Decorative sheet
The decorative sheet achieves a smooth and uniform texture through a surface protective layer with controlled ridges, enhancing tactile experience and durability while avoiding gloss adjusters, thus improving fingerprint resistance and stain resistance.
Patent Information
- Application Number
- JP2024522411
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-01-04
- Filing Date
- 2023-12-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2043-12-26
AI Technical Summary
Existing decorative sheets lack uniformity in texture and smoothness, and often require gloss adjusters that can lead to susceptibility to fingerprints and reduced oil repellency.
A decorative sheet with a surface protective layer featuring a unique uneven structure, comprising ridges with specific peak heights and compositions, formed using ionizing radiation-curable resins and silica particles, ensuring uniform texture and low gloss without the need for gloss adjusters.
The decorative sheet provides a smooth, uniform tactile sensation with excellent fingerprint resistance, stain resistance, and scratch resistance, maintaining a low gloss appearance.
Smart Images

Figure 0007582559000005 
Figure 0007582559000006 
Figure 0007582559000007
Abstract
Description
[Technical Field]
[0001] The present invention relates to a decorative sheet. [Background technology]
[0002] Decorative sheets are used to decorate the surfaces of interior and exterior materials such as building fixtures, furniture, fixtures, and flooring materials, for the purpose of imparting design and durability to these materials. Decorative sheets are generally widely used as decorative panels that are attached via an adhesive or the like to the surface of substrates such as wood, wood boards, metal plates, non-combustible boards, paper substrates, and resin substrates.
[0003] Designs can be added by forming patterns such as wood grain or stone grain using various printing methods. Plain decorative sheets without patterns are sometimes preferred. The choice of whether to have a pattern or not and the type of pattern vary depending on the application and preference.
[0004] The glossiness of the surface is also important for the design of decorative sheets. There are a variety of decorative sheets to choose from depending on the application and preference, ranging from high gloss like a mirror to low gloss that does not reflect light at all.
[0005] As mentioned above, durability is an important function of decorative sheets, along with providing design. Durability is a comprehensive assessment of scratch resistance, stain resistance, and whether these can be maintained over a long period of time. Requirements vary depending on the environment and situation in which the decorative sheet is used, but decorative sheets with high performance are always in demand.
[0006] To impart durability, a surface protective layer is generally formed on the outermost surface of the decorative sheet. Furthermore, to adjust the aforementioned gloss, particularly to achieve low gloss, a gloss adjuster (matt additive) is generally added to the surface protective layer.
[0007] Furthermore, decorative sheets are generally subjected to processes such as cutting and bending in order to form decorative materials such as decorative plates, and therefore it is preferable that the decorative sheets have processability that can withstand these processes.
[0008] As such, a decorative sheet that takes into consideration design (low gloss), scratch resistance, and stain resistance is disclosed in Patent Document 1, for example. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Publication No. 2019-119138 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a decorative sheet that gives a smooth feel and has excellent uniformity of feel. [Means for solving the problem]
[0011] According to one aspect of the present invention, there is provided an insulating film comprising an original fabric layer and a surface protective layer provided on one surface of the original fabric layer, wherein the surface of the surface protective layer is provided with an uneven structure including a plurality of ridge-like portions each protruding in a ridge-like shape, the uneven structure of the surface protective layer has a protruding peak height Rpk of less than 3.5 μm, and the surface protective layer has a mass concentration C (mass %) of carbon atoms, a mass concentration O (mass %) of oxygen atoms, and a mass concentration Si (mass %) of silicon atoms that satisfy the following relationship: 0.5≦{Si / (C+O+Si)}×100 A decorative sheet that satisfies the above requirements is provided.
[0012] According to another aspect of the present invention, there is provided a decorative sheet according to the above aspect, wherein the protruding peak height Rpk is 0.5 μm or more.
[0013] According to yet another aspect of the present invention, the surface protective layer has a mass concentration C (mass %) of carbon atoms, a mass concentration O (mass %) of oxygen atoms, and a mass concentration Si (mass %) of silicon atoms that satisfy the following relationship: 0.5≦{Si / (C+O+Si)}×100≦5.0 There is provided a decorative sheet according to any of the above aspects that satisfies the above.
[0014] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the uneven structure of the surface protective layer has a mean length RSm of roughness curve elements of 800 μm or less. According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the uneven structure of the surface protective layer has a mean length RSm of roughness curve elements of 350 μm or less.
[0015] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the average length RSm is 10 μm or more.
[0016] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the thickness of the surface protective layer is 2 μm or more and 15 μm or less.
[0017] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the thickness of the surface protective layer is not less than 2 μm and less than 10 μm.
[0018] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the gloss of the surface protective layer is 20.0 or less.
[0019] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the gloss of the surface protective layer is 10.0 or less.
[0020] According to yet another aspect of the present invention, there is provided a decorative sheet relating to any of the above aspects, wherein at least some of the multiple ridge portions are adjacent in the width direction, and at the position where at least some of the multiple ridge portions are adjacent in the width direction, a cross section parallel to the width direction and the thickness direction of the surface protection layer has a sinusoidal shape in the portion where the uneven structure is provided.
[0021] According to yet another aspect of the present invention, there is provided a decorative sheet according to any one of the above aspects, wherein the surface protective layer contains a cured product of an ionizing radiation curable resin.
[0022] According to yet another aspect of the present invention, there is provided a decorative sheet according to the above aspect, wherein the ionizing radiation curable resin is an acrylate containing a repeating structure as a main component, the repeating structure is any one of ethylene oxide, propylene oxide, and ε-caprolactone, and the number of repetitions of the repeating structure is 3 or more.
[0023] According to yet another aspect of the present invention, there is provided a decorative sheet according to the above aspect, wherein the ionizing radiation curable resin is primarily composed of an acrylate, the acrylate being composed of a first acrylate containing a repeating structure and a mono- to hexa-functional second acrylate, the repeating structure being any one of ethylene oxide, propylene oxide, and ε-caprolactone, and the number of repetitions of the repeating structure being 3 or more.
[0024] According to yet another aspect of the present invention, there is provided a decorative material comprising a decorative sheet according to any one of the above aspects and a substrate to which the decorative sheet is attached. [Effects of the Invention]
[0025] According to the present invention, it is possible to provide a decorative sheet that provides a smooth feel and has excellent uniformity of feel. [Brief explanation of the drawings]
[0026] [Figure 1]FIG. 1 is a cross-sectional view of a decorative material including a decorative sheet according to one embodiment of the present invention. [Figure 2] FIG. 2 is a cross-sectional view of the surface protective layer included in the decorative sheet of FIG. [Figure 3] FIG. 3 is a microscope image of a surface protective layer included in a decorative sheet according to one example of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0027] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects, either singly or in combination.
[0028] Furthermore, the embodiments shown below are merely examples of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of the present invention within the technical scope defined by the claims.
[0029] In the drawings, elements having the same or similar functions are denoted by the same reference numerals, and redundant explanations will be omitted. Furthermore, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, and the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual relationship.
[0030] <1> Decorative materials and decorative sheets Fig. 1 is a cross-sectional view of a decorative material including a decorative sheet according to one embodiment of the present invention. Fig. 2 is a cross-sectional view of a surface protective layer included in the decorative sheet of Fig. 1. Fig. 3 is a micrograph of a surface protective layer included in a decorative sheet according to one example of the present invention.
[0031] The cross section shown in Fig. 2 is a cross section along the thickness direction of the surface protection layer. The micrograph in Fig. 3 is a plan view photograph obtained by a laser microscope (OLS-4000 manufactured by Olympus Corporation).
