Metal film deposition equipment

By maintaining a 10 mm distance between the anode and the side wall in the film forming apparatus, the apparatus addresses non-uniform film thickness issues, achieving improved surface uniformity of the metal film.

JP7582152B2Active Publication Date: 2024-11-13TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021166257
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-08
Publication Date
2024-11-13
Estimated Expiration
2041-10-08

AI Technical Summary

Technical Problem

The existing metal film forming apparatuses suffer from non-uniform film thickness distribution on the base material surface due to the influence of electric field lines from both the anode and the side wall of the housing, leading to uneven film formation.

Method used

The apparatus includes a design with a ceiling wall and a side wall that partially surrounds the anode, maintaining a minimum distance of 10 mm between the anode's outer surface and the side wall's inner surface, thereby reducing the influence of electric field lines from the side wall on the film forming area.

Benefits of technology

This design ensures improved surface uniformity of the metal film by minimizing the impact of electric field lines from both the anode and the side wall, resulting in a more uniform film thickness distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582152000002
    Figure 0007582152000002
  • Figure 0007582152000003
    Figure 0007582152000003
  • Figure 0007582152000004
    Figure 0007582152000004
Patent Text Reader

Abstract

To provide a metal film deposition apparatus capable of depositing a metal film with improved surface uniformity.SOLUTION: A film deposition apparatus 1 includes: an anode 11; a solid electrolyte membrane 13 disposed below the anode 11; a power supply part 14 that applies a voltage between the anode 11 and the substrate B, with the substrate B, which is located below the solid electrolyte membrane 13, as the cathode; and a liquid housing section 15, provided between the anode 11 and the solid electrolyte membrane 13, for housing a metal ion-containing electrolyte L. The liquid housing 15 includes: a ceiling wall 15a on which the anode 11 is installed; and a side wall 15b extending downward from the ceiling wall 15a to surround the anode 11 at least partially, wherein the distance between an inner surface 15b1 facing the anode 11 in the side wall 15b, and the outer surface 11a of the anode 11 opposite the inner surface 15b1 is set at 10 mm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film forming apparatus for forming a metal film on a surface of a substrate. [Background technology]

[0002] Conventionally, metal ions have been deposited on the surface of a substrate to form a metal coating (for example, see Patent Document 1). Patent Document 1 describes a metal coating forming device that includes an anode, a solid electrolyte membrane disposed below the anode, a power supply unit that applies a voltage between the anode and the substrate, with the substrate disposed below the solid electrolyte membrane as the cathode, and a housing that contains an electrolytic solution containing metal ions between the anode and the solid electrolyte membrane. This film forming device pressurizes the electrolytic solution in the housing while the solid electrolyte membrane is in contact with the substrate from above, and applies a voltage between the anode and the substrate to reduce the metal ions contained inside the solid electrolyte membrane, thereby forming a metal coating on the surface of the substrate.

[0003] The housing of the film forming apparatus has a recess for accommodating the anode. The recess is formed by a ceiling wall on which the anode is placed and a side wall extending from the ceiling wall to surround the anode. An opening is provided at the bottom of the housing, and the opening is sealed by the solid electrolyte membrane.

[0004] The anode may be shaped according to the deposition region of the substrate, and depending on the shape of the anode, the anode may be installed on the ceiling wall of the housing with a predetermined gap between it and the side wall of the housing. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-111807 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, since the housing contains an electrolyte solution containing metal ions, the side wall of the housing is constantly in contact with the electrolyte solution and is positively charged. Therefore, when a voltage is applied between the anode and the substrate in the film-forming device to form a metal film on the surface of the substrate, the substrate surface may include a mixture of a portion formed under the influence of electric field lines from the anode and a portion formed under the influence of electric field lines not only from the anode but also from the side wall of the housing. In this case, there is a risk that the distribution of the film thickness on the substrate surface (hereinafter also referred to as "surface uniformity") may become uneven.

