Liquid quick-setting agent, sprayed concrete composition, sprayed concrete, and spraying method

The liquid quick-setting agent with controlled aluminum, sulfur, sodium, and pH, along with polyethylene oxide, addresses insoluble precipitate issues, ensuring stable and effective shotcrete performance.

JP7583826B2Active Publication Date: 2024-11-14DENKA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022558870
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-30
Filing Date
2021-08-17
Publication Date
2024-11-14
Estimated Expiration
2041-08-17

AI Technical Summary

Technical Problem

Liquid quick-setting agents often generate insoluble precipitates, particularly natroalunite, which inhibit rapid setting and decrease workability, and are difficult to handle due to their alkalinity.

Method used

A liquid quick-setting agent with specific compositions and conditions to minimize natroalunite precipitation, including controlled amounts of aluminum, sulfur, sodium, and pH, along with polyethylene oxide, to ensure good workability and stability.

Benefits of technology

Prevents quick-setting inhibition by natroalunite precipitation, enhancing workability and allowing for effective use in shotcrete applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583826000001
    Figure 0007583826000001
Patent Text Reader

Abstract

Provided are: a liquid quick-setting agent that can prevent the inhibition of quick-setting of a quick-setting agent due to the precipitation of natroalunite, and exhibit good workability; a sprayed concrete composition; a sprayed concrete; and a spraying construction method. The liquid quick-setting agent is mixed with a sprayed concrete composition that includes: a polyethylene oxide having a mass average molecular weight of 100,000-300,000; and a cement concrete. The liquid quick-setting agent contains aluminum, sulfur, and sodium, wherein the content of natroalunite is 0.3-3 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid quick-setting admixture, a shotcrete composition, a shotcrete, and a shotcrete application method. [Background technology]

[0002] Conventionally, it has been known that silicates, aluminates, chlorides, etc. are effective for reducing rebound of shotcrete, filling voids underground or behind tunnels, and instantly eliminating fluidity and preventing leakage in places where water is present or cracks are present, etc. However, most of these are highly alkaline liquid quick-setting additives, which pose problems in terms of handling and practical operation.

[0003] As a result, various non-alkaline liquid quick-setting admixtures have been investigated. For example, Patent Document 1 proposes a cement quick-setting admixture containing a soluble aluminum salt and a fluoride, which exhibits good quick-setting properties and strength development and allows for sufficient construction. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-261393 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, liquid quick-setting admixtures generally produce precipitates depending on the storage temperature. Among these precipitates, insoluble precipitates (insoluble precipitates) cannot be redissolved, so if they are added directly to concrete, the quick-setting admixture's effectiveness is reduced, which can cause problems during construction. In Patent Document 1, too, after a certain period of storage, the above-mentioned insoluble precipitates (insoluble precipitates) may occur, and these precipitates need to be removed before application, which is one of the factors that reduces workability.

[0006] In light of these problems, the present inventors conducted various investigations and studies on the above-mentioned insoluble precipitates, and first discovered that the insoluble precipitates were natroalunite (sodium alum).Then, they newly discovered that the precipitated natroalunite inhibits the quick-setting of the accelerator, thereby reducing the workability when the accelerator is used.

[0007] In view of the above, the present invention aims to provide a liquid quick-setting admixture, a sprayed concrete composition, a sprayed concrete, and a spraying method that can prevent inhibition of quick-setting of the quick-setting admixture due to precipitation of sodium alunite and exhibit good workability. Another object of the present invention is to reduce the dust of the sprayed concrete from the viewpoint of the working environment. [Means for solving the problem]

[0008] As a result of various investigations to solve the above problems, the present inventors have found that the problem can be solved by controlling the amount of sodium alunite precipitated in a liquid quick-setting admixture having a specific composition to a predetermined value or less. That is, the present invention is as follows.

