermic peak due to crystallization is observed between 100°C and 200°C. Since it depends on the size of the measuring device used, the length of the test piece in the longitudinal direction of this embodiment is preferably 4.5 to 5.5 cm. The length of the minor axis (= width) of the test piece in this embodiment is preferably 2.5 to 3.5 cm. Furthermore, the thickness of the test piece in this embodiment is preferably 0.05 to 0.15 mm. In this specification, the "length and width of the test piece" are measured using a vernier caliper, while the "thickness of the test piece" refers to the average value of the thicknesses of a total of 25 points, which are obtained by cutting the test piece at 5 points at 8 mm intervals along the longitudinal direction in a direction perpendicular to the longitudinal direction, and measuring the thickness of the test piece at 5 points at 5 mm intervals along the width direction on each cut surface using a TH-104 film thickness measuring instrument (manufactured by Tester Sangyo Co., Ltd.).

[0054] In this embodiment, the surface of the test piece or the surface of the sheet may be subjected to a surface treatment in order to suppress fluctuations in the measured values. The above-mentioned surface treatment method is not particularly limited, and can be appropriately selected from known methods as long as it does not impair the properties of the test piece. For example, degreasing with an organic solvent such as acetone in which PAS resin is insoluble can be included.

[0055] (Zeta potential measurement process) The zeta potential measurement step in this embodiment is a step of measuring the zeta potential of the surface of the test piece obtained in the above test piece preparation step by a streaming potential method. By using the zeta potential value as an index of the surface properties of the PAS resin, the surface properties of the evaluation sample can be measured relatively easily, and the properties of the PAS resin can be easily understood. In addition, when the zeta potential value of the same PAS resin sample is measured multiple times, the fluctuation range (coefficient of variation) of the zeta potential value due to measurement is smaller than that of the conventional viscosity increase measurement using MFR. The zeta potential measurement step in this embodiment is a step of measuring the zeta potential of the surface of the test piece by a streaming potential method, preferably at a pH of 3 to 9, more preferably at a pH of 4.0 to 8.5, even more preferably at a pH of 6.5 to 8.4, and even more preferably at a pH of 7.8 to 8.2. In another embodiment, the zeta potential measurement step is preferably a step of measuring by a streaming potential method, preferably at a pH of 4.5 to 6.0, and more preferably at a pH of 4.8 to 5.2. Setting the zeta potential measurement conditions within the pH range of 3 to 9 not only reduces the variance in the measured values, but also increases the absolute value of the observed zeta potential. This increases the difference in zeta potential values, making it easier to detect the difference in zeta potential values ​​between the same or different PAS resins, and facilitating the evaluation of the properties of the PAS resin with higher accuracy. In particular, by setting the zeta potential measurement conditions within the pH range of 7.8 to 8.2, the variability in the measured values ​​can be significantly reduced and the absolute value of the observed zeta potential value itself can be significantly increased, making it easier to evaluate the properties of the PAS resin with extremely high accuracy. In the zeta potential measurement step in this embodiment, the zeta potential of the surface of the test piece may be measured under a plurality of different pH ranges by a streaming potential method. Furthermore, for example, when it is difficult to adjust the pH near pH=8 (e.g., pH 6.5 to 8.4) close to the inflection point of the titration curve, the zeta potential of the surface of the test piece may be measured near pH=5 (e.g., pH 4.5 to 6.0).

[0056] <Zeta potential> The zeta potential in this embodiment is preferably measured using a streaming potential method in a pH range of 3 to 9. Hereinafter, measurement of the zeta potential using the streaming potential method will be described with reference to Fig. 1. For ease of explanation, the case of about pH=8 in the preferred pH range of 3 to 9 will be described with reference to Fig. 1 as an example.