[0007] The present invention has been made in consideration of the above points, and an object of the present invention is to provide a metal film forming apparatus that can form a metal film with improved surface uniformity. [Means for solving the problem]

[0008] In view of the above problems, a metal film forming apparatus according to the present invention includes an anode, a solid electrolyte membrane disposed below the anode, a power supply unit configured to apply a voltage between the anode and a substrate using a substrate disposed below the solid electrolyte membrane as a cathode, and a liquid storage unit configured to store an electrolytic solution containing metal ions between the anode and the solid electrolyte membrane, the liquid storage unit storing an electrolytic solution containing metal ions, the liquid storage unit applying a voltage between the anode and the substrate while the solid electrolyte membrane is in contact with the substrate from above, thereby reducing the metal ions contained inside the solid electrolyte membrane to form a metal film on a surface of the substrate, the liquid storage unit including a ceiling wall portion on which the anode is disposed, and a side wall portion extending downward from the ceiling wall portion so as to at least partially surround the anode, and a distance between an inner surface of the side wall portion that faces the anode and an outer surface of the anode that faces the inner surface is set to 10 mm or more. Effect of the Invention

[0009] According to the present invention, the liquid storage section includes a ceiling wall section on which the anode is installed, and a side wall section extending downward from the ceiling wall section so as to at least partially surround the anode, and the distance between the inner surface of the side wall section, which is the surface facing the anode, and the outer surface of the anode facing the inner surface, is set to 10 mm or more. Thus, in the film formation device of the present invention, a sufficient distance is provided between the film formation area of ​​the substrate arranged below the anode and the side wall section of the liquid storage section. Therefore, when a metal coating is formed on the surface of the substrate using the film formation device, the influence of the electric field lines from the side wall section of the housing on the film formation area of ​​the substrate can be reduced. Therefore, when a film is formed using the film formation device, the mixture of the part on the surface of the substrate formed under the influence of the electric field lines from the anode and the part formed under the influence of the electric field lines from not only the anode but also the side wall section of the housing is suppressed. Therefore, a metal coating with improved surface uniformity can be formed on the substrate. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of a metal film forming apparatus according to an embodiment of the present invention, showing an additional mechanism for circulating an electrolyte in the film forming apparatus. [Diagram 2] 2 is a partially enlarged cross-sectional view of the film forming apparatus shown in FIG. 1, showing an enlarged view of part A in FIG. [Diagram 3] FIG. 2 is a partially enlarged cross-sectional view of the film formation apparatus shown in FIG. 1, illustrating the visualized effect of electric field lines on the film formation region of the substrate. [Figure 4] FIG. 1 is a partially enlarged cross-sectional view of a conventional film forming apparatus, illustrating the visualization of the influence of electric field lines on a film forming region of a substrate. [Diagram 5] FIG. 4 is a schematic cross-sectional view of a metal film forming apparatus according to another embodiment of the present invention. [Figure 6] FIG. 2 is a schematic plan view showing a film thickness measurement position of a substrate in an embodiment of the present invention. [Figure 7] 6 is a graph showing the relationship between the surface uniformity calculated based on the film thickness measurement positions in FIG. 5 and the distance between the anode and the side wall portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, a metal film forming apparatus according to an embodiment of the present invention will be described. Fig. 1 is a schematic cross-sectional view of a metal film forming apparatus 1 according to an embodiment of the present invention, and shows an additional mechanism for circulating an electrolytic solution L in the film forming apparatus 1. Fig. 2 is a partially enlarged cross-sectional view of the film forming apparatus 1 shown in Fig. 1, and shows an enlarged view of part A in Fig. 1.

[0012] As shown in FIG. 1, the film forming apparatus 1 includes a metallic anode 11, a solid electrolyte membrane 13 arranged below the anode 11, a power supply unit 14 that applies a voltage between the anode 11 and a substrate B arranged below the solid electrolyte membrane 13, with the substrate B serving as a cathode, and an upper casing (liquid storage unit) 15 that stores an electrolytic solution L containing metal ions between the anode 11 and the solid electrolyte membrane 13.

[0013] The film forming apparatus 1 is an apparatus that applies a voltage between the anode 11 and the substrate B in a state in which the solid electrolyte membrane 13 is in contact with the substrate B from above, reduces metal ions contained inside the solid electrolyte membrane 13 to precipitate a metal, and forms a metal coating F made of the precipitated metal on the surface of the substrate B. Note that Fig. 1 shows a state before the solid electrolyte membrane 13 comes into contact with the substrate B.