[0009] [1] A liquid quick-setting admixture to be mixed with a sprayed concrete composition containing cement concrete and polyethylene oxide having a mass average molecular weight of 100,000 to 3,000,000, the liquid quick-setting admixture containing aluminum, sulfur, and sodium and having a sodium alunite content of 0.3 to 3 mass%. [2] The liquid quick-setting admixture according to [1], wherein the content of the natroalunite is 0.3 to 3 mass % after storage at 0 to 40° C. for 48 hours immediately after preparation. [3] The liquid quick-setting admixture according to [1] or [2], wherein the sodium alunite is derived from cryolite and / or sodium sulfate. [4] The liquid quick-setting admixture according to any one of [1] to [3], which has a pH of 1 to 4. [5] The liquid quick-setting admixture according to any one of [1] to [4], wherein the aluminum is 1 to 20 parts by mass in terms of Al2O3, the sulfur is 10 to 30 parts by mass in terms of SO3, and the sodium is 0.1 to 3 parts by mass in terms of Na2O. [6] The liquid quick-setting admixture according to any one of [1] to [5], having a solids concentration of 20 to 50 mass %. [7] The liquid quick-setting admixture according to any one of [1] to [6], which has a viscosity at 20°C of 1,000 mPa s or less. [8] The liquid quick-setting admixture according to any one of [1] to [7], wherein the mass ratio of aluminum in terms of Al2O3 to sulfur in terms of SO3 (Al2O3 / SO3) is 0.3 to 0.7. [9] A sprayed concrete composition comprising the liquid quick-setting admixture according to any one of [1] to [8], cement concrete, and polyethylene oxide having a mass average molecular weight of 100,000 to 3,000,000.

[10] A sprayed concrete composition as described in [9], in which the cement concrete and the polyethylene oxide are mixed in advance.

[11] A sprayed concrete composition according to [9] or

[10] , which is obtained by mixing the liquid quick-setting admixture with the cement concrete containing the polyethylene oxide.

[12] A sprayed concrete obtained by spraying the sprayed concrete composition according to any one of [9] to

[11] .

[13] A spraying method, comprising spraying the sprayed concrete composition according to any one of [9] to

[11] . Effect of the Invention

[0010] According to the present invention, it is possible to provide a liquid quick-setting admixture, a sprayed concrete composition, a sprayed concrete, and a spraying method which are capable of preventing inhibition of quick-setting of the quick-setting admixture due to precipitation of sodium alunite and exhibiting good workability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited to the embodiment. In this specification, "parts" and "%" are based on mass unless otherwise specified.

[0012] [Sprayed concrete composition and sprayed concrete] The shotcrete composition according to an embodiment (present embodiment) of the present invention and the shotcrete obtained by hardening the composition contain a liquid quick-setting admixture, cement concrete, and polyethylene oxide. Hereinafter, embodiments of the sprayed concrete composition, the liquid quick-setting admixture used in the sprayed concrete, the cement concrete, and the polyethylene oxide of the present invention will be described.

[0013] [Liquid quick-setting agent] The liquid quick-setting admixture according to the present embodiment contains aluminum, sulfur, and sodium. By containing these, quick-setting properties and strength development can be improved.

[0014] Moreover, the liquid quick-setting admixture according to this embodiment has a natroalunite content of 0.3 to 3 mass%. If the natroalunite content exceeds 3 mass%, the quick-setting properties that the liquid quick-setting admixture can exhibit in the sprayed concrete are inhibited, and this makes it difficult to exhibit good workability. The natroalunite content is preferably 2.5 mass% or less, and more preferably 2 mass% or less. Although it is preferable that natroalunite is absent, since it is produced by thermal hydrolysis, in practice it may be present at about 0.3 mass%.

[0015] It is preferable that the natroalunite content is 3 mass% or less at least after storing the liquid quick-setting admixture at 0 to 40°C for 48 hours immediately after preparation. If the natroalunite content is 3 mass% or less at this point, inhibition of rapid hardening by natroalunite is suppressed during subsequent storage at 0 to 40°C. Note that "0 to 40°C" is the assumed temperature range during actual use of the liquid quick-setting admixture. The natroalunite content can be measured by the method described in the Examples.