[0032] The decorative material 11 shown in FIG. 1 includes a substrate B and a decorative sheet 1 attached thereto. Here, the decorative material 11 is a decorative board. The decorative board may be a flat plate, or may be curved or folded. The decorative material 11 may have a shape other than a plate.
[0033] Here, the substrate B is a plate material. The plate material is, for example, a wood board, an inorganic board, a metal plate, or a composite board made of multiple materials. The substrate B may have a shape other than a plate.
[0034] The decorative sheet 1 includes a base fabric layer 2, a design layer 3, a transparent resin layer 4, a surface protective layer 5, an adhesive layer 7, a primer layer 6, and a masking layer 8. The design layer 3, adhesive layer 7, transparent resin layer 4, and surface protective layer 5 are provided in this order from the base fabric layer 2 side on the surface of the base fabric layer 2 opposite the surface facing the substrate B. The masking layer 8 and primer layer 6 are provided in this order from the base fabric layer 2 side on the surface of the base fabric layer 2 facing the substrate B. One or more of the design layer 3, transparent resin layer 4, primer layer 6, adhesive layer 7, and masking layer 8 may be omitted. The elements included in the decorative sheet 1 will be explained below in order.
[0035] <1.1> Raw fabric layer The raw fabric layer 2 or its material can be any material selected from, for example, paper, synthetic resin, synthetic resin foam, rubber, nonwoven fabric, synthetic paper, metal foil, etc. Examples of paper include tissue paper, titanium paper, and resin-impregnated paper. Examples of synthetic resins include polyethylene, polypropylene, polybutylene, polystyrene, polycarbonate, polyester, polyamide, ethylene-vinyl acetate copolymer, polyvinyl alcohol, and acrylic. Examples of rubber include ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, styrene-butadiene copolymer rubber, styrene-isoprene-styrene block copolymer rubber, styrene-butadiene-styrene block copolymer rubber, and polyurethane. Examples of nonwoven fabrics include organic and inorganic nonwoven fabrics. Examples of metals for the metal foil include aluminum, iron, gold, and silver.
[0036] The thickness of the raw fabric layer 2 is preferably within the range of 20 μm to 250 μm, taking into consideration the ease of printing and costs.
[0037] <1.2> Primer layer When an olefin-based resin is used as the material of the raw fabric layer 2, the surface of the raw fabric layer 2 is often in an inactive state. Therefore, in this case, it is preferable to provide a primer layer 6 between the raw fabric layer 2 and the substrate B. When the raw fabric layer 2 is made of an olefin-based material, the primer layer 6 may be omitted, and the raw fabric layer 2 may be subjected to a surface modification treatment such as corona treatment, plasma treatment, ozone treatment, electron beam treatment, ultraviolet treatment, or dichromate treatment in order to improve the adhesion between the raw fabric layer 2 and the substrate B.
[0038] Materials that can be used for the primer layer 6 include, for example, the materials described below for the design layer 3. Since the primer layer 6 is applied to the back surface of the decorative sheet 1, and considering that the decorative sheet 1 will be wound up in web form, an inorganic filler may be added to the primer layer 6 to avoid blocking and increase adhesion to the adhesive. Examples of inorganic fillers include silica, alumina, magnesia, titanium oxide, and barium sulfate.
[0039] <1.3> Hidden layer To impart the decorative sheet 1 with the ability to conceal the substrate B, for example, a colored sheet can be used as the base layer 2, or an opaque concealing layer 8 can be provided. The concealing layer 8 can be made of, for example, the same material as that used for the design layer 3, which will be described later. However, since the purpose of the concealing layer 8 is to provide concealment, it is preferable to use, for example, an opaque pigment, titanium oxide, iron oxide, or the like, as the pigment. Furthermore, to enhance the concealing ability, metals such as gold, silver, copper, and aluminum can also be added to the material of the concealing layer 8. Generally, flake-shaped aluminum pieces are often added.
[0040] <1.4> Picture layer The design layer 3 is a layer formed by printing a design onto the base layer 2 using ink. Examples of ink binders include soluble nitrocellulose, cellulose, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral, polyurethane, acrylic, polyesters, and modified products thereof, either alone or in combination. The binder may be aqueous, solvent-based, or emulsion-based, and may be a one-component type or a two-component type that includes a curing agent. The design layer 3 may be formed by curing a layer formed with a curable ink by irradiation with ultraviolet light, electron beams, or the like. The most common method is to use a urethane-based ink that is cured with an isocyanate. The ink used to form the design layer 3 may further contain, in addition to the binder, pigments, colorants such as dyes, extender pigments, solvents, and various additives, which are commonly found in inks. Examples of versatile pigments include condensed azo, insoluble azo, quinacridone, isoindoline, anthraquinone, imidazolone, cobalt, phthalocyanine, carbon, titanium oxide, iron oxide, and pearl pigments such as mica.
[0041] In addition to applying ink, it is also possible to apply a design to the pattern layer 3 by vapor deposition or sputtering of various metals. In particular, it is preferable that a light stabilizer be added to the ink. This can suppress deterioration of the decorative sheet 1 itself caused by light degradation of the ink, and extend the life of the decorative sheet 1.
[0042] <1.5>Adhesive layer The adhesive layer 7 is also called a heat-sensitive adhesive layer, an anchor coat layer, or a dry lamination adhesive layer.
[0043] The resin material for the adhesive layer 7 is not particularly limited, and may be appropriately selected from acrylic, polyester, polyurethane, epoxy, and other resin materials. Alternatively, an ethylene-vinyl acetate copolymer resin adhesive may be used as the resin material for the adhesive layer 7. The coating method may be appropriately selected depending on the viscosity of the adhesive. Generally, gravure coating is used, and the adhesive layer 7 is formed on the upper surface of the design layer 3 by gravure coating, followed by lamination of the transparent resin layer 4. The adhesive layer 7 may be omitted if sufficient adhesive strength is obtained between the transparent resin layer 4 and the design layer 3.
[0044] <1.6>Transparent resin layer An olefin-based resin is preferably used as the resin material of the transparent resin layer 4. Examples of the olefin-based resin include polypropylene, polyethylene, polybutene, and the like, as well as α-olefins (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3 Examples of the copolymer include homopolymers of α-olefins (e.g., 9-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene) or copolymers of two or more of these, and copolymers of ethylene or α-olefins with other monomers, such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-butyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-butyl acrylate copolymer.
[0045] Furthermore, in order to improve the surface strength of the decorative sheet 1, it is preferable to use highly crystalline polypropylene as the resin for the transparent resin layer 4. Note that various additives such as heat stabilizers, light stabilizers, antiblocking agents, catalyst scavengers, colorants, light scattering agents, and gloss adjusters can also be added to the transparent resin layer 4 as needed. Generally, phenol-based, sulfur-based, phosphorus-based, and hydrazine-based heat stabilizers are used, and hindered amine-based and other light stabilizers are used, each added in any combination.
[0046] <1.7>Surface protective layer The surface protection layer 5 includes a core portion 5A and a plurality of ridge portions 5B each protruding in a ridge shape from one surface of the core portion 5A. These ridge portions 5B form an uneven structure.
[0047] Here, in the decorative sheet 1 according to this embodiment, the term "ridge-like" refers to a convex shape that is linear in plan view. The ridge portions 5B may be curved or linear in plan view, but are preferably curved in view of the fingerprint resistance of the decorative sheet 1. Each ridge portion 5B may or may not be branched in plan view. In addition, in the present disclosure, the ridge portions 5B refer to, for example, the portion from the lowest point to the tip of the uneven shape provided on the surface of the surface protective layer 5, and the core portion 5A refers to the portion of the surface protective layer 5 excluding the ridge portions 5B.
