Non-oriented electrical steel sheet and its manufacturing method

A non-oriented electrical steel sheet with optimized elemental composition and manufacturing processes forms favorable ferrite textures, addressing the challenge of high magnetic flux density and reduced iron loss, enhancing motor efficiency and torque.

JP7583814B2Active Publication Date: 2024-11-14CLEANSOLUTION CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022537553
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-19
Filing Date
2020-12-17
Publication Date
2024-11-14
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing non-oriented electrical steel sheets face challenges in achieving high magnetic flux density and reduced iron loss without increasing manufacturing costs, particularly due to the limitations of elements like Si, Ni, and anisotropy issues between rolling and diagonal directions.

Method used

A non-oriented electrical steel sheet composition with controlled amounts of Si, Mn, P, S, Al, N, Cu, Ca, Mg, Sb, Sn, and other impurities, along with specific manufacturing processes, including hot rolling, cold rolling, and final annealing, to form favorable ferrite textures and improve magnetic properties.

Benefits of technology

The solution enhances magnetic flux density and reduces anisotropy, making it suitable for high-efficiency motors and generators with improved torque and output characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583814000001
    Figure 0007583814000001
  • Figure 0007583814000002
    Figure 0007583814000002
  • Figure 0007583814000003
    Figure 0007583814000003
Patent Text Reader

Abstract

An object of the present invention is to provide a non-oriented electrical steel sheet having improved magnetic flux density by forming a large amount of ferrite texture that is advantageous for magnetic properties through the segregation of S and P in a steel composition containing Cu, and a method for manufacturing the same. [Solution] The non-oriented electrical steel sheet of the present invention contains, by weight, Si: 1.5% or less, C: 0.01% or less (excluding 0%), Mn: 0.03 to 3%, P: 0.01 to 0.2%, S: 0.001 to 0.02%, Al: 0.01% or less (excluding 0%), N: 0.005% or less (excluding 0%), and Cu: 0.02 to 0.3%, and is characterized by containing Ca and Mg, each alone or in a combined amount of 0.0001 to 0.005% by weight, Sb and Sn, each alone or in a combined amount of 0.001 to 0.2% by weight, with the balance being Fe and unavoidable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-oriented electrical steel sheet and a manufacturing method thereof, and more particularly to a non-oriented electrical steel sheet having improved magnetic flux density by forming a large amount of ferrite texture that is advantageous for magnetic properties through segregation of S and P in a steel composition containing Cu, and a manufacturing method thereof. [Background technology]

[0002] Non-oriented electrical steel sheets are used as iron core materials in rotating equipment such as motors and generators, and stationary equipment such as small transformers, and play an important role in determining the energy efficiency of electrical equipment. Recently, the use of high-efficiency motors has increased significantly due to the tightening of motor efficiency regulations. In order to improve the efficiency of such motors, it is necessary to reduce iron loss and copper loss. Both of these methods can have a significant impact on the magnetism of the magnetic steel sheet, which is the core material. As a result, motor manufacturers are tending to use magnetic steel sheets with low iron loss instead of the existing magnetic steel sheets with high iron loss.

[0003] To reduce copper loss, methods are used such as lowering the design magnetic flux density below the conventional level or lowering the excitation current at the design magnetic flux. However, to use the latter method, it is necessary to improve the magnetic flux density of the electrical steel sheet. In particular, in the case of electromagnetic steel sheets with high magnetic flux density, there is the advantage that the torque can be improved, and in the case of motors that are frequently turned on and off, there is the advantage that large output can be produced in a short time. As an example of an electrical steel sheet with high magnetic flux density, a non-oriented electrical steel sheet with a low Si content and a large amount of Ni added is known. However, the addition of Ni lowers the stable temperature of austenite, and therefore the temperature at which heat treatment can be performed in the ferrite phase. This makes it impossible to perform high-temperature annealing, which is advantageous for iron loss and magnetism. In addition, there is a problem that the content of Si, an element that increases resistivity, is low, resulting in high iron loss. Therefore, it is necessary to develop a non-oriented electrical steel sheet that has low iron loss and high magnetic flux density without increasing manufacturing costs.

