Ferritic stainless steel and exhaust gas parts
A ferritic stainless steel with controlled Al/Si-based oxides on the surface addresses the limitations of conventional alloying element methods, enhancing red scale resistance and maintaining manufacturability and cost-effectiveness.
Patent Information
- Application Number
- JP2022557621
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-23
- Filing Date
- 2021-10-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-10-22
AI Technical Summary
Conventional methods for improving red scale resistance in stainless steel by adding alloying elements like Cr and Si lead to increased manufacturing costs and reduced manufacturability, and there is a need for alternative methods to enhance red scale resistance without these elements.
A ferritic stainless steel with specific chemical compositions and controlled surface oxides, including Al/Si-based oxides, is developed to improve red scale resistance, maintaining manufacturability and reducing costs.
The solution provides ferritic stainless steel with excellent red scale resistance, improved workability, high-temperature strength, and corrosion resistance, while avoiding the drawbacks of alloying element additions.
Smart Images

Figure 0007584533000003 
Figure 0007584533000004 
Figure 0007584533000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel and an exhaust gas part, more specifically to a ferritic stainless steel having excellent resistance to red scale in a high-temperature steam atmosphere, and an exhaust gas part obtained by using the ferritic stainless steel as a raw material. This application claims priority based on Japanese Patent Application No. 2020-178302, filed on October 23, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] When stainless steel is used for applications such as exhaust gas path components, stove combustion equipment, fuel cell components, or plant-related materials, it is usually heated to high temperatures of 300 to 900°C. In addition, in the above applications, the stainless steel is used in an environment containing water vapor, which can cause red scale (Fe-based oxides) to form. In some cases, this red scale may fly off and adhere to other parts, causing adverse effects, and there is also a risk of reducing high-temperature strength due to thinning caused by oxidation.
[0003] Therefore, a ferritic stainless steel having red scale resistance in a high-temperature steam atmosphere is desired. Conventionally, various methods have been known for improving red scale resistance.
[0004] Patent Documents 1 and 2 describe that the addition of Si promotes the diffusion of Cr, increases the amount of Cr-based oxides produced, and strengthens the oxide film, thereby improving the steam oxidation resistance and red scale resistance of the inventions described in Patent Documents 1 and 2. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2003-160844 [Patent Document 2] Japanese Patent Application Publication No. 2003-160842 Summary of the Invention [Problem to be solved by the invention]
[0006] The above-mentioned conventional techniques focus on Cr and Si in steel and optimize the Cr and Si contents in the steel. However, such control by adding alloy elements leads to deterioration of manufacturability and increase in cost. Therefore, the present inventors have investigated ways to improve red scale resistance other than by adding alloy elements. Specifically, the present inventors have focused on oxides of a specific composition on the surface of stainless steel in order to improve red scale resistance.
[0007] An object of the present invention is to provide a ferritic stainless steel having excellent red scale resistance and an exhaust gas part made of the ferritic stainless steel and having excellent red scale resistance. [Means for solving the problem]
[0008] In order to solve the above problems, the gist of the present invention is as follows. [1] The ferritic stainless steel according to one embodiment of the present invention has a chemical composition of 0.05% by mass or more and 2.50% by mass or less of Si, 0.05% by mass or more and 1.50% by mass or less of Mn, 0.025% by mass or less of C, 0.040% by mass or less of P, 0.003% by mass or less of S, 0.025% by mass or less of N, 0.01% by mass or more and 0.50% by mass or less of Ni, 10.50% by mass or more and 25.00% by mass or less of Cr, 0.01% by mass or more and 1.80% by mass or less of Cu, 0.002% by mass or more and 0.200% by mass or less of Al, 0.001% by mass or more and 1.00% by mass or less of Nb, 0% by mass or more and 2.5% by mass or less of W, 0% by mass or more and 3.00% by mass or less of Mo, 0% by mass or more and 0.500% by mass or less of Ti, 0% by mass or more and 0. 0 to 0.100% by mass or less of B, 0 to 0.0030% by mass of Ca, 0 to 0.50% by mass of Hf, 0 to 0.40% by mass of Zr, 0 to 0.50% by mass of Sb, 0 to 0.30% by mass of Co, 0 to 1.0% by mass of Ta, 0 to 1.00% by mass of Sn, 0 to 0.30% by mass of Ga, 0 to 0.50% by mass of V, 0 to 0.003% by mass of Mg, and 0 to 0.20% by mass of REM, with the balance being Fe and impurities, and at least one of an oxide containing 5% by mass or more of Al and an oxide containing 5% by mass or more of Si is present on the surface, and In the observation field The number of oxides present on the surface having a diameter D represented by the following formula (1) of 0.1 μm or more and 2.0 μm or less is 93 μm 2 There are 10 or more per prize. D = (Dmax + Dmin) / 2 (1) (In the formula (1), Dmax is the maximum diameter of the oxide on the surface, and Dmin is the minimum diameter of the oxide on the surface.)
[0009] According to the above-mentioned configuration, a ferritic stainless steel having excellent red scale resistance can be realized.