[0014] The material of the substrate B is not particularly limited as long as it functions as a cathode (i.e., a surface having electrical conductivity), and may be made of a metal material such as aluminum or iron, or the surface of a resin, ceramic, or the like may be coated with a metal layer such as copper, nickel, silver, or iron.

[0015] 1, the film forming apparatus 1 includes a lower casing 21 on which a substrate B is placed. The substrate B is electrically connected to the negative electrode of the power supply unit 14 via a negative electrode side conductor 14a extending inside the lower casing 21. For example, the lower casing 21 may be formed from a non-conductive material. When the lower casing 21 is made of a conductive material (for example, a metal), the substrate B may be electrically connected to the negative electrode of the power supply unit 14 via the lower casing 21 and the negative electrode side conductor 14a.

[0016] The anode 11 has a shape corresponding to the film-forming region of the substrate B. That is, the film-forming region of the substrate B means the surface portion of the substrate B facing the anode 11. The anode 11 is a non-porous (for example, non-porous) anode made of the same metal as the metal of the metal coating F, and is a block-shaped or flat anode. Examples of the material of the anode 11 include copper, nickel, silver, and iron. In this embodiment, the anode 11 is dissolved by applying a voltage using the power supply unit 14, but the anode 11 does not need to be dissolved if the film is formed using only the electrolyte solution L containing metal ions, for example. The anode 11 may be porous, but is more preferably non-porous. By using the non-porous anode 11, the metal coating F formed on the substrate B is less susceptible to the surface state of the anode 11.

[0017] The anode 11 is connected to a first connection pin 18 made of a conductive material (e.g., metal), and the first connection pin 18 is connected to an upper casing 15 also made of a conductive material (e.g., metal). The positive electrode of the power supply unit 14 is connected to the upper casing 15 via a positive electrode side conductor 14b. Thus, the anode 11 is electrically connected to the positive electrode of the power supply unit 14 via the first connection pin 18, the upper casing 15, and the positive electrode side conductor 14b.

[0018] As described above, the electrolyte L is a liquid containing the metal of the metal coating F to be formed in an ionic state, and examples of the metal include copper, nickel, silver, and iron. The electrolyte L is an aqueous solution in which these metals are dissolved (ionized) with an acid such as nitric acid, phosphoric acid, succinic acid, nickel sulfate, or pyrophosphoric acid. For example, when the metal is nickel, examples of the electrolyte L include aqueous solutions of nickel nitrate, nickel phosphate, nickel succinate, nickel sulfate, or nickel pyrophosphate.

[0019] The solid electrolyte membrane 13 is impregnated (contains) metal ions therein by contacting it with the above-mentioned electrolytic solution L. The solid electrolyte membrane 13 is not particularly limited as long as the metal ions can be reduced in the substrate B when a voltage is applied from the power supply unit 14, and a metal derived from the metal ions can be precipitated. Examples of the material of the solid electrolyte membrane 13 include fluorine-based resins such as Nafion (registered trademark) manufactured by DuPont, hydrocarbon-based resins, polyamic acid resins, and resins having an ion exchange function such as Selemion (CMV, CMD, CMF series) manufactured by Asahi Glass Co., Ltd.

[0020] As shown in FIG. 1 and FIG. 2, the upper casing 15 includes a ceiling wall portion 15a on which the anode 11 is installed, a side wall portion 15b extending downward from the ceiling wall portion 15a so as to at least partially surround the anode 11, and an accommodating recess 15c which is a space formed by the ceiling wall portion 15a and the side wall portion 15b. As shown in FIG. 1, the anode 11 is installed on the ceiling wall portion 15a via a first connection pin 18. The anode 11 may be installed directly on the ceiling wall portion 15a. The side wall portion 15b extends downward from the edge of the ceiling wall portion 15a and surrounds the outside of the anode 11 partially or entirely. As a result, as shown in FIG. 2, a predetermined gap having a distance D is formed between an inner surface 15b1, which is a surface of the side wall portion 15b facing the anode 11, and an outer surface 11a of the anode 11 facing the inner surface 15b1. Distance D is the shortest distance (the horizontal distance in this embodiment) between the outer surface 11a of the anode 11 and the inner surface 15b1 of the side wall portion 15b, and is set to 10 mm or more.

