Grain-oriented electrical steel sheet and its manufacturing method

The grain-oriented electrical steel sheet with a forsterite film and optimized Ti content in the annealing separator addresses twinning deformation, ensuring minimal processing issues and preserved magnetic properties for applications like small generators and wound cores.

JP7582455B2Active Publication Date: 2024-11-13JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023513545
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-20
Filing Date
2022-10-17
Publication Date
2024-11-13
Estimated Expiration
2042-10-17

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheets suffer from twinning deformation during processing, leading to cracks, chips, and deterioration of magnetic properties, particularly in applications requiring high-strength processing like small generators and wound cores.

Method used

A grain-oriented electrical steel sheet with a specific composition and manufacturing process, including a forsterite film containing Ti, optimized oxygen basis weight, and Ti content in the annealing separator, to reduce twinning deformation and maintain magnetic properties.

Benefits of technology

The solution effectively reduces twinning deformation, minimizing cracks and chips during processing while maintaining high magnetic properties, suitable for applications like small generators and wound cores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582455000001
    Figure 0007582455000001
  • Figure 0007582455000002
    Figure 0007582455000002
  • Figure 0007582455000003
    Figure 0007582455000003
Patent Text Reader

Abstract

The present invention provides a grain-oriented electromagnetic steel sheet which is free from defects such as cracking and chipping due to twinning deformation even if applied to a winding core or an iron core of a small power generator or the like, thereby being subjected to intense processing, and which is also free from deterioration in the magnetic characteristics. This grain-oriented electromagnetic steel sheet has a component composition that contains 2.8 mass% to 3.5 mass% of Si and 0.01 mass% to 1.0 mass% of Mn, with the balance being made up of Fe and unavoidable impurities, while having a base coating film that is mainly composed of forsterite and contains Ti, and a top coating film that is formed on the base coating film. With respect to this grain-oriented electromagnetic steel sheet, the base coating film has an oxygen weight per square meter of 3.8 g / m2 or more and a Ti weight per square meter of 0.06 g / m2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to grain-oriented electrical steel sheets that are primarily used for the cores of transformers, electric motors, generators, and the like, and in particular to grain-oriented electrical steel sheets that are resistant to twinning even when subjected to relatively strong bending, shearing, and the like, such as for the cores of small generators and small electric motors, or wound cores and EI cores, and to a method for manufacturing the same. [Background technology]

[0002] Grain-oriented and non-oriented electrical steel sheets are widely used as iron core materials for various transformers, electric motors, generators, etc. Grain-oriented electrical steel sheets have a crystal orientation called the Goss orientation {110} <001> Because it is highly concentrated in one direction, it has a high magnetic flux density and low iron loss, which gives it excellent iron loss characteristics that directly translate into reduced energy loss in transformers, generators, etc.

[0003] When using such grain-oriented electrical steel sheets to manufacture the cores of small generators and small electric motors, or EI cores, punching and shearing are often performed after a leveling process to correct the coil shape. However, during the leveling process, punching and shearing, the steel sheet may undergo twinning deformation, resulting in cracks, chips and warping, which may cause manufacturing problems. In addition, when manufacturing wound cores, twinning may occur when the steel sheet is wound and deformed into the core shape, which may cause deterioration of the magnetic properties.

[0004] Therefore, various techniques have been proposed to improve processability. For example, Patent Document 1 describes a method for reducing S and N in the raw material components and adding SO to the annealing separator. 3 The compound is SO 3 A technology has been proposed in which the addition of 0.5 to 5.0 mass% of the component mass suppresses the occurrence of twins.

[0005] Furthermore, Patent Document 2 proposes a technology in which a forsterite coating with excellent coating properties is formed by incorporating a Ti compound in an annealing separator, in which the Ti concentration of the steel sheet including the forsterite coating is set in the range of 1.0 to 2.0 times the N concentration to reduce the N in the steel, thereby preventing cracks during shearing or bending.

[0006] Patent Document 3 discloses a technology for reducing the number of starting points for twin generation by refining the secondary recrystallized grain size in the direction perpendicular to the rolling direction (C direction) and reducing the unevenness of the coating / base steel interface. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2000-256810 A [Patent Document 2] Japanese Patent Application Publication No. 06-179977 [Patent Document 3] Special Publication No. 2013-58239 Summary of the Invention [Problem to be solved by the invention]

[0008] By applying the above-mentioned conventional techniques, it is possible to improve the workability of grain-oriented electrical steel sheets without deteriorating their magnetic properties. However, further improvement is required in terms of suppressing the occurrence of twin crystals. For example, when the technology described in Patent Document 1 is applied, the twin crystal occurrence rate is significantly reduced, but the rate can reach a high value of about 10%, which is within the range of variation, and improvement in this regard is required.

[0009] In addition, by optimizing the concentration ratio of Ti and N according to Patent Document 2, bending workability is improved. However, since no consideration is given to twins that occur during bending, further consideration is required to reduce the occurrence rate of twins.

[0010] Refining the secondary grain size in the direction perpendicular to the rolling direction, as described in Patent Document 3, is effective in reducing twins. However, if there is a slight temperature gradient or change in the heating rate in the coil during finish annealing, the secondary recrystallized grains become coarse, which requires strict control, and there is room for improvement.

