Manufacturing method of decorative sheet and decorative sheet

By mixing thermoplastic resin with a white pigment and a liquid colorant to form decorative sheets, the method addresses the inefficiencies of preparing colored pellets and extensive cleaning, enhancing workability and color change efficiency.

JP7584351B2Active Publication Date: 2024-11-15C I TAKIRON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021079328
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-07
Publication Date
2024-11-15
Estimated Expiration
2041-05-07

AI Technical Summary

Technical Problem

The existing manufacturing methods for decorative sheets require preparation of colored color master resin pellets for each color tone, leading to increased workload and the need for extensive cleaning when changing colors, which burdens the coloring process.

Method used

A method involving mixing thermoplastic resin with a white pigment to form a first resin composition, adding a liquid colorant to create a second resin composition, and extruding it into a sheet shape, eliminating the need for colored pellets and reducing equipment cleaning during color changes.

Benefits of technology

This approach reduces the burden of coloring work and improves workability by allowing for easy color changes without extensive cleaning, while maintaining excellent hiding and sheet formability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584351000001
    Figure 0007584351000001
Patent Text Reader

Abstract

To provide a manufacturing method of a decorative sheet, which is capable of reducing a load of coloring work and having an excellent workability in changing colors, and to provide the decorative sheet.SOLUTION: A manufacturing method of a decorative sheet at least comprises the steps of: mixing a thermoplastic resin and a white pigment to form a first resin composition; supplying the first resin composition to an extruder, and adding dropwise a liquid colorant to the first resin composition supplied to the extruder to form a second resin composition comprising the first resin composition and the colorant; and extruding and molding the second resin composition into a sheet using the extruder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a decorative sheet colored with a colorant, and to a decorative sheet. [Background technology]

[0002] Decorative sheets are used to enhance design by providing surface decoration for various applications, such as wall materials, construction materials, building materials such as fittings, surface decoration of furniture, etc., automotive interiors, low-voltage electrical coverings, etc. Known decorative sheets include those that are simply colored with a coloring agent to enhance design.

[0003] As a method for producing such a colored decorative sheet, for example, a method has been proposed in which color master resin pellets (pigments or dyes uniformly kneaded into a base resin) are blended with base resin pellets and extruded into a sheet using an extruder. It is described that this type of configuration can prevent the pellets from separating, and allows the production of molded products with good color tones. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-81200 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the manufacturing method described in Patent Document 1, it is necessary to prepare colored color master resin pellets that are mixed for each color tone, and it is also necessary to prepare excess colorant and remove the excess colorant, which results in a heavy coloring work load.

[0006] Furthermore, since the system is configured to supply colored color master resin pellets to the extruder, when changing colors by changing the colorant, it is necessary to clean the equipment that supplies the color master resin pellets to the extruder, and it is also necessary to clean the entire extruder, which creates the problem of a heavy workload when changing colors.

[0007] Therefore, the present invention has been made in consideration of the above problems, and aims to provide a manufacturing method for a decorative sheet and a decorative sheet that can reduce the burden of coloring work and have excellent workability when changing colors. [Means for solving the problem]

[0008] In order to achieve the above-mentioned object, the manufacturing method for decorative sheets of the present invention is characterized by including at least the steps of mixing a thermoplastic resin and a white pigment to form a first resin composition, supplying the first resin composition to an extruder and dripping a liquid colorant onto the first resin composition supplied to the extruder to form a second resin composition consisting of the first resin composition and the colorant, and extruding the second resin composition into a sheet shape using the extruder.

[0009] The decorative sheet of the present invention is a decorative sheet containing at least a thermoplastic resin, a white pigment, and a colorant other than the white pigment, characterized in that the content of the white pigment is 0.5 parts by mass to 15 parts by mass per 100 parts by mass of the thermoplastic resin, and the colorant is liquid. Effect of the Invention

[0010] According to the present invention, the burden of coloring work can be reduced and the workability when changing colors can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The decorative sheet of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.