[0057] As an example of zeta potential measurement by the streaming potential method, Fig. 1 is a schematic diagram showing the state of an electric double layer at the solid-liquid interface between an evaluation sample (=measurement subject) that is a flat (including film) test piece 2 and an electrolyte solution 3. For ease of explanation, Fig. 1 shows an example in which the test piece 2 made of PAS resin is negatively charged. In measuring the zeta potential using the streaming potential method of the present disclosure, a PAS film as a test piece 2 is set on at least one side of a clamp cell 1 shown in FIG. 1, an electrolyte 3 (1 mmol KCl aqueous solution) adjusted to a pH of 8 is passed through it, the voltage generated by the pressure difference (Δp) is measured, and the zeta potential is calculated using the Helmholtz-Smoluchowski equation (equation (II)) described below.

[0058] As shown in FIG. 1, when the test piece 2 is negatively charged, positively charged particles or ions gather on the surface of the test piece 2 in the electrolyte solution 3, forming a so-called electric double layer. When an electric field is applied between the electrodes 4a and b in this state, the positively charged particles or ions cause a flow (laminar flow) toward the negative electrode 4a near the surface of the test piece 2. As a result, a flow (laminar flow) in the opposite direction occurs in the center of the clamp cell 1 to compensate for this flow (laminar flow). In FIG. 1, the arrows indicate the direction of the flow of the electrolyte solution 3. Alternatively, the electrolyte solution 3 may be pushed away by a constant pressure difference (ΔP) using compressed air or an inert gas to cause a flow. Then, using values ​​of the laminar flow velocity difference (or pressure difference), the viscosity of the electrolytic solution 3, the dielectric constant of the electrolytic solution 3, and the like measured according to the above principle, the following Helmholtz-Smoluchowski equation is used:

number

[0059] <Zeta potential measurement conditions> In this embodiment, the electrolyte solution that can be used for measuring the zeta potential is preferably an aqueous solution containing a monovalent-monovalent electrolyte, such as an aqueous solution of potassium chloride, an aqueous solution of sodium chloride, an aqueous solution of lithium chloride, an aqueous solution of potassium hydroxide, an aqueous solution of sodium hydroxide, or an aqueous solution of lithium hydroxide. In this specification, an aqueous solution of potassium chloride is used. In addition, as the acid or alkali for adjusting the pH when measuring the zeta potential, a general acid or alkali aqueous solution is used, and HCl or KOH is mainly used. The concentration of the electrolyte in the electrolytic solution is preferably 0.1 to 1000 mmol / L. In this specification, 1 mmol / L is used as an example of the concentration of the electrolyte in the electrolytic solution. In this embodiment, when the zeta potential measurement is performed under a condition of a specific pH range, a buffer solution may be used as a usable electrolyte solution. The buffer solution can be appropriately selected according to the pH condition to be measured. The buffer solution refers to a solution in which a weak acid and its salt (conjugate base) or a weak base and its salt (conjugate acid) are mixed, and the desired pH can be adjusted by combining these. For example, when the pH is set to 4 or more and less than 6, acetic acid and sodium acetate, acetic acid and potassium acetate, acetic acid and ammonium acetate, disodium hydrogen phosphate and potassium dihydrogen phosphate, disodium hydrogen phosphate and citric acid, citric acid and sodium citrate, citric acid and potassium citrate, hydrochloric acid and sodium citrate, or succinic acid and sodium succinate can be mentioned. When the pH is set to 6 or more and less than 8, phosphate buffer solution, MES buffer solution, Tris buffer solution, or HEPES buffer solution can be mentioned. When the pH is set to 8 or more and less than 9, CHES buffer solution, TAPS buffer solution, or Bicine buffer solution can be mentioned. On the other hand, Britton-Robinson buffer solution can be used to set the pH range from 2.6 to 12.

[0060] The pH of the electrolytic solution used in the zeta potential measurement step in this embodiment is preferably in the range of 3 to 9, and in a preferred example of this embodiment, an electrolytic solution with a pH of 4.8 to 8.2 is used. The conductivity of the electrolytic solution for the zeta potential in this embodiment may be in the range of 14 to 15 mS / m. In this specification, the pH and conductivity are measured using a pH and conductivity meter (SurPASS3 (Anton Paar)). In this embodiment, the measurement temperature for the zeta potential is preferably around room temperature (22 to 28° C.).