[0004] In addition, when the motor rotates, the excitation direction rotates within the plate surface, but generally the best magnetism is observed in the rolling direction, and the worst magnetism is observed in the direction at 45 degrees from the rolling direction. Therefore, not only is it extremely advantageous in terms of improving motor efficiency to have excellent magnetic properties in both the rolling direction and the diagonal direction of the rolling compared to an electrical steel sheet that is excellent only in the rolling direction, but also because the difference in magnetic properties between the two directions is small, it is preferred in the case of motors based on rotating bodies. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a non-oriented electrical steel sheet and a manufacturing method thereof, and more specifically, to provide a non-oriented electrical steel sheet and a manufacturing method thereof in which a large amount of ferrite texture that is advantageous for magnetic properties is formed by the segregation of S and P in a steel composition to which Cu is added, thereby improving magnetic flux density. [Means for solving the problem]

[0006] The non-oriented electrical steel sheet of the present invention is characterized by containing, by weight, Si: 1.5% or less, C: 0.01% or less (excluding 0%), Mn: 0.03 to 3%, P: 0.005 to 0.2%, S: 0.001 to 0.02%, Al: 0.7% or less (excluding 0%), N: 0.005% or less (excluding 0%) and Cu: 0.02 to 0.06%, Ca and Mg, each alone or in a combined amount, 0.0001 to 0.005% by weight, Sb and Sn, each alone or in a combined amount, 0.02 to 0.2% by weight, and the balance being Fe and unavoidable impurities.

[0007] The non-oriented electrical steel sheet of the present invention may contain 0.0001 to 0.003% by weight of Mg. The non-oriented electrical steel sheet of the present invention may contain 0.01 to 0.1% by weight of Sn and 0.001 to 0.1% by weight of Sb. The non-oriented electrical steel sheet of the present invention may further contain Ni: 0.05% by weight or less. The non-oriented electrical steel sheet of the present invention may have an average crystal grain size of 13 to 100 μm. The non-oriented electrical steel sheet of the present invention may have an average of the magnetic flux density B50L in the rolling direction and the magnetic flux density B50C in a direction forming an angle of 90 degrees with the rolling direction of 1.76 T or more, and a ratio (B50L / B50D) of the magnetic flux density B50L in the rolling direction to the magnetic flux density B50D in a direction forming an angle of 45 degrees with the rolling direction of 1.07 or less.

[0008] The method for producing a non-oriented electrical steel sheet of the present invention comprises the steps of: Si: 1.5% or less; C: 0.01% or less (excluding 0%); Mn: 0.03 to 3%; P: 0.005 The method comprises the steps of heating a slab, hot rolling the slab to produce a hot-rolled sheet, cold rolling the hot-rolled sheet to produce a cold-rolled sheet, and final annealing the cold-rolled sheet. The method comprises the steps of: heating a slab comprising: 0.001 to 0.02% S; 0.7% or less by weight of Al (except 0%); 0.005% or less by weight of N (except 0%); 0.02 to 0.06% Cu; 0.0001 to 0.005% by weight of Ca and Mg, each of which is alone or in a combined amount of 0.02 to 0.2% by weight of Sb and Sn, with the balance being Fe and unavoidable impurities. The thickness of the hot-rolled sheet may be 2.0 to 3.5 mm. The cold rolled sheet may have a thickness of 0.3 to 1.0 mm. Effect of the Invention

[0009] The non-oriented electrical steel sheet of the present invention can improve the magnetic flux density by forming a large amount of ferrite texture that is advantageous for magnetic properties due to the segregation of S and P in the steel composition to which Cu has been added. In addition, the anisotropy of the magnetic flux density can be improved. Furthermore, the non-oriented electrical steel sheet of the present invention can be used in a variety of applications, such as as a core material for high-efficiency motors, or motors with high output and high torque characteristics, and generators. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The term "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components. When we refer to an item as being "on" another item, it means that it is exactly on top of the other item, or there may be other items between them. In contrast, when we refer to an item as being "directly on" another item, there are no other items between them. Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless defined.

[0011] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight. In one embodiment of the present invention, the term "additionally contain an additional element" means that the additional amount of the additional element is substituted for the remaining iron (Fe). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein.

[0012] In one embodiment of the present invention, in a steel composition to which Cu is added, the segregation of S and P forms a large amount of ferrite texture that is advantageous for magnetic properties, thereby improving the magnetic flux density of a non-oriented electrical steel sheet.