[0011] The present invention has been made in consideration of the above-mentioned problems faced by the conventional technology, and has as its object to provide a grain-oriented electrical steel sheet which is free from cracks, chips, etc. due to twin deformation and from deterioration of magnetic properties, even in applications that undergo strong processing, such as iron cores and wound cores for small generators, by developing a manufacturing technology for grain-oriented electrical steel sheet which can reduce the rate of twinning compared to the conventional technology, and to propose a manufacturing method for the same. [Means for solving the problem]

[0012] In order to solve the above problems, the inventors conducted numerous experiments on grain-oriented electrical steel sheets with good coating properties, which have a Ti-containing forsterite coating as a base coating formed by applying an annealing separator containing a Ti compound, and investigated ways to reduce the twinning rate compared to the conventional techniques. As a result, they discovered that the oxygen weight of the base coating and the amount of Ti contained in the base coating have a significant effect on the occurrence of twinning, and that in order to suppress the occurrence of twinning, it is effective to increase the oxygen weight of the base coating and limit the amount of Ti in the base coating, which led to the development of the present invention. That is, the gist and configuration of the present invention are as follows.

[0013] 1. A steel sheet having a composition containing 2.8-3.5 mass% Si and 0.01-1.0 mass% Mn, with the balance being Fe and unavoidable impurities, a base coating containing Ti and mainly composed of forsterite, and a top coating formed on the base coating, wherein the base coating has an oxygen coverage of 3.8 g / m 2 or more and Ti weight is 0.06g / m 2 The following is grain-oriented electrical steel sheet.

[0014] 2. The composition further includes Al: more than 0 mass% and not more than 0.015 mass%, N: more than 0 mass% and not more than 0.007 mass%, Cu: more than 0 mass% and not more than 0.14 mass%, Ni: more than 0 mass% and not more than 0.3 mass%, Cr: more than 0 mass% and not more than 0.06 mass%, Sb: more than 0 mass% and not more than 0.04 mass%, Sn: more than 0 mass% and not more than 0.04 mass%, Mo: more than 0 mass% and not more than 0.1 mass%, B: more than 0 mass% and not more than 0.01 mass%, P 2. The grain-oriented electrical steel sheet according to 1, containing one or more selected from the group consisting of Al: more than 0 mass% and 0.06 mass% or less, Nb: more than 0 mass% and 0.02 mass% or less, Bi: more than 0 mass% and 0.01 mass% or less, Ge: more than 0 mass% and 0.05 mass% or less, As: more than 0 mass% and 0.05 mass% or less, Te: more than 0 mass% and 0.02 mass% or less, Ti: more than 0 mass% and 0.04 mass% or less, and V: more than 0 mass% and 0.03 mass% or less.

[0015] 3. A method for producing a grain-oriented electrical steel sheet, comprising the steps of hot rolling a steel slab having a composition containing 0.001-0.10 mass% C, 2.8-3.5 mass% Si, 0.01-1.0 mass% Mn, one or two selected from S and Se in total at 0.005-0.03 mass%, with the balance being Fe and unavoidable impurities, and cold rolling the hot rolled sheet once or at least two times with intermediate annealing in between to obtain a cold rolled sheet, subjecting the cold rolled sheet to primary recrystallization annealing, applying an annealing separator thereto and then finish annealing to obtain a finish annealed sheet, and applying a coating liquid to the finish annealed sheet and then flattening annealing to obtain a grain-oriented electrical steel sheet, The oxygen coverage on the steel sheet surface after the primary recrystallization annealing is 1.5 g / m 2 More than 2.1g / m 2 The annealing separator is preferably TiO relative to 100 parts by mass of MgO. 2 and the temperature rise rate during the final annealing between 700 and 950°C is 15°C / h or more.

[0016] 4. The composition of the steel slab is further selected from the group consisting of Al: 0.003 to 0.015 mass%, N: 0.001 to 0.007 mass%, Cu: 0.01 to 0.14 mass%, Ni: 0.01 to 0.3 mass%, Cr: 0.01 to 0.06 mass%, Sb: 0.004 to 0.04 mass%, Sn: 0.005 to 0.04 mass%, Mo: 0.01 to 0.1 mass%, B: 0.001 to 0.01 mass%, P: 0.0 4. The method for producing a grain-oriented electrical steel sheet according to 3 above, containing one or more elements selected from the group consisting of Nb: 0.05 to 0.06 mass%, Nb: 0.002 to 0.02 mass%, Bi: 0.001 to 0.01 mass%, Ge: 0.001 to 0.05 mass%, As: 0.005 to 0.05 mass%, Te: 0.005 to 0.02 mass%, Ti: 0.005 to 0.04 mass%, and V: 0.005 to 0.03 mass%. Effect of the Invention