[0012] The decorative sheet of the present invention is a sheet-like molded article containing a thermoplastic resin, a white pigment, and a colorant other than the white pigment.

[0013] <Thermoplastic resin> The decorative sheet of the present invention is mainly composed of a thermoplastic resin, and examples of the thermoplastic resin include polyvinyl chloride resin, glycol-modified polyethylene terephthalate resin (PETG), amorphous crystalline polyethylene terephthalate resin (APET), polyolefin resin (polyethylene resin, polypropylene resin, etc.), acrylonitrile-butadiene-styrene resin (ABS), polycarbonate resin, etc. Examples of amorphous crystalline polyethylene terephthalate resin (APET) include recycled polyethylene terephthalate (RPET) made from PET bottles and the like. These thermoplastic resins may be used alone or in combination of two or more.

[0014] As the thermoplastic resin, glycol-modified polyethylene terephthalate resin is preferred from the viewpoint of ease of processing into a quadratic curved surface and excellent three-dimensional moldability. Glycol-modified polyethylene terephthalate resin is a type of polyethylene terephthalate resin, and is a non-crystalline polyester resin that contains, as a glycol component, ethylene glycol as well as a diol other than ethylene glycol (1,4-cyclohexanedimethanol), whereas the glycol component of polyethylene terephthalate resin is ethylene glycol.

[0015] The thickness of the decorative sheet of the present invention, which is mainly composed of a thermoplastic resin, is not particularly limited, but is preferably 50 to 500 μm, more preferably 100 to 400 μm. If the thickness of the decorative sheet is 50 μm or more, the mechanical strength and hiding power can be sufficiently improved. If the thickness of the decorative sheet is 500 μm or less, the three-dimensional moldability is more excellent, and it is easier to ensure flexibility and printability.

[0016] <White pigment> The white pigment is for improving the hiding power of the decorative sheet, and examples thereof include titanium oxide, zinc oxide, calcium carbonate, magnesium oxide, and ritbon. Among these, it is preferable to use titanium oxide, which has a high hiding power. Examples of the titanium oxide include rutile type titanium oxide and anatase type titanium oxide, and rutile type titanium oxide is preferable from the viewpoint of low catalytic activity. These white pigments may be used alone or in combination of two or more.

[0017] The content of the white pigment is preferably 0.5 to 15 parts by mass relative to 100 parts by mass of the thermoplastic resin, because if it is less than 0.5 parts by mass, the hiding power may decrease, and if it is more than 15 parts by mass, the viscosity of the molten resin may decrease significantly, resulting in a decrease in the formability of the decorative sheet.

[0018] The average particle size of the white pigment is preferably 50 nm to 500 nm, because if it is less than 50 nm, the transparency of the decorative sheet increases, which may decrease the hiding power, and if it is greater than 500 nm, the coloring degree (whiteness) may decrease.

[0019] The term "average particle size" used here refers to the 50% particle size (D50), and can be measured as the volume average particle size using a laser diffraction / scattering type particle size distribution analyzer (Microtrac (registered trademark) particle size distribution analyzer MT3200, manufactured by Nikkiso Co., Ltd.) or the like.

[0020] <Coloring agent> The colorant is intended to improve the design of the decorative sheet, and in the present invention, a liquid colorant containing an inorganic pigment or an organic pigment is used. Examples of inorganic pigments include carbon black, iron oxide, nickel titanium yellow, ultramarine, and titanium black, and examples of organic pigments include phthalocyanine, quinacridone, and anthraquinone. These colorants may be used alone or in combination of two or more. In addition, organic coloring dyes are prone to fading and have poor weather resistance, so they are not used as colorants in the decorative sheet of the present invention.

[0021] The content of the colorant is preferably 9 parts by mass or less per 100 parts by mass of the thermoplastic resin, because if it is more than 9 parts by mass, the viscosity of the molten resin will be significantly reduced, which may result in a decrease in the formability of the decorative sheet.