[0021] The accommodation recess 15c is open downward. The solid electrolyte membrane 13 is attached to the upper casing 15 via, for example, a sealant (not shown) so as to seal the accommodation recess 15c while the anode 11 and the electrolytic solution L are accommodated in the accommodation recess 15c. The anode 11 and the solid electrolyte membrane 13 are arranged apart from each other and are not in contact with each other, and the space between them is filled with the electrolytic solution L. In this way, the upper casing 15 is structured so that the electrolytic solution L accommodated in the accommodation recess 15c comes into direct contact with the anode 11 and the solid electrolyte membrane 13. The upper casing 15 is made of a material that is insoluble in the electrolytic solution L.

[0022] Furthermore, the upper casing 15 is formed with a supply flow path 16 for supplying the electrolytic solution L to the accommodating recess 15c, and a discharge flow path 17 for discharging the electrolytic solution L from the accommodating recess 15c. As shown in Fig. 1, the supply flow path 16 and the discharge flow path 17 are holes penetrating the side wall portion 15b of the upper casing 15 in the left-right direction. The supply flow path 16 is fluidly connected to a supply pipe line 32, which will be described later, and the discharge flow path 17 is fluidly connected to a discharge pipe line 34, which will be described later.

[0023] Next, a mechanism for circulating the electrolytic solution L in the film forming apparatus 1 will be described. As shown in FIG. 1, one end of a supply pipe 32 is fluidly connected to the supply flow passage 16 of the upper casing 15 on the upstream side of the film forming apparatus 1. The other end of the supply pipe 32 is connected to a tank 31 in which the electrolytic solution L is stored. A pump P is interposed in the supply pipe 32, and the electrolytic solution L is pumped up from the tank 31 into the supply pipe 32 by driving the pump P, and the electrolytic solution L is pressure-fed to the accommodation recess 15c of the upper casing 15. In addition, one end of a discharge pipe 34 is fluidly connected to the discharge flow passage 17 of the upper casing 15 on the downstream side of the film forming apparatus 1. The other end of the discharge pipe 34 is connected to the tank 31. A pressure regulating valve 35 is interposed in the discharge pipe 34, which prevents the pressure (liquid pressure) of the electrolytic solution L accommodated in the accommodation recess 15c from exceeding a predetermined pressure, and can keep the accommodation recess 15c sealed at or below that pressure. By using this type of circulation mechanism, the electrolyte solution L, whose metal ion concentration has been adjusted to a predetermined concentration, can be supplied from the supply flow path 16 to the accommodating recess 15c, and the electrolyte solution L used during film formation in the accommodating recess 15c can be returned to the tank 31 via the discharge flow path 17.

[0024] In this embodiment, the film forming apparatus 1 is provided with a lifting mechanism (not shown) on the upper part of the upper casing 15. The lifting mechanism may be a hydraulic or pneumatic cylinder, and this makes it possible to move the solid electrolyte membrane 13 toward and away from the substrate B.

[0025] A film forming method using the film forming apparatus 1 according to this embodiment will be described below. First, the substrate B is placed in the lower casing 21, the alignment of the substrate B with respect to the anode 11 is adjusted, and the temperature of the substrate B is adjusted. Next, the upper casing 15 is lowered using a lifting mechanism (not shown) to bring the solid electrolyte membrane 13 into contact with the substrate B from above. After that, the electrolyte L is introduced from the tank 31 into the accommodation recess 15c of the upper casing 15 using the pump P. At this time, the liquid pressure of the electrolyte L in the accommodation recess 15c is increased to a predetermined pressure by the pump P and the pressure regulating valve 35, and the solid electrolyte membrane 13 presses the substrate B with the liquid pressure of the electrolyte L.