[0013] The non-oriented electrical steel sheet according to one embodiment of the present invention contains, by weight percent, Si: 1.5% or less, C: 0.01% or less (excluding 0%), Mn: 0.03 to 3%, P: 0.005 0.0001-0.005% by weight, S: 0.001-0.02%, Al: 0.01% or less (excluding 0%), N: 0.005% or less (excluding 0%), Cu: 0.02-0.3%, Ca and Mg are each independently or in a combined amount of 0.0001-0.005% by weight, Sb and Sn are each independently or in a combined amount of 0.001-0.2% by weight, and the balance is Fe and unavoidable impurities. First, the reasons for limiting the components of non-oriented electrical steel sheets will be explained.

[0014] Si: 1.50% by weight or less Silicon (Si) is an element effective in increasing the inherent resistance of steel and reducing iron loss, and the more it is added, the better. However, it is an element that forms a BCC structure in place of iron atoms in steel, and is the main element that deteriorates magnetic flux density. When a large amount of Si is added, the saturation magnetic flux is greatly reduced, and as a result, the B50 magnetic flux density may also be deteriorated. Therefore, Si can be contained within the above-mentioned range. More specifically, Si can be contained in an amount of 1.00% by weight or less. More specifically, Si can be contained in an amount of 0.10 to 0.50% by weight.

[0015] C: 0.0100% by weight or less Carbon (C) is an element that causes magnetic aging and greatly increases core loss. Therefore, C can be contained in an amount of 0.0100% by weight or less. More specifically, C can be contained in an amount of 0.005% by weight or less. More specifically, C can be contained in an amount of 0.0010 to 0.0050% by weight.

[0016] Mn:0.03~3.00wt% Manganese (Mn) needs to be added in consideration of the amount of Cu added to prevent brittleness during hot rolling. If the Mn content is too low, problems due to brittleness during hot rolling may occur. If the Mn content is too high, the saturation magnetic flux density decreases, and the ratio of Fe in the steel decreases, causing the saturation magnetic flux density to decrease. Therefore, Mn can be contained within the above-mentioned range. More specifically, Mn can be contained in an amount of 0.05 to 1.00% by weight. More specifically, Mn can be contained in an amount of 0.10 to 0.50% by weight.

[0017] P: 0.005 ~0.20wt% Phosphorus (P) acts together with Cu and S to improve the texture in the ferrite structure of the steel and to increase the magnetic flux density. If the P content is too low, the above-mentioned effects may not be properly exhibited. If the P content is too high, P precipitates alone in the steel, resulting in poor magnetic flux density and maximizing the brittleness of the steel, making it difficult to roll the steel. Therefore, P may be contained within the above-mentioned range. More specifically, P may be contained in an amount of 0.03 to 0.15% by weight. More specifically, P may be contained in an amount of 0.05 to 0.10% by weight.

[0018] S:0.0010~0.0200wt% Sulfur (S) is an element that segregates on the surface and grain boundaries. S is an element that influences the development of texture due to surface segregation during annealing, and is useful for improving magnetic flux density and reducing anisotropy. When S is contained in an excessively small amount, the above-mentioned effects may not be properly exhibited. When S is contained in an excessively large amount, a large amount of sulfides such as MnS and CuS are formed, and the grain growth may be inhibited by these sulfides. As a result, the iron loss may increase. Therefore, S can be contained within the above-mentioned range. More specifically, S can be contained in 0.00150 to 0.0100 wt %. More specifically, S can be contained in 0.0020 to 0.0050 wt %.

[0019] Al: 0.700% by weight or less Aluminum (Al) is an element effective in increasing the specific resistance of steel and reducing iron loss, and is a useful element that can prevent phase transformation to austenite even at high temperatures depending on the amount added as a ferrite stabilizing element, and is an element that increases the resistivity of steel sheet to the same extent as Si. However, if too much Al is added, the saturation magnetic flux decreases significantly, and the excitation effective current may increase significantly when the motor is manufactured and driven. Therefore, Al may be contained within the above-mentioned range. More specifically, Al may be contained at 0.100% by weight or less. More specifically, Al may be contained at 0.005% by weight or less.

[0020] N: 0.0050% by weight or less Nitrogen (N) is a harmful element that forms nitrides, inhibits grain growth, and increases core loss. Therefore, N may be contained in an amount of 0.0050% by weight or less. More specifically, N may be contained in an amount of 0.0030% by weight or less.