[0048] The ridge portions 5B are curved, and at least some of them are adjacent to each other in the width direction, as shown in Fig. 3. At a position where at least some of the ridge portions 5B are adjacent to each other in the width direction, the cross section of the surface protective layer 5 parallel to the width direction and the thickness direction of the surface protective layer 5 has a wave shape, such as a sine wave shape, in the portion where the uneven structure is provided, as shown in Fig. 2.
[0049] The uneven structure of the surface protective layer 5 has a protruding peak height Rpk of less than 3.5 μm. Here, "protruding peak height Rpk" is a surface texture parameter defined in JIS B0671-2:2002. This protruding peak height Rpk is more preferably 3.0 μm or less, and even more preferably 2.8 μm or less. A decorative sheet with a large protruding peak height Rpk can provide a user with a rough tactile sensation when they slide their skin over the surface of the surface protective layer, for example, when they slide their finger over the surface of the surface protective layer.
[0050] This protruding peak height Rpk is preferably 0.5 μm or more, more preferably 0.8 μm or more, and even more preferably 1.0 μm or more. A decorative sheet with a small protruding peak height Rpk can generate a large frictional force when a user slides their skin over the surface of the surface protective layer, for example, when they slide their finger over the surface of the surface protective layer.
[0051] The uneven structure of the surface protective layer 5 preferably has a mean length RSm of roughness curve elements of 800 μm or less, more preferably 550 μm or less, even more preferably 350 μm or less, even more preferably 320 μm or less, and even more preferably 300 μm or less. Here, the "mean length RSm of roughness curve elements" is a surface texture parameter defined in JIS B0601:2013. When a user slides their skin over the surface of the surface protective layer, for example, when they slide their finger over the surface of the surface protective layer, the mean length RSm of the roughness curve elements is preferably within the above range in order to provide the user with a smooth feel.
[0052] This average length RSm is preferably 10 μm or more, more preferably 50 μm or more, and even more preferably 80 μm or more. It is difficult to manufacture a structure in which this average length RSm is small and the protruding peak height Rpk is relatively large.
[0053] In the surface protective layer 5, the mass concentration C (mass %) of carbon atoms, the mass concentration O (mass %) of oxygen atoms, and the mass concentration Si (mass %) of silicon atoms satisfy the following relational expression (1). 0.5≦{Si / (C+O+Si)}×100 (1) Here, the surface protective layer 5 contains an ionizing radiation curable resin and silica particles, which will be described later. When the surface protective layer 5 satisfies the above relational expression (1), the ridge portions 5B can be uniformly formed over a wide area, improving the uniformity of the tactile feel. From the same viewpoint, the value of {Si / (C+O+Si)}×100 is preferably 0.75 or more, and more preferably 1.0 or more.
[0054] In the surface protective layer 5, the C (mass %), O (mass %), and Si (mass %) preferably satisfy the following relational formula (2). 0.5≦{Si / (C+O+Si)}×100≦5.0 (2) It is preferable that the value of {Si / (C+O+Si)}×100 is 5.0 or less from the viewpoints of scratch resistance, contamination resistance, weather resistance, etc. From the same viewpoint, the value of {Si / (C+O+Si)}×100 is more preferably 3.5 or less, and even more preferably 2.0 or less.
[0055] SEM-EDX analysis (scanning electron microscope-energy dispersive X-ray analysis) The C (mass %), O (mass %), and Si (mass %) contained in the surface protective layer 5 can be measured by observation with a scanning electron microscope (SEM) and energy dispersive X-ray spectroscopy (EDX). EDX is a method for elemental analysis by detecting characteristic X-rays generated by electron beam irradiation and analyzing them by energy. Here, a Hitachi High-Tech Regulus 8220 SEM was used, and an Oxford AZtecLive / Ultim Max 170 attached to the SEM was used as the EDX device. Analysis was performed under the following conditions.
[0056] ·Analysis conditions The surface of the surface protective layer 5 was subjected to a conductive treatment (Pt sputtering at 40 mA for 20 seconds), and the topcoat surface was subjected to SEM-EDX analysis under the following conditions. Accelerating voltage: 15 kV Emission current: 10μA Probe Current: High Condenser lens: 1 Measurement time: 60 seconds Measurement magnification: 500x
[0057] As will be explained below, the decorative sheet 1 according to this embodiment has excellent uniformity in its smooth feel. 3 is a micrograph obtained by imaging a decorative sheet according to one example of the present invention. This micrograph shows a rectangular microscopic region with a side length of about several hundred micrometers.
[0058] In the microscopic region shown in the micrograph of Figure 3, the wrinkles corresponding to the ridge portions 5B are uniformly formed. Uniformity of the wrinkles contributes to uniformity of the feel to the touch. Therefore, a decorative sheet that has excellent uniformity in the smooth feel to the touch must have uniform wrinkles, for example, as shown in the micrograph of Figure 3.
[0059] However, even if wrinkles are uniformly present in such a specific microregion, other regions may have wrinkles of a different form than those shown in Figure 3, or may include areas where no wrinkles are formed. Whether wrinkles are uniformly present across the entire surface of surface protective layer 5 may not be possible to determine by observing a microscopic image obtained by imaging a specific microregion having the dimensions described above or by observing the decorative sheet with the naked eye. Furthermore, if wrinkles are not uniformly present on the surface of surface protective layer 5, even if the unevenness of the wrinkles cannot be confirmed by observing a microscopic image obtained by imaging a specific microregion or by observing the decorative sheet with the naked eye, this unevenness may be perceived as a different tactile sensation when a user slides their skin over the surface of surface protective layer 5.
[0060] The decorative sheet 1 can be obtained by the method described below. This decorative sheet 1 has the above-mentioned characteristics. When a user slides their skin over the surface of the surface protective layer 5, this decorative sheet 1 provides the user with a smooth and silky feel, and the smooth and silky feel is highly uniform.
[0061] The thickness of the surface protective layer 5 is preferably 2 μm or more and 15 μm or less, more preferably 2 μm or more and less than 10 μm, and even more preferably 2 μm or more and less than 8 μm. If the thickness of the surface protective layer 5 is reduced, it becomes difficult to increase the protruding peak height Rpk and the average length RSm. If the thickness of the surface protective layer 5 is increased, the protruding peak height Rpk and the average length RSm tend to increase.
[0062] Here, the thickness of the surface protective layer 5 is the thickness of a layer that has the same apparent area and volume as the surface protective layer 5 and a flat surface. The thickness of the surface protective layer 5 is determined, for example, by the following method. First, a cross section parallel to the thickness direction of the surface protective layer 5 and perpendicular to the length direction of the ridge portions 5B is imaged. Next, from this cross-sectional image, the dimension of the surface protective layer 5 in the width direction of the ridge portions 5B and the area of the cross section of the surface protective layer 5 are determined. The thickness of the surface protective layer 5 is a value obtained by dividing this area by the above dimension.
[0063] When the coating liquid for forming a surface protective layer, which will be described later, does not contain a solvent, the thickness of the coating film made of the coating liquid for forming a surface protective layer is equal to the thickness of the surface protective layer 5 .
[0064] The glossiness of the surface protective layer 5 is preferably 20.0 or less, more preferably 10.0 or less, and even more preferably 8.0 or less. Here, the "glossiness" is a value measured at an incident angle of 60 degrees using a glossmeter conforming to JIS Z8741:1997.