[0010] [2] The ferritic stainless steel described in [1] has a CIE 1976 lightness L measured on the surface using a D65 light source in a diffuse lighting method, receiving light at an angle of 8° to the normal to the surface, with a viewing angle of 10° and a measurement time of 1 second. * may be 60 or more.
[0011] According to the above configuration, a ferritic stainless steel having excellent design properties can be realized.
[0012] [3] The ferritic stainless steel according to [1] or [2] has a chemical composition of 0.01% by mass or more and 2.5% by mass or less of W, 0.01% by mass or more and 3.00% by mass or less of Mo, 0.001% by mass or more and 0.500% by mass or less of Ti, 0.0002% by mass or more and 0.0100% by mass or less of B, 0.0002% by mass or more and 0.0030% by mass or less of Ca, 0.001% by mass or more and 0.50% by mass or less of Hf, 0.01% by mass or more and 0.40% by mass or less of Zr, 0.00 It may contain one or more of 5 mass% or more and 0.50 mass% or less of Sb, 0.01 mass% or more and 0.30 mass% or less of Co, 0.001 mass% or more and 1.0 mass% or less of Ta, 0.002 mass% or more and 1.00 mass% or less of Sn, 0.0002 mass% or more and 0.30 mass% or less of Ga, 0.01 mass% or more and 0.50 mass% or less of V, 0.0003 mass% or more and 0.003 mass% or less of Mg, and 0.001 mass% or more and 0.20 mass% or less of REM.
[0013] According to the above-mentioned configuration, it is possible to improve the workability, high-temperature strength, corrosion resistance, oxidation resistance of the steel plate, and secondary workability of the molded products produced using the ferritic stainless steel.
[0014] [4] The ferritic stainless steel according to any one of [1] to [3] may satisfy the following formula (2) in a range from the surface to 1.0 μm after being held in an atmosphere of 300 to 900°C for 100 hours or more, where the Cr content is [Cr], the Si content is [Si], and the Al content is [Al], all in unit mass%: [Cr] + [Si] + [Al] ≧ 18.0…(2)
[0015] [5] In the ferritic stainless steel according to another embodiment of the present invention, the following formula (2) is satisfied in the range from the surface to 1.0 μm, where the Cr content is [Cr], the Si content is [Si], and the Al content is [Al], all in unit mass%. 36.7≧ [Cr] + [Si] + [Al] ≧ 18.0…(2)
[0016] [6] An exhaust gas component according to one aspect of the present invention includes the ferritic stainless steel according to any one of [1] to [5]. Effect of the Invention
[0017] According to the above aspects of the present invention, it is possible to provide a ferritic stainless steel having excellent red scale resistance and an exhaust gas part having excellent red scale resistance. [Brief description of the drawings]
[0018] [Figure 1] 1 is a flowchart showing an example of a method for producing a ferritic stainless steel according to an embodiment of the present invention. [Figure 2A] FIG. 2 is a diagram showing an example of an SEM photograph of the surface of the ferritic stainless steel of the example steel No. 6. [Figure 2B] FIG. 2 is a diagram showing an example of an SEM photograph of the surface of ferritic stainless steel material No. 8 of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, a ferritic stainless steel according to one embodiment of the present invention (the ferritic stainless steel according to this embodiment), a manufacturing method for the ferritic stainless steel according to this embodiment, and an exhaust gas part obtained by using the ferritic stainless steel according to this embodiment as a raw material (the exhaust gas part according to this embodiment) will be described. The following description is for a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified. In addition, in this specification, "A to B" indicates A or more and B or less.
[0020] In addition, in this specification, the term "stainless steel" refers to a stainless steel material whose specific shape is not limited. Examples of the stainless steel material include steel plates, steel pipes, and bar steel.
[0021] <<Ferritic stainless steel>> <Chemical composition> The composition (chemical composition) of components contained in the ferritic stainless steel according to one embodiment of the present invention is as follows. In addition to the components shown below, the ferritic stainless steel is made up of iron (Fe) and / or small amounts of impurities (impurities) that may be mixed in from the raw materials or during the manufacturing process.
[0022] (Chromium: Cr) Cr is an essential element for forming a passive film and ensuring corrosion resistance. It is also effective for ensuring red scale resistance. To obtain this effect, the Cr content is 10.50 mass% or more. The Cr content is preferably 12.50 mass% or more. On the other hand, excessive Cr content increases material costs and causes a decrease in toughness, so the Cr content is set to 25.00 mass% or less, and preferably 23.00 mass% or less.
[0023] (Silicon: Si) Silicon is an element effective in improving red scale resistance. To obtain this effect, the silicon content is 0.05 mass % or more. The silicon content is preferably 0.10 mass % or more. On the other hand, if the Si content is excessive, it will cause a decrease in toughness and workability. Therefore, the Si content is set to 2.50 mass% or less. The Si content is preferably set to 2.00 mass% or less.
[0024] (Copper: Cu) Cu is an element that is contained to ensure high-temperature strength. To obtain this effect, the Cu content is 0.01 mass% or more. The Cu content is preferably 0.02 mass% or more. On the other hand, if the Cu content is excessive, the ferrite phase becomes unstable and the material cost increases. Therefore, the Cu content is 1.80 mass% or less. The Cu content is preferably 1.60 mass% or less.