[0061] In the zeta potential measurement step in this embodiment, the following conditions are used as an example. -Type of electrolyte: KCl aqueous solution Ultrapure water used for electrolyte: ASTM I grade (ASTM D 1193-06(2018) type 1) Electrolyte concentration: 1mmol / L Conductivity of electrolyte solution: 14~15mS / m ·Measurement temperature: 20~28℃ pH: 4.8~8.2 Cell type: Clamp cell Cell material: PVDF -Gap between cell and test piece (evaluation sample): Adjusted to 100-120μm Measurement pressure range: 200~450mbar

[0062] "Discrimination process" In the method for evaluating a PAS resin according to this embodiment, it is preferable to further include a determination step (1) of determining whether or not the zeta potential value of the surface of the test piece measured in the zeta potential measurement step is within the range of -1 to -80 mV at pH 3 to 9. By providing the determination step (1) of determining whether the zeta potential value of the surface of the test piece measured under conditions of pH 3 to 9 is within the range of −1 to −80 mV, it becomes easier to evaluate the properties of the PAS resin with higher accuracy. In this embodiment, a preferred aspect of the determination step (1) may be a determination step (2) of determining whether or not the zeta potential value measured under conditions of pH 7.8 to 8.2 (e.g., pH = 8.0) in the zeta potential measurement step is within the range of -50 to -65 mV. This allows evaluation of PAS resins with a specific magnitude of zeta potential value, and therefore provides PAS resins with superior reactivity with higher accuracy than PAS resins quantified by conventional viscosity increase methods such as MFR. When the zeta potential of the surface of a test piece is measured at a specific pH (e.g., pH 3 to 9), a high zeta potential value indicates a tendency for the number of reactive functional groups (e.g., functional groups containing oxygen atoms or nitrogen atoms) present at the molecular ends of the PAS resin constituting the test piece to be large, and therefore the reactivity of the prepared PAS resin is naturally considered to be high. In particular, when the zeta potential values ​​of test pieces each having a PAS resin of the same molecular weight as a constituent component are compared, it is confirmed that the PAS resin used for the test piece with a high zeta potential value tends to have a high reactivity. In another aspect of the present embodiment, instead of or in combination with the determining step (2), a determining step (3) may be provided in which it is determined whether or not the zeta potential value of the surface of the test piece measured in the zeta potential measurement step under conditions of pH 4.8 to 5.2 (e.g., pH=5.0) is within the range of -30 to -45 mV. If the zeta potential value is within this range, a PAS resin with excellent reactivity can be provided. Furthermore, since the zeta potential values ​​and the difference between the zeta potentials of the same or different PPS resins are greater in a measurement system of pH 7.8 to 8.2 (e.g., pH = 8.0) than in a measurement system of pH 4.8 to 5.2 (e.g., pH = 5.0), it becomes easier to evaluate the properties of the PPS resin with higher accuracy. In addition, the relationship between the pH value used in the measurement of the zeta potential of the surface of the test piece and the zeta potential value varies depending on the pH value measured. Therefore, in the present disclosure, the above-mentioned discrimination steps (1) to (3) are merely given as an example of a particularly suitable method for evaluating a PAS resin, and in particular, the discrimination steps (2) and (3) are discrimination steps in which the pH used to measure the zeta potential value is different. Therefore, the scope of the present disclosure also includes other pHs and the zeta potential values ​​at those pHs, and is not limited to only exhibiting a zeta potential value in the range of -50 to -65 mV at pH 7.8 to 8.2 (particularly, pH = 8.0) or exhibiting a zeta potential value in the range of -30 to -45 mV at pH 4.8 to 5.2 (for example, pH = 5.0).