[0021] Cu:0.020~0.060wt% Copper (Cu) facilitates crystal growth during coiling after hot rolling. In addition, the segregation of Sn, S, and P on the surface and grain boundaries has an effect on improving magnetic flux density. In addition, by combining with S to form coarse sulfides during final annealing, it suppresses the inferiority of iron loss due to fine MnS, improves magnetic flux density, and reduces iron loss, making it possible to manufacture an electrical steel sheet with excellent magnetic properties. When Cu is contained in an excessively small amount, the above-mentioned effects may not be properly expressed. When Cu is contained in an excessively large amount, it may cause hot shortening defects at high temperatures and may cause the formation of a Cu secondary phase in the steel, thereby deteriorating the magnetic flux density. Therefore, Cu may be contained within the above-mentioned range. More specifically, Cu may be contained in an amount of 0.020 to 0.050 wt%. At this time, Cu is one of the most commonly used metallic elements, and is either mixed in from scrap, which is the raw material for steel, or added as an alloy element.

[0022] Ca and Mg, either alone or in combination: 0.0001 to 0.005% by weight Calcium (Ca) is an element that forms sulfides and oxides. When Ca is added, it can coarsen sulfides and promote particle growth. When Ca and Mg are contained in excessively small amounts, the above-mentioned effects may not be properly exhibited. When Ca is contained in excessively large amounts, it combines with Ca and oxygen in the steel to form precipitates, slowing down the crystal growth rate, which can cause a problem of suppressing the texture control effect during annealing by P. Therefore, Ca can be added together with Mg in the above-mentioned range. More specifically, when Ca is contained, it can contain 0.0005 to 0.005 wt % Ca. More specifically, it can contain 0.0005 to 0.0015 wt % Ca.

[0023] Magnesium (Mg) acts similarly to Ca during annealing in Cu, S and P added steel. That is, when Mg is added, it can coarsen sulfides and promote particle growth. When Mg and Ca are contained in excessively small amounts, the above-mentioned effects may not be properly exhibited. When Mg is added in excessively large amounts, the texture control effect during annealing by P can be suppressed. Therefore, Mg can be added in the above-mentioned range together with Ca. More specifically, when Mg is contained, Mg can be contained in 0.0001 to 0.003 wt %. More specifically, Mg can be contained in 0.0005 to 0.002 wt %.

[0024] Since Ca has a similar effect to Mg, they are treated as one element and when contained alone, separately, or simultaneously, the total amount of these elements can be contained in the range of 0.0001 to 0.005 wt %. That is, when Ca is contained alone, it can contain 0.0001 to 0.005 wt % Ca; when Mg is contained alone, it can contain 0.0001 to 0.005 wt % Mg; and when Ca and Mg are contained simultaneously, it can contain 0.0001 to 0.005 wt % of Ca and Mg in total.

[0025] Sb and Sn, either singly or in combination: 0.02 to 0.2% by weight Antimony (Sb) and tin (Sn) are both grain boundary segregation elements, and have the effect of controlling the texture caused by crystal growth during annealing and improving magnetic flux density. When the Sb and Sn content is too low, the above-mentioned effects may not be properly manifested. In particular, in steels to which Cu is added, they have the effect of inducing texture that greatly improves magnetic properties through mutual interaction at grain boundaries and favoring crystal growth. However, when Sb and Sn are included in excessive amounts, they may segregate at grain boundaries, reducing toughness and decreasing productivity compared to improving magnetic properties. Since Sb and Sn have similar functions, they are treated as one element, and when they are contained alone, each of them, or both of them can be contained in a total amount of 0.02 to 0.2 wt %. That is, when Sb is contained alone, it can contain 0.02 to 0.2 wt % Sb, when Sn is contained alone, it can contain 0.02 to 0.2 wt % Sn, or when Sb and Sn are contained simultaneously, it can contain 0.001 to 0.2 wt % of Sb and Sn in total. More specifically, it may contain 0.020 to 0.100% by weight of Sn and 0.0001 to 0.100% by weight of Sb at the same time.

[0026] The non-oriented electrical steel sheet according to an embodiment of the present invention may further include Ni: 0.05 wt % or less. Ni: 0.05% by weight or less Nickel (Ni) is known as an element that increases saturation magnetic flux density. In one embodiment of the present invention, the addition of Cu, S, and P can sufficiently improve the saturation magnetic flux density, and the addition of Ni can rather inhibit the growth of crystal grains, resulting in low core loss and the formation of a texture that is unfavorable to magnetism. Therefore, when Ni is further included, it may be included in an amount of 0.05% by weight or less. More specifically, it may be included in an amount of 0.02% by weight or less.