[0025] (Niobium: Nb) Nb is an element that is contained to ensure high-temperature strength. To obtain this effect, the Nb content is 0.001% or more. The Nb content is preferably 0.05% by mass or more, and more preferably 0.10% by mass or more. On the other hand, if Nb is contained excessively, there is a possibility that workability and toughness may deteriorate. Therefore, the Nb content is 1.00 mass% or less. The Nb content is preferably 0.70 mass% or less, and more preferably 0.45 mass% or less.
[0026] (Manganese: Mn) Mn is an element that improves the adhesion of scale in ferritic stainless steel. To obtain this effect, the Mn content is 0.05 mass% or more. The Mn content is preferably 0.10 mass% or more. On the other hand, excessive Mn content destabilizes the ferrite phase and promotes the generation of MnS, which is the starting point of corrosion. Therefore, the Mn content is set to 1.50 mass% or less. The Mn content is preferably 1.20 mass% or less.
[0027] (Nickel: Ni) Ni is an element that improves the corrosion resistance of ferritic stainless steel. To obtain this effect, the Ni content is 0.01 mass% or more. The Ni content is preferably 0.05 mass% or more. On the other hand, if Ni is contained excessively, the ferrite phase becomes unstable and the material cost increases. Therefore, the Ni content is 0.50 mass% or less. The Ni content is preferably 0.30 mass% or less.
[0028] (Carbon:C) If C is contained excessively, the amount of carbides in the ferritic stainless steel increases, and the corrosion resistance of the steel decreases. Therefore, the C content is 0.025 mass% or less. The C content is preferably 0.020 mass% or less. The lower the C content, the better, and 0% may be acceptable; however, lowering the C content more than necessary increases the cost, so the C content may be 0.002 mass % or more.
[0029] (Rin:P) If P is contained excessively, the workability of ferritic stainless steel decreases. Therefore, the P content is 0.040 mass% or less. The P content is preferably 0.030 mass% or less. The lower the P content, the better, and 0% is also acceptable, but if the P content is reduced more than necessary, the cost increases, so the P content may be 0.001 mass% or more.
[0030] (Sulfur: S) If S is contained in an excessive amount, the generation of corrosion starting points is promoted in ferritic stainless steel. Therefore, the S content is 0.003 mass% or less. The S content is preferably 0.002 mass% or less. The lower the S content, the better, and 0% is also acceptable, but if the S content is reduced more than necessary, the cost increases, so the S content may be 0.0001 mass% or more.
[0031] (Nitrogen: N) If N is contained excessively, N will form nitrides with other elements, which will lead to the hardening of the ferritic stainless steel. Therefore, the N content is 0.025 mass% or less. The N content is preferably 0.020 mass% or less. The lower the N content, the better, and 0% is acceptable, but if the N content is reduced more than necessary, the cost will increase, so the N content may be 0.003 mass% or more.
[0032] (Aluminum: Al) Al is an element effective for improving the corrosion resistance of ferritic stainless steel and for improving red scale resistance. Furthermore, Al is an element effective as a deoxidizer during steelmaking. To obtain these effects, the Al content is 0.002 mass% or more. The Al content is preferably 0.008 mass% or more. On the other hand, if the Al content is excessive, the surface quality may deteriorate, so the Al content is set to 0.200 mass% or less.
[0033] (Other Ingredients) The ferritic stainless steel according to one embodiment of the present invention contains 0.01 mass % or more and 2.5 mass % or less of W, 0.01 mass % or more and 3.00 mass % or less of Mo, 0.001 mass % or more and 0.500 mass % or less of Ti, 0.0002 mass % or more and 0.0100 mass % or less of B, 0.0002 mass % or more and 0.0030 mass % or less of Ca, 0.001 mass % or more and 0.50 mass % or less of Hf, 0.01 mass % or more and 0.40 mass % or less of Zr, 0.005 mass % or more and 0.05 mass % or less of Hf, 0.01 mass % or more and 0.05 mass % or less of Zr, 0.005 mass % or more and 0.05 mass % or less of Hf, 0.01 mass % or more and 0.05 mass % or less of Hf, 0.01 mass % or more and 0.05 mass % or less of Zr, 0.005 mass % or more and 0.05 mass % or less of Hf ... The ferritic stainless steel according to the present embodiment may further contain one or more of the following elements: 0.50% by mass or less Sb, 0.01% by mass or more and 0.30% by mass or less Co, 0.001% by mass or more and 1.0% by mass or less Ta, 0.002% by mass or more and 1.00% by mass or less Sn, 0.0002% by mass or more and 0.30% by mass or less Ga, 0.01% by mass or more and 0.50% by mass or less V, 0.001% by mass or more and 0.20% by mass or less REM, and 0.0003% by mass or more and 0.003% by mass or less Mg. The ferritic stainless steel according to the present embodiment may further contain 0.20% by mass or less, preferably 0.10% by mass or less La, or 0.20% by mass or less, preferably 0.05% by mass or less Ce, as REM. However, since the inclusion of these elements is not essential, the content may be 0% or may be less than the range described below.