[0063] [Preferable form of evaluation method for PAS resin] The present disclosure relates to a method for producing a PAS resin, the method comprising the steps of: a polymerization step for obtaining a PAS resin; a purification step for purifying the PAS resin; and an evaluation step for evaluating a test piece formed from at least a part of the purified PAS resin obtained through the purification step. How to evaluate The method for evaluating a PAS resin is characterized in that the evaluation step comprises a test piece preparation step of obtaining the test piece by melting the PAS resin and solidifying the molten PAS resin, and a zeta potential measurement step of measuring the zeta potential of the surface of the test piece by a streaming potential method under conditions of pH 3 to 9. The method for evaluating a PAS resin in this embodiment uses a test piece having a specific shape and specific physical properties as a standard sample to measure the zeta potential value, and therefore not only can the zeta potential value be measured easily, but also has higher measurement accuracy than conventional evaluation methods (e.g., the degree of viscosity increase using MFR, etc.). In this embodiment, the zeta potential value of the surface of the test piece is preferably in the range of −51 to −64 mV at pH 7.8 to 8.2 (for example, pH=8.0), more preferably −53 to −63 mV, and further preferably −55 to −62 mV. In this embodiment, the isoelectric point pH of the test piece containing PAS resin as a constituent is preferably in the range of 1 to 6.0, and more preferably 2 to 3.

[0064] Although the embodiments of the present disclosure have been described above, the method for evaluating the PAS resin of the present disclosure is not limited to the above examples and can be modified as appropriate. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. In the following, unless otherwise specified, "%" or "parts" are based on mass.

[0066] (PPS resin manufacturing) [Synthesis Example 1] 22.050 kg (150 mol) of p-dichlorobenzene (p-DCB), 2.974 kg (30 mol) of N-methyl-2-pyrrolidone (NMP), 12.362 kg (150 mol) of 68% NaSH, and 12.500 kg (150 mol) of 48% NaOH were fed to a 150-liter autoclave equipped with an agitator and a bottom valve, which was connected to a pressure gauge, a thermometer, a condenser, and a decanter, and the temperature was raised to 173°C under a nitrogen atmosphere while stirring. After 12.353 kg of water was distilled off, the kettle was sealed. At that time, the p-DCB distilled by azeotropy was separated in a decanter and returned to the kettle as needed. After the dehydration was completed, the temperature inside the autoclave was cooled to 160°C, 29.486 kg (297 mol) of NMP was fed, and the temperature was raised to 220°C and stirred for 2 hours, and then the temperature was raised to 250°C and stirred for 1 hour. The final pressure was 0.28 MPa. After the reaction, the bottom valve of the autoclave was opened, and NMP was extracted into a 150-liter vacuum agitation dryer equipped with an agitator while still in a reduced pressure state, and then the NMP was thoroughly removed by stirring at 150°C under reduced pressure for 2 hours to obtain a mixture (A-1) of powdered PPS resin and salts. 1000g of 70°C ion-exchanged water was added to 417g of the mixture (A-1), stirred for 20 minutes, and then filtered. This process was repeated twice. The obtained water-containing cake and 600g of ion-exchanged water were fed into a 1-liter autoclave equipped with a stirrer and stirred at 160°C for 30 minutes. After cooling to room temperature, 800g of 70°C ion-exchanged water was further added to the water-containing cake obtained by filtration, and filtered. The obtained hydrous cake and 600 g of ion-exchanged water were charged into a 1-liter autoclave equipped with a stirrer, stirred at 220°C for 30 minutes, cooled to room temperature, and filtered. 600 g of ion-exchanged water at 70°C was added to the hydrous cake obtained by filtration and filtered. Then, 600 g of carbonated water with a pH of 4 at 20°C was added and filtered, and 600 g of ion-exchanged water at 70°C was added and filtered. The obtained hydrous cake was dried in a hot air circulation dryer at 120°C for 6 hours to obtain a white powdery PPS resin. The viscosity increase degree and zeta potential of the PPS resin obtained in Synthesis Example 1 were measured three times each, and the results are shown in Table 1.