[0027] Other impurities In addition to the elements mentioned above, impurities are inevitably mixed in. The balance is iron (Fe), and when additional elements other than the elements mentioned above are added, they are included to replace the balance of iron (Fe). Inevitably added impurities may be Cr, Zr, Mo, V, and the like. Cr may be contained in an amount of 0.05% by weight or less. Cu, Ni, and Cr react with impurity elements to form fine sulfides, carbides, and nitrides, which have a detrimental effect on magnetic properties, so their contents are each limited to 0.05% by weight or less. The steel may further contain 0.01% by weight or less of one or more of Zr, Mo, and V. Since Zr, Mo, V, etc. are strong carbonitride-forming elements, it is preferable to avoid adding them as much as possible, and each of them is contained in an amount of 0.01% by weight or less.

[0028] As described above, the non-oriented electrical steel sheet according to an embodiment of the present invention contains appropriate Cu, S, P, Ca, and Mg as alloy components, and sulfides of appropriate size and density are formed. These sulfides can promote grain growth, ultimately improving the magnetic properties and anisotropy of the non-oriented electrical steel sheet. The average crystal grain size in the microstructure of the electrical steel sheet may be 13.0 to 100.0 μm. If the crystal grain size is too small, the hysteresis loss increases and the core loss deteriorates. In addition, it is preferable to have an appropriate crystal grain size in order to improve the magnetic flux density by the effect of fine precipitates and segregation. However, if the crystal grain size is too large, there may be a problem in processing during punching in a product coated after annealing. More specifically, the average crystal grain size may be 13.0 to 40.0 μm. The crystal grains constituting non-oriented electrical steel sheet are composed of a non-recrystallized structure processed in the cold rolling process and then recrystallized in the final annealing process, with the recrystallized structure accounting for 99% or more by volume.

[0029] As described above, the non-oriented electrical steel sheet according to one embodiment of the present invention has excellent magnetic properties and anisotropy. Specifically, the non-oriented electrical steel sheet according to an embodiment of the present invention has a magnetic flux density (B 50), the average of the magnetic flux density B50L in the rolling direction (RD direction) and the magnetic flux density B50C in the direction forming an angle of 90 degrees with the rolling direction (TD direction) may be 1.76 T or more, and the ratio (B50L / B50D) of the magnetic flux density B50L in the rolling direction to the magnetic flux density B50D in the direction forming an angle of 45 degrees with the rolling direction may be 1.07 or less. More specifically, the average of B50L and B50C may be 1.78 to 1.85 T, and (B50L / B50D) may be 1.00 to 1.05. The non-oriented electrical steel sheet according to an embodiment of the present invention is also excellent in terms of iron loss. Specifically, the iron loss (W 15 / 50 ) may be 5.5 W / kg or less.

[0030] A method for producing a non-oriented electrical steel sheet according to an embodiment of the present invention comprises the steps of: (a) preparing a steel sheet having a composition, by weight percent, of Si: 1.5% or less; C: 0.01% or less (excluding 0%); Mn: 0.03 to 3%; P: 0.005 The method may include the steps of heating a slab comprising: heating the slab; hot rolling the slab to produce a hot-rolled sheet; cold rolling the hot-rolled sheet to produce a cold-rolled sheet; and final annealing the cold-rolled sheet. The method may include the steps of heating a slab comprising: 0.001 to 0.02% S; 0.7% or less (excluding 0%) Al; 0.005% or less (excluding 0%) N; 0.02 to 0.06% Cu; 0.0001 to 0.005% by weight of Ca and Mg, each of which is alone or in a combined amount; 0.001 to 0.2% by weight of Sb and Sn, each of which is alone or in a combined amount; and the balance being Fe and unavoidable impurities. Each step will be explained in detail below.

[0031] First, the slab is heated. The reason for limiting the addition ratio of each component in the slab is the same as the reason for limiting the composition of the non-oriented electrical steel sheet described above, so a repeated explanation will be omitted. The composition of the slab does not substantially change during the manufacturing process such as hot rolling, hot-rolled sheet annealing, cold rolling, and final annealing described below, so the composition of the slab and the composition of the non-oriented electrical steel sheet are substantially the same. The slabs can be produced by melting steel having a suitable composition in a converter or a degassing treatment device, and then performing continuous casting or rolling of the lump or powder. The slab is placed in a heating furnace and heated to 1,100 to 1,250°C. When heated to a temperature exceeding 1,250°C, precipitates such as AlN and MnS present in the slab are redissolved and then finely precipitate during hot rolling, suppressing grain growth and possibly reducing magnetic properties. When the slab is heated, it is hot-rolled to 2.0-3.5 mm, and the hot-rolled sheet is coiled. During hot rolling, the finish rolling ends in the ferrite phase region. During hot rolling, a large amount of ferrite phase expanding elements such as Si, Al, and P is added, or elements that suppress the ferrite phase such as Mn and C are added in small amounts. When rolling in the ferrite phase in this way, many {100} planes are formed in the texture, which can improve the magnetic properties.