[0022] <Manufacturing method> Next, a method for producing the decorative sheet of the present invention will be described. When producing the decorative sheet of the present invention, a thermoplastic resin and a white pigment are first mixed to form a first resin composition. This configuration makes it possible to reliably disperse the white pigment, which is difficult to disperse in a liquid colorant, and therefore improves the hiding power of the decorative sheet.

[0023] Next, the first resin composition is fed to an extruder, and a liquid colorant is dripped onto the first resin composition fed to the extruder to form a second resin composition consisting of the first resin composition and the colorant.

[0024] More specifically, the first resin composition is supplied to an extruder from equipment in which the first resin composition is compounded via supply equipment such as piping, and at the same time, for example, a liquid colorant prepared in advance is supplied to the feed section of the extruder, and the liquid colorant is dripped onto the first resin composition supplied to the extruder, thereby forming a second resin composition consisting of the first resin composition and the colorant.

[0025] Therefore, it is only necessary to prepare and drip a liquid colorant for each color tone, and there is no need to prepare color master resin pellets that have been pre-colored and mixed for each color tone, as in the conventional technology described above, which makes it possible to reduce the burden of the coloring work.

[0026] Furthermore, it is only necessary to drip the required amount of liquid colorant, eliminating the need for the prior art technique of preparing excess colorant and then removing the excess colorant, thereby reducing the burden of the coloring work.

[0027] In addition, unlike the above-mentioned conventional technology in which colored color master resin pellets are supplied to the extruder, a liquid colorant is supplied to the feed section of the extruder and dripped, so the color is fixed from the blending of the first resin composition until the first resin composition is supplied to the extruder. Therefore, when changing the colorant, it is not necessary to clean the equipment for blending the first resin composition and the equipment for supplying the first resin composition to the extruder, and the workability when changing the color can be improved.

[0028] Furthermore, because the liquid colorant is supplied to the feed section of the extruder and dripped, it is only necessary to clean the equipment following the feed section of the extruder when changing colorants, eliminating the need to clean the entire extruder as in the prior art described above, thereby improving workability when changing colors.

[0029] The second resin composition is then extruded into a sheet shape by an extruder, thereby producing a colored decorative sheet mainly made of a thermoplastic resin.

[0030] As described above, in the decorative sheet manufacturing method of the present invention, when manufacturing a decorative sheet having excellent hiding power and sheet formability, the burden of coloring work can be reduced and workability when changing colors can be improved. EXAMPLES

[0031] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.

[0032] Example 1 (Making decorative sheets) First, 15 parts by mass of titanium oxide (manufactured by Ishihara Sangyo Kaisha, product name: CR-60, average particle size: 0.21 μm) was added to 100 parts by mass of A-PET resin (manufactured by China Run Co., Ltd., product name: CR8816), which is the main component, to form a first resin composition. Next, the first resin composition was supplied to an extruder (OSE-35φmm extruder) manufactured by Nagata Manufacturing Co., Ltd., and 0.3 parts by mass of liquid colorant 1 (L*: 96.32, a*: -0.32, b*: 3.65) prepared in advance was dropped into the feed section of the extruder at a rate of 100 parts by mass of A-PET resin to form a second resin composition consisting of the first resin composition and colorant 1. Using the above-mentioned extruder, the second resin composition was extruded into a sheet shape under conditions of a temperature of 265°C and a screw rotation speed of 44 rpm, and a colored decorative sheet (width: 340 mm, thickness: 0.2 mm) mainly composed of A-PET resin was produced.

[0033] "L*" is a correlation value of lightness defined in JIS Z 8781-4:2013 "Colorimetry - Part 4: CIE 1976 L*a*b* color space" (corresponding international standard ISO 11664-4:2008). "a*" and "b*" are color coordinates defined in JIS Z 8781-4:2013 "Colorimetry - Part 4: CIE 1976 L*a*b* color space" (corresponding international standard ISO 11664-4:2008).