[0067] [Synthesis Example 2] 19.413 kg of flake sodium sulfide (60.3 wt% Na2S) and 45.0 kg of NMP were supplied to a 150-liter autoclave equipped with an agitator blade and a bottom valve, which was connected to a pressure gauge, a thermometer, and a condenser. The temperature was raised to 209°C while stirring under a nitrogen stream, and 4.644 kg of water was distilled off (the remaining water content was 1.13 moles per mole of sodium sulfide). The autoclave was then sealed and cooled to 180°C, and further cooled while supplying 22.185 kg of p-DCB and 18.0 kg of NMP. At a liquid temperature of 150°C, the inside of the autoclave was pressurized to a gauge pressure of 0.1 MPa with nitrogen gas, and heating was started again. The liquid temperature was raised from 200°C to 250°C over 3 hours, and the mixture was kept at 250°C for 1 hour to react, after which 0.635 kg of water was pressure-injected and cooled to 220°C over 40 minutes. After that, cooling was continued, and 0.284 kg (2.25 moles) of oxalic acid dihydrate and 0.663 kg of NMP were pressure-injected at 200°C. Cooling was continued, and at 100°C, the bottom valve was opened and the reaction slurry was transferred to a 150-liter plate filter and pressure-filtered at 120°C. Next, 16 kg of NMP was added and pressure-filtered. After filtration, the mixture was stirred at 150°C under reduced pressure for 2 hours using a 150-liter vacuum dryer equipped with a stirring blade to remove NMP, and a mixture (B-1) of powdered PPS resin and salts was obtained. 1000 g of 70°C ion-exchanged water was added to 417 g of the mixture (B-1), stirred for 20 minutes, and then filtered. This operation was repeated once more, and the obtained wet cake and 600 g of ion-exchanged water were fed to a 1-liter autoclave equipped with a stirrer and stirred at 160°C for 30 minutes. After cooling to room temperature, the mixture was filtered, and 600 g of 70°C ion-exchanged water was added to the resulting wet cake, followed by further filtration. The resulting wet cake was dried for 6 hours in a hot air circulating dryer at 120°C to obtain a white powdery PPS resin. The viscosity increase and zeta potential of the PPS resin obtained in Synthesis Example 2 were measured three times each, and the results are shown in Table 1.

[0068] (Evaluation method for PPS resin) (1) Measurement of viscosity increase of PPS resin The degree of increase in viscosity of the PPS resins obtained in Synthesis Examples 1 and 2 upon addition of epoxysilane was measured by the following method. The degree of increase in melt viscosity was evaluated when 1.0% (mass ratio of γ-glycidoxypropyltrimethoxysilane to the solid content of PPS resin) was added and melt-kneaded. The melt-kneading was carried out at 320°C and 100 rpm for 5 minutes using a Labo Plastomill (20-200C, using R-60 type mixer, manufactured by Toyo Seiki Seisakusho Co., Ltd.). The degree of increase in melt viscosity when epoxysilane was added and melt-kneaded is expressed by the following formula. Viscosity increase rate (multiplication factor) = (MFR after adding epoxy silane) / (MFR without adding epoxy silane)

[0069] (2) Measurement of the zeta potential (ζ potential) of PPS resin (2-1) Method for preparing test specimens for zeta potential measurement After weighing out 0.5 g of each of the PPS resins produced in Synthesis Examples 1 and 2, each PPS resin was sandwiched between two Teflon sheets containing glass fiber (Nitto Denko Corporation, Nitoflon) and heated for 1 minute using a hot plate preheated to 350° C. During this process, the PPS resin melted, so it was pressed from above with a metal plate heated to 350° C. to form a film having a thickness of 0.1 cm. After heating the film-like PPS resin for an additional minute, the two Teflon sheets sandwiching the film-like molten PPS resin were transferred from the hot plate onto a metal plate at room temperature (28°C), immediately sandwiched between the metal plates at room temperature (28°C) from above, and cooled to room temperature (28°C) to solidify the molten PPS resin. The solidified film-like PPS resin was then cut into 5 cm x 3 cm pieces to prepare amorphous test pieces each containing at least a portion of the PPS resin produced in Synthesis Example as a constituent component. (2-2) Zeta potential measurement method The surface of each amorphous test piece containing the PPS resin obtained above was degreased with acetone, and then the zeta potential value of the surface of each amorphous test piece was measured three times using a solid-specific zeta potential meter SurPASS3 (Anton Paar) by the streaming potential method under the following measurement conditions. "Measurement conditions" Electrolyte: 1mmol / L KCl aqueous solution ·Measurement temperature: 22~26℃ pH: 8.0 or 5.0

[0070] (3)DSC measurement 4 mg of the film-like PPS resin test piece prepared for the zeta potential measurement was taken and heated from 40°C to 350°C at 20°C / min using a PerkinElmer DSC8500 differential scanning calorimeter (DSC). Since no exothermic peak associated with resin crystallization was observed between 100°C and 200°C, it was confirmed that each film-like test piece was in an amorphous state.