[0017] According to the present invention, it is possible to provide a grain-oriented electrical steel sheet which is less prone to twin deformation and which exhibits little deterioration in magnetic properties even when used in applications where strong processing is performed. Therefore, by using the grain-oriented electrical steel sheet of the present invention, it is possible to reduce problems such as cracking and chipping when processing into iron cores and wound cores for small generators, and also to manufacture generators, transformers, and the like with little energy loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] First, the experimental results that led to the present invention will be described. A steel slab containing C: 0.04 mass%, Si: 2.9 mass%, Mn: 0.06 mass%, Se: 0.01 mass%, and Sb: 0.01 mass%, with the balance being Fe and unavoidable impurities, was hot-rolled by a known method to obtain a hot-rolled sheet, which was then annealed at 850°C for 30 seconds. The steel slab was then cold-rolled at least twice, with an intermediate annealing at 900°C for 1 minute, to obtain a cold-rolled sheet with a final thickness of 0.30 mm. Next, the PH 2 O / PH 2The cold-rolled sheet was subjected to primary recrystallization annealing, which also served as decarburization annealing, at 840°C for 140 seconds in various atmospheres with a MgO content of 0.39 to 0.61. At this time, the oxygen coverage on the surface of the cold-rolled sheet after primary recrystallization annealing (hereinafter also referred to as decarburization annealed sheet) was changed in various ways, as shown in Table 1. An annealing separator was then applied to both the front and back surfaces of the decarburization annealed sheet. The annealing separator was a mixture of TiO per 100 parts by mass of MgO. 2 The powder was prepared by varying the amount of addition as shown in Table 1, and the resulting slurry was used at 15 g / m2 so that the hydration amount was 2.0 mass%. 2 After coating, the sheet was dried, wound into a coil, and subjected to final annealing. In the final annealing, the temperature was raised from 700 to 950°C at a rate of 15°C / h, followed by a holding treatment at 1160°C for 5 hours for purification. In this final annealing, a base coat was formed on the surface of the decarburized annealed sheet. After that, a coating liquid consisting of magnesium phosphate, colloidal silica, and chromic anhydride was applied on the base coat, and the coating was baked and subjected to flattening annealing, which also served to correct the shape of the steel sheet, to obtain a product coil (grain-oriented electrical steel sheet). In this flattening annealing, a top coat was formed on the base coat.

[0019] For each steel sheet thus obtained, the measurement results of the oxygen weight of the decarburization annealed sheet after primary recrystallization annealing (hereinafter also referred to as the oxygen weight after decarburization annealing), the oxygen weight and Ti weight of the base coating, as well as the investigation results of the magnetic flux density and twin occurrence rate of the steel sheets are shown in Table 1.

[0020] Here, the oxygen weight per unit area can be measured by a fusion-infrared absorption method, and the Ti weight per unit area can be measured by an emission spectrometry.

[0021] The magnetic flux density when excited with 800A / m is: B 8 (T) to JIS Measurement was performed according to the method specified in C2550.

[0022] Furthermore, the twinning rate is the ratio (%) of the number of specimens with twinning to the total number of specimens subjected to the tensile test, which is obtained by taking 60 or more JIS No. 5 test pieces (samples) from each steel plate, subjecting each JIS No. 5 test piece to a tensile test at room temperature and a tensile speed of 10 m / min, visually observing the pickled and macro-etched surface, and judging the specimen in which a twin line is found to be a specimen with twinning to be a specimen with twinning.

[0023] [Table 1]

[0024] From Table 1, the oxygen coverage of the undercoat is 3.8 g / m 2 or more and Ti weight is 0.06g / m 2 It can be seen that if this value is less than 1.5%, the occurrence rate of twins is effectively reduced to 1.5% or less.

[0025] Furthermore, as shown in Table 1, the oxygen weight of the undercoat was 3.8 g / m 2 In order to control the above, it is necessary to increase the oxygen content after decarburization annealing and to add TiO 2 However, if the oxygen weight after decarburization annealing was too high, the oxygen weight of the undercoat dropped sharply. Similarly, the oxygen weight after decarburization annealing and the amount of TiO in the annealing separator also contributed to the control of the Ti weight of the undercoat. 2 Both the amount of Ti and the amount of Ti contributed to the reduction, especially the 0.06 g / m 2 In order to keep the above value, the TiO in the annealing separator must be 2 In addition to reducing the content, it was also effective to reduce the oxygen weight after decarburization annealing.

[0026] The reason why such results were obtained is unclear, but the present inventors consider it as follows. Grain-oriented electrical steel sheets have secondary recrystallized grains oriented in {110} <001> However, in steel sheets with such a crystal orientation, when deformation is applied in the rolling direction, the {112} <111> The slip system acts to cause twin deformation. However, twin deformation occurs only when the strain rate is high or deformation is performed at a low temperature because the deformation energy is high. In general, it is considered effective to reduce such twins by, for example, reducing coarse inclusions or making the grain size fine to reduce local stress concentration, or by reducing impurities to reduce the strength against material deformation. In relation to the coating, it is known that it is effective to increase the strength of the coating by introducing S into the coating as described in Patent Document 1 above, or by adjusting the ratio of Ti and N as described in Patent Document 2. In contrast, the above findings suggest that factors other than the coating strength are involved. In other words, the inventors considered it important not to directly transmit the coating tension of the topcoat coating to the base steel. In other words, the steel sheet is subjected to a tensile stress by the topcoat coating, and twins occur when further deformation stress is applied under this condition. Conversely, if the coating stress is not applied, twins are unlikely to occur even with a small deformation stress.

[0027] If the oxygen weight of the undercoat is increased beyond a certain level, the stress of the upper topcoat is relaxed in the undercoat, and the stress applied to the steel substrate is reduced. Also, the higher the Ti content in the undercoat, the higher the tension of the undercoat itself, making it more likely for twin crystals to occur.

[0028] Next, a method for controlling the oxygen coverage of the undercoat will be described. Since the oxygen weight of the base coating roughly correlates with the oxygen weight of the steel sheet surface after decarburization annealing, increasing this will also increase the oxygen weight of the base coating. However, if the oxygen weight after decarburization annealing is too high, too much of the base coating will be formed, and the base coating will partially peel off, which will in turn decrease the oxygen weight of the base coating. Therefore, there is an appropriate range for the oxygen weight after decarburization annealing.