[0034] (Tungsten: W) W is an element that may be contained to ensure high-temperature strength. To obtain this effect, the W content is preferably 0.01 mass % or more, and more preferably 0.1 mass % or more. On the other hand, excessive W content increases material costs. Therefore, in the ferritic stainless steel according to this embodiment, the W content is 2.5 mass% or less. The W content is preferably 1.5 mass% or less, and more preferably 1.3 mass% or less.
[0035] (Molybdenum: Mo) Mo is an element that may be contained to ensure high-temperature strength and red scale resistance. To obtain this effect, the Mo content is preferably 0.01 mass % or more. On the other hand, excessive Mo content hardens the steel, reduces workability, and increases material costs. Therefore, the Mo content is set to 3.00 mass% or less. The Mo content is preferably set to 2.50 mass% or less.
[0036] (Titanium: Ti) Ti is an element that can convert ferritic stainless steel into a ferritic single phase at 900 to 1000°C by reacting with C and / or N, and improves red scale resistance and workability. Therefore, Ti may be contained. To obtain this effect, the Ti content is preferably 0.001 mass% or more. The Ti content is preferably 0.010 mass% or more, and more preferably 0.050 mass% or more. On the other hand, if the Ti content is excessive, the workability and surface quality may deteriorate. Therefore, the Ti content is 0.500 mass% or less. The Ti content is preferably 0.300 mass% or less, and more preferably 0.250 mass% or less.
[0037] (Boron: B) B is an element that improves the secondary workability of molded articles produced using ferritic stainless steel. To obtain this effect, the B content is preferably 0.0002 mass % or more. On the other hand, if B is contained in excess, Cr 2 Compounds such as B are easily formed, which may deteriorate the red scale resistance. Therefore, the B content is 0.0100% by mass or less. The B content is preferably 0.0080% by mass or less, and more preferably 0.0030% by mass or less.
[0038] (Calcium: Ca) Ca is an element that promotes high-temperature oxidation resistance. Therefore, Ca may be contained as necessary. To obtain this effect, the Ca content is preferably 0.0002 mass % or more. On the other hand, an excessive Ca content leads to a decrease in corrosion resistance, so the Ca content is set to 0.0030 mass% or less.
[0039] (Hafnium: Hf) Hf is an element that improves corrosion resistance, high-temperature strength, and oxidation resistance. Hf may be contained as necessary. To obtain this effect, the Hf content is preferably 0.001 mass% or more. The Hf content is more preferably 0.01 mass% or more. On the other hand, an excessive Hf content may deteriorate workability and manufacturability, so the Hf content is set to 0.50 mass% or less.
[0040] (Zirconium: Zr) Zr is an element that improves high-temperature strength, corrosion resistance, and high-temperature oxidation resistance. Therefore, Zr may be contained as necessary. To obtain this effect, the Zr content is preferably 0.01 mass% or more. On the other hand, an excessive Zr content leads to deterioration of workability and manufacturability, so the Zr content is set to 0.40 mass% or less.
[0041] (Antimony: Sb) Sb is an element that improves high-temperature strength. Therefore, Sb may be contained as necessary. To obtain this effect, the Sb content is preferably 0.005 mass% or more. The Sb content is more preferably 0.01 mass% or more. On the other hand, excessive Sb content reduces weldability and toughness, so the Sb content is set to 0.50 mass% or less.
[0042] (Cobalt: Co) Co is an element that improves high-temperature strength. Therefore, Co may be contained as necessary. To obtain this effect, the Co content is preferably 0.01 mass % or more. On the other hand, an excessive Co content reduces toughness and hence manufacturability, so the Co content is set to 0.30 mass % or less.
[0043] (Tantalum: Ta) Ta is an element that improves high-temperature strength. Therefore, Ta may be contained as necessary. To obtain this effect, the Ta content is preferably 0.001 mass% or more. The Ta content is more preferably 0.01 mass% or more, and further preferably 0.1 mass% or more. On the other hand, excessive Ta content reduces weldability and toughness, so the Ta content is set to 1.0 mass % or less.
[0044] (Tin: Sn) Sn is an element that improves corrosion resistance and high-temperature strength. Therefore, Sn may be contained as necessary. To obtain this effect, the Sn content is preferably 0.002 mass% or more. The Sn content is more preferably 0.01 mass% or more. On the other hand, an excessive Sn content may cause a decrease in toughness and manufacturability, so the Sn content is set to 1.00 mass% or less.
[0045] (Gallium: Ga) Ga is an element that improves corrosion resistance and hydrogen embrittlement resistance. Therefore, Ga may be contained as necessary. To obtain this effect, the Ga content is preferably 0.0002 mass% or more. The Ga content is more preferably 0.01 mass% or more. On the other hand, excessive Ga content reduces weldability and toughness, so the Ga content is set to 0.30 mass% or less.
[0046] (Vanadium: V) V is an element that fixes the solute C and N in steel as compounds and improves the ductility and workability of the steel. Therefore, V may be contained as necessary. To obtain this effect, the V content is preferably 0.01 mass% or more. On the other hand, an excessive V content reduces the workability of the steel, so the V content is set to 0.50 mass% or less.
[0047] (Magnesium: Mg) Mg is a deoxidizing element and also an element that refines the structure of the slab and improves the formability. Therefore, Mg may be contained as necessary. To obtain this effect, the Mg content is preferably 0.0003 mass% or more. On the other hand, since an excessive Mg content leads to deterioration of corrosion resistance, weldability, and surface quality, the Ca content is 0.003 mass % or less.