[0016] Here, natroalunaite is also called sodalite, and is (NaAl3(SO4)2(OH)6, (Na,K)Al3(SO4)2(OH)6, or [Na + ][Al 3+ ][Al 3+ 2][(OH)6|(SO4)2] 10- According to the present inventors, natroalunite is mainly derived from the raw material cryolite, and in particular, thiolite (Na5Al3F 14 ) and elpasolite (K2NaAlF6). Natroalunite is mainly derived from the raw material sodium sulfate, and since more sodium sulfate precipitates in the liquid quick-setting admixture as the content increases, the amount of sodium sulfate is preferably 0.5 parts by mass or more and less than 7 parts by mass, and more preferably 1 part by mass or more and less than 6 parts by mass. Therefore, in order to make the content of natroalunite in the liquid quick-setting admixture 3% by mass or less, it is sufficient to carry out a treatment such as reducing the amount of thiolite and elpasolite in the cryolite. In addition, the temperature conditions when preparing the liquid quick-setting admixture may be adjusted as described later.

[0017] The liquid quick-setting admixture according to the present embodiment is preferably acidic, and more preferably has a pH of 1 to 4. When the liquid quick-setting admixture is acidic, it is easier to handle than an alkaline hardening accelerator.

[0018] The contents of aluminum, sulfur, and sodium in the liquid quick-setting admixture are not particularly limited, and from the viewpoint of rapid hardening, it is preferable that aluminum is 1 to 20 parts by mass in terms of Al2O3, sulfur is 10 to 30 parts by mass in terms of SO3, and sodium is 0.1 to 3 parts by mass in terms of Na2O. It is more preferable that aluminum is 5 to 10 parts by mass in terms of Al2O3. It is more preferable that sulfur is 12 to 25 parts by mass in terms of SO3. It is more preferable that sodium is 0.1 to 2 parts by mass in terms of Na2O.

[0019] Furthermore, from the viewpoint of the storage stability of the liquid quick-setting admixture and the mixability when added to paste, mortar, or concrete, the mass ratio of aluminum in Al2O3 conversion to sulfur in SO3 conversion (Al2O3 / SO3) is preferably 0.3 to 0.7, and more preferably 0.4 to 0.6.

[0020] The solids concentration of the liquid quick-setting admixture according to this embodiment is preferably 20 to 50 mass %, and more preferably 25 to 45 mass %, from the viewpoints of the storage stability of the liquid quick-setting admixture and the mixability when added to paste, mortar, or concrete.

[0021] The liquid quick-setting admixture according to this embodiment preferably has a viscosity of 1,000 mPa·s or less at 20°C, more preferably 1 to 900 mPa·s. A viscosity of 1,000 mPa·s or less improves mixability and provides stable physical properties. The viscosity can be measured by the method described in the examples.

[0022] The liquid quick-setting admixture according to the present embodiment can be prepared by mixing raw materials such as aluminum sulfate, various alums, aluminum hydroxide, sodium hydroxide, sulfuric acid, natural or synthetic cryolite, sodium fluoride, and aluminum fluoride in a liquid, and heating at 80 to 95° C. for 30 to 120 minutes. From the viewpoint of good productivity, it is preferable to use sulfuric acid, aluminum hydroxide, aluminum sulfate, or various alums, and natural or synthetic cryolite as the raw materials. In addition, it is preferable to use water or the like as the liquid.

[0023] Here, when cryolite is used as a raw material for preparing the liquid quick-setting admixture according to the present embodiment, insoluble precipitates are likely to occur. In particular, it is presumed that thiolite and elpasolite contained in cryolite contribute to the generation of insoluble precipitates. It has also been found that the generation of insoluble precipitates can be suppressed by carrying out a specific operation when preparing the hardening accelerator. Taking into consideration any of these factors, it is preferable to carry out, for example, the following operation (1) or (2) in order to make the content of natroalunite in the liquid quick-setting admixture 0.3 to 3 mass%.