[0032] After the step of producing the hot-rolled sheet, the method may further include a step of annealing the hot-rolled sheet. At this time, the annealing temperature of the hot-rolled sheet may be 950 to 1,200°C. If the annealing temperature of the hot-rolled sheet is too low, the structure does not grow or grows finely, resulting in little increase in magnetic flux density, and if the annealing temperature is too high, the magnetic properties may rather decrease and rolling workability may become poor due to deformation of the sheet shape. The annealing of the hot-rolled sheet is performed to increase the orientation favorable to magnetism as necessary, and may be omitted.

[0033] Next, the hot-rolled sheet is pickled and cold-rolled to a predetermined sheet thickness. Although different reduction rates can be applied depending on the thickness of the hot-rolled sheet, cold rolling can be applied to a final thickness of 0.3 to 1.0 mm by applying a rolling reduction of 50 to 95%. Cold rolling can be performed in a single cold rolling pass, or can be performed in two or more cold rolling passes with intermediate annealing in between as necessary. The cold-rolled sheet is subjected to final annealing (cold-rolled sheet annealing). In the process of final annealing the cold-rolled sheet, the soaking temperature during annealing is set to 800 to 1,150°C. If the annealing temperature of the cold-rolled sheet is too low, it may be difficult to obtain crystal grains large enough to obtain low core loss. If the annealing temperature is too high, the sheet shape during annealing may not be uniform, and the precipitates may be redissolved at high temperature and then precipitate finely during cooling, which may adversely affect the magnetic properties. The steel sheet that has been subjected to the final annealing is subjected to an insulating coating treatment. The method of forming the insulating layer is widely known in the technical field of non-oriented electrical steel sheets, and therefore a detailed description thereof will be omitted. Specifically, as the insulating layer forming composition, either a chromium-based (Cr-type) or a chromium-free (Cr-free) type can be used without any restrictions.

[0034] Preferred examples and comparative examples of the present invention will be described below. However, the following examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples. EXAMPLES

[0035] Molten steel blown in a converter was degassed to produce steel consisting of the weight percentages shown in Tables 1 and 2 below, with the balance being Fe and unavoidable impurities, and then the steel was continuously cast to produce slabs. The slabs were reheated by holding at 1200°C for 1 hour, and then hot rolled at a finish rolling temperature of 860°C to the thicknesses listed in Table 3 to produce hot-rolled sheets. Each hot-rolled sheet produced was coiled at a temperature of 700°C and annealed in air for 60 minutes to replicate the temperature of the hot-rolled coil during coiling. This was cold-rolled to a thickness of 0.5 mm, and then annealed at 850°C for 35 seconds in a nitrogen atmosphere containing 5% hydrogen to produce a non-oriented electrical steel sheet. From this, SST test pieces with a width of 60 mm and a length of 60 mm were cut out in the rolling direction (L direction) and in a direction at 45 degrees to the rolling direction (D direction), and the core loss W was measured according to IEC 60404-3. 15 / 50 For magnetic flux density B50 and anisotropy, the following (B50L / B50D) was measured, and the results are shown in Table 3.

[0036] [Table 1]

[0037] [Table 2]

[0038] [Table 3]

