Bi-directional electrical steel sheet and its manufacturing method

By controlling alloy composition and rolling conditions, the bidirectional electrical steel sheet achieves improved magnetic properties in both rolling and perpendicular directions, addressing the limitations of existing sheets and enhancing generator performance.

JP7583815B2Active Publication Date: 2024-11-14CLEANSOLUTION CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022537561
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-19
Filing Date
2020-12-17
Publication Date
2024-11-14
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing electrical steel sheets exhibit poor magnetic properties in directions perpendicular to the rolling direction, limiting their application in generators with varying rotation speeds and requiring complex, low-productivity manufacturing methods.

Method used

A bidirectional electrical steel sheet with controlled alloy composition (Si: 2.0~4.0%, Al: 0.01~0.04%, S: 0.0004~0.02%, Mn: 0.05~0.3%, N: 0.01% or less, C: 0.005% or less, P: 0.005~0.15%, Ti: 0.001~0.005%, Ca: 0.0001~0.005%, Mg: 0.0001~0.005%) and adjusted rolling conditions to enhance the fraction of {100} oriented crystal grains, ensuring excellent magnetism in both rolling and perpendicular directions.

Benefits of technology

The solution results in a steel sheet with enhanced magnetic properties in both directions, suitable for generators with slow rotation speeds, and allows for continuous production, improving productivity and energy efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583815000009
    Figure 0007583815000009
  • Figure 0007583815000010
    Figure 0007583815000010
  • Figure 0007583815000001
    Figure 0007583815000001
Patent Text Reader

Abstract

The object of the present invention is to appropriately control the contents of Ti, Mg, and Ca in the alloy composition and adjust the rolling conditions to obtain a {100} <001> The present invention aims to provide a bi-directional electrical steel sheet having excellent magnetic properties in both the rolling direction and the direction perpendicular to the rolling direction by increasing the fraction of oriented crystal grains, and a method for manufacturing the same. The present invention provides a two-dimensional electrical steel sheet containing, by weight, 2.0 to 4.0% Si, 0.01 to 0.04% Al, 0.0004 to 0.02% S, 0.05 to 0.3% Mn, 0.01% or less (excluding 0%) N, 0.005% or less (excluding 0%) C, 0.005 to 0.15% P, 0.001 to 0.005% Ti, 0.0001 to 0.005% Ca, and 0.0001 to 0.005% Mg, with the remainder being Fe and other unavoidable impurities. <001> The area fraction of crystal grains with orientations within 15° of {100} is 60 to 99%. <025> The area fraction of crystal grains having an orientation within 15° from the center is within 1 to 30%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bi-directional electrical steel sheet and a manufacturing method thereof. More specifically, the present invention relates to a method for producing the same, which is characterized in that the contents of Ti, Mg, and Ca in the alloy composition are appropriately controlled and the rolling conditions are adjusted to produce a {100} <001> The present invention relates to a bi-directional electrical steel sheet having excellent magnetic properties in both the rolling direction and the direction perpendicular to the rolling direction by increasing the fraction of oriented crystal grains, and a method for manufacturing the same. [Background technology]

[0002] In order to improve the magnetic flux density of electrical steel sheets, it is necessary to improve the texture of the steel and to align it in the magnetization direction. <100> The most effective method is to align the axes parallel to each other. In addition, a method is used to improve the magnetic flux density by reducing the amount of alloy in the steel and increasing the proportion of Fe atoms in the steel to bring the saturation magnetic flux closer to that of pure iron. Among these, in the case of grain-oriented electrical steel sheets, the Goss orientation, known as {110} <001> This is a method that uses the orientation of the steel, and is usually obtained by the process of slab - hot rolling - hot rolled sheet annealing - cold rolling - decarburization during the first recrystallization - nitriding - second high temperature annealing. However, this method has excellent magnetic properties only in the rolling direction (Rd direction) and is extremely poor in the direction perpendicular to the rolling direction (TD direction), making it difficult to use it in anything other than transformers in which the magnetization direction is set to the rolling direction. For this reason, <100> There is a demand for the production of electrical steel sheets with a controlled texture that makes the axes parallel.

[0003] The magnetization direction in rotating equipment usually rotates within the plate plane, <100> The axis must be parallel to the plate surface, but among the orientations under this condition, the orientation commonly observed in steel materials is {100} <011> This is the direction that is shifted 45 degrees from the rolling direction to the direction perpendicular to the rolling direction (TD direction). <100> Since the axes are parallel, the most magnetic properties are achieved when the magnetization direction is at 45 degrees to the rolling direction of the sheet. However, this orientation is a stable orientation during cold rolling, and is completely lost during recrystallization annealing, so it is not used in electrical steel sheet materials. Similarly, <001> There is a certain orientation, known as the Cube orientation, which has long been recognized as useful, but the only known methods of producing it are those that involve cross rolling and vacuum annealing, which are not feasible for large-scale industrial production. In particular, the cross rolling method cannot be used because continuous production of the material is not possible. In the case of large generators, cylindrical cores with diameters of several meters must be manufactured, so it cannot be applied to a process in which the core is divided into several to several tens of pieces on a plate and then assembled, and productivity is extremely low.