[0024] (1) When using cryolite as the raw material, the cryolite to be used must contain 3 mass% or less of thiolite and elpasolite. (2) After heating at 80 to 95°C as described above, the mixture is rapidly cooled to room temperature (e.g., 25°C) within 60 minutes.

[0025] The liquid quick-setting admixture prepared in the manner described above is suitable for use in a sprayed concrete composition and sprayed concrete, as described below.

[0026] The amount of the liquid quick-setting admixture used in the sprayed concrete composition and the sprayed concrete of the present invention is preferably 5 to 20 parts by mass, more preferably 7 to 15 parts by mass, per 100 parts by mass of cement in the cement concrete. By using 5 to 20 parts by mass, a good quick-setting effect is exhibited and early strength development can be improved.

[0027] [Cement concrete] The cement concrete according to the present embodiment is a general term for cement paste, cement mortar, and concrete.

[0028] The cement for cement concrete is not particularly limited, and examples include various Portland cements such as normal, high-early-strength, extra-high-early-strength, medium-heat, and low-heat, filler cements made by mixing Portland cement with blast furnace slag, fly ash, and limestone powder, and environmentally friendly cements (eco-cement) made from municipal waste incineration ash and sewage sludge incineration ash, and these can also be used in a fine powder form. The ratio of the mixture and cement in the mixed cement is not particularly limited, and it is also possible to use a mixture of more of these admixtures than are assumed by the JIS.

[0029] The cement concrete of this embodiment contains cement and aggregate, and the aggregate preferably has low water absorption and high aggregate strength. The aggregate is not particularly limited as long as it can be sprayed, but river sand, mountain sand, sea sand, lime sand, silica sand, etc. can be used as fine aggregate, and river gravel, mountain gravel, lime gravel, etc. can be used as coarse aggregate, and crushed sand and crushed stone can also be used.

[0030] [Polyethylene oxide] The polyethylene oxide according to the present embodiment is blended and contained in the sprayed concrete composition as a dust reducing component. If the mass average molecular weight of the polyethylene oxide is high, the viscosity of the concrete increases and the mixing with the quick-setting agent tends to deteriorate, so the dust reducing performance decreases, and if the mass average molecular weight is low, the polyethylene oxide cannot be involved in the concrete viscosity and the dust reducing performance decreases, so in the present invention, the mass average molecular weight of the polyethylene oxide is preferably 100,000 to 3,000,000, more preferably 300,000 to 2,500,000, and even more preferably 500,000 to 2,000,000. The mass average molecular weight of polyethylene oxide can be determined by gel permeation chromatography (GPC) under the following measurement conditions. Measurement conditions: Equipment: Product name "LC-10AD" (manufactured by Shimadzu Corporation) Detector: Refractive index detector (RID) Column: Product name "SHODEX KF-804" (manufactured by Showa Denko K.K.) ·Measurement temperature: 30℃ ·Eluent:THF ·Flow rate: 1.0mL / min Sample concentration: 0.2% by mass (THF) Sample injection volume: 100μL Conversion standard: Polyethylene oxide

[0031] The content of polyethylene oxide in this embodiment is preferably 0.02 to 0.4 parts by mass, more preferably 0.05 to 0.3 parts by mass, and even more preferably 0.1 to 0.25 parts by mass, relative to 100 parts by mass of water used in cement concrete. When the content of polyethylene oxide is equal to or more than the above lower limit, dust reduction performance is easily obtained. In addition, when the content of polyethylene oxide is equal to or less than the above upper limit, the mixability with the liquid quick-setting admixture is improved, the adhesion property at the very initial stage is improved, and rebound can be suppressed. By using the liquid quick-setting admixture of the present invention in combination, it is possible to spray thickly or under spring water, which was a problem with the liquid quick-setting admixture so far.