[0065] <2> Manufacturing method of decorative sheet The decorative sheet 1 is produced, for example, by the following method: For the sake of brevity, explanations regarding the design layer 3, transparent resin layer 4, primer layer 6, adhesive layer 7, and hiding layer 8 will be omitted here.
[0066] First, a coating film made of a coating liquid for the surface protective layer is formed on one surface of the raw fabric layer 2. This coating film can be formed by various printing methods such as gravure printing, offset printing, screen printing, electrostatic printing, and inkjet printing, or various coating methods such as roll coating, knife coating, microgravure coating, and die coating.
[0067] The coating liquid for the surface protective layer contains an ionizing radiation curable resin. Here, "ionizing radiation" refers to charged particle radiation such as an electron beam. The ionizing radiation curable resin is cured by irradiation with ionizing radiation. The ionizing radiation curable resin can also be cured by irradiation with ultraviolet light. The ionizing radiation curable resin used here is cured by irradiation with light having a wavelength of 200 nm or less, and has a high absorption coefficient for this light.
[0068] In the coating liquid for surface protection layer, when the total solid content is taken as 100 parts by mass, the amount of ionizing radiation curable resin is preferably 60 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more. As the ionizing radiation curable resin, known resins such as various monomers and commercially available oligomers can be used, for example, (meth)acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins. The ionizing radiation curable resin may be either an aqueous resin or a non-aqueous (organic solvent-based) resin.
[0069] The main component of the ionizing radiation curable resin is preferably an acrylate. Here, the main component of the ionizing radiation curable resin means that the main component is 60 parts by mass or more, based on 100 parts by mass of the total solid content of the ionizing radiation curable resin. The ionizing radiation curable resin preferably contains 70 parts by mass or more of the acrylate, and more preferably 80 parts by mass or more.
[0070] The acrylate is preferably a difunctional or higher acrylate, and more preferably a trifunctional or higher acrylate. In order to obtain a surface protective layer 5 with excellent scratch resistance, the acrylate is preferably a trifunctional or higher acrylate. There is no upper limit to the number of functional groups of the acrylate, but according to one example, it is hexafunctional or lower.
[0071] The acrylate preferably contains a repeating unit. This repeating unit is, for example, any one of an ethylene oxide (EO) unit, a propylene oxide (PO) unit, and an ε-caprolactone (CL) unit. The repeating unit is preferably ethylene oxide or propylene oxide. In a tri- or higher functional acrylate containing a repeating unit, the repeating unit may be present between an acryloyl group and a methylol group in an open ring state.
[0072] The number of repetitions of the repeating structure is preferably three or more. Using an acrylate with a high number of repetitions makes it easier for the cured film to expand in the in-plane direction during the second irradiation step described below, which makes it easier for wrinkles corresponding to the ridges 5B to form on the coating film surface. It also makes it possible to form wrinkles uniformly over a wide area, contributing to improved uniformity of the tactile feel. However, increasing the number of repetitions reduces the crosslink density and the scratch resistance of the surface protective layer.
[0073] Examples of trifunctional acrylates containing repeating units include EO-modified, PO-modified, or CL-modified trimethylolpropane triacrylate, glycerin triacrylate, isocyanurate triacrylate, or pentaerythritol triacrylate. In trifunctional acrylates containing repeating units, the number of repeating units is preferably 3 or more and 30 or less, and more preferably 3 or more and 20 or less.
[0074] The tetrafunctional acrylate containing a repeating unit is, for example, EO-modified, PO-modified, or CL-modified pentaerythritol tetraacrylate. In the tetrafunctional acrylate containing a repeating unit, the number of repeating units is preferably 12 or more, more preferably 12 to 50, and even more preferably 20 to 50.
[0075] The repeat number of the repeating structure can be analyzed using MALDI-TOF-MS. Ionizing radiation curable resins may have a molecular weight distribution. If there is a molecular weight distribution, the repeat number is determined to be the repeat number corresponding to the molecular weight with the strongest peak in the MALDI-TOF-MS mass spectrum.
[0076] As described above, the main component of the ionizing radiation curable resin is preferably an acrylate. The acrylate may be composed of the acrylate described above. Alternatively, the acrylate may be composed of the acrylate described above (hereinafter referred to as the first acrylate) and a second acrylate different from the first acrylate. In this case, the blending ratio of the first acrylate to the second acrylate is not particularly limited, but can be, for example, a mass ratio within the range of 90:10 to 20:80. The second acrylate is, for example, a mono- to hexa-functional acrylate.
[0077] According to one example, the acrylate may be composed of a first acrylate containing a repeating unit and a second acrylate having one to six functionalities. In this example, the repeating unit of the first acrylate is any one of ethylene oxide, propylene oxide, and ε-caprolactone, and the number of repetitions of the repeating unit is three or more.
[0078] The second acrylate preferably does not contain a repeating unit. That is, the second acrylate is preferably a mono- to hexa-functional acrylate that does not contain a repeating unit. Specifically, the second acrylate preferably does not contain any of the repeating units of ethylene oxide, propylene oxide, and ε-caprolactone.
[0079] Examples of the second acrylate include trimethylolpropane triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, and dipentaerythritol hexaacrylate.
[0080] The use of the second acrylate in addition to the first acrylate tends to decrease the peak height Rpk and increase the average length RSm of the roughness curve element, which can increase the glossiness of the surface protective layer 5 and increase the glossiness variation, or can increase the thickness of the surface protective layer 5 and increase the thickness variation.
[0081] As described above, the coating liquid for a surface protective layer contains silica particles. When the coating liquid for a surface protective layer contains silica particles, wrinkles can be more uniformly formed on the coating surface in the second irradiation step described below, which contributes to improving the uniformity of the tactile feel.
[0082] The coating liquid for forming a surface protective layer may further contain particles other than silica particles. Examples of the particles other than silica particles include particles made of organic materials such as polyethylene (PE) wax, polypropylene (PP) wax, and resin beads, and particles made of inorganic materials such as glass, alumina, titania, zirconia, calcium carbonate, and barium sulfate. The particles other than silica particles may be contained in the coating liquid for forming a surface protective layer in an amount of, for example, 20% by mass or less of the total particles.
[0083] The average particle size (D50) of the particles, including silica particles, is preferably 10 μm or less. The average particle size (D50) of the particles is more preferably 1 μm or more and 8 μm or less, and even more preferably 2 μm or more and 6 μm or less. If large particles are used, the particles are likely to fall off from the surface protective layer 5, which may make it difficult to achieve high scratch resistance. If the particles are small, the effect of generating wrinkles uniformly is small.
[0084] Here, the "average particle size (D50)" refers to the median size (D50) measured using a laser diffraction / scattering particle size distribution analyzer. If the coating liquid for the surface protective layer contains particles, the surface protective layer 5 obtained from this coating liquid will also contain particles. The average particle size of the particles contained in the surface protective layer 5 can be determined by observing the cross section of the layer and averaging the particle sizes of multiple particles. The value obtained in this manner is essentially the same as the median size (D50) measured using a laser diffraction / scattering particle size distribution analyzer. Therefore, the above-mentioned range of average particle size can also be interpreted as the range of average particle sizes of the particles contained in the surface protective layer 5.
[0085] The amount of particles, including silica particles, added is preferably 1.3 to 22 parts by mass, more preferably 1.3 to 15 parts by mass, and even more preferably 3 to 10 parts by mass, per 100 parts by mass of the ionizing radiation curable resin. When the coating liquid for surface protection layer does not contain particles other than silica particles, the above-mentioned amount refers to the amount of silica particles added. When the amount of particles is within the above range, the effect of generating uniform wrinkles is particularly great.