[0004] In the case of generators, typical turbine generators produce electricity at the commercial electrical frequency of 50 Hz or 60 Hz in each country, so the magnetic properties at 50 Hz and 60 Hz are important, but for generators with slow rotational speeds such as wind turbines, the magnetic properties at DC and frequencies below 30 Hz are important. Therefore, in the above equipment, the magnetic flux density characteristic, which indicates the degree of magnetization, is more important than the iron loss generated by AC magnetic field, and this is generally evaluated by B8 magnetic flux density. B8 magnetic flux density means the magnetic flux density value of a steel sheet when the magnetic field strength is 800A / m, which is mainly measured with 50Hz AC magnetic field, but in some cases it is measured with DC or at frequencies below 50Hz. Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to provide a bi-directional electrical steel sheet and a method for producing the same. More specifically, the contents of Ti, Mg, and Ca in the alloy composition are appropriately controlled and the rolling conditions are adjusted to produce a {100} <001> The present invention provides a bi-directional electrical steel sheet having excellent magnetic properties in both the rolling direction and the direction perpendicular to the rolling direction by increasing the fraction of oriented crystal grains, and a method for manufacturing the same. [Means for solving the problem]

[0006] The grain-oriented electrical steel sheet of the present invention contains, by weight, 2.0 to 4.0% Si, 0.01 to 0.04% Al, 0.0004 to 0.02% S, 0.05 to 0.3% Mn, 0.01% or less (excluding 0%) N, 0.005% or less (excluding 0%) C, 0.005 to 0.15% P, 0.001 to 0.005% Ti, 0.0001 to 0.005% Ca, and 0.0001 to 0.005% Mg, with the balance being Fe and other unavoidable impurities, <001> The area fraction of crystal grains having an orientation within 15° of {100} is 60 to 99%. <025> The crystal grains having an orientation within 15° from the above range have an area fraction of 1 to 30%.

[0007] The grain-oriented electrical steel sheet of the present invention satisfies the following formula 1. [Formula 1] 10×([Ti]+[Ca]+[Mg])≧[Al] (In formula 1, [Ti], [Ca], [Mg] and [Al] represent the contents (wt%) of Ti, Ca, Mg and Al, respectively.)

[0008] The grain-oriented electrical steel sheet of the present invention may further contain one or more of Sn: 0.1% by weight or less, Sb: 0.001 to 0.1% by weight, and Mo: 0.01 to 0.2% by weight. The grain-oriented electrical steel sheet of the present invention may further contain one or more of Bi: 0.01 wt % or less, Pb: 0.01 wt % or less, As: 0.01 wt % or less, Be: 0.01 wt % or less, and Sr: 0.01 wt % or less. The grain-oriented electrical steel sheet of the present invention may have an average crystal grain size that is 20 times or more the thickness of the steel sheet. The bidirectional electrical steel sheet of the present invention may include an oxide layer formed from the surface of a substrate of the steel sheet toward the inside of the substrate, and an insulating layer formed on the surface of the substrate. The surface of the base material and the insulating layer can be in contact with each other. It may further include a forsterite layer interposed between the surface of the substrate and the insulating layer.

[0009] In the grain-oriented electrical steel sheet of the present invention, Br in both the rolling direction and the direction perpendicular to the rolling direction may be 1.65 T or more, and Br in the circumferential direction may be 1.58 T or more. Br is calculated by the following formula 2. [Formula 2] Br=7.87 / (7.87-0.065×[Si]-0.1105×[Al])×B8 (In formula 2, [Si] and [Al] indicate the contents (wt%) of Si and Al, respectively. B8 indicates the strength (Tesla) of the induced magnetic field when induced at 800 A / m.)

[0010] The method for producing a grain-oriented electrical steel sheet of the present invention comprises, by weight%, Si: 2.0 to 4.0%, Al: 0.01 to 0.04%, S: 0.0004 to 0.02%, Mn: 0.05 to 0.3%, N: 0.02% or less (excluding 0%), C: 0.05% or less (excluding 0%), P: 0.005 to 0.15%, Ti: 0.001 to 0.005%, Ca: 0.0001 to 0.005%, and Mg: 0.0001 to 0.005%, with the balance The method includes the steps of producing a slab containing Fe and other unavoidable impurities, hot rolling the slab to produce a hot-rolled sheet, rolling the hot-rolled sheet to produce a steel sheet, subjecting the steel sheet to primary recrystallization annealing, and subjecting the steel sheet that has been primarily recrystallized annealed to secondary recrystallization annealing, wherein the total reduction in the step of producing the hot-rolled sheet is 95% or more, and the step of producing the hot-rolled sheet includes a plurality of passes, with the reduction in each pass being 50% or less. The slab can satisfy the following formula 3. [Formula 3] [C] / [Si]≧0.0067 (In formula 3, [C] and [Si] represent the C and Si contents (wt%) in the slab, respectively.)

[0011] The step of producing the hot rolled sheet may be carried out at a temperature of 700° C. or higher. The step of manufacturing the steel sheet may include a step of first rolling the hot-rolled sheet; a step of intermediate annealing, and a step of second rolling the intermediate-annealed steel sheet.

[0012] The first rolling step and the second rolling step may each have a rolling reduction of 75% or less. The first rolling step and the second rolling step may include a plurality of passes, with the reduction in each pass being 45% or less. The first rolling step and the second rolling step may be performed at a temperature of 50°C or more and less than 700°C.

[0013] The step of performing the first recrystallization annealing may include a step of decarburizing at a dew point temperature of 50 to 70°C. The first recrystallization annealing step may include a nitriding step, and the amount of nitriding may be 0.01 to 0.03 wt %. After the step of performing the primary recrystallization annealing, the average grain size of the steel sheet that has been subjected to the primary recrystallization annealing may be 30 to 50 μm. After the first recrystallization annealing step, the method may further include applying an annealing separator. After the second recrystallization annealing step, the method may further include removing a forsterite layer formed on the surface of the steel sheet. Effect of the Invention

[0014] The grain-oriented electrical steel sheet of the present invention has excellent magnetic properties in both the rolling direction and the direction perpendicular to the rolling direction by appropriately controlling the contents of Ti, Mg, and Ca in the alloy composition and adjusting the rolling conditions. It is particularly useful for generators with slow rotation speeds, such as wind power generators. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic diagram of a cross section of a grain-oriented electrical steel sheet according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a grain-oriented electrical steel sheet according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, the first part, component, region, layer or section described below may be referred to as the second part, component, region, layer or section without departing from the scope of the present invention. The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The term "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components. When an element is referred to as being "on" another element, it means that it is directly on top of the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them. Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless defined.

[0017] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight. In one embodiment of the present invention, the term "additionally contain an additional element" refers to the addition of an additional amount of the additional element in place of the remaining iron (Fe). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein.