[0026] In this state, a voltage is applied between the anode 11 and the substrate B using the power supply unit 14. As a result, the metal ions contained in the solid electrolyte membrane 13 move to the surface of the substrate B in contact with the solid electrolyte membrane 13 and are reduced on the surface of the substrate B. As a result, metal is precipitated on the surface of the substrate B, and a metal film F is formed on the surface of the substrate B. At this time, since the electrolyte solution L is contained in the containing recess 15c, the metal ions can be constantly supplied to the solid electrolyte membrane 13. When the formation of the metal film F is completed, the application of the voltage by the power supply unit 14 is stopped, and then the pumping of the electrolyte solution L by the pump P is stopped, and the solid electrolyte membrane 13 is separated from the substrate B using the lifting mechanism.

[0027] Next, the action and effect of the film forming apparatus 1 according to this embodiment will be described in comparison with the conventional film forming apparatus 1a. FIG. 3 is a partially enlarged cross-sectional view of the film forming apparatus 1 shown in FIG. 1, and shows the visual effect of the electric field lines E on the film forming region of the substrate B. FIG. 4 is a partially enlarged cross-sectional view of the conventional film forming apparatus 1a, and shows the visual effect of the electric field lines E on the film forming region of the substrate B. As shown in FIGS. 3 and 4, the conventional film forming apparatus 1a has a different width of the side wall portion 15b of the upper casing 15 compared to the film forming apparatus 1 according to this embodiment. Specifically, the conventional film forming apparatus 1a has a wider side wall portion 15b compared to the film forming apparatus 1 according to this embodiment, and thus the distance between the outer surface 11a of the anode 11 and the inner surface 15b1 of the side wall portion 15b is shorter. The same reference numerals are used for components having the same or similar functions in the film forming apparatus 1 according to this embodiment and the conventional film forming apparatus 1a.

[0028] As described above, according to the film forming apparatus 1 of this embodiment, the distance between the inner surface 15b1 of the side wall portion 15b and the outer surface 11a of the anode 11 is set to 10 mm or more. Specifically, the shortest distance (horizontal distance in this embodiment) between the outer surface 11a of the anode 11 and the inner surface 15b1 of the side wall portion 15b is set to 10 mm or more. Thus, in the film forming apparatus 1 of this embodiment, a sufficient distance is provided between the film forming area of ​​the substrate B disposed below the anode 11 and the side wall portion 15b of the upper casing 15. Therefore, when the metal film F is formed on the surface of the substrate B using the film forming apparatus 1, the influence of the electric field lines E from the side wall portion 15b on the film forming area of ​​the substrate B can be suppressed. Therefore, when the metal coating F is formed on the surface of the substrate B using the film forming apparatus 1, the mixture of a portion formed under the influence of the electric field lines E from the anode 11 and a portion formed under the influence of the electric field lines E not only from the anode 11 but also from the side wall portion 15b of the upper casing 15 is suppressed on the surface of the substrate B. Thus, the metal coating F with improved surface uniformity can be formed on the substrate B.

[0029] In contrast, in the conventional film forming apparatus 1a, the shortest distance between the inner surface 15b1 of the side wall portion 15b and the outer surface 11a of the anode 11 is short, and a sufficient distance is not provided between the film forming area of ​​the substrate B and the side wall portion 15b of the upper casing 15. In this case, as shown in FIG. 4, the influence of the electric field lines E from the side wall portion 15b on the film forming area of ​​the substrate B may increase. For this reason, in the film forming apparatus 1a, when a voltage is applied between the anode 11 and the substrate B to form a metal film F on the surface of the substrate B, the surface of the substrate B may include a mixture of a portion formed under the influence of the electric field lines E from the anode 11 and a portion formed under the influence of the electric field lines E from not only the anode 11 but also the side wall portion 15b of the upper casing 15. As a result, a metal film F with reduced surface uniformity may be formed on the substrate B. In particular, in the conventional film forming apparatus 1a, the current density flowing from the anode 11 to the substrate B is set to 4.8 A / dm 2If the distance exceeds this, the surface uniformity is likely to decrease due to the influence of the electric field lines E from the side wall portion 15b of the upper casing 15. However, in this embodiment, a sufficient distance is provided between the film formation area of ​​the substrate B and the side wall portion 15b of the upper casing 15, so that the surface uniformity of the metal film can be ensured even under such film formation conditions.