[0039] As shown in Tables 1 to 3, it can be confirmed that the inventive examples, which all satisfy the alloy components according to one embodiment of the present invention, are excellent in both magnetism and anisotropy. In contrast, it can be seen that Steel Type 1 contains an excessive amount of C, which results in poor magnetic properties and anisotropy. It can be seen that steel type 2 contains an excess of Si, which results in poor magnetic properties and anisotropy. It can be seen that Steel Type 3 and Steel Type 19 have poor magnetic properties and anisotropy due to their excessive or insufficient Mn content. It can be seen that steel type 4 and steel type 20 contain excessive or insufficient P, and therefore have poor magnetic properties and anisotropy. It can be seen that steel types 5 and 6 contain excessive Al, which results in poor magnetic properties and anisotropy. It can be seen that steel types 9, 23, and 24 contain excessive or insufficient S, and therefore have poor magnetic properties and anisotropy. It can be confirmed that steel type 8 contains an excessive amount of N, and therefore has poor magnetic properties and anisotropy. It can be seen that steel types 9, 10 and 12 have poor magnetic properties and anisotropy due to their excessive or insufficient Cu content. It can be confirmed that steel types 13, 14, 15 and 18 contain excessive or insufficient amounts of Sb and Sn, and therefore have poor magnetic properties and anisotropy. It can be confirmed that steel types 11, 16 and 17 have poor magnetic properties and anisotropy due to their excessive or insufficient Ca and Mg content.

[0040] The present invention is not limited to the above-mentioned embodiments, and can be manufactured in various different forms, and a person skilled in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-mentioned embodiments are illustrative in all respects and not limiting.

Claims

1. In weight percent, it contains Si: 0.10 to 0.50%, C: 0.010% or less (excluding 0%), Mn: 0.03 to 3%, P: 0.005 to 0.20%, S: 0.0010 to 0.020%, Al: 0.7% or less (excluding 0%), N: 0.005% or less (excluding 0%), and Cu: 0.02 to 0.06%; Ca and Mg are each contained alone or in a combined amount of 0.0001 to 0.005% by weight, The alloy contains 0.02 to 0.20% by weight of Sb and Sn, either singly or in combination, with the remainder being Fe and unavoidable impurities, A non-oriented electrical steel sheet, characterized in that the average of the magnetic flux density B50L in the rolling direction and the magnetic flux density B50C in a direction forming an angle of 90 degrees with the rolling direction is 1.76 T or more, and the ratio (B50L / B50D) of the magnetic flux density B50L in the rolling direction to the magnetic flux density B50D in a direction forming an angle of 45 degrees with the rolling direction is 1.07 or less.

2. 2. The non-oriented electrical steel sheet according to claim 1, further comprising: 0.0001 to 0.003 wt. % Mg.

3. 3. The non-oriented electrical steel sheet according to claim 1, comprising: 0.02 to 0.1% by weight of Sn and 0.001 to 0.1% by weight of Sb.

4. The non-oriented electrical steel sheet according to any one of claims 1 to 3, further comprising Ni: 0.05% by weight or less.

5. The non-oriented electrical steel sheet according to any one of claims 1 to 4, characterized in that the average crystal grain size is 13 to 100 µm.

6. heating a slab containing, by weight, 0.10-0.50% Si, 0.010% or less (excluding 0%) C, 0.03-3% Mn, 0.005-0.20% P, 0.0010-0.020% S, 0.7% or less Al (excluding 0%), 0.005% or less N (excluding 0%) and 0.02-0.06% Cu, 0.0001-0.005% by weight of Ca and Mg, each of which is singly or in a combined amount, 0.02-0.20% by weight of Sb and Sn, and the balance being Fe and unavoidable impurities; hot rolling the slab to produce a hot rolled sheet; cold rolling the hot rolled sheet to produce a cold rolled sheet; and final annealing of the cold rolled sheet; The non-oriented electrical steel sheet produced has an average of a magnetic flux density B50L in the rolling direction and a magnetic flux density B50C in a direction forming an angle of 90 degrees with the rolling direction of 1.76 T or more, and a ratio (B50L / B50D) of a magnetic flux density B50L in the rolling direction to a magnetic flux density B50D in a direction forming an angle of 45 degrees with the rolling direction of 1.07 or less.

7. The method for producing a non-oriented electrical steel sheet according to claim 6, characterized in that the hot-rolled sheet has a thickness of 2.0 to 3.5 mm.

8. The method for producing a non-oriented electrical steel sheet according to claim 6 or 7, characterized in that the cold rolled sheet has a thickness of 0.3 to 1.0 mm.

Citation Information

Patent Citations

  • Non-oriented silicon steel sheet excellent in magnetic property

    JP2001271147A

  • Non-oriented electromagnetic steel sheet extremely excellent in core loss and magnetic flux density

    JP2010174376A

  • Non-oriented silicon steel sheet excellent in recyclability and method for producing the same

    JP2016125134A

  • Non-oriented magnetic electromagnetic steel sheet and manufacturing method therefor

    JP2017057462A