[0018] A grain-oriented electrical steel sheet according to an embodiment of the present invention contains, by weight, 2.0-4.0% Si, 0.01-0.04% Al, 0.0004-0.02% S, 0.05-0.3% Mn, 0.01% or less (excluding 0%) N, 0.005% or less (excluding 0%) C, 0.005-0.15% P, 0.001-0.005% Ti, 0.0001-0.005% Ca, and 0.0001-0.005% Mg, with the remainder being Fe and other unavoidable impurities. First, the reasons for limiting the composition of the bidirectional electrical steel sheet will be explained.

[0019] Si:2.00~4.00wt% Silicon (Si) is an element that forms austenite during hot rolling, and the amount of addition must be limited to provide an austenite fraction of about 10% near the slab heating temperature and the hot-rolled sheet annealing temperature. In addition, in secondary recrystallization annealing, only when the secondary recrystallization microstructure is a single phase ferrite can be smoothly formed during annealing, so the amount of addition must be limited to a single phase ferrite. In pure iron, when 2.0 wt% or more is added, a single phase ferrite is formed, and the austenite fraction can be adjusted by adding C, so the lower limit of the Si content can be limited to 2.0 wt%. Furthermore, when the Si content exceeds 4 wt%, cold rolling is difficult and the saturation magnetic flux is poor, so this is limited. More specifically, the Si content is 2.2 to 3.3 wt%. More specifically, in order to obtain a steel sheet with high magnetic flux density, the Si content is 2.4 to 2.9 wt%.

[0020] Al:0.010~0.040wt% Aluminum (Al) forms AlN and is used as an inhibitor of secondary recrystallization. In one embodiment of the present invention, the cube texture can be obtained even when using inhibitors other than those used in the nitriding process of normal grain-oriented electrical steel sheets, so the amount of Al added can be controlled in a wider range than that of normal grain-oriented electrical steel sheets. However, when less than 0.01 wt% is added, the oxides in the steel increase significantly, deteriorating the magnetic properties, and the secondary recrystallization temperature is changed to prevent the formation of the cube orientation, so the lower limit is set to 0.01 wt%. When the amount exceeds 0.04 wt%, the secondary recrystallization temperature increases significantly, making industrial production difficult. More specifically, the Al content is 0.015 to 0.035 wt%.

[0021] S:0.0004~0.0200% by weight Sulfur (S) combines with Cu and Mn in steel to form fine MnS, and the finely formed precipitates aid secondary recrystallization, so the amount of S added can be 0.0004 to 0.02 wt%. If S is added in excess, the Goss fraction in the steel increases during secondary recrystallization due to segregation of S, and the precipitates in the hot-rolled sheet are not controlled, so that the desired texture during secondary recrystallization may not be obtained. More specifically, S is contained in an amount of 0.0005 to 0.006 wt%.

[0022] Mn:0.05~0.30wt% Manganese (Mn) is unavoidably present in molten steel, but a small amount of Mn can be used as a precipitate, and can be added to steel as an element that changes to MnS after the formation of FeS. However, if too much Mn is added, Mn maintains a strong bond with S even during high-temperature annealing, preventing the bond between Mg, Ca, and S that form fine precipitates. Conversely, if too little Mn is added, it may become difficult to control the texture during secondary recrystallization. Therefore, Mn is contained in an amount of 0.05 to 0.3 wt%. More specifically, Mn is contained in an amount of 0.08 to 0.2 wt%.

[0023] N: 0.0100% by weight or less Nitrogen (N) is an element that forms AlN, and since AlN is used as an inhibitor, it is necessary to ensure that the content is appropriate. If the N content is too low, it will sufficiently increase the degree of non-uniform deformation of the structure during cold rolling, promote cube growth during primary recrystallization, and make it impossible to suppress the growth of goss. If the N content is excessive, not only will it cause surface defects such as blisters due to nitrogen diffusion during processes after hot rolling, but it will also form excess nitrides in the hot-rolled steel sheet state, making rolling difficult and causing an increase in manufacturing costs. The slab contains 0.02 wt% or less N. In one embodiment of the present invention, a nitriding process is included during the first recrystallization annealing, but when 0.01 wt% to 0.02 wt% is added to the hot-rolled steel sheet, this nitriding process can be omitted to create a sufficient inhibitor. Since some of the N is removed during the second recrystallization annealing, the N content of the slab and the final manufactured electrical steel sheet differ.

[0024] C: 0.0050% by weight or less If carbon (C) is contained in a large amount even after the secondary recrystallization annealing, magnetic aging occurs and iron loss increases significantly, so the upper limit is set to 0.005 wt %. More specifically, C can be contained in an amount of 0.0001 to 0.005 wt %. The slab contains C at 0.05 wt% or less. This can suppress stress concentration and goss formation in the hot-rolled sheet, and can refine precipitates. C also increases the degree of non-uniform deformation of the structure during cold rolling, promotes cube growth during primary recrystallization, and suppresses the growth of goss. However, if excessive C is added, although stress concentration in the hot-rolled sheet can be eliminated, goss formation cannot be suppressed, and refinement of precipitates is difficult. Since it significantly deteriorates cold rolling properties during cold rolling, there is a limit to the amount of addition. In one embodiment of the present invention, the C content of the slab and the final manufactured electrical steel sheet is different because a decarburization process is included during primary recrystallization annealing.

[0025] The C and Si contents in the slab can satisfy Eq. [Formula 3] [C] / [Si]≧0.0067 (In formula 3, [C] and [Si] represent the C and Si contents (wt%) in the slab, respectively.) If the C content is too low or the Si content is too high, it may be difficult to promote the growth of cubes and suppress the growth of goss. More specifically, the left side of Equation 3 may be 0.0083 or more.

[0026] P:0.005~0.150wt% Phosphorus (P) improves the resistivity of steel, improves the cube fraction during secondary recrystallization, and increases the amount of non-uniform deformation during cold rolling, so it is preferable to add at least 0.005% by weight. However, when added in excess of 0.15% by weight, the cold rolling properties become extremely weak, so the amount of addition is limited. More specifically, P is contained in an amount of 0.01 to 0.08% by weight.