[0086] The coating liquid for the surface protective layer may further contain a solvent and additives for improving the functionality of the final product, such as antibacterial agents and antifungal agents. The coating liquid for the surface protective layer may further contain other additives such as an ultraviolet absorber and a light stabilizer. Examples of ultraviolet absorbers that can be used include benzotriazoles, benzoates, benzophenones, and triazines. Examples of light stabilizers that can be used include hindered amines. Note that, according to the method described herein, a surface protective layer 5 having low gloss can be formed without the use of a gloss adjuster (matt additive).
[0087] When carrying out the first irradiation step described below or when curing the entire coating film made of the coating liquid for surface protective layer by ultraviolet irradiation in the third irradiation step described below, it is preferable that the coating liquid for surface protective layer further contains a photoinitiator. The photoinitiator is not particularly limited, but examples thereof include benzophenone-based, acetophenone-based, benzoin ether-based, and thioxanthone-based photoinitiators.
[0088] The amount of photoinitiator added is preferably 0.1 to 10 parts by mass, more preferably 0.25 to 8 parts by mass, and even more preferably 0.5 to 6 parts by mass, relative to 100 parts by mass of the ionizing radiation-curable resin. If the amount of photoinitiator is less than 0.1 part by mass, the effect of the first irradiation step described below is less likely to be achieved. If the amount of photoinitiator is more than 10 parts by mass, the coating film will be completely cured, making it less likely that wrinkles will form in the subsequent second irradiation step.
[0089] After forming a coating film made from the coating liquid for the surface protective layer, the coating film is preferably semi-cured by carrying out a first irradiation step. In the first irradiation step, the coating film is irradiated with light having a wavelength of approximately 200 nm or more and 400 nm or less (hereinafter referred to as first irradiation light). By semi-curing the coating film by carrying out the first irradiation step, it is possible to form wrinkles more uniformly in the second irradiation step described below. Furthermore, it is possible to design the depth of the wrinkle shape and adjust the texture by adjusting the irradiation conditions of the first irradiation step. The first irradiation step is not essential, and its implementation can be determined depending on the desired properties of the product.
[0090] In the first irradiation step, a lamp selected from a high-pressure mercury lamp, a metal halide lamp, a single-wavelength LED lamp having light with a wavelength of 200 nm or more and 400 nm or less can be used.
[0091] The cumulative light intensity of the first irradiation light is 2 mJ / cm 2 More than 100mJ / cm 2 It is preferable that the dose is 10 mJ / cm or less. 2 More than 80mJ / cm 2 More preferably, it is 20 mJ / cm or less.2 More than 60mJ / cm 2 It is more preferable to set the integrated light amount to the following: If the integrated light amount is small, the effect of the first irradiation step is less likely to be achieved; if the integrated light amount is large, the coating film is completely cured, making it difficult for wrinkles to form in the subsequent second irradiation step.
[0092] After forming a coating film made of the coating liquid for surface protective layer or after carrying out the first irradiation step, the second irradiation step is carried out. In the second irradiation step, the coating film is irradiated with light having a wavelength of 200 nm or less (hereinafter referred to as the second irradiation light). The ionizing radiation curable resin contained in the coating liquid for surface protective layer has a large absorption coefficient for the second irradiation light. Therefore, the second irradiation light incident on the coating film can only reach a position several tens to several hundreds of nm away from the outermost surface. Therefore, in the second irradiation step, the crosslinking reaction proceeds in the surface region of the coating film, forming an extremely thin cured film, while the crosslinking reaction does not proceed in other regions, leaving the coating film uncured.
[0093] The coating film after the second irradiation step has wrinkles on its surface that correspond to the ridge portions 5 B. The present inventors believe that the reason why wrinkles are formed on the coating film surface by the second irradiation step is as follows.
[0094] As described above, the second exposure light can only reach a position several tens to several hundreds of nanometers from the outermost surface of the coating film. That is, the crosslinking reaction of the ionizing radiation curable resin occurs only on the surface of the coating film. When irradiated with the second exposure light, the monomers and the like present on the surface of the coating film crosslink via the functional groups they possess to form a cured film, but not all of these functional groups are used to crosslink the monomers present on the surface of the coating film. That is, uncrosslinked functional groups may remain in the cured film.
[0095] The second irradiation light does not reach the monomers present at positions away from the surface of the coating film, so the crosslinking reaction does not occur. However, some of the monomers present at positions away from the surface of the coating film migrate to the cured film and undergo crosslinking reaction there. In this way, the number of molecules involved in the crosslinking reaction increases.
[0096] As the number of molecules involved in the crosslinking reaction at the coating surface increases, the volume of the cured film increases. Because the crosslinking reaction occurs only at the surface of the coating, the cured film cannot increase in volume in the thickness direction, but expands in the in-plane direction. As a result, wrinkles appear on the surface of the coating.
[0097] The second irradiation light can be extracted from excimer VUV (Vacuum Ultra Violet) light. Excimer VUV light can be produced from lamps using rare gases or rare gas halide compounds. When high-energy electrons are externally applied to a lamp filled with rare gases or rare gas halide compounds, a large number of discharge plasmas (dielectric barrier discharges) are generated. This plasma discharge excites the atoms of the discharge gas (rare gas), momentarily transforming them into an excimer state. When returning from this excimer state to the ground state, light is emitted in a wavelength range specific to that excimer.
[0098] The gas used in the excimer lamp may be any conventional gas that emits light of 200 nm or less. Examples of gases that can be used include rare gases such as Xe, Ar, and Kr, and mixtures of rare gases such as ArBr and ArF with halogen gases. Excimer lamps have different wavelengths (center wavelengths) depending on the gas used, such as approximately 172 nm (Xe), approximately 126 nm (Ar), approximately 146 nm (Kr), approximately 165 nm (ArBr), and approximately 193 nm (ArF).
[0099] Considering the magnitude of photon energy and the difference between wavelength and bond energy of organic matter, it is preferable to use a xenon lamp that emits excimer light with a central wavelength of 172 nm as the light source. Also, considering the cost of maintaining the equipment and the availability of materials, it is preferable to use a xenon lamp as the light source.
[0100] The second irradiation step is carried out in an atmosphere with a low oxygen concentration. Oxygen has a high absorption coefficient for light of 200 nm or less. Therefore, the second irradiation step is preferably carried out in, for example, a nitrogen gas atmosphere. The oxygen concentration in the gas phase during the second irradiation step, i.e., the residual oxygen concentration in the reaction atmosphere, is preferably 2000 ppm or less, and more preferably 1000 ppm or less.
[0101] Furthermore, oxygen in the atmosphere inhibits radical polymerization. Therefore, the residual oxygen concentration in the reaction atmosphere affects the formation of wrinkles on the coating surface. Therefore, changing the residual oxygen concentration in the reaction atmosphere can also change the surface properties of the surface protective layer 5.
[0102] The cumulative light intensity of the second irradiation light is 0.5 mJ / cm 2 More than 200mJ / cm 2 It is preferable that the dose is 1 mJ / cm or less. 2 More than 100mJ / cm 2 More preferably, it is 3 mJ / cm or less. 2 More than 50mJ / cm 2 It is more preferable that the integrated light amount is set to the following: If the integrated light amount is small, the expansion of the cured film in the in-plane direction is small, whereas if the integrated light amount is large, the surface condition of the coating film is deteriorated.