[0029] In addition to adjusting the oxygen content after decarburization annealing, the TiO 2 The oxygen coverage of the undercoat can also be increased by increasing the amount of TiO 2 During the final annealing, it decomposes to generate oxygen, which oxidizes the steel sheet and increases the amount of the base coating formed.

[0030] Furthermore, a method for controlling the Ti coating weight of the undercoat is described. The Ti content is determined by the Ti source being TiO in the annealing separator. 2 Therefore, this TiO 2 It is roughly correlated with the amount of TiO 2 In addition to adjusting the amount of oxygen, the amount of oxygen after decarburization annealing also has an effect. This is because if the amount of oxygen after decarburization annealing is high, the oxides present on the surface layer of the subscale, such as Fe 2 SiO 4 Materials such as TiO 2 undergoes a substitution reaction to form FeTiO 3 This allows Ti to easily penetrate into the coating, which is thought to increase the Ti content in the coating.

[0031] As described above, the oxygen coverage after decarburization annealing and the TiO in the annealing separator 2 Both amounts of addition affect both the oxygen weight and Ti weight of the undercoat. Therefore, the oxygen weight after decarburization annealing and the TiO 2 By optimizing the amount of each added, the oxygen weight and Ti weight of the undercoating can be kept within appropriate ranges, and the rate of twinning can be reduced.

[0032] The present invention will be described in detail below. First, the grain-oriented electrical steel sheet to which the present invention is directed will be described. The grain-oriented electrical steel sheet to which the present invention relates has a component composition containing 2.8-3.5 mass% Si and 0.01-1.00 mass% Mn, with the balance being Fe and unavoidable impurities, and has a base coating that contains Ti and is mainly composed of forsterite, and a top coating that is formed on the base coating.

[0033] This grain-oriented electrical steel sheet has an oxygen coverage of 3.8 g / m2 in the base coating. 2 or more, and the Ti weight is 0.06 g / m 2 This is based on the above-mentioned new finding that strain due to tension in the topcoat film promotes twinning, and that the rate of twinning can be suppressed if the base film can relieve the stress caused by the topcoat film. In other words, the oxygen coverage of the undercoat is 3.8 g / m 2 If the Ti weight is less than 0.06 g / m, the ability of the undercoat to relax the tension of the coating decreases, resulting in an increase in the occurrence of twins. 2 If the oxygen content exceeds 3.8 g / m, the tension of the undercoat itself increases, and the occurrence rate of twins also increases. 2 or more, and the Ti weight is 0.06 g / m 2 The following applies.

[0034] On the other hand, in the undercoating, there is no need to particularly limit the upper limit of the oxygen weight per unit area and the lower limit of the Ti weight per unit area. However, from the viewpoint of the coating adhesion, the oxygen weight per unit area of ​​the undercoating is set to 5.0 g / m 2 From the same viewpoint, the Ti coating weight in the undercoat is preferably 0.01 g / m or less. 2 More preferably, it is equal to or greater than this.

[0035] The topcoat film formed on the above-mentioned undercoat film can be of any type, and can be any coating commonly used for topcoats of grain-oriented electrical steel sheets, such as a tension-imparting coating made by applying and baking a coating liquid consisting of magnesium phosphate-colloidal silica-titanium sulfate.

[0036] Furthermore, the grain-oriented electrical steel sheet to which the present invention is directed has a magnetic flux density of B 8It is preferable that the magnetic flux density is 1.88T or less. The reason why it is preferable to lower the magnetic flux density is that, in general, when the magnetic flux density is high, the secondary recrystallized grain size becomes large, the grain boundary density decreases, and twins tend to develop. If the magnetic flux density is set low to refine the secondary recrystallized grain size, it is possible to prevent the strain applied during processing from concentrating locally, and to make it easier to prevent twin deformation. Therefore, the present invention cannot be applied to a technique in which, for example, the coil is annealed under a temperature gradient to elongate the secondary recrystallized grains. In addition, a technique in which the secondary recrystallized grains are grown by holding the coil in the secondary recrystallization temperature range during the finish annealing is also inappropriate for the present invention.

[0037] The composition of the grain-oriented electrical steel sheet may further contain one or more elements selected from Al, N, Cu, Ni, Cr, Sb, Sn, Mo, B, P, Nb, Bi, Ge, As, Te, Ti, and V. Specifically, the composition of the grain-oriented electrical steel sheet is as follows: Al: more than 0 mass% and not more than 0.015 mass%, N: more than 0 mass% and not more than 0.007 mass%, Cu: more than 0 mass% and not more than 0.14 mass%, Ni: more than 0 mass% and not more than 0.3 mass%, Cr: more than 0 mass% and not more than 0.06 mass%, Sb: more than 0 mass% and not more than 0.04 mass%, Sn: more than 0 mass% and not more than 0.04 mass%, Mo: more than 0 mass% and not more than 0.1 mass%, B: more than 0 mass% and not more than 0.01 mass%, and mass% or less, P: more than 0 mass% and 0.06 mass% or less, Nb: more than 0 mass% and 0.02 mass% or less, Bi: more than 0 mass% and 0.01 mass% or less, Ge: more than 0 mass% and 0.05 mass% or less, As: more than 0 mass% and 0.05 mass% or less, Te: more than 0 mass% and 0.02 mass% or less, Ti: more than 0 mass% and 0.04 mass% or less, and V: more than 0 mass% and 0.03 mass% or less.