[0034] (Evaluation of color matching workability) Regarding the workability of color mixing, cases where there was no need to prepare a master batch with a color mixture for each color tone and the workload was low were marked with an ◯, and cases where it was necessary to prepare a master batch with a color mixture for each color tone and the workload was high were marked with an X. The results are shown in Table 1.

[0035] (Evaluation of colorant preparation) The cases where only the necessary amount of colorant had to be prepared were marked with an ◯, and the cases where more than the necessary amount of colorant had to be prepared were marked with an X. The results are shown in Table 1.

[0036] (Evaluation of cleaning ability) When changing the color tone, the equipment for compounding the first resin composition and the equipment for supplying the first resin composition to the extruder did not need to be cleaned, and was marked with an "O" when it was necessary to clean them, and a "X" when it was necessary to clean them. The results are shown in Table 1.

[0037] (Evaluation of color changeability) When changing the colorant, the case where only a part of the extruder needed to be cleaned was marked with an ◯, and the case where the whole extruder needed to be cleaned was marked with an X. The results are shown in Table 1.

[0038] (Evaluation of Concealment) For the prepared decorative sheet, the color difference ΔE between the chromaticity measured on a MDF (Medium Density Fiberboard) (L*: 66.03, a*: 9.24, b*: 21.90) as a color measurement stand and the chromaticity measured on a white substrate (white-painted MDF, L*: 93.38, a*: -0.85, b*: 4.99) as a color measurement stand was 0.6 or less, and the rest was marked as ×. More specifically, a spectrophotometer (CCM) (Kurabo, product name: COLOR-7) was used to measure three arbitrary points of the sample under conditions of a light source of D65, a viewing angle of 10°, and a color measurement range of φ28 mm, and the average value was used as the color coordinate. The above results are shown in Table 1.

[0039] (Evaluation of sheet formability) The decorative sheet (width: 340 mm) produced was evaluated based on the variation in sheet width over the entire decorative sheet. More specifically, when the variation in sheet width over the entire decorative sheet was less than 10 mm (i.e., when the sheet width over the entire decorative sheet was greater than 330 mm and less than 350 mm), it was evaluated as ○, and when the variation in sheet width was 10 mm or more (i.e., when there was a portion in the entire decorative sheet where the sheet width was 330 mm or less, or 350 mm or more), it was evaluated as ×. The results are shown in Table 1.

[0040] Example 2 (Making decorative sheets) First, 1.5 parts by mass of titanium oxide (manufactured by Ishihara Sangyo Kaisha, product name: CR-60, average particle size: 0.21 μm) was added to 100 parts by mass of PVC resin (manufactured by Taiyo PVC, product name: TH700), which is the main component, to form a first resin composition. Next, the first resin composition was supplied to an extruder (OSE-35φmm extruder) manufactured by Nagata Manufacturing Co., Ltd., and 2 parts by mass of liquid colorant 2 (brightness L*: 75.86, chromaticity a*: 1.32, chromaticity b*: 5.45) prepared in advance was dropped into the feed section of the extruder to form a second resin composition consisting of the first resin composition and colorant 2. Using the above-mentioned extruder, the second resin composition was extruded into a sheet shape under conditions of a temperature of 190° C. and a screw rotation speed of 44 rpm, and a colored decorative sheet (width: 340 mm, thickness: 0.2 mm) mainly composed of PVC resin was produced.