[0071] [Table 1]

[0072] In Table 1, when Examples 1 to 4 are compared with Comparative Examples 1 and 2, the CV value (%), which is the coefficient of variation, is reduced by about 10 times, and the change amount [%] of the difference between the average values ​​of Synthesis Example 1 and Synthesis Example 2, which corresponds to an index of measurement accuracy (= [average value of Synthesis Example 2-average value of Synthesis Example 1] / [average value of Synthesis Example 2]×100), is improved by up to 5.1%. Therefore, it was confirmed that the evaluation method of this embodiment has less variation and can evaluate reactive PPS resins with high accuracy compared to the conventional evaluation method using the viscosity increase degree. In addition, when Examples 1 and 2 are compared with Examples 3 and 4, it was confirmed that setting the pH to around 8 not only reduces the variation but also increases the zeta potential value and the difference between the same or different PPS resins, making it easier to evaluate the properties of the PPS resins with high accuracy. [Industrial Applicability]

[0073] According to the present disclosure, the surface characteristics of PAS resin can be quantified, thereby providing a method for evaluating the reactivity of PAS resin with less variation and higher accuracy than conventional evaluation methods that use viscosity. [Explanation of symbols]

[0074] 1 Clamp Cell 2. Test specimens 3 Electrolyte solution 4a Negative electrode 4b Positive electrode

Claims

1. A preparation step of preparing a polyarylene sulfide resin; and evaluating a test piece formed from at least a portion of the polyarylene sulfide resin, The evaluation step includes a test piece preparation step of melting the polyarylene sulfide resin and solidifying the molten polyarylene sulfide resin to obtain the test piece; and a zeta potential measuring step of measuring the zeta potential of the surface of the test piece by a streaming potential method.

2. The method for evaluating a polyarylene sulfide resin according to claim 1 , wherein the zeta potential measuring step measures the zeta potential of the surface of the test piece under a condition of pH 3 to 9.

3. The evaluation method for a polyarylene sulfide resin according to claim 1 or 2, wherein the evaluation step further includes a determination step (2) of determining whether or not the zeta potential value of the surface of the test piece measured in the zeta potential measurement step is within a range of -50 to -65 mV at pH 7.8 to 8.

2.

4. The method for evaluating a polyarylene sulfide resin according to any one of claims 1 to 3, characterized in that, when the test piece is subjected to DSC measurement while heating the test piece in a temperature range from 40°C to 350°C at a rate of 20°C / min, no exothermic peak due to crystallization is observed between 100°C and 200°C.

5. The method for evaluating a polyarylene sulfide resin according to any one of claims 1 to 4, wherein the preparation step includes a polymerization step of obtaining the polyarylene sulfide resin to prepare the polyarylene sulfide resin.

6. A polymerization step for obtaining a polyarylene sulfide resin; a purification step of purifying the polyarylene sulfide resin; and an evaluation step of evaluating a test piece formed from at least a part of the purified polyarylene sulfide resin obtained through the purification step, The evaluation step includes a test piece preparation step of melting the polyarylene sulfide resin and solidifying the molten polyarylene sulfide resin to obtain the test piece; and a zeta potential measuring step of measuring the zeta potential of the surface of the test piece under conditions of pH 3 to 9 by a streaming potential method.

Citation Information

Patent Citations

  • Zeta potential measuring instrument

    JP1992050758A

  • Polyarylene sulfide having high reactivity with epoxysilane and resin composition containing the resin

    JP1994256517A

  • Polyarylene sulfide copolymer and composition containing the same copolymer

    JP1995247429A

  • Sample storage container

    JP2002360237A

  • Semiconductor package and manufacturing method thereof

    WO2008078899A1