[0038] Next, a method for producing the above-mentioned grain-oriented electrical steel sheet will be described. First, the chemical composition of the steel slab will be described.

[0039] C: 0.001 to 0.10 mass% C is a necessary component for generating Goss-oriented crystal grains, and in order to realize this effect, it is necessary to add 0.001 mass% or more. On the other hand, if the amount of C added exceeds 0.10 mass%, it becomes difficult to decarburize to a level that does not cause magnetic aging in the subsequent decarburization annealing. Therefore, the C content is set to a range of 0.001 to 0.10 mass%. The C content is preferably 0.015 mass% or more, and preferably 0.08 mass% or less.

[0040] Si: 2.8~3.5mass% Silicon is a necessary component for increasing the electrical resistance of steel and reducing iron loss, stabilizing the BCC structure, and enabling high-temperature heat treatment, and must be added in an amount of at least 2.8 mass%. However, the addition of more than 3.5 mass% reduces workability and makes it difficult to manufacture by cold rolling. Therefore, the silicon content is set to a range of 2.8 to 3.5 mass%. Taking into account the effect of preventing twinning, the silicon content is preferably 2.8 mass% or more, and preferably 3.3 mass% or less.

[0041] Mn: 0.01 to 1.0 mass% Mn is an element that is effective in improving the hot brittleness of steel, and also functions as an inhibitor by forming precipitates such as MnS and MnSe when S or Se is contained. The above effect can be obtained by adding 0.01 mass% or more. However, if it is added in an amount exceeding 1.0 mass%, the precipitates such as MnSe become coarse, and the inhibitor effect is lost. Therefore, the Mn content is set to the range of 0.01 to 1.0 mass%. The Mn content is preferably 0.03 mass% or more and 0.50 mass% or less.

[0042] S, Se: 0.005-0.03 mass% for one or both types in total S and Se combine with Mn and Cu to form MnSe, MnS, and Cu. 2-x Se,Cu 2-xIt is a useful component that forms S, precipitates as a dispersed second phase in steel, and exerts an inhibitor effect. If the total content of S and Se is less than 0.005 mass%, the above-mentioned addition effect is insufficient, while addition exceeding 0.03 mass% causes the secondary grain size to become coarse, which is disadvantageous for the generation of twins. Therefore, the amount of these elements added is in the range of 0.005 to 0.03 mass% whether added alone or in combination. The total content of S and Se is preferably 0.006 mass% or more, and preferably 0.020 mass% or less.

[0043] In addition to the above-mentioned chemical composition, the steel slab used in the production of the grain-oriented electrical steel sheet of the present invention further contains Al (sol.Al): 0.003 to 0.015 mass%, N: 0.001 to 0.007 mass%, Cu: 0.01 to 0.14 mass%, Ni: 0.01 to 0.3 mass%, Cr: 0.01 to 0.06 mass%, Sb: 0.004 to 0.04 mass%, Sn: 0.005 to 0.04 mass%, Mo: 0.01 to 0.1 mass%, B: 0.004 to 0.04 mass%, and Sn: 0.005 to 0.04 mass%. It may contain one or more selected from the group consisting of C: 0.001 to 0.01 mass%, P: 0.005 to 0.06 mass%, Nb: 0.002 to 0.02 mass%, Bi: 0.001 to 0.01 mass%, Ge: 0.001 to 0.05 mass%, As: 0.005 to 0.05 mass%, Te: 0.005 to 0.02 mass%, Ti: 0.005 to 0.04 mass%, and V: 0.005 to 0.03 mass%.

[0044] The elements sol.Al, N, Cu, Ni, Cr, Sb, Sn, Mo, B, P, Nb and Bi segregate at the grain boundaries and on the steel sheet surface to act as auxiliary inhibitors and have the effect of moderately improving the magnetic properties, so they can be added as necessary. However, in order to prevent the magnetic flux density from increasing too much beyond a certain level as in the present invention, the amount added must be lower than in the past. Therefore, when adding these elements, it is preferable to keep the amount within the above range.

[0045] In addition, the elements Ge, As, Te, Ti and V all have a stable inhibitor effect (suppressing power) and can be present uniformly even in processes where temperature variations occur within the steel sheet, such as slab heating and finish annealing, and therefore have the effect of stabilizing the magnetic flux density over the entire length of the coil, so they can be added as needed.

[0046] Of the above-mentioned components, C is decarburized and removed from the steel during the manufacturing process, while S and Se are purified and removed from the steel during final annealing, so that the contents of both are at the unavoidable impurity level at the product stage.

[0047] Next, the manufacturing conditions of the grain-oriented electrical steel sheet according to the present invention will be described in detail. The grain-oriented electrical steel sheet of the present invention is prepared by melting steel having the above-described composition in a conventionally known refining process, forming a steel material (steel slab) using a continuous casting method or an ingot casting-blooming rolling method, and then hot rolling the steel material to form a hot-rolled sheet, which is annealed as necessary, and then cold rolling once or twice or more times with intermediate annealing in between to form a cold-rolled sheet of the final thickness. In the present invention, in order to refine secondary grains and suppress the occurrence of twins without increasing the magnetic flux density too much, it is preferable that the final cold rolling reduction is relatively low. Specifically, the final cold rolling reduction is preferably 50 to 70%, and more preferably 55 to 66%.