[0027] Ca: 0.0001 to 0.0050% by weight and Mg: 0.0001 to 0.0050% by weight Calcium (Ca) and magnesium (Mg) are alloy elements with very high reactivity in steel, and even when added in small amounts, they have a significant effect on the properties of steel. In steel with an appropriate amount of S added, Ca and Mg combine with S to form fine sulfides at high temperatures. These are stable even at low temperatures, so when these fine precipitates are formed in a hot-rolled sheet, they act as inhibitors for texture control during secondary recrystallization. However, when excessive amounts of Ca and Mg are added, they also combine with oxygen in the steel to form oxides, which can cause surface defects and magnetic defects. Therefore, the steel contains 0.0001 to 0.005 weight percent Ca and 0.0001 to 0.005 weight percent Mg. More specifically, the steel contains 0.001 to 0.003 weight percent Ca and 0.0005 to 0.0025 weight percent Mg.

[0028] Ti:0.0010~0.0050wt% Titanium (Ti) is an alloying element with high reactivity in steel, and reacts with C, N, O, etc. in steel to rapidly form inclusions and precipitates from continuous casting. By adding Ti, the dissolved oxygen in steel is first removed, and then the solid solubility of C, N, etc. is reduced. Since it is necessary to control the amount of dissolved oxygen in steel for the growth of cubes, the amount of Ti added is preferably 0.001 wt% or more. On the other hand, in order not to play a role in reducing the solid solubility of C and N, which affect the deformation during rolling in steel, it is preferable to add 0.005 wt% or less. More specifically, Ti can be contained at 0.002 to 0.004 wt%.

[0029] The grain-oriented electrical steel sheet according to an embodiment of the present invention can satisfy the following formula 1. [Formula 1] 10×([Ti]+[Ca]+[Mg])≧[Al] (In formula 1, [Ti], [Ca], [Mg] and [Al] represent the contents (wt%) of Ti, Ca, Mg and Al, respectively.)

[0030] When Ca and Mg combine with S to form fine sulfides, they can act as inhibitors in secondary recrystallization. Ti also combines very easily with many impurities in steel, such as O, C, N, and S, and acts as an inhibitor. To act as an inhibitor, a sufficient amount must be present, of an appropriate size, and with little deviation in distribution. Another inhibitor, Al, mainly combines with nitrogen to form AlN, and plays a role in inhibiting recrystallization growth. AlN smoothly causes secondary recrystallization, but in order for secondary recrystallization to occur in the Cube orientation, not the Goss orientation, it is necessary to slow down the crystal growth rate by decomposing the inhibitor. Abnormal grain growth during secondary recrystallization is explosive grain growth, so it is very difficult to suppress it, and this requires the use of inhibitors other than AlN. Therefore, the amount of inhibitors such as Ti, Ca, and Mg must be present in the steel in sufficient amounts to satisfy the above-mentioned formula 1. More specifically, it is preferable that the total amount of Ca, Mg, and Ti is 5 times or more the amount of Al in the steel. In other words, it is preferable that 5 × ([Ti] + [Ca] + [Mg]) ≥ [Al].

[0031] The grain-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of Sn: 0.1 wt % or less, Sb: 0.001 to 0.1 wt %, and Mo: 0.01 to 0.2 wt %. Sn: 0.10% by weight or less Tin (Sn) reduces the stability of the Goss orientation during rolling, decreasing the post-rolling fraction of Goss and increasing the fraction of Cube orientation. Sn also increases Goss during recrystallization. Therefore, in order to remove the Goss orientation with an appropriate rolling reduction and keep the Goss fraction low even after recrystallization, the amount of Sn added must be 0.1 wt% or less.

[0032] Sn has the effect of slowing down the recrystallization rate and suppressing the crystal growth during recrystallization, and is effective in matching the growth rate of the grain boundaries, which grow rapidly at the grain boundaries, with the growth rate of the crystal grains, which grow by recrystallization within the grains, so the amount of Sn added can be adjusted. More specifically, Sn can be contained in an amount of 0.001 to 0.1% by weight. More specifically, Sn can be contained in an amount of 0.01 to 0.05% by weight.

[0033] Sb:0.0010~0.1000wt%, Mo:0.0100~0.2000wt% Antimony (Sb) is an element that can be added to control the primary recrystallization texture. When added in an amount of 0.001 wt% or more, it is an element that changes the thickness of the oxide layer formed and reduces the magnetic difference between the rolling direction and the rolling direction, but when added in an amount exceeding 0.1 wt%, the slip on the rolls increases significantly during cold rolling, so this is limited. More specifically, Sb: 0.005 to 0.05 wt% is suitable. Mo is an element that helps the high-temperature phase stability of carbides and nitrides in steel when added, and can help increase the secondary recrystallization temperature and make precipitates finer during continuous casting and hot-rolled sheet annealing. Therefore, its addition amount is limited to 0.01 to 0.2 wt%. More specifically, Mo can be contained in an amount of 0.02 to 0.05% by weight.

[0034] As described above, when an additional element is contained, it is contained in place of the balance Fe. For example, a grain-oriented electrical steel sheet further containing 0.001 to 0.1 weight % Sb has a composition, in weight %, of Si: 2.0 to 4.0%, Al: 0.01 to 0.04%, S: 0.0004 to 0.002%, Mn: 0.05 to 0.3%, N: 0.005% or less (excluding 0%), C: 0.005% or less (excluding 0%), P: 0.005 to 0.15%, Ca: 0.0001 to 0.005%, Mg: 0.0001 to 0.005%, and Sb: 0.001 to 0.1%, with the balance being Fe and other unavoidable impurities.

[0035] The grain-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of Bi: 0.0100 wt % or less, Pb: 0.0100 wt % or less, As: 0.0100 wt % or less, Be: 0.0100 wt % or less, and Sr: 0.0100 wt % or less. Bismuth (Bi), lead (Pb), arsenic (As), beryllium (Be) and strontium (Sr) are elements that form fine oxides, nitrides and carbides in steel and are useful for secondary recrystallization, so they can be added. However, adding more than 0.01% by weight can cause problems with the formation of secondary recrystallization becoming unstable, so the amount added must be limited. The balance of the grain-oriented electrical steel sheet of the present invention other than the above-mentioned components is Fe and unavoidable impurities, however, this does not exclude the inclusion of other elements as long as they do not impair the effects of the present invention.