[0030] Next, another embodiment of the present invention will be described. 5 is a schematic cross-sectional view of a metal film forming apparatus 100 according to another embodiment of the present invention. The film forming apparatus 100 is different from the above-mentioned film forming apparatus 1 in at least one of the configurations of the first connection pin 18 and the second connection pin 19, the materials of the upper casing 15 and the lower casing 21, and the configuration of the side wall portion 15b of the upper casing 15. Hereinafter, components having the same or similar functions as those of the above-mentioned film forming apparatus 1 are denoted by the same reference numerals as those of the film forming apparatus 1 and their description is omitted, and only different parts will be described.

[0031] In a film forming apparatus 100 according to another embodiment, the anode 11 is connected to a first connection pin 18 made of a conductive material (e.g., metal), and the first connection pin 18 is connected to a second connection pin 19 made of a similarly conductive material (e.g., metal). The second connection pin 19 extends through the ceiling wall portion 15a of the upper casing 15 in the vertical direction. The positive electrode of the power supply unit 14 is connected to the second connection pin 19 via the positive electrode side conductor 14b. Thus, the anode 11 is electrically connected to the positive electrode of the power supply unit 14 via the first connection pin 18, the second connection pin 19, and the positive electrode side conductor 14b. The outer periphery of each of the first connection pin 18 and the second connection pin 19 is insulated.

[0032] In addition, in a film forming apparatus 100 according to another embodiment, each of the upper casing 15 and the lower casing 21 is formed of a non-conductive material such as resin. Furthermore, in the film forming apparatus 100, the side wall portion 15b of the upper casing 15 is formed by coating the inner surface 15b1 with an insulating ceramic (for example, by cold spraying, thermal spraying, passivation treatment, etc.).

[0033] Thus, in the film forming apparatus 100 according to another embodiment, the outer circumference of each of the first connection pin 18 and the second connection pin 19 is insulated, each of the upper casing 15 and the lower casing 21 is made of a non-conductive material such as resin, and the inner surface 15b1 of the side wall portion 15b of the upper casing 15 is coated with insulating ceramics. This prevents the side wall portion 15b of the upper casing 15 from being positively charged. Therefore, in the film forming apparatus 100, when a voltage is applied between the anode 11 and the substrate B to form a metal coating F on the surface of the substrate B, the influence of the electric field lines from the side wall portion 15b of the upper casing 15 on the surface of the substrate B is suppressed. Therefore, a metal coating F with improved surface uniformity can be formed on the substrate B. EXAMPLES

[0034] The invention is illustrated by the following examples. A glass epoxy board (FR-4) measuring 10 cm x 10 cm was prepared as a substrate for forming a film on its surface. The substrate was made of a layer of glass fiber cloth impregnated with epoxy resin. Copper foil was formed on the surface of this glass epoxy board.

[0035] Next, a copper film was formed using the film forming apparatus 1 according to this embodiment shown in FIG. 1. A copper sulfate aqueous solution (Cu-BRITE-SED) manufactured by JCU Corporation was used as the electrolyte, and a Cu plate was used as the anode. The film forming conditions were as follows: the electrode distance between the substrates serving as the anode and cathode was 2 mm, the temperature of the electrolyte was 42°C, a solid electrolyte membrane (Nafion (manufactured by DuPont)) with a thickness of 8 μm was adhered to the substrate, the liquid pressure of the electrolyte was 0.6 MPa, and the current density was 7 A / dm. 2 , film forming area 100cm 2 The copper film was formed for a cumulative film formation time of 388 seconds. In this example, the copper film was formed while maintaining the above-mentioned film formation conditions and changing the distance D between the outer surface of the anode and the inner surface of the side wall portion to 7.2 mm, 10 mm, 58 mm, and 68 mm.

[0036] <Confirmation of surface uniformity> The film thickness was measured at nine points on the substrate on which the film was formed as described above, as shown in FIG. 6. FIG. 6 is a schematic plan view showing the film thickness measurement positions of the substrate B in the embodiment of the present invention. Specifically, the thickness of the copper film was measured three times at each of the nine points shown in FIG. 6 using a film thickness meter, and the surface uniformity of each substrate was calculated by the formula "(maximum film thickness - minimum film thickness) / average value". The evaluation was based on the surface uniformity (±15%) required for PCB. The results are shown in Table 1. FIG. 7 is a graph in which the distance D in Table 1 is set on the horizontal axis and the surface uniformity is set on the vertical axis, and the graph shows the relationship between the surface uniformity calculated based on the film thickness measurement positions in FIG. 6 and the distance between the anode 11 and the side wall portion 15b.