[0103] After the second irradiation step is completed, the third irradiation step is carried out. In the third irradiation step, the coating film is irradiated with a third radiation or irradiation light to cure the entire coating film. In this way, the surface protective layer 5 is obtained.
[0104] The third radiation or irradiation light is ionizing radiation such as an electron beam, or ultraviolet light having a longer wavelength than the second irradiation light.
[0105] If the third radiation or irradiation light is ultraviolet light, the integrated light intensity of the third irradiation light is 10 mJ / cm 2 More than 500mJ / cm 2 It is preferable that the dose is 50 mJ / cm or less. 2 More than 400mJ / cm 2 It is more preferable that the dose is 100 mJ / cm or less, and 2More than 300mJ / cm 2 It is more preferable that:
[0106] The decorative sheet 1 can be produced by, for example, the method described above. The decorative sheet 1 may also be produced by other methods. For example, a plate may be formed using the method described above for the surface protective layer 5, and the surface protective layer 5 having a relief structure on its surface may be formed by transfer using this plate.
[0107] <3> effect The decorative sheet 1 described with reference to Figures 1 to 3 has the surface properties of the surface protective layer 5. Such a decorative sheet 1 provides the user with a smooth and uniform feel when the user slides their skin over the surface of the surface protective layer 5, for example, when they slide their finger over the surface of the surface protective layer 5. In other words, this decorative sheet 1 allows the user to slide their finger or the like over the entire surface of the surface protective layer 5 with little friction, without the user being aware of the presence of large irregularities.
[0108] The decorative sheet 1, which provides a smooth feel to the user, is suitable for use in applications where it frequently comes into contact with the user's skin or where the user's skin is in contact with it for long periods of time, such as furniture. Articles using the decorative sheet 1 do not cause discomfort to the user when they come into contact with the user's skin.
[0109] The surface protective layer 5 of the decorative sheet 1 has the above-described surface properties, and therefore can achieve a low gloss even without containing a gloss adjuster (matt additive). Gloss adjusters reduce the oil repellency of layers formed from resin materials, making surface protective layers containing gloss adjusters more susceptible to fingerprints. A surface protective layer 5 that does not contain a gloss adjuster is less likely to absorb oil and therefore less susceptible to fingerprints. Furthermore, a surface protective layer 5 with excellent oil repellency is less likely to develop oil stains or adsorb contaminants. Furthermore, a surface protective layer 5 that does not contain a gloss adjuster does not lose gloss adjuster particles when its surface is scratched, and therefore a decorative sheet 1 containing such a surface protective layer 5 is less likely to develop gloss changes or scratches.
[0110] The reason why the surface protection layer 5 having the above-described surface properties can be obtained by the above-described method is as follows.
[0111] Oxygen in the gas phase not only absorbs short-wavelength ultraviolet light but also inhibits radical polymerization. The effect of oxygen in the gas phase on radical polymerization is greatest in the portion of the coating film made of ionizing radiation-curable resin adjacent to the gas phase, and decreases as the distance from the coating surface increases. Therefore, by changing the oxygen concentration in the gas phase in the second irradiation step, the relationship between the distance from the coating surface and the progress of the crosslinking reaction can be changed.
[0112] If this relationship changes, the thickness of the cured film formed on the surface of the coating film by the second irradiation step and the degree of in-plane expansion of the cured film as the crosslinking reaction progresses will change. The integrated light dose in the second irradiation step also affects the thickness of the cured film and the degree of in-plane expansion of the cured film. The thickness of the cured film and the degree of in-plane expansion of the cured film also affect the surface properties of the surface protective layer. Furthermore, the thickness of the coating film also affects the formation of wrinkles.
[0113] Therefore, for example, by appropriately setting the composition of the ionizing radiation curable resin, the thickness of the coating film, the oxygen concentration in the gas phase in the second irradiation step, and the integrated light amount in the second irradiation step, it is possible to obtain a surface protection layer having the desired surface properties. [Example]
[0114] The following describes examples of the present invention. <Example 1> The decorative sheet 1 described with reference to Figures 1 to 3 was produced by the following method: In this example, the transparent resin layer 4, primer layer 6, adhesive layer 7 and masking layer 8 were omitted.
[0115] First, the basis weight is 50 g / m 2An impregnated paper (GFR-506, manufactured by Kojin Co., Ltd.) was prepared as the raw fabric layer 2. On one side of the raw fabric layer 2, a picture layer 3 was formed using an oil-based nitrocellulose resin gravure printing ink (PCNT (PCRNT) various colors, manufactured by Toyo Ink Co., Ltd.).
[0116] Next, a coating liquid for a surface protective layer was applied onto the design layer 3. The coating liquid for the surface protective layer was prepared by blending the following particles with the following ionizing radiation curable resin. ·Ionizing radiation curable resin Type: Ethylene glycol diacrylate (EO 9 moles added) Product name: Light Acrylate 9EG-A (Kyoeisha Chemical Co., Ltd.) Blend: 100 parts by mass ·particle Product name: Silysia (registered trademark) 250N (manufactured by Fuji Silysia Chemical Ltd.) Particle size: 5μm Blend: 2 parts by mass Photoinitiators Product name: Irgacure 184 (BASF Japan Ltd.) Blend: 1 part by mass The coating film made of the coating liquid for the surface protective layer was formed to a thickness of 5 μm.
[0117] Thereafter, the first irradiation step was carried out. Specifically, in the atmosphere, a high-pressure mercury lamp with a main wavelength of ultraviolet light of 365 nm was used to irradiate the surface of the coating film made of the coating liquid for the surface protective layer with an accumulated light amount of 50 mJ / cm. 2 This caused the coating film to be semi-cured.
[0118] Next, the second irradiation step was carried out. Specifically, under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm, ultraviolet rays with a wavelength of 172 nm were irradiated onto the surface of the coating film made of the coating liquid for the surface protective layer using a Xe excimer lamp at an integrated light intensity of 50 mJ / cm. 2 This caused wrinkles to form on the surface of the coating film.
[0119] Finally, the third irradiation step was carried out. Specifically, the coating film was irradiated with ionizing radiation to cure the entire coating film, thereby forming a surface protective layer 5. In this manner, a decorative sheet 1 was obtained.