[0048] (Rare earth elements: REM) REM refers to a collective term for 15 elements (lanthanoid elements) ranging from scandium (Sc) and lanthanum (La) to lutetium (Lu). REM may contain any one of the lanthanoid elements alone, or may contain two or more of the lanthanoid elements. When any one of the lanthanoid elements is contained as REM, for example, as described below, it may contain either La or Ce, or a lanthanoid element other than La and Ce alone. When two or more of the lanthanoid elements are contained as REM, there is no particular restriction on the combination of elements, but as an example, La and Ce may be contained, or a plurality of lanthanoid elements contained in the misch metal may be contained as REM by adding the misch metal. REM is an element that improves the cleanliness of stainless steel and also improves high-temperature oxidation resistance. Therefore, REM may be contained as necessary. To obtain these effects, the REM content is preferably 0.001 mass% or more. The REM content is more preferably 0.01 mass% or more. On the other hand, an excessive REM content increases the alloy cost and reduces manufacturability, so the REM content is set to 0.20 mass% or less.
[0049] (Lantern: La) La may be contained as an REM. La is an element that improves the cleanliness of stainless steel and also improves high-temperature oxidation resistance, and further improves red scale resistance and scale spalling resistance. When La is contained (using metallic La or the like) to obtain this effect, the La content is preferably 0.001 mass% or more. The La content is more preferably 0.01 mass% or more. On the other hand, excessive La content increases material costs. Therefore, the La content is 0.20 mass% or less. The La content is preferably 0.10 mass% or less, and in consideration of costs, the La content is more preferably 0.05 mass% or less, and further preferably 0.03 mass% or less.
[0050] (Cerium: Ce) As REM, Ce may be contained. Ce is an element that improves the cleanliness of stainless steel and also improves high-temperature oxidation resistance. Furthermore, it is an element that improves red scale resistance and scale peeling resistance. When Ce is contained (using metallic Ce or the like) to obtain this effect, the Ce content is preferably 0.001% by mass or more. The Ce content is more preferably 0.01% by mass or more. On the other hand, if Ce is contained excessively, the material cost increases. Therefore, the Ce content is 0.20% by mass or less. The Ce content is preferably 0.05% by mass or less.
[0051] The chemical composition of the ferritic stainless steel according to this embodiment is obtained by performing elemental analysis by a general method such as ICP-AES from a position 1 / 4 of the plate thickness from the surface (a range of 1 / 8 to 3 / 8 of the thickness from the surface in the thickness direction is acceptable). Also, C and S may be measured using the combustion-infrared absorption method, N may be measured using the inert gas fusion-thermal conductivity method, and O may be measured using the inert gas fusion-infrared absorption method.
[0052] <Oxide containing Al or Si> In the ferritic stainless steel according to this embodiment, at least one of the oxides containing 5% by mass or more of Al and the oxides containing 5% by mass or more of Si exists on the surface, and among the oxides existing on the surface, the number of oxides (hereinafter referred to as "Al / Si-based oxides") having a diameter D represented by the following formula (1) of 0.1 μm or more and 2.0 μm or less is 93 μm 2 10 or more per hit. This oxide improves red scale resistance. D = (Dmax + Dmin) / 2 ···(1) (In the above formula (1), Dmax is the maximum diameter of each oxide on the surface, and Dmin is the minimum diameter of each oxide on the surface.)
[0053] The size of the oxide on the surface of the ferritic stainless steel can be measured, for example, by a scanning electron microscope (SEM). Specifically, a scanning electron microscope (SEM) is used to take SEM photographs of the surface of the steel material. The area of one field of view is 93 μm 2 From this SEM photograph, the maximum diameter and the minimum diameter of the oxide are calculated using image analysis software, for example, "Photoshop (registered trademark)" (manufactured by Adobe Co., Ltd.). Here, the Al and Si contents in the oxides on the surface of the ferritic stainless steel can be measured, for example, by an energy dispersive X-ray spectroscopy (EDS). That is, EDS can be used to determine whether the oxides are oxides whose number is counted (oxides containing 5% or more by mass of Al or oxides containing 5% or more by mass of Si). In this embodiment, the "maximum diameter" of an oxide means the maximum width between two parallel lines when the oxide is sandwiched between the two parallel lines when the oxide is viewed in a plan view. Also, in this specification, the "minimum diameter" of an oxide means the minimum width between two parallel lines when the oxide is sandwiched between the two parallel lines when the oxide is viewed in a plan view.
[0054] The reasons why oxides containing 5% or more by mass of Al or oxides containing 5% or more by mass of Si (sometimes called Al / Si-based oxides) improve red scale resistance are believed to be as follows. First, Al / Si-based oxides act as a protective coating. Second, Al / Si-based oxides grow when heated, lowering the oxygen partial pressure around the Al / Si-based oxide. Al, Si, Cr, and Fe are more likely to be oxidized in that order, so Al, Si, and Cr are oxidized preferentially over Fe. Therefore, the growth of Al / Si-based oxides can reduce the formation of red scale, which is an Fe-based oxide.