[0037] [Table 1]

[0038] (Results and Discussion) From Table 1 and FIG. 7, when the distance D is 7.2 mm, the shortest distance between the outer surface of the anode and the inner surface of the side wall is short, and there is not enough distance between the film-forming area of ​​the substrate and the side wall of the upper casing, so that it is considered that the influence of the electric field lines E from the side wall 15b on the film-forming area of ​​the substrate B is increased. Therefore, when a voltage is applied between the anode and the substrate to form a metal film on the substrate surface, it is considered that the substrate surface includes a mixture of a portion formed under the influence of the electric field lines from the anode and a portion formed under the influence of the electric field lines from not only the anode but also the side wall of the upper casing. As a result, it is considered that a metal film with surface uniformity exceeding the standard (15%) was formed on the substrate.

[0039] On the other hand, when the distance D is 10 mm or more, i.e., 10 mm, 58 mm, and 68 mm, the shortest distance between the outer surface of the anode and the inner surface of the side wall is long, and a sufficient distance is provided between the coating area of ​​the substrate and the side wall of the upper casing, so that it is considered that the influence of the electric field lines E from the side wall on the coating area of ​​the substrate is suppressed. Therefore, when a metal coating is formed on the surface of the substrate, it is considered that the mixture of the part on the substrate surface that is formed under the influence of the electric field lines from the anode and the part that is formed under the influence of the electric field lines from not only the anode but also the side wall of the upper casing is suppressed. Therefore, it is considered that a metal coating with surface uniformity that meets the standard (15%) was formed on the substrate.

[0040] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the film forming apparatuses 1 and 100 according to the above-mentioned embodiments, and includes all aspects included in the concept of the present invention and the scope of the claims. In addition, each configuration may be appropriately and selectively combined to achieve the above-mentioned problems and effects. For example, the shape, material, arrangement, size, etc. of each component in the above-mentioned embodiments may be appropriately changed according to the specific aspects of the present invention. [Explanation of symbols]

[0041] 1, 1a, 100: film forming apparatus, 11: anode, 11a: outer surface, 13: solid electrolyte membrane, 14: power supply unit, 14a: negative electrode side conductor, 14b: positive electrode side conductor, 15: upper casing (liquid storage unit), 15a: ceiling wall, 15b: side wall, 15b1: inner surface, 15c: storage recess, 16: supply flow path, 17: discharge flow path, 18: first connection pin, 19: second connection pin, 21: lower casing, 31: tank, 32: supply pipe, 34: discharge pipe, 35: pressure regulating valve, B: substrate, F: metal coating, L: electrolyte, P: pump

Claims

[Claim 1] An anode; a solid electrolyte membrane disposed below the anode; a power supply unit that applies a voltage between the anode and the substrate, the substrate being disposed below the solid electrolyte membrane as a cathode; a liquid storage portion for storing an electrolytic solution containing metal ions between the anode and the solid electrolyte membrane; a metal coating forming apparatus for forming a metal coating on a surface of the substrate by applying a voltage between the anode and the substrate while the solid electrolyte membrane is in contact with the substrate from above, and reducing metal ions contained in the solid electrolyte membrane, the liquid containing portion includes a ceiling wall portion on which the anode is disposed, and a side wall portion extending downward from the ceiling wall portion so as to at least partially surround the anode, a distance between an inner surface of the sidewall portion facing the anode and an outer surface of the anode opposite the inner surface is set to 10 mm or more.

Citation Information

Patent Citations

  • Continuously oneeside electroplating apparatus

    JP1979130444A

  • Formation of bump and plating device

    JP1998275811A

  • Film formation apparatus for metallic film

    JP2020111807A

  • Electroplating apparatus and electroplating method

    JP2020147831A

  • Method and apparatus for dynamic current distribution control during electroplating

    US20140144781A1