[0048] Next, the cold-rolled sheet is subjected to primary recrystallization annealing or primary recrystallization annealing that also serves as decarburization annealing. At this time, a nitriding treatment may be performed as necessary. The first feature of the present invention and one of the main elements of the present invention is that the oxygen weight of the oxide film formed at this time is adjusted to be higher than that of the conventional method. That is, the oxygen coverage on the steel sheet surface after primary recrystallization annealing is 1.5 to 2.1 g / m 2 At least one of the temperature, time and atmosphere in the primary recrystallization annealing is adjusted so that the oxygen coverage on the steel sheet surface after the primary recrystallization annealing is 1.5 to 2.1 g / m 2The reason for this is to set the oxygen weight and Ti weight in the undercoat in an appropriate range. In particular, the oxygen weight is set to 1.5 g / m 2 If the oxygen content is less than 2.1 g / m, the formation of the undercoat film becomes insufficient. 2 If it exceeds this value, the formation of the undercoat film will be excessive, eventually resulting in spot-like peeling, and sufficient effect will not be obtained.

[0049] As conditions for the primary recrystallization annealing to set the oxygen weight per unit area in the above range after the primary recrystallization annealing, the annealing temperature is preferably set to 700 to 900°C and the annealing time is preferably set to the range of 30 to 300 seconds. If the annealing temperature is less than 700°C or the annealing time is less than 30 seconds, the desired oxygen weight per unit area may not be secured or decarburization may be insufficient. On the other hand, if the annealing temperature exceeds 900°C or the annealing time exceeds 300 seconds, the oxygen weight per unit area may become excessive. In addition, a wet hydrogen atmosphere is used during the decarburization annealing. The dew point is set to the range of 45 to 60°C, and the H 2 Concentration is the same as in the conventional method, and can be in the range of 40% to 80%. 2 From the concentration, the oxidizing pH of the atmosphere 2 O / PH 2 By adjusting the pH, the amount of oxygen per unit area can be adjusted. 2 O / PH 2 The range of 0.40 to 0.55 is preferable, and it is also possible to change the range at each stage of the heating zone and the soaking zone.

[0050] The above-mentioned soaking area can be divided into two stages, the front stage and the rear stage. The front stage and the rear stage have different soaking temperatures, oxidizing atmosphere, pH 2 O / PH 2 If the temperature is changed, the temperature difference between the front and rear stages should be 20℃ or more. If it is oxidizing, the pH 2 O / PH 2 The difference between the temperature and the temperature is changed by 0.2 or more. Generally, there is no particular limitation regarding the temperature, but it is better to make the latter stage higher in temperature than the former stage. Regarding the oxidizing atmosphere, the latter stage has a lower pH than the former stage. 2 O / PH 2In this case, the temperature and / or pH can be adjusted between the final stage and the stage before it. 2 O / PH 2 The difference between temperature and pH should be within the above range. 2 O / PH 2 The final soaking region when the temperature is changed is defined as the final stage.

[0051] In order to achieve the high oxygen weight defined in the present invention, it is possible to devise a pretreatment for the primary recrystallization annealing. For example, when cleaning the rolled sheet (cold rolled sheet), electrolytic degreasing is performed with a degreasing solution (electrolyte) containing sodium silicate. This results in a reduction in the amount of SiO 2 The compound is electrodeposited on the surface of the steel sheet, and serves as the starting point of oxidation during decarburization annealing, thereby increasing the oxygen coverage.

[0052] Since the oxygen weight after primary recrystallization annealing varies depending on the material composition and previous processes, it is necessary to adjust the annealing conditions according to each process. For example, if the Si content in the steel material is low, at 3 mass% or less, the oxygen weight tends to decrease, so the dew point is set higher. In addition, if the oxygen weight on the surface of the steel sheet before primary recrystallization annealing is 0.1 g / m 2 If the above conditions are high, it is also effective to set the dew point lower.

[0053] Furthermore, in order to increase the oxygen weight per unit area after the primary recrystallization annealing, it is also possible to set the dew point of the heating region higher and the dew point of the soaking region lower. These treatments are not particularly limited, and any conditions may be used as long as the oxygen weight per unit area can be kept within a desired range.

[0054] After the primary recrystallization annealing, an annealing separator containing MgO as the main component is applied to the surface of the steel sheet. 2 Here, TiO 2 The main reason for adding TiO is to improve the adhesion of the coating. 2In the present invention, the addition of TiO 2 The second feature is that the amount of TiO added is kept to a very small amount. 2 The amount of TiO added is in the range of 0.6 to 2.7 parts by mass when the amount of MgO is 100 parts by mass. 2 If the amount added (content) is less than 0.6 parts by mass, the coating adhesion decreases and a base pattern occurs. 2 When the amount added is more than 2.7 parts by mass, the amount of Ti contained in the base coating is 0.06 g / m2 in terms of Ti basis weight. 2 If the thickness exceeds this value, the occurrence rate of twins increases.