[0055] However, if there is an excess of Al / Si oxides on the surface of ferritic stainless steel, the Al / Si oxides may reduce the brightness of the surface of the ferritic stainless steel, which may deteriorate the design of the ferritic stainless steel. 2 It is preferable that the number of particles is 25 or less, and more preferably 22 or less per one. In this case, the lightness of the surface of the ferritic stainless steel is improved, and the designability can be maintained at a good level. In this embodiment, "lightness" refers to the CIE 1976 lightness L measured by using a D65 light source in a diffuse lighting system, receiving light at a direction of 8° with respect to the normal line of the surface of the ferritic stainless steel, with a viewing angle of 10° and a measurement time of 1 second. * means...
[0056] When the diameter D of oxides containing 5 mass% or more of Al or Si on the surface of ferritic stainless steel is less than 0.1 μm, the effect of improving red scale resistance by the oxides is low. Therefore, in this embodiment, the target is oxides having a diameter D of 0.1 μm or more. On the other hand, among oxides containing 5% or more by mass of Al or Si, the presence of oxides having a diameter D exceeding 2.0 μm may reduce the brightness of the surface of the ferritic stainless steel, which may deteriorate the design properties of the ferritic stainless steel. Therefore, it is preferable to control the number of oxides containing 5% or more by mass of Al or Si and having a diameter D of 0.1 μm or more and 2.0 μm or less on the surface of the ferritic stainless steel to within a specified range.
[0057] In addition, on the surface of ferritic stainless steel, there are few oxides that contain 5 mass% or more of Al or Si and have a diameter D exceeding 2.0 μm (for example, 93 μm 2 It is preferable that the number of grains per grain is 5 or less, and it is most preferable that the grains are absent. In this case, the brightness of the surface of the ferritic stainless steel can be improved, and the design of the ferritic stainless steel can be improved.
[0058] The present inventors have focused on Al / Si-based oxides on the surface of ferritic stainless steel and have discovered that by controlling the number of Al / Si-based oxides within a predetermined range, it is possible to realize a ferritic stainless steel with excellent red scale resistance.
[0059] In addition to the Al / Si oxides, a passive film is present on the surface of the ferritic stainless steel according to this embodiment with a thickness of 2.0 to 8.0 nm. The passive film is a very dense and highly adhesive film made of hydrated chromium oxyhydroxide and chromium oxide, mainly composed of Cr.
[0060] The thickness of the passive film can be determined using a high-frequency glow discharge optical emission spectrometer (GDS). Specifically, a GDS analyzer (e.g., HORIBA GD-Profiler2 or an equivalent device) is used to analyze the oxygen concentration at 2.5 nm pitches from the surface in the thickness direction, and the passive film is determined by measuring its thickness from the surface to the position where the oxygen concentration is half the peak value. For example, other GDS measurement conditions are as follows: Gas replacement time: 200 seconds, Pre-sputtering time: 30 seconds, Background: 5 seconds, Depth: 1.01μm, Pressure: 600Pa, Output: 35W, Effective value: 8.75W, Module: 8V, Phase: 4V, Frequency: 100Hz Duty Cycle: 0.25.
[0061] In the ferritic stainless steel according to this embodiment, when used at high temperatures in the presence of water vapor, Al / Si oxides grow and reduce the oxygen partial pressure around the Al / Si oxides. As a result, unlike ordinary ferritic stainless steel, the generation of Fe oxides, which are the main component of red scale, is reduced, and the surface morphology has an increased generation of Cr, Al, and Si oxides, resulting in excellent red scale resistance. For example, after being held in an atmosphere of 300 to 900°C for 100 hours or more, the following formula (2) is satisfied in the range from the surface to 1.0 μm (surface layer), where the Cr content is [Cr], the Si content is [Si], and the Al content is [Al], all in unit mass%. [Cr] + [Si] + [Al] ≧ 18.0…(2) If formula (2) is not satisfied, it is believed that the surface is dominated by Fe-based oxides, i.e., excessive red scale is formed. [Cr]+[Si]+[Al] is preferably 20.0 (mass %) or more.
[0062] There is no need to limit the Cr content [Cr], Si content [Si], and Al content [Al] within the range from the surface to 1.0 μm, but from the standpoint of the effect of suppressing red scale, it is preferable that the Si content and / or Al content is each 3.0 mass% or more.
[0063] In a high-temperature atmosphere, Al / Si oxides grow gradually up to a certain time, but after 100 hours or more, there is no significant change, and it is believed that the states of Cr, Si, and Al also do not change significantly. In other words, when the ferritic stainless steel according to this embodiment is used as a component such as an exhaust gas path component, a stove combustion equipment component, a fuel cell component, or a plant-related material, it is considered that the Cr, Al, and Si contents in the surface layer satisfy formula (2). On the other hand, even if the above-mentioned holding is performed, the chemical composition at the 1 / 4 depth position does not change.