[0041] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0042] Example 3 (Making decorative sheets) First, 2.4 parts by mass of titanium oxide (manufactured by Ishihara Sangyo Kaisha, product name: CR-60, average particle size: 0.21 μm) was added to 100 parts by mass of A-PET resin (manufactured by China Run Co., Ltd., product name: CR8816), which is the main component, to form a first resin composition. Next, the first resin composition was supplied to an extruder (OSE-35φmm extruder) manufactured by Nagata Manufacturing Co., Ltd., and 3 parts by mass of liquid colorant 2 (brightness L*: 75.86, chromaticity a*: 1.32, chromaticity b*: 5.45) prepared in advance was dropped into the feed section of the extruder with respect to 100 parts by mass of A-PET resin to form a second resin composition consisting of the first resin composition and colorant 2. Using the above-mentioned extruder, the second resin composition was extruded into a sheet shape under conditions of a temperature of 265°C and a screw rotation speed of 44 rpm, and a colored decorative sheet (width: 340 mm, thickness: 0.2 mm) mainly composed of A-PET resin was produced.

[0043] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0044] Example 4 A decorative sheet was produced in the same manner as in Example 3, except that the amount of titanium oxide added was changed to 1.2 parts by mass, and the amount of Colorant 2 dropped was changed to 5 parts by mass.

[0045] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0046] Example 5 A decorative sheet was produced in the same manner as in Example 3, except that the amount of titanium oxide added was changed to 0.6 parts by mass, and the amount of Colorant 2 dropped was changed to 8 parts by mass.

[0047] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0048] Comparative Example 1 A decorative sheet was produced in the same manner as in Example 1, except that the amount of titanium oxide added was changed to 18 parts by mass, and the amount of Colorant 1 dropped was changed to 0.5 parts by mass.

[0049] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0050] Comparative Example 2 A decorative sheet was produced in the same manner as in Example 1, except that the amount of titanium oxide added was changed to 18 parts by mass, and the amount of Colorant 1 dropped was changed to 2 parts by mass.

[0051] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0052] Comparative Example 3 A decorative sheet was produced in the same manner as in Example 3, except that the amount of titanium oxide added was changed to 0.12 parts by mass, and the amount of Colorant 2 dropped was changed to 10 parts by mass.

[0053] Then, evaluations of color matching workability, colorant preparation, cleaning ability, color changeability, hiding power, and sheet formability were performed in the same manner as in Example 1. The results are shown in Table 1.

[0054] Comparative Example 4 Except for not using titanium oxide, a decorative sheet was produced in the same manner as in Comparative Example 3. More specifically, 100 parts by mass of A-PET resin (manufactured by Huarun Co., Ltd., product name: CR8816) was supplied to an extruder (OSE-35φmm extruder) manufactured by Nagata Manufacturing Co., Ltd., and 10 parts by mass of liquid colorant 2 (brightness L*: 75.86, chromaticity a*: 1.32, chromaticity b*: 5.45) prepared in advance was dropped into the feed section of the extruder at 10 parts by mass per 100 parts by mass of A-PET resin to form a resin composition consisting of A-PET resin and colorant 2, and the resin composition was extruded into a sheet shape using the above-mentioned extruder under conditions of a temperature of 265°C and a screw rotation speed of 44 rpm to produce a colored decorative sheet (width: 340 mm, thickness: 0.2 mm) mainly composed of A-PET resin.

[0055] Comparative Example 5 First, colored pellets were prepared using A-PET resin (CR8816, manufactured by China Run Co., Ltd.) and colorant 2, with a coloring of L*: 75.86, a*: 1.32, and b*: 5.45. Next, 2.4 parts by mass of titanium oxide and 3 parts by mass of the prepared colored pellets were fed to an extruder (OSE-35φmm extruder) manufactured by Nagata Manufacturing Co., Ltd., per 100 parts by mass of A-PET resin (CR8816, manufactured by China Run Co., Ltd.), and molding was performed using this extruder under conditions of a temperature of 265°C and a screw rotation speed of 44 rpm, to prepare a colored decorative sheet (width 340 mm, thickness 0.200 mm) mainly made of A-PET resin.