[0055] TiO 2 The conditions of the annealing separator other than the amount of addition may be as known in the art. For example, the additives of the annealing separator include TiO 2 In addition, borates, sulfates, carbonates, hydroxides, chlorides, etc. of Li, Na, K, Mg, Ca, Sr, Sn, Sb, Cr, Fe, Ni, etc. can be added alone or in combination. The amount of the annealing separator applied to the steel sheet surface is 8 to 16 g / m on both sides. 2 The hydration amount is preferably in the range of 0.5 to 3.7 mass %. Furthermore, the annealing separator is usually prepared by forming a slurry with water, applying the slurry with a roll coater, and then drying. This method can also be used in the present invention.

[0056] After the application of the annealing separator, final annealing is performed. The third feature of the present invention is that the heating rate at this time is specified. That is, the heating rate between 700 and 950°C during final annealing must be 15°C / h or more. This temperature range is where the formation of the base coating begins in earnest, and also where the TiO 2 This is also the temperature range just before Fe decomposes and Ti penetrates into the undercoat. If the heating rate in this temperature range is slow, Fe 2 SiO 4 From FeTiO 3If the substitution reaction that forms the above-mentioned occurs too quickly, Ti will penetrate into the film too quickly, increasing the Ti content in the undercoat. In addition, the activity of MgO at this temperature is lost, making it difficult for the subsequent coating reaction to proceed, and the oxygen coverage of the undercoat will also decrease. Furthermore, the growth of secondary recrystallized grains is promoted at this temperature, resulting in coarsening of the grain size. Therefore, the heating rate between 700 and 950°C during the final annealing is set to 15°C / h or more, and preferably 20°C / h or more.

[0057] Other conditions for the final annealing may be the same as in the conventional method. For example, the atmosphere is H 2 ,N 2 , Ar, or a mixture of these conditions may be used. Finish annealing (holding treatment) is generally performed at a temperature of 1150°C to 1250°C for a time of 3 hours to 50 hours, and this range may also be used in the present invention. If the temperature is lower than 1150°C or the time is shorter than 3 hours, purification will be insufficient and precipitates will remain, which may increase the rate of twinning. On the other hand, if the temperature is higher than 1250°C or the time is longer than 50 hours, the coil may buckle and the yield may decrease.

[0058] Furthermore, after the final annealing, an insulating film is applied and then annealed for flattening, which also serves as baking, and these may be performed by known methods. By using the manufacturing method consisting of the series of steps as described above, it is possible to obtain a grain-oriented electrical steel sheet in which twin crystals are unlikely to occur even when subjected to severe working. EXAMPLES

[0059] A steel slab containing C: 0.05 mass%, Si: 3.2 mass%, Mn: 0.06 mass%, S: 0.01 mass%, Al: 0.006 mass%, N: 0.004 mass%, and Mo: 0.01 mass%, with the balance being Fe and unavoidable impurities, was heated at 1410°C for 30 minutes, hot-rolled to a hot-rolled sheet with a thickness of 2.5 mm, and hot-rolled sheet annealed at 1000°C for 1 minute. The sheet was then cold-rolled to a thickness of 0.9 mm, intermediate annealed at 980°C for 1 minute, and cold-rolled to a final thickness of 0.35 mm.

[0060] Next, pH 2 O / PH 2 The decarburization annealed sheet was subjected to primary recrystallization annealing, which also served as decarburization annealing, at 850°C for 120 seconds in an atmosphere of 0.51. At this time, the oxygen weight of the decarburization annealed sheet was 2.0 g / m 2 Further, after that, TiO was added to 100 parts by mass of MgO as an annealing separator. 2 2.4 parts by mass of Li 2 SO 4 The powder was made into a slurry and applied at 11 g / m2 on both sides of the steel sheet so that the hydration amount was 1.3 mass%. 2 After coating, the wire was dried, wound into a coil, and subjected to final annealing. The final annealing was performed by increasing the temperature from 700 to 950°C at various heating rates shown in Table 2, followed by a holding treatment at 1160°C for 5 hours for purification.

[0061] Thereafter, a coating liquid consisting of magnesium phosphate-colloidal silica-titanium sulfate was applied, and the coating was baked and subjected to flattening annealing, which also served to correct the shape of the steel sheet, to obtain a product coil (grain-oriented electrical steel sheet). The magnetic flux density B 8 The results are shown in Table 2 together with the oxygen weight and Ti weight of the undercoat. 8 The twinning rate was measured according to the above-mentioned measurement method.

[0062] From Table 2, it can be seen that when the heating rate is slow, the oxygen coverage of the undercoating decreases and the Ti content increases, and accordingly the twinning rate also increases.

[0063] [Table 2] EXAMPLES

[0064] A steel slab containing the various components shown in Table 3, with the remainder being Fe and unavoidable impurities, was heated at 1380°C for 60 minutes, then hot rolled to a hot rolled sheet with a thickness of 2.2 mm, and hot rolled sheet annealed at 1000°C for 1 minute. It was then cold rolled to an intermediate thickness of 0.8 mm, intermediate annealed at 1000°C for 2 minutes, and further cold rolled to a cold rolled sheet with a final thickness of 0.27 mm. This was then cooled at 10C / dm in an electrolyte containing 2% sodium silicate. 2 After electrolytic degreasing, 2 O / PH 2 The specimens were subjected to primary recrystallization annealing, which also served as decarburization annealing, at 820°C for 100 seconds in an atmosphere of 0.46. After that, TiO was added to 100 parts by mass of MgO as an annealing separator. 2 The powder was made into a slurry form by adding 1.5 parts by mass of ammonium nitrate and 2.5 parts by mass of calcium hydroxide, and the hydration amount was 1.0 mass%. The slurry was applied to both sides of the steel sheet at 10 g / m 2 After coating, the strip was dried and wound into a coil, which was then subjected to final annealing. The final annealing was performed by raising the temperature between 700 and 950°C at a rate of 20°C / h, followed by a holding treatment at 1180°C for 10 hours for purification. After that, a coating liquid consisting of magnesium phosphate, colloidal silica, and titanium sulfate was applied, and the coating was baked and subjected to flattening annealing, which also served to correct the shape of the steel sheet, to obtain the product coil (grain-oriented electrical steel sheet).