[0064] <<Exhaust gas parts>> The exhaust gas component according to the present embodiment is obtained by processing the ferritic stainless steel according to the present embodiment as a raw material. Therefore, the exhaust gas component according to the present embodiment has a chemical composition at the stage obtained by processing or the like (before being used as a component) of 0.05% to 2.50% by mass of Si, 0.05% to 1.50% by mass of Mn, 0.025% by mass or less of C, 0.040% by mass or less of P, 0.003% by mass or less of S, 0.025% by mass or less of N, 0.01% to 0.50% by mass of Ni, 1.0% by mass or less of Zn, 0.01% by mass or less of Fe, 0.02% by mass or less of H, 0.03% by mass or less of H, 0.02% by mass or less of H, 0.03% by mass or less of H, 0.04% by mass or less of H, 0.05% by mass or less of H ...5% by mass or less of H, 0.06% by mass or less of H, 0.07% by mass or less of H, 0.08% by mass or less of H, 0.09% by mass or less of H, 0.1% by mass or less of H, 0.1% by mass or less of H, 0.2% by mass or less of H, 0.2% by mass or less of H, 0.3% by mass or less of H, 0.4% by mass or less of H, 0.5% by mass or less of H, 0.6 0.50 mass% or more and 25.00 mass% or less of Cr, 0.01 mass% or more and 1.80 mass% or less of Cu, 0.002 mass% or more and 0.200 mass% or less of Al, 0.001 mass% or more and 1.00 mass% or less of Nb, 0 mass% or more and 2.5 mass% or less of W, 0 mass% or more and 3.00 mass% or less of Mo, 0 mass% or more and 0.500 mass% or less of Ti, 0 mass% or more and 0.0100 mass% or less of B, 0 mass% or more and 0 0.0030% by mass or less Ca, 0% by mass or more and 0.50% by mass or less Hf, 0% by mass or more and 0.40% by mass or less Zr, 0% by mass or more and 0.50% by mass or less Sb, 0% by mass or more and 0.30% by mass or less Co, 0% by mass or more and 1.0% by mass or less Ta, 0% by mass or more and 1.00% by mass or less Sn, 0% by mass or more and 0.30% by mass or less Ga, 0% by mass or more and 0.50% by mass or less V, 0% by mass or more and 0.003% by mass or less Mg, and 0% by mass or more and 0.20% by mass or less REM, with the balance being Fe and impurities, and at least one of an oxide containing 5% by mass or more of Al and an oxide containing 5% by mass or more of Si is present on the surface, and the number of oxides present on the surface having a diameter D represented by the following formula (1) of 0.1 μm or more and 2.0 μm or less is 93 μm 2 There are 10 or more per prize. D = (Dmax + Dmin) / 2 (1) In the formula (1), Dmax is the maximum diameter of the oxide on the surface, and Dmin is the minimum diameter of the oxide on the surface. Furthermore, the surface is measured using a D65 light source in a diffuse illumination mode at an angle of 8° to the normal to the surface, with a CIE 1976 lightness L measured at a viewing angle of 10° and a measurement time of 1 second. * In some cases, the number is 60 or more. In addition, after the exhaust gas part according to this embodiment is held in an atmosphere of 300 to 900°C for 100 hours or more, the following formula (2) is satisfied in the range from the surface to 1.0 μm, where [Cr] is the Cr content, [Si] is the Si content, and [Al] is the Al content, all in unit mass %: [Cr] + [Si] + [Al] ≧ 18.0…(2) In other words, the exhaust gas part according to this embodiment is, for example, an exhaust gas path component, a stove combustion equipment, a fuel cell component, or a plant-related material, and when used for a certain period of time under normal conditions for such applications (after use), in the range from the surface to 1.0 μm, the following formula (2) is satisfied, where the Cr content is [Cr], the Si content is [Si], and the Al content is [Al], all in unit mass %. [Cr] + [Si] + [Al] ≧ 18.0…(2)
[0065] In both the ferritic stainless steel according to this embodiment and the exhaust gas component according to this embodiment, the Cr content [Cr], Si content [Si], and Al content [Al] in the range from the surface to a depth of 1.0 μm can be measured using GDS. Specifically, the analysis area is φ4 mm, and all elements contained in each steel are selected and measured at 2.5 nm pitches up to a depth of 1.0 μm, except for C and N. From the measurement results, the contents of Cr, Al, and Si are calculated at the positions where Cr, Al, and Si each show a peak within the range of 1.0 μm deep.
[0066] <<Method of manufacturing ferritic stainless steel>> Conventional methods for improving red scale resistance include surface polishing as a finishing process to promote Cr diffusion in the steel and encourage the production of Cr oxides, or forming a hot-dip galvanized layer on the surface.
[0067] The present inventors have found that the number of Al / Si oxides on the surface is 93 μm by the following manufacturing method, for example. 2 It has been found that a ferritic stainless steel having excellent red scale resistance and having 10 or more particles per square inch can be obtained.
[0068] The ferritic stainless steel according to one embodiment of the present invention is obtained, for example, as a ferritic stainless steel strip. Fig. 1 is a flow chart showing an example of a method for producing a ferritic stainless steel according to this embodiment. As shown in Fig. 1, the method for producing a ferritic stainless steel strip according to this embodiment includes a pretreatment step S1, a hot rolling step S2, an annealing step S3, a first pickling step S4, a cold rolling step S5, a final annealing step S6, a nitric acid electrolysis step S7, and a final pickling step S8. The preferred conditions for each step will be described below. For conditions not described below, known conditions can be used.