[0056] [Table 1]

[0057] As shown in Table 1, in Examples 1 to 5, it is only necessary to prepare a liquid colorant for each color tone, and there is no need to prepare a colored master batch with a mixed color tone for each color tone as in Comparative Example 5, so it is clear that the burden of the coloring work is low.

[0058] Furthermore, in Examples 1 to 5, it is only necessary to drip only the required amount of liquid colorant, and there is no need to prepare excess colorant and then remove the excess colorant after producing the decorative sheet, as in Comparative Example 5. This simplifies the work involved in preparing the colorant, and reduces the burden of the coloring work.

[0059] Furthermore, in Examples 1 to 5, unlike Comparative Example 5 in which colored pellets are supplied to the extruder, a liquid colorant is dripped into the feed section of the extruder, eliminating the need to clean the equipment for compounding the first resin composition and the equipment for supplying the first resin composition to the extruder, and thus demonstrating excellent operability when changing colors.

[0060] Furthermore, in Examples 1 to 5, since a liquid colorant is dropped into the feed section of the extruder, it is only necessary to clean the equipment following the feed section of the extruder, and cleaning of the entire extruder, as in Comparative Example 5, is not required, which shows that the workability when changing colors is excellent.

[0061] Moreover, the decorative sheets of Examples 1 to 5 have a color difference ΔE of 0.6 or less, indicating excellent hiding power. On the other hand, the decorative sheet of Comparative Example 3 contains a small amount of titanium oxide, less than 0.5 parts by mass (0.12 parts by mass), and the decorative sheet of Comparative Example 4 does not contain titanium oxide, so the color difference is greater than 0.6 and the hiding power is poor.

[0062] In addition, the decorative sheets of Examples 1 to 5 have excellent sheet moldability because the colorant content is 9 parts by mass or less. On the other hand, the decorative sheets of Comparative Examples 1 and 2 have poor sheet moldability because the titanium oxide (powder) content is greater than 15 parts by mass (18 parts by mass). In addition, the decorative sheets of Comparative Examples 3 and 4 have poor sheet moldability because the colorant content is greater than 9 parts by mass (10 parts by mass). [Industrial Applicability]

[0063] As described above, the present invention is suitable for a manufacturing method of a decorative sheet colored with a colorant and for a decorative sheet.

Claims

1. mixing a thermoplastic resin and a white pigment to form a first resin composition; supplying the first resin composition to an extruder and dripping a liquid colorant onto the first resin composition supplied to the extruder to form a second resin composition comprising the first resin composition and the colorant; a step of extruding the second resin composition into a sheet shape by the extruder; At least A method for producing a decorative sheet, characterized in that the content of the white pigment is 0.5 parts by mass to 15 parts by mass per 100 parts by mass of the thermoplastic resin.

2. A decorative sheet comprising at least a thermoplastic resin, a white pigment, and a colorant other than the white pigment, the thermoplastic resin is a polyvinyl chloride resin or an amorphous crystalline polyethylene terephthalate resin, The content of the white pigment is 0.5 parts by mass to 15 parts by mass relative to 100 parts by mass of the thermoplastic resin, The decorative sheet is characterized in that the colorant is a liquid.

3. 3. The decorative sheet according to claim 2, wherein the colorant is a liquid containing an inorganic pigment or an organic pigment.

4. 4. The decorative sheet according to claim 2, wherein the content of the colorant is 9 parts by mass or less per 100 parts by mass of the thermoplastic resin.

5. The decorative sheet according to any one of claims 2 to 4, wherein the white pigment has an average particle size of 50 nm to 500 nm.

Citation Information

Patent Citations

  • A decorative sheet sheet -

    JP1984126634U

  • Improved colored articles and compositions and methods for making them

    JP2000507309A

  • Method for producing colored molded product and colored master resin pellet using same and having sheath-core structure

    JP2001081200A

  • Colored (METH)acrylic film, marking film, receptor sheet and production method thereof

    JP2008214445A

  • System and method for forming various plastic products from a single molten material

    JP2015503470A