[0120] <Example 2> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 50 mJ / cm 2 using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0121] <Example 3> Decorative sheet 1 was produced in the same manner as in Example 2, except for the following points: In this example, the blending amounts of the following particles were changed. ·particle Product name: Silysia 250N (Fuji Silysia Chemical) Particle size: 5μm Blend: 1.3 parts by mass
[0122] <Example 4> Decorative sheet 1 was produced in the same manner as in Example 2, except for the following points: In this example, the blending amounts of the following particles were changed. ·particle Product name: Silysia 250N (Fuji Silysia Chemical) Particle size: 5μm Blend: 15 parts by mass
[0123] <Example 5> Decorative sheet 1 was produced in the same manner as in Example 2, except for the following points: In this example, the blending amounts of the following particles were changed. ·particle Product name: Silysia 250N (Fuji Silysia Chemical) Particle size: 5μm Blend: 22 parts by mass
[0124] <Example 6> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 15 moles added) Product name: SR9035 (Sartomer) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 50 mJ / cm 2 using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0125] <Example 7> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 3 moles added) Product name: Miramer M3130 (Miwon) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 100 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0126] <Example 8> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Trimethylolpropane PO modified triacrylate (PO 6 moles added) Product name: NK Ester A-TMPT-6PO (manufactured by Shin-Nakamura Chemical Co., Ltd.) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 50 mJ / cm 2 using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0127] <Example 9> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Caprolactone-modified tris-(2-acryloxyethyl) isocyanurate (caprolactone (CL) 3 moles added) Product name: NK Ester A-9300-3CL (manufactured by Shin-Nakamura Chemical Co., Ltd.) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 100 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0128] <Example 10> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for the surface protective layer was formed to a thickness of 1 μm. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 10 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0129] <Example 11> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for the surface protective layer was formed to a thickness of 2 μm. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 10 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0130] <Example 12> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for surface protection layer was formed to a thickness of 9 μm. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 3 moles added) Product name: Miramer M3130 (Miwon) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 150 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0131] <Example 13> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (35 moles of EO added) Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd.) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 50 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0132] <Example 14> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (EO 50 moles added) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 50 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0133] <Example 15> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (20 moles of EO added) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 100 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 100 ppm. 2 The irradiation was carried out so that
[0134] <Example 16> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Propoxylated pentaerythritol tetraacrylate (PO35 moles added) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 50 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0135] <Example 17> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Caprolactone-modified pentaerythritol tetraacrylate (CL 20 moles added) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 100 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 100 ppm. 2 The irradiation was carried out so that
[0136] <Example 18> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for the surface protective layer was formed to a thickness of 1 μm. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (35 moles of EO added) Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd.) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 10 mJ / cm 2 using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0137] <Example 19> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for the surface protective layer was formed to a thickness of 2 μm. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (35 moles of EO added) Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd.) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 10 mJ / cm 2 using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0138] <Example 20> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for surface protection layer was formed to a thickness of 9 μm. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (20 moles of EO added) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 150 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0139] <Example 21> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin Type: Ethoxylated dipentaerythritol hexaacrylate (12 moles of EO added) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 150 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 100 ppm. 2 The irradiation was carried out so that
[0140] <Example 22> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin 1 Trimethylolpropane EO modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) Blend: 60 parts by mass ·Ionizing radiation curable resin 2 Type: Dipentaerythritol hexaacrylate Product name: Miramer M600 (Miwon) Blend: 40 parts by mass The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 10 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0141] <Example 23> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points: In this example, the following ionizing radiation curable resin was used. ·Ionizing radiation curable resin 1 Trimethylolpropane EO modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) Blend: 40 parts by mass ·Ionizing radiation curable resin 2 Type: Dipentaerythritol hexaacrylate Product name: Miramer M600 (Miwon) Blend: 60 parts by mass The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 10 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0142] <Example 24> Decorative sheet 1 was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. The coating film made of the coating liquid for the surface protective layer was formed to a thickness of 14 μm. ·Ionizing radiation curable resin 1 Trimethylolpropane EO modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) Blend: 40 parts by mass ·Ionizing radiation curable resin 2 Type: Dipentaerythritol hexaacrylate Product name: Miramer M600 (Miwon) Blend: 60 parts by mass The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 100 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 100 ppm. 2 The irradiation was carried out so that
[0143] <Comparative Example 1> A decorative sheet was produced in the same manner as in Example 1, except for the following points: In this example, the coating liquid for the surface protective layer was a mixture of the following ionizing radiation curable resin and the following particles. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) Blend: 100 parts by mass ·particle Product name: Silysia 250N (Fuji Silysia Chemical) Particle size: 5μm Blend: 15 parts by mass Then, the first and second irradiation steps were not carried out, and the coating film made of the coating liquid for forming the surface protective layer was cured only by the third irradiation step.
[0144] <Comparative Example 2> A decorative sheet was produced in the same manner as in Example 1, except for the following points: In this example, the coating liquid for the surface protective layer was a mixture of the following ionizing radiation curable resin and the following particles. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (35 moles of EO added) Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd.) Blend: 100 parts by mass ·particle Product name: Silysia 250N (Fuji Silysia Chemical) Particle size: 5μm Blend: 15 parts by mass Then, the first and second irradiation steps were not carried out, and the coating film made of the coating liquid for forming the surface protective layer was cured only by the third irradiation step.
[0145] <Comparative Example 3> A decorative sheet was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. A coating film made of the coating liquid for the surface protective layer was formed to a thickness of 10 μm. ·Ionizing radiation curable resin Type: Trimethylolpropane EO-modified triacrylate (EO 6 moles added) Product name: Miramer M3160 (Miwon) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 150 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 500 ppm. 2 The irradiation was carried out so that
[0146] <Comparative Example 4> A decorative sheet was produced in the same manner as in Example 1, except for the following points. That is, in this example, the following ionizing radiation curable resin was used. A coating film made of the coating liquid for the surface protective layer was formed to a thickness of 10 μm. ·Ionizing radiation curable resin Type: Ethoxylated pentaerythritol tetraacrylate (35 moles of EO added) Product name: NK Ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd.) The second irradiation step is carried out by irradiating the surface of the coating film made of the surface protective layer coating liquid with ultraviolet light having a wavelength of 172 nm at an integrated light intensity of 150 mJ / cm using a Xe excimer lamp under atmospheric pressure in a nitrogen gas atmosphere with an oxygen concentration of 200 ppm. 2 The irradiation was carried out so that
[0147] <Comparative Example 5> A decorative sheet was produced in the same manner as in Example 1, except for the following points: In this example, particles (Sylysia 250N) were not blended.
[0148] <Evaluation> Each of the decorative sheets described above was subjected to the following evaluations.
[0149] (1) Glossiness The glossiness was measured at 60 degrees using a Rhopoint IQ (manufactured by Konica Minolta, Inc.) The "60 degree glossiness value" in Tables 1 to 3 below represents this 60 degree glossiness.
[0150] (2) Skin feel The skin feel was evaluated by the following method. First, preliminary preparations were made to ensure that the evaluation criteria were consistent across evaluators. Specifically, 10 standard test pieces with different surface textures were prepared. Next, 20 evaluators were asked to run their fingers over the surface of the standard test pieces while blindfolded, and then classify the tactile sensations into the following five groups. Group 1: The presence of unevenness was barely felt, and the friction force was felt to be small. Group 2: felt the presence of small irregularities or felt that the friction force was somewhat large. Group 3: The texture was intermediate between that of Group 1 and Group 2. Group 4: Felt the presence of large bumps. Group 5: They did not feel any unevenness, but felt that the friction was great. The above procedure was repeated until the ratings by each rater were consistent for three or more consecutive times, and the ratings between raters were consistent for three consecutive times.
[0151] Next, for each of the decorative sheets, each of the evaluators was asked to run their fingers over the surface of the surface protective layer while blindfolded, and then classify the tactile sensation into one of the five groups. This procedure was repeated until the evaluations by each evaluator were consistent for three or more consecutive evaluations, and the evaluation results between the evaluators were consistent for three consecutive evaluations. From these results, the skin sensation was evaluated according to the following criteria. AAA (smooth): Group 1 AA (smooth): 3rd group A (Smooth): Group 2 B (rough or smooth): Group 4 or 5
[0152] (3) Uniformity of texture After evaluating the skin feel, the 20 evaluators evaluated the uniformity of the feel using the following method. Test pieces measuring 10 cm long x 10 cm wide were cut from each decorative sheet. Each of the 20 evaluators was blindfolded and asked to freely run their fingers over the entire surface of the surface protection layer of each test piece, and to classify the uniformity of the texture into the following three groups based on the presence or absence of change in the texture (smooth texture) and the degree of change.
[0153] Group 1: There was no area where the texture (smooth texture) felt different. Group 2: There were some areas where the texture (smooth texture) felt different, but the degree of change was slight. Group 3: There were some areas where the texture (smooth texture) felt clearly different.