[0036] In this way, the grain-oriented electrical steel sheet according to one embodiment of the present invention precisely controls the alloy composition to form a large number of cube textures. <001> The area fraction of crystal grains having an orientation within 15° from the surface may be 60 to 99%. In this case, exceeding 99% means suppressing the formation of island grains that are inevitably formed during secondary recrystallization and completely removing precipitates, but this requires a large increase in the annealing time at high temperature, so this is limited to 60 to 99%. More specifically, it may be 70 to 97%. Even more specifically, it may be 80 to 95%.

[0037] Also, <025> For grains with orientation, {100} <001> The orientation is rotated by about 22.5° from the {100} direction. By increasing this orientation, the bidirectional property of the steel sheet decreases and the properties in the circumferential direction become uniform. Therefore, in order to ensure the bidirectional property, the area fraction of crystal grains having the above orientation may be within 30%. On the other hand, the above orientation has a {100} plane parallel to the steel sheet surface, which has little adverse effect on magnetic properties, and the {100} <001> Since it is rotated 22.5° from the <001> The grains with orientations within 15° of {100} <025> The area fraction is considered to be within 15° of the grains, and cannot be 0%. When assuming a Gaussian distribution of 15°, the minimum value can include 1% or more. More specifically, it can be 3 to 20%. More specifically, it can be 5 to 15%. {100} <001> and {100} <025> The amount of non-crystalline grains may be less than 10%. The grain oriented electrical steel sheet according to an embodiment of the present invention may have an average grain size of 20 times or more the thickness of the steel sheet. In an embodiment of the present invention, secondary recrystallization is used, and it is advantageous for the grain size of the secondary recrystallization to be more than 20 times the thickness of the sheet in order to obtain a desired orientation. The grain size can be measured based on a plane parallel to the rolled surface (ND surface) of the steel sheet. The grain size means the diameter of an imaginary circle having the same area as the grain.

[0038] FIG. 1 is a schematic diagram of a cross section of a grain-oriented electrical steel sheet 100 according to an embodiment of the present invention. 1, the steel plate may include an oxide layer 11 formed from the surface of the steel plate substrate 10 toward the inside of the substrate 10, and an insulating layer 30 formed on the surface of the steel plate. In this case, the surface of the steel plate substrate 10 may refer to one or both sides (upper and lower sides) of the steel plate. The oxide layer 11 is formed by the penetration of oxygen into the inside of the base material. Specifically, in addition to the above-mentioned composition of the steel sheet, oxygen (O) can be contained in an amount of 10% by weight or more. The base material 10 and the oxide layer 11 can be distinguished from each other in terms of the oxygen content. The oxide layer 11 can be present to a thickness of 5 μm or less. If the oxide layer 11 is present too thick, the oxygen fraction in the steel inhibits the growth of cube crystal grains, lowering the cube fraction and ultimately deteriorating the magnetic properties. More specifically, the thickness of the oxide layer 11 may be 0.01 to 2.5 μm. An insulating layer 30 is formed on the surface of the substrate 10. The insulating layer 30 helps to ensure insulation. The insulating layer 30 is formed from an organic or inorganic coating composition, and in some cases, from an organic-inorganic composite coating composition. The insulating layer 30 may have a thickness of 0.2 to 8 μm. If the thickness is too thin, it is difficult to achieve the required insulating properties. If the thickness is too thick, magnetization is not easily performed because it is difficult for magnetic domains to move during surface magnetization, and ultimately magnetism may deteriorate. If the insulating layer 30 is formed on both sides of the substrate 10, each of the insulating layers 30 formed on both sides can satisfy the above-mentioned thickness range. More specifically, the insulating layer 30 may have a thickness of 0.4 to 5 μm.

[0039] FIG. 2 shows a schematic diagram of a cross section of a bi-directional electrical steel sheet 100 according to another embodiment of the present invention. As shown in FIG. 2, in one embodiment of the present invention, a forsterite layer 20 interposed between the surface of the substrate 10 and the insulating layer 30 may be further included. In order to apply tension in the rolling direction, the grain-oriented electrical steel sheet forms an oxide layer containing forsterite (Mg2SiO4) to a thickness of 2 to 3 μm from the surface, and applies tension by utilizing the difference between the thermal expansion coefficient of this layer and that of the base material. However, in the case of one embodiment of the present invention, the tension in the rolling direction means compression in the direction perpendicular to the rolling direction, and it is preferable to reduce this extremely. Since a thin forsterite layer 20 of 2.0 μm or less has a significantly reduced tension application effect, it is possible to remove the tension applied to the entire sheet by forming such a thin forsterite layer 20. The forsterite layer 20 is formed from an annealing separator applied before the secondary recrystallization annealing. The annealing separator contains MgO as a main component, which is widely known, and therefore a detailed description will be omitted. After the second recrystallization anneal, the forsterite layer 20 can be removed, resulting in the formation of an insulating layer 30 abutting the surface of the substrate 10, as shown in FIG.