[0032] The sprayed concrete composition and sprayed concrete of the present invention can use bentonite, stone powder, and various cement admixtures and cement admixtures in addition to liquid quick-setting admixtures, cement concrete, and polyethylene oxide. In particular, when applying to places where water is present, such as underground or behind a tunnel, or places where leakage into cracks must be prevented, the combined use of fine powders such as bentonite and stone powder and underwater anti-separation admixtures is effective in improving underwater anti-separation resistance.

[0033] In addition, the liquid quick-setting agent of the present invention is also effective in producing quick-setting aerated mortar. Usually, in the case of quick-setting aerated mortar, the quick-setting action of the quick-setting agent is faster than necessary, for example, instantaneously fast, so that while the quick-setting agent is being added and mixed, the bubbles in the aerated mortar are broken, making it difficult to obtain the desired physical properties such as specific gravity and strength. The liquid quick-setting agent of the present invention has a setting time of several seconds to several tens of seconds, so that quick-setting air mortar can be produced without breaking the bubbles, and it is possible to carry out the work sufficiently, and it has excellent quick-setting properties after setting. This makes it possible to prevent the leakage into cracks and the like, which were previously considered to be disadvantages of air mortar, and the separation of materials when cast in a place where water is present.

[0034] The water used in the cement concrete is not particularly limited, and the amount of water used is also not particularly limited, but usually, 40 to 150 parts by mass is preferable for 100 parts by mass of cement. If it is 40 to 150 parts by mass, good fluidity and strength development are easily exhibited.

[0035] In the present invention, when the cement concrete mixed with water and the liquid quick-setting admixture are mixed, the fluidity may be lost within a few seconds after mixing. Therefore, when a long pumping distance is required or when workability is taken into consideration, it is preferable to feed the liquid quick-setting admixture and the cement concrete mixed with water separately and then mix them together at the tip of the feed pipe for construction.

[0036] In the present invention, the method of mixing the liquid quick-setting admixture, the cement concrete, and the polyethylene oxide to prepare the concrete composition is not particularly limited, and for example, a method of mixing and merging the liquid quick-setting admixture and the cement concrete containing the polyethylene oxide can be mentioned. Specific mixing and merging methods include, for example, a method of using a mixing pipe such as a Y-shaped pipe, a method of using a double pipe, and a method of using an inlet piece that mixes and mixes the liquid quick-setting admixture in a shower-like manner. In addition, a method of setting a spiral mixer in the pipe after the merging and mixing to further mix is ​​also possible. If the liquid quick-setting admixture and the cement concrete are mixed sufficiently, adhesion and plasticity are obtained, and workability is improved, and if the mixing is insufficient, it may flow partially, making it difficult to completely apply the material.

[0037] [Spraying method] The sprayed concrete composition according to this embodiment is mainly used in a spraying method, although a simple pouring method is sufficient when filling voids underground or behind a tunnel. As for the spraying method according to this embodiment, when spraying in a place where water is present or where leakage into cracks must be prevented, it is also effective to blow the sprayed concrete composition with compressed air. The point where the compressed air is introduced is not particularly limited, but it is preferable to introduce it into a mixing pipe. EXAMPLES

[0038] The present invention will be described in more detail below based on experimental examples, but the present invention is not limited to these.

[0039] (Examples 1 to 11) Aluminum sulfate, an aluminum source, a sulfur source, a fluorine source, and a sodium source were mixed in water so that the ratios of aluminum in terms of Al2O3, sulfur in terms of SO3, and sodium in terms of Na2O were as shown in Table 1, and the mixture was heated at 90°C for 60 minutes. After heating, the mixture was rapidly cooled to 25°C in 50 minutes using a circulating cooling device to produce a liquid quick-setting admixture as a hardening accelerator. The solids concentration of the liquid quick-setting admixture and the viscosity of the liquid quick-setting admixture at 20°C were measured as described below. The pH of the supernatant of the liquid quick-setting admixture was also measured using a pH meter. The results are shown in Table 1.