[0154] This procedure was repeated until the evaluations by each evaluator were consistent for three or more consecutive evaluations, and the evaluation results were consistent between the evaluators for three consecutive evaluations. From these results, the uniformity of the tactile sensation was evaluated according to the following criteria. Note that this evaluation was not performed for the decorative sheets of Comparative Examples 1 to 4, which were rated B for the tactile sensation. AA: Group 1 A: 2nd group B: Group 3.
[0155] (4) Fingerprint resistance To evaluate fingerprint resistance, the ability to wipe off fingerprints was evaluated. Specifically, the 60-degree gloss of the surface of each decorative sheet was first measured, and this 60-degree gloss was designated as the initial gloss. Subsequently, a fingerprint-resistant evaluation liquid was applied to the surface protective layer, and the fingerprint-resistant evaluation liquid applied to the surface of the decorative sheet was wiped off. Here, a higher fatty acid was used as the fingerprint-resistant evaluation liquid. Thereafter, the 60-degree gloss of the area from which the fingerprint-resistant evaluation liquid had been wiped off was measured, and this 60-degree gloss was designated as the gloss after wiping.
[0156] The fingerprint removal rate was calculated using the following formula: Fingerprint removal rate (%) = (glossiness after wiping / initial glossiness) x 100
[0157] The evaluation criteria were as follows: AA: 70% or more but less than 250% A: 50% or more but less than 70%, or 250% or more but less than 300% B: Less than 50% or 300% or more
[0158] (5) Stain resistance To evaluate stain resistance, the Staining A Test specified in the Japanese Agricultural Standards (JAS) was conducted. Specifically, 10 mm wide lines were drawn on the surface protective layer of each decorative sheet using blue ink, black quick-drying ink, and red crayon, and the sheets were left for 4 hours. The blue ink, black quick-drying ink, and red crayon lines were then wiped off with a cloth soaked in ethanol.
[0159] The evaluation criteria were as follows: AA: Lines of each color could be easily wiped off. A: I was able to wipe off some of the lines of each color, but some stains remained. B: I couldn't wipe off the lines of each color.
[0160] (6) Scratch resistance test Each decorative sheet was attached to wood substrate B using a urethane adhesive. A steel wool rubbing test was then conducted to evaluate scratch resistance. Specifically, the decorative sheet was rubbed back and forth 20 times with steel wool while applying a load of 100 g, and the surface of the decorative sheet was visually inspected for scratches and changes in gloss.
[0161] The evaluation criteria were as follows: AA: No scratches or changes in gloss occurred on the surface. A: Minor scratches or changes in gloss have occurred on the surface. B: Significant scratches or changes in gloss occurred on the surface.
[0162] [Table 1]
[0163] [Table 2]
[0164] [Table 3]
[0165] [Table 4]
[0166] As shown in Tables 1 to 3, the decorative sheets according to Examples 1 to 24 provided the evaluators with a smooth feel and uniformity of the feel. Furthermore, the decorative sheets according to Examples 1 to 24 were low gloss and excellent in fingerprint resistance, stain resistance, and scratch resistance. In contrast, the decorative sheets according to Comparative Examples 1 and 2, as shown in Table 4, did not provide the evaluators with a smooth feel and were poor in fingerprint resistance, stain resistance, and scratch resistance. Furthermore, the decorative sheets according to Comparative Examples 3 and 4 were low gloss and excellent in fingerprint resistance, stain resistance, and scratch resistance, but did not provide the evaluators with a smooth feel. Furthermore, the decorative sheet according to Comparative Example 5 was low gloss and excellent in fingerprint resistance, stain resistance, and scratch resistance, and provided the evaluators with a smooth feel, but was poor in uniformity of the feel. [Explanation of symbols]
[0167] 1...decorative sheet, 2...base layer, 3...pattern layer, 4...transparent resin layer, 5...surface protection layer, 5A...core portion, 5B...ridge portion, 6...primer layer, 7...adhesive layer, 8...hiding layer, 11...decorative material, B...base material.
Claims
1. A base fabric layer and a surface protective layer provided on one surface or above the base fabric layer, a concave-convex structure including a plurality of ridge-like portions each protruding in a ridge shape is provided on a surface of the surface protection layer; The uneven structure of the surface protective layer has a protruding peak height Rpk of less than 3.5 μm, In the surface protective layer, the mass concentration C (mass %) of carbon atoms, the mass concentration O (mass %) of oxygen atoms, and the mass concentration Si (mass %) of silicon atoms satisfy the following relational expression: 0.5≦{Si / (C+O+Si)}×100 Satisfy your cosmetic needs.
2. 2. The decorative sheet according to claim 1, wherein said protruding peak height Rpk is 0.5 μm or more.
3. In the surface protective layer, the mass concentration C (mass %) of carbon atoms, the mass concentration O (mass %) of oxygen atoms, and the mass concentration Si (mass %) of silicon atoms satisfy the following relational expression: 0.5≦{Si / (C+O+Si)}×100≦5.0 The decorative sheet according to claim 1 , which satisfies the above.
4. 2. The decorative sheet according to claim 1, wherein the uneven structure of the surface protective layer has a mean length RSm of roughness curve elements of 800 μm or less.
5. 2. The decorative sheet according to claim 1, wherein the uneven structure of the surface protective layer has a mean length RSm of roughness curve elements of 350 μm or less.
6. The decorative sheet according to claim 4, wherein said average length RSm is 10 µm or more.
7. 2. The decorative sheet according to claim 1, wherein the thickness of said surface protective layer is from 2 μm to 15 μm.
8. 2. The decorative sheet according to claim 1, wherein the thickness of said surface protective layer is 2 μm or more and less than 10 μm.
9. 2. The decorative sheet according to claim 1, wherein the surface protective layer has a glossiness of 20.0 or less.
10. 2. The decorative sheet according to claim 1, wherein the surface protective layer has a glossiness of 10.0 or less.
11. The decorative sheet according to claim 1, wherein at least a portion of the plurality of ridge portions are adjacent to each other in the width direction, and at a position where at least a portion of the plurality of ridge portions are adjacent to each other in the width direction, a cross section parallel to the width direction and the thickness direction of the surface protection layer has a sinusoidal shape in the portion where the uneven structure is provided.
12. the surface protective layer contains a cured product of an ionizing radiation curable resin, The ionizing radiation curable resin is mainly composed of an acrylate containing a repeating unit structure, the repeating unit is any one of ethylene oxide, propylene oxide, and ε-caprolactone, 2. The decorative sheet according to claim 1, wherein the repeating structure is repeated three or more times.
13. the surface protective layer contains a cured product of an ionizing radiation curable resin, The decorative sheet according to claim 1, wherein the ionizing radiation curable resin is mainly composed of an acrylate, the acrylate being composed of a first acrylate containing a repeating structure and a second acrylate having mono- to hexa-functionality, the repeating structure being any one of ethylene oxide, propylene oxide, and ε-caprolactone, and the number of repetitions of the repeating structure is 3 or more.
14. A decorative material comprising the decorative sheet according to any one of claims 1 to 13 and a substrate to which the decorative sheet is attached.
Citation Information
Patent Citations
Forming method of design coating film, board for building material and aqueous coating composition
JP2007185606A
Decorative sheet and method for producing decorative sheet
JP2018144437A
Decorative sheet and manufacturing method thereof
JP2020075420A
Decorative sheet, decorative plate, and method for producing decorative sheet
JP2021137990A
Decorative sheet
WO2017033972A1