[0040] The bi-directional electrical steel sheet according to an embodiment of the present invention has excellent magnetic properties in both the rolling direction and the direction perpendicular to the rolling direction. Specifically, the Br in both the rolling direction and the direction perpendicular to the rolling direction is 1.65T or more, and the Br in the circumferential direction is 1.58T or more, and Br is calculated by the following formula 2. [Formula 2] Br=7.87 / (7.87-0.065×[Si]-0.1105×[Al])×B8 (In formula 2, [Si] and [Al] indicate the contents (wt%) of Si and Al, respectively. B8 indicates the strength (Tesla) of the induced magnetic field when induced at 800 A / m.) In the case of large generators, the diameter of the ring frame is several meters, and the ring frame is formed by cutting the magnetic steel sheet with T-shaped teeth. In this case, the T-shaped teeth part can be in the rolling direction vertical and the rolling direction can be placed on the ring frame, or conversely, the T-shaped teeth part can be in the rolling direction and the rolling direction can be placed on the ring frame vertical. Such design changes are determined by the length of the teeth, the diameter of the ring frame, and the width of the ring frame. Usually, the teeth part is a part where a large magnetic flux flows when the generator is in operation, and this magnetic flux escapes to the ring part. In consideration of the energy generated at this time, it is decided whether the rolling direction and the rolling vertical direction are the teeth part or the ring part. However, in the case of materials with very high magnetic flux density such as Br of 1.63 T or more, there is no need to distinguish which part is used for the rolling direction and which part is used for the rolling vertical direction, and in either case, it has very high energy efficiency. In addition, when the circumferential magnetic flux density Br is increased to 1.56T or more, the energy loss due to magnetic flux at the connection between the Teeth part of the T-shape and the ring frame is significantly reduced. This improves the efficiency of the generator, and by reducing the width of the ring frame and the size of the Teeth part, a highly efficient generator can be created even with a small core size.

[0041] A method for producing a grain-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of producing a slab containing, by weight, 2.0-4.0% Si, 0.01-0.04% Al, 0.0004-0.02% S, 0.05-0.3% Mn, 0.02% or less (excluding 0%), 0.05% or less C (excluding 0%), 0.005-0.15% P, 0.001-0.005% Ti, 0.0001-0.005% Ca, 0.0001-0.005% Mg, and the balance being Fe and other unavoidable impurities, hot rolling the slab to produce a hot-rolled sheet, rolling the hot-rolled sheet to produce a steel sheet, subjecting the steel sheet to primary recrystallization annealing, and subjecting the steel sheet that has been subjected to primary recrystallization annealing to secondary recrystallization annealing. Each step will be explained in detail below.

[0042] First, a slab is manufactured. The reason for limiting the addition ratio of each component in the slab is the same as the reason for limiting the composition of the grain-oriented electrical steel sheet described above, so a repeated explanation will be omitted. The composition of the slab other than C and N does not substantially change during the manufacturing process such as hot rolling, hot-rolled sheet annealing, cold rolling, primary recrystallization annealing, and secondary recrystallization annealing described below, so the composition of the slab other than C and N is substantially the same as the composition of the grain-oriented electrical steel sheet. The slabs can be produced using thin slab or strip casting techniques. The thickness of the slabs may be 200-300mm. The slabs can be heated as required.

[0043] The slab is then hot rolled to produce a hot rolled sheet. The total reduction in the step of producing the hot rolled sheet is 95% or more, and the step of producing the hot rolled sheet includes a plurality of passes, with each pass having a reduction of 50% or less. As described above, only by controlling the reduction rate can the size distribution of the microstructure and the distribution of precipitates be controlled, and the relationship between each crystal grain and its neighboring crystal grains in an appropriate size distribution can be controlled so that a target texture can be obtained when recrystallization occurs after rolling. The reduction ratio is calculated as follows: ([Thickness of steel plate before reduction] - [Thickness of steel plate after reduction]) / [Thickness of steel plate before reduction]. For example, the total reduction ratio at the stage of manufacturing hot-rolled plate is calculated as ([Thickness of slab] - [Thickness of hot-rolled plate]) / [Thickness of hot-rolled plate]. The step of producing the hot-rolled sheet may include a plurality of passes, with the reduction in each pass being 50% or less. In this case, a pass means rolling with one rolling mill. Specifically, the step of producing the hot-rolled sheet may include 3 to 12 passes. As described above, the reduction in each pass in the step of producing the hot-rolled sheet may be 50% or less. More specifically, the total rolling reduction in the stage of producing the hot rolled sheet may be 97.0% to 99.9%, and the rolling reduction in each pass may be 30% to 50%.

[0044] The process for producing a hot-rolled sheet includes a step of rough rolling a slab, a step of heating the rough-rolled bar, and a step of finish rolling the heated bar. In the heating step, the temperature can be maintained at 1050°C or higher for 10 to 300 minutes. If the maintenance time is too short, the precipitates in the slab cannot be properly arranged to achieve a required level of precipitate distribution in the hot-rolled sheet, and a uniform microstructure cannot be obtained for the subsequent process. On the other hand, if the maintenance time is too long, the precipitates become very coarse, and the amount of C in the slab can decrease as it reacts with oxygen during reheating of the slab. The hot rolling end temperature may be 1050℃ or less. When the hot rolling end temperature is high, more shear deformation is applied during hot rolling, but the recrystallization and crystal growth rate is fast, so more crystal grains with recrystallized cube orientation can be secured. This allows the cube fraction to increase during annealing of the hot rolled sheet.

[0045] The thickness of the hot rolled sheet may be 1 to 3.5 mm. The step of producing the hot rolled sheet may be carried out at a temperature of 700° C. or more. After the step of producing the hot-rolled sheet, the method may further include a step of annealing the hot-rolled sheet. The annealing temperature in the step of annealing the hot-rolled sheet may be 1000 to 1200°C. Next, the hot-rolled sheet is rolled to produce a steel sheet.

[0046] The step of manufacturing the steel sheet may include a step of first rolling the hot-rolled sheet, a step of intermediate annealing, and a step of second rolling the intermediate-annealed steel sheet. In the first rolling step, the hot rolled sheet is cold or warm rolled to a thickness of 0.5 to 1.8 mm. In the first rolling step, the rolling reduction may be 75% or less. The first rolling step may include a plurality of passes, with the rolling reduction in each pass being 45% or less. If the rolling reduction is excessively large, the Goss fraction increases after recrystallization. Specifically, the first rolling step may include 2 to 8 passes. More specifically, in the first rolling stage, the reduction may be 60 to 75%, and in each pass, the reduction may be 35 to 45%.