[0040] <Materials used> Water: Tap water Aluminum sulfate: Aluminum sulfate powder, reagent (aluminum source, sulfur source) Sulfuric acid: Sulfuric acid, reagent (sulfur source) Aluminum hydroxide: Reagent (aluminum source) Cryolite: Reagent (fluorine source), Chiolite: 2%, Elpasolite: 0.5% (measured by XRD) Sodium sulfate: Reagent, anhydrous, (sodium source)

[0041] <Measurement method> Solids concentration: The total amount of SO3, Al2O3, Na2O, and F from the raw materials was calculated. Viscosity (20℃): Measured using a B rotational viscometer.

[0042] 50 g of the liquid quick-setting admixture was stored at 20° C. for 48 hours. After that, the content of sodium alunite was measured as described below. The results are shown in Table 1.

[0043] <Measurement method> -Natroalunite content 50g of the stored liquid quick-setting admixture was poured into a glass filter, suction filtered, and then dried in a vacuum desiccator for 24 hours to obtain a sample, which was then subjected to X-ray diffraction measurement. The peak intensity of the Natroalunite alone was compared with the peak intensity of the Natroalunite sample to determine the Natroalunite content.

[0044] Next, 100 parts by mass of cement, 50 parts by mass of water, 250 parts by mass of sand, 150 parts by mass of gravel, and 0.15 parts by mass of polyethylene oxide per 100 parts by mass of water were mixed in a mixer to produce cement concrete. The produced cement concrete and the above-mentioned liquid quick-setting admixture were separately fed into a mixing pipe, and the quick-setting mortar, which is a quick-setting cement concrete, was continuously prepared while mixing in a non-driven line mixer so that the liquid quick-setting admixture was 10 parts by mass per 100 parts of cement. The quick-setting mortar was subjected to a setting test as described below to evaluate the quick-setting property and mixability. The results are shown in Table 1.

[0045] <Materials used> Cement: Commercially available ordinary Portland cement (Denka, density 3.15 g / cm 3 ) Water: Tap water Sand: River sand from the Himekawa River in Niigata Prefecture, density 2.61g / cm 3 Polyethylene oxide: Mass average molecular weight 1.8 million, commercially available

[0046] <Evaluation method> -Evaluation of quick setting and mixability According to ASTM C403, the quick-setting mortar was penetrated 10 times with a Proctor needle 2 minutes after the addition of the liquid accelerator. 2 Those who met all 10 criteria were given an "A," those who met the criteria 7 to 9 times were given a "B," those who met the criteria 4 to 6 times were given a "C," and those who met the criteria less than 4 times were given a "D."

[0047] Example 12 A liquid quick-setting admixture was produced under the same conditions as in Example 1, except that the amount of cryolite was reduced to two-thirds. The results are shown in Table 1.

[0048] Example 13 A liquid quick-setting admixture was produced under the same conditions as in Example 1, using one-third the amount of cryolite. The results are shown in Table 1.

[0049] Example 14 A liquid quick-setting admixture was produced under the same conditions as in Example 1, using one-sixth the amount of cryolite. The results are shown in Table 1.

[0050] Example 15 The amount of cryolite was halved and the amount of sodium sulfate was halved in Example 1, and a liquid quick-setting admixture was produced under the same conditions. The results are shown in Table 1.

[0051] Comparative Example 1 In the same manner as in Example 1, aluminum sulfate, an aluminum source, a sulfur source, a fluorine source, and a sodium source were mixed with water and heated at 90°C for 60 minutes. After heating, the mixture was left as it was and cooled to 25°C for 240 minutes to produce a liquid quick-setting admixture. The solids concentration of the liquid quick-setting admixture and the viscosity of the liquid quick-setting admixture at 20°C were measured. In addition, the pH of the supernatant of the liquid quick-setting admixture was measured with a pH meter. The results are shown in Table 1.