[0065] The magnetic flux density B 8The results are shown in Table 3 together with the oxygen weight after the primary recrystallization annealing, the oxygen weight and Ti weight in the base coat. 8 The twinning rate was measured according to the above-mentioned measurement method.

[0066] From Table 3, it can be seen that under conditions in which electrolytic degreasing is performed and the oxygen weight per unit area after primary recrystallization annealing is kept within the appropriate range, the oxygen weight per unit area of ​​the base coating increases and the Ti weight per unit area decreases for steel sheets of any composition, and the twin occurrence rate is also improved accordingly.

[0067] [Table 3]

Claims

1. The steel sheet has a composition containing 2.8 to 3.5 mass% Si and 0.01 to 1.0 mass% Mn, with the balance being Fe and unavoidable impurities, an undercoat film containing Ti and mainly composed of forsterite, and a topcoat film formed on the undercoat film, and the undercoat film has an oxygen coverage of 3.8 g / m 2 or more and Ti weight is 0.01 g / m2 or more and 0.06 g / m 2 The following is grain-oriented electrical steel sheet.

2. The composition further includes Al: more than 0 mass% and not more than 0.015 mass%, N: more than 0 mass% and not more than 0.007 mass%, Cu: more than 0 mass% and not more than 0.14 mass%, Ni: more than 0 mass% and not more than 0.3 mass%, Cr: more than 0 mass% and not more than 0.06 mass%, Sb: more than 0 mass% and not more than 0.04 mass%, Sn: more than 0 mass% and not more than 0.04 mass%, Mo: more than 0 mass% and not more than 0.1 mass%, B: more than 0 mass% and not more than 0.01 mass%, P: 0 2. The grain-oriented electrical steel sheet according to claim 1, comprising one or more elements selected from the group consisting of Al: more than 0 mass% and 0.06 mass% or less, Nb: more than 0 mass% and 0.02 mass% or less, Bi: more than 0 mass% and 0.01 mass% or less, Ge: more than 0 mass% and 0.05 mass% or less, As: more than 0 mass% and 0.05 mass% or less, Te: more than 0 mass% and 0.02 mass% or less, Ti: more than 0 mass% and 0.04 mass% or less, and V: more than 0 mass% and 0.03 mass% or less.

3. A method for producing a grain-oriented electrical steel sheet, comprising the steps of hot rolling a steel slab having a component composition containing 0.001 to 0.10 mass% C, 2.8 to 3.5 mass% Si, 0.01 to 1.0 mass% Mn, 0.005 to 0.03 mass% in total of one or two selected from S and Se, with the balance being Fe and unavoidable impurities, and cold rolling the hot rolled sheet once or at least two times with intermediate annealing between them to form a cold rolled sheet, subjecting the cold rolled sheet to primary recrystallization annealing, applying an annealing separator thereto and then finish annealing to form a finish annealed sheet, and applying a coating liquid to the finish annealed sheet and then flattening annealing to obtain a grain-oriented electrical steel sheet, The oxygen coverage on the steel sheet surface after the primary recrystallization annealing is 1.5 g / m 2 2.1g / m or more 2 The annealing separator contains TiO relative to 100 parts by mass of MgO. 2 and the temperature rise rate in the final annealing between 700 and 950° C. is 15° C. / h or more.

4. The composition of the steel slab further includes Al: 0.003 to 0.015 mass%, N: 0.001 to 0.007 mass%, Cu: 0.01 to 0.14 mass%, Ni: 0.01 to 0.3 mass%, Cr: 0.01 to 0.06 mass%, Sb: 0.004 to 0.04 mass%, Sn: 0.005 to 0.04 mass%, Mo: 0.01 to 0.1 mass%, B: 0.001 to 0.01 mass%, P: 0.001 to 0.01 mass%, and 4. The method for producing a grain-oriented electrical steel sheet according to claim 3, further comprising one or more selected from the group consisting of Nb: 0.5 to 0.06 mass%, Nb: 0.002 to 0.02 mass%, Bi: 0.001 to 0.01 mass%, Ge: 0.001 to 0.05 mass%, As: 0.005 to 0.05 mass%, Te: 0.005 to 0.02 mass%, Ti: 0.005 to 0.04 mass%, and V: 0.005 to 0.03 mass%.

Citation Information

Patent Citations

  • Silicon steel sheet excelling in high-frequency characteristic and its production

    JP1986238939A

  • Grain-oriented silicon steel sheet excellent in bendability and core loss property

    JP1994179977A

  • Forsterite film of grain oriented silicon steel sheet with high magnetic flux density and its formation

    JP1997184017A

  • Production of grain oriented silicon steel sheet excellent in magnetic property and coating characteristics

    JP1998060533A

  • Grain oriented silicon steel sheet excellent in magnetic property in low magnetic field and high-frequency and punching workability and its production

    JP2000256810A