[0047] The intermediate annealing step can be performed at 1000 to 1200°C. In the second rolling step, the steel sheet after the first rolling may be cold or warm rolled to a thickness of 0.15 to 0.65 mm. In the second rolling step, the rolling reduction may be 75% or less. In addition, the second rolling step may include a plurality of passes, with the rolling reduction in each pass being 45% or less. If the rolling reduction is excessively large, the Goss fraction increases after recrystallization. Specifically, the second rolling step may include 1 to 6 passes. More specifically, in the second rolling stage, the reduction may be 60 to 75%, and the reduction in each pass may be 35 to 45%. The first rolling step and the second rolling step may be performed at a temperature of 50°C or more and less than 700°C.

[0048] The first recrystallization annealing step may include a step of decarburization at a dew point temperature of 50 to 70°C. If a large amount of carbon remains even after the second recrystallization annealing, it may cause magnetic aging and greatly increase core loss, so in the first recrystallization annealing step, carbon may be partially removed through decarburization. This is carried out at a dew point temperature of 50 to 70°C in a mixed atmosphere of hydrogen and nitrogen. In the step of the primary recrystallization annealing, the amount of nitride may be 0.01 to 0.03 wt %. If the amount of nitride is not adequately ensured, the secondary recrystallization may not be smoothly formed, which may cause a problem of deterioration of magnetic properties. The decarburization and nitridation may be carried out simultaneously or sequentially, in which case the decarburization may be followed by nitridation or the nitridation may be followed by decarburization. After the step of performing the primary recrystallization annealing, the average grain size of the steel sheet that has been subjected to the primary recrystallization annealing may be 30 to 50 μm. If the average grain size of the steel sheet that has been subjected to the primary recrystallization annealing is not appropriately ensured, the secondary recrystallization may not be smoothly formed, which may cause a problem of deterioration in magnetic properties. The primary recrystallization annealing is carried out in the temperature range of 800 to 900°C. After the first recrystallization annealing step, the method may further include applying an annealing separator containing MgO. The forsterite layer formed by application of the annealing separator is the same as that described above, and therefore a duplicated description will be omitted.

[0049] The secondary recrystallization annealing is performed by heating the steel at an appropriate heating rate to {100} <001> The secondary recrystallization of the cube orientation occurs, and the subsequent purification annealing, which is a process for removing impurities, is then performed before cooling. In this process, the annealing atmosphere gas is a mixture of hydrogen and nitrogen gas during the heating process, as in the normal case, and 100% hydrogen gas is used for a long period of time during purification annealing to remove impurities. The temperature of the secondary recrystallization annealing may be 1000 to 1300°C, and the time may be 10 to 25 hours. In one embodiment of the present invention, as described above, it may be advantageous for the forsterite layer to be thin or removed. Therefore, the method may further include removing the forsterite layer formed on the surface of the steel sheet after the secondary recrystallization annealing. The removal method may be a physical or chemical method.

[0050] Preferred examples and comparative examples of the present invention will be described below. However, the following examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples.

[0051] [Experimental Example 1] A slab consisting of the components shown in Tables 1 and 2 and the balance being Fe and unavoidable impurities was produced, heated at 1200°C, and hot-rolled in eight passes to produce a hot-rolled coil with a thickness of 2.3 mm. The hot-rolled sheet was annealed at 1050°C to 1140°C for 30 seconds, annealed at 930°C for 90 seconds, and then quenched. The hot-rolled annealed sheet was first rolled at 200°C in three passes to a thickness of 1.3 mm. The reduction ratio at this time was 40%. This was again annealed at 1050°C to 1140°C for 30 seconds, annealed at 930°C for 90 seconds, and then quenched. The annealed sheet was secondarily rolled at 200°C in four passes to the thickness shown in Table 4. The rolled sheet was nitrided by the mass shown in Table 3 by weight %, and at the same time, the dew point was decarburized in a 75% hydrogen atmosphere by volume, as shown in Table 3, by a primary recrystallization annealing process. The grain size was then measured and shown in Table 3. Thereafter, the sheet was heated to 1200°C at a heating rate of 20°C per hour with or without an annealing separator containing MgO, and then secondary recrystallization annealing was performed for 20 hours. The cooled sheet was measured for magnetic properties with or without removing the forsterite layer after removing the MgO annealing separator, and the results are shown in Table 3. Table 3 shows the reduction ratios in hot rolling (rolling at 700°C or higher) and the primary / secondary cold / warm rolling (rolling at less than 700°C) and the reduction ratios of the passes with the largest reduction ratios. The reduction ratios in the first / second cold / warm rolling (rolling at less than 700°C) represent the cases where the reduction ratios are large in the first and second rolling, which are separated based on intermediate annealing. Table 4 shows the fraction of the cube ({100} <001> The area fraction of oriented crystal grains and the Br value were measured and summarized.

[0052] [Table 1] TIFF0007583815000002.tif78168

[0053] [Table 2] TIFF0007583815000004.tif60163

[0054] [Table 3] TIFF0007583815000006.tif52154

[0055] [Table 4] TIFF0007583815000008.tif52161

[0056] As shown in Tables 1 to 4, the inventive examples, which satisfy the alloy composition of the present invention and have an appropriately adjusted rolling reduction, have a large average crystal grain size, a high cube fraction, and excellent magnetic properties. In contrast, the comparative examples, which do not satisfy the alloy composition of the present invention or do not have an appropriately adjusted rolling reduction, have a small average crystal grain size, a low cube fraction, and poor magnetic properties.

[0057] The present invention is not limited to the above-mentioned embodiments, and can be manufactured in various different forms, and a person skilled in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-mentioned embodiments are illustrative in all respects and not limiting. [Explanation of symbols]

[0058] 10: Steel plate base material 11: Oxide layer 20: Forsterite layer 30: Insulating layer 100: Bidirectional electrical steel sheet

Claims

1. A bi-directional electrical steel sheet, the alloy comprises, by weight, 2.0-4.0% Si, 0.01-0.04% Al, 0.0004-0.02% S, 0.05-0.3% Mn, 0.01% or less (excluding 0%) N, 0.005% or less (excluding 0%) C, 0.005-0.15% P, 0.001-0.005% Ti, 0.0001-0.005% Ca, and 0.0001-0.005% Mg, with the balance being Fe and other unavoidable impurities; the area fraction of crystal grains having an orientation within 15° of {100}<001> is 60-99% and the area fraction of crystal grains having an orientation within 15° of {100}<025> is 1-30%, The following formula 1 is satisfied: A bi-directional electrical steel sheet, characterized in that the average crystal grain size is 20 times or more the thickness of the steel sheet. [Formula 1] 10×([Ti]+[Ca]+[Mg])≧[Al] (In formula 1, [Ti], [Ca], [Mg] and [Al] represent the contents (wt%) of Ti, Ca, Mg and Al, respectively.)