[0052] Comparative Example 2 A liquid quick-setting admixture was produced under the same conditions, except that sodium sulfate was used in place of cryolite in Comparative Example 1. The results are shown in Table 1.

[0053] Comparative Example 3 A liquid quick-setting admixture was produced under the same conditions as in Comparative Example 1, except that the amount of cryolite was reduced to half and the amount of sodium sulfate was reduced to half. The results are shown in Table 1.

[0054] Comparative Example 4 A liquid quick-setting admixture was produced under the same conditions as in Comparative Example 1, using 1 / 20 the amount of cryolite. The results are shown in Table 1.

[0055] Comparative Example 5 A liquid quick-setting admixture was produced under the same conditions, using 1 / 40th the amount of cryolite used in Comparative Example 1. The results are shown in Table 1.

[0056] [Table 1] [Industrial Applicability]

[0057] The liquid quick-setting admixture of the present invention can be suitably used for cement concrete to be sprayed onto exposed natural ground surfaces such as tunnels for roads, railways, and waterways, and slopes.

Claims

1. A liquid quick-setting admixture to be mixed with a sprayed concrete composition containing cement concrete and polyethylene oxide having a mass average molecular weight of 100,000 to 3,000,000, The liquid quick-setting admixture contains aluminum, sulfur, and sodium, and has a sodium alunite content of 0.3 to 3 mass%.

2. The liquid quick-setting admixture according to claim 1, wherein the content of the natroalunite is 0.3 to 3 mass% after storage at 0 to 40°C for 48 hours immediately after preparation.

3. The liquid quick-setting admixture according to claim 1 or 2, which has a pH of 1 to 4.

4. The aluminum in 100 parts by mass of the liquid quick-setting agent is Al 2 O 3 The sulfur is 1 to 20 parts by mass in terms of SO 3 The sodium is 10 to 30 parts by mass in terms of Na 2 The liquid quick-setting admixture according to any one of claims 1 to 3, wherein the content is 0.1 to 3 parts by mass in terms of O.

5. The liquid quick-setting admixture according to any one of claims 1 to 4, having a solids concentration of 20 to 50 mass%.

6. The liquid quick-setting admixture according to any one of claims 1 to 5, having a viscosity at 20°C of 1,000 mPa·s or less.

7. A 2 O 3 Aluminum and SO 3 Mass ratio of sulfur in terms of Al 2 O 3 / SO 3 7. The liquid quick-setting admixture according to claim 1, wherein the ratio of the viscosity of the liquid quick-setting admixture to the viscosity of the liquid quick-setting admixture is 0.3 to 0.

7.

8. A sprayed concrete composition comprising the liquid quick-setting admixture according to any one of claims 1 to 7, cement concrete, and polyethylene oxide having a mass average molecular weight of 100,000 to 3,000,000.

9. A method for producing the sprayed concrete composition according to claim 8, comprising the steps of: mixing the polyethylene oxide into the cement concrete; and mixing the liquid quick-setting admixture with the cement concrete containing the polyethylene oxide.

10. A method for producing a sprayed concrete composition as described in Claim 9, wherein, in the process of mixing the liquid quick-setting admixture with the cement concrete containing the polyethylene oxide, the liquid quick-setting admixture and the cement concrete containing the polyethylene oxide are mixed and joined together.

11. A sprayed concrete obtained by spraying the sprayed concrete composition according to claim 8.

12. A spraying method, comprising spraying the sprayed concrete composition according to claim 8.

Citation Information

Patent Citations

  • Quick-setting agent for cement, quick-setting cement concrete produced by using the agent, and method of producing the same

    JP2001261393A

  • Liquid curing accelerator, rapid curing cement / Concrete using the same and method of producing rapid curing cement / Concrete

    JP2002047048A

  • Spray material and spraying method using it

    JP2007055831A

  • Sprayed concrete manufacturing equipment, sprayed concrete spraying method and sprayed concrete manufacturing method, using the same

    JP2010007230A