2. 2. The bi-directional electrical steel sheet according to claim 1, further comprising one or more of Sn: 0.1 wt % or less, Sb: 0.001 to 0.1 wt %, and Mo: 0.01 to 0.2 wt %.

3. 3. The bidirectional electrical steel sheet according to claim 1, further comprising one or more of Bi: 0.01 wt % or less, Pb: 0.01 wt % or less, As: 0.01 wt % or less, Be: 0.01 wt % or less, and Sr: 0.01 wt % or less.

4. 4. The bidirectional electrical steel sheet according to claim 1 , further comprising an oxide layer formed from a surface of a substrate of the steel sheet toward the inside of the substrate, and an insulating layer formed on the surface of the substrate.

5. The bidirectional electrical steel sheet according to claim 4, wherein a surface of the substrate and the insulating layer are in contact with each other.

6. The bi-directional electrical steel sheet according to claim 4 , further comprising a forsterite layer interposed between the surface of the substrate and the insulating layer.

7. 7. The bidirectional electrical steel sheet according to claim 1 , wherein Br in the rolling direction and the direction perpendicular to the rolling direction are all 1.65 T or more, Br in the circumferential direction is 1.58 T or more, and Br is calculated by the following formula 2: [Formula 2] Br=7.87 / (7.87-0.065×[Si]-0.1105×[Al])×B8 (In formula 2, [Si] and [Al] represent the contents (wt%) of Si and Al, respectively. B8 represents the strength (Tesla) of the induced magnetic field when induced at 800 A / m.)

8. a step of producing a slab containing, by weight percent, 2.0-4.0% Si, 0.01-0.04% Al, 0.0004-0.02% S, 0.05-0.3% Mn, 0.02% or less (excluding 0%) N, 0.05% or less (excluding 0%) C, 0.005-0.15% P, 0.001-0.005% Ti, 0.0001-0.005% Ca, and 0.0001-0.005% Mg, with the balance being Fe and other unavoidable impurities, and satisfying the following formula 1; hot rolling the slab to produce a hot rolled sheet; rolling the hot-rolled sheet to produce a steel sheet; subjecting the steel sheet to a first recrystallization annealing; and The steel sheet subjected to the first recrystallization annealing is subjected to a second recrystallization annealing, The total rolling reduction in the step of producing the hot rolled sheet is 95% or more, The step of producing the hot-rolled sheet includes a plurality of passes, each of which has a rolling reduction of 50% or less; The produced bidirectional electrical steel sheet has an area fraction of crystal grains having an orientation within 15° of {100}<001> of 60 to 99%, and an area fraction of crystal grains having an orientation within 15° of {100}<025> of 1 to 30%, A method for producing a bi-directional electrical steel sheet, characterized in that the average crystal grain size is 20 times or more the thickness of the steel sheet. [Formula 1] 10×([Ti]+[Ca]+[Mg])≧[Al] (In formula 1, [Ti], [Ca], [Mg] and [Al] represent the contents (wt%) of Ti, Ca, Mg and Al, respectively.)

9. The method for producing a bi-directional electrical steel sheet according to claim 8, wherein the slab satisfies the following formula 3: [Formula 3] [C] / [Si]≧0.0067 (In formula 3, [C] and [Si] represent the C and Si contents (wt%) in the slab, respectively.)

10. The method of claim 8 or 9, wherein the step of producing the hot-rolled sheet is performed at a temperature of 700° C. or more.

11. 11. The method for producing a bi-directional electrical steel sheet according to claim 8, wherein the step of producing the steel sheet includes the steps of: first rolling a hot-rolled sheet; intermediate annealing; and second rolling the intermediate annealed steel sheet.

12. The method of claim 11, wherein the reduction ratio in each of the first rolling and the second rolling is 75% or less.

13. The method for producing a bi-directional electrical steel sheet according to claim 11 or 12, wherein the first rolling and the second rolling include a plurality of passes, and the reduction in each pass is 45% or less.

14. The method of claim 11, wherein the first rolling and the second rolling are performed at a temperature of 50°C or more and less than 700°C.

15. The method for producing a grain-oriented electrical steel sheet according to any one of claims 8 to 14, wherein the step of performing the primary recrystallization annealing includes a step of decarburizing at a dew point temperature of 50 to 70°C.

16. The method for producing a grain-oriented electrical steel sheet according to any one of claims 8 to 15, characterized in that the primary recrystallization annealing step includes a nitriding step, and the amount of nitriding is 0.01 to 0.03 wt%.

17. The method for manufacturing a bi-directional electrical steel sheet according to any one of claims 8 to 16, wherein after the primary recrystallization annealing, the steel sheet that has been subjected to the primary recrystallization annealing has an average grain size of 30 to 50 μm.

18. The method of claim 8 , further comprising the step of applying an annealing separator after the primary recrystallization annealing. 19 . The method of claim 8 , further comprising the step of applying an annealing separator after the primary recrystallization annealing.

19. The method of claim 18, further comprising removing a forsterite layer formed on the surface of the steel sheet after the secondary recrystallization annealing.

Citation Information

Patent Citations

  • Method for producing bi-directional silicon steel sheet

    JP2005179745A

  • Method for manufacturing electromagnetic steel sheet

    JP2007031793A

  • Method for producing double oriented silicon steel sheet

    JP2007262519A

  • Double oriented silicon steel sheet

    JP2008106367A

  • Grain-oriented electrical steel sheet and its manufacturing method

    JP2019506528A