[0069] <Pretreatment process> In the pretreatment step S1, first, a melting furnace in a vacuum or argon atmosphere is used to melt steel having a chemical composition adjusted to fall within the range of the present invention described above, and the steel is cast to produce a slab. Then, a slab piece for hot rolling is cut out from the slab. The slab piece is then heated to a temperature range of 1100°C to 1300°C in an air atmosphere. The time for which the slab piece is heated and held is not limited. When the pretreatment step is carried out industrially, the casting may be continuous casting.
[0070] <Hot rolling process> The hot rolling step S2 is a step of producing a hot rolled steel strip of a predetermined thickness by hot rolling the slab (steel ingot) obtained in the pretreatment step S1. The hot rolling conditions are not limited and may be adjusted according to the required mechanical properties, etc.
[0071] <Annealing process> The annealing step S3 is a step for softening the hot-rolled steel strip obtained in the hot rolling step S2 by heating the steel strip. This annealing step S3 is a step that is performed as necessary, and does not necessarily have to be performed.
[0072] <First pickling process> The first pickling step S4 is a step in which scale adhering to the surface of the steel strip is washed off using a pickling solution such as hydrochloric acid or a mixture of nitric acid and hydrofluoric acid.
[0073] <Cold rolling process> The cold rolling step S5 is a step in which the steel strip that has been descaled in the first pickling step S4 is further rolled to a thinner thickness.
[0074] <Final annealing process> The final annealing step S6 is a step in which the steel strip that has been thinly rolled in the cold rolling step S5 is heated to remove distortion and soften the steel strip. 3 O 4 or Cr 2 O 3 This is a process for forming an inner oxide, which is an oxide of Al or Si, etc., together with an outer oxide such as SiO2. For the above purpose, the annealing in the final annealing step S6 is performed at a temperature of about 900 to 1100° C. for a time period of 30 to 90 seconds depending on the alloy components in an atmosphere of air or a combustion gas such as liquefied combustion gas (LNG).
[0075] <Nitric acid electrolysis process> The nitric acid electrolysis step S7 is a step in which the steel strip obtained in the final annealing step S6 is electrolyzed in an aqueous nitric acid solution. In the nitric acid electrolysis step S7, oxides adhering to the surface of the steel strip are partially removed. Specifically, the surface of the steel strip obtained in the final annealing step S6 is provided with, for example, (Fe, Cr) 3 O 4 or Cr 2 O 3An outer oxide layer such as aluminum or silicon is formed between the outer oxide layer and the base material. In the nitric acid electrolysis step S7, nitric acid electrolysis is performed under conditions that remove most of the outer oxide layer while leaving most of the inner oxide. Although most of the inner oxide remains, it is preferable that some of the inner oxide peels off to be easily removed in the final pickling step S8.
[0076] The nitric acid concentration in the nitric acid electrolysis step S7 is preferably 150 g / L or less. In this case, after the final pickling step S8, a 93 μm thick film is formed on the surface of the steel strip. 2 It is easy to leave 10 or more Al / Si oxide particles per unit area. On the other hand, if more Al / Si-based oxides than necessary remain, the brightness of the surface decreases. Therefore, in order to keep the amount of Al / Si-based oxides on the surface after the final pickling step within a preferred range, the nitric acid concentration in the nitric acid electrolysis step S7 is preferably 100 g / L or more. In order to efficiently remove the outer layer oxides in a short time, the nitric acid concentration in the nitric acid electrolysis step S7 is preferably 130 g / L or more.
[0077] The solution temperature in the nitric acid electrolysis step S7 is preferably 70° C. or less, more preferably 60° C. or less. In this case, after the final pickling step S8, a 93 μm thick layer is formed on the surface of the steel strip. 2 It is easy to leave 10 or more Al / Si oxide particles per unit area. On the other hand, the solution temperature in the nitric acid electrolysis step S7 is preferably 50° C. or higher, and more preferably 60° C. or higher, in which case the outer oxide layer can be efficiently removed in a short time.
[0078] The current density in the nitric acid electrolysis step S7 is 150 mA / cm 2 In this case, after the final pickling step S8, the surface of the steel strip is preferably 93 μm or less. 2 It is easy to leave 10 or more Al / Si oxide particles per unit area. On the other hand, the current density in the nitric acid electrolysis step S7 is 100 mA / cm 2It is preferable that the current is 120mA / cm or more. 2 More preferably, it is 130 mA / cm or more. 2 It is more preferable that the above-mentioned condition is satisfied. In this case, the outer oxide layer can be efficiently removed in a short period of time.
[0079] The electrolysis time in the nitric acid electrolysis step S7 is more preferably 120 seconds or less. In this case, after the final pickling step S8, a 93 μm thick layer is formed on the surface of the steel strip. 2 It is possible to leave 10 or more Al / Si oxide particles per one sample. On the other hand, the electrolysis time in the nitric acid electrolysis step S7 is preferably 60 seconds or more, which can reliably remove most of the outer oxide layer, while making part of the inner oxide easily peelable, and can keep the amount of remaining Al / Si-based oxides in a preferred range after the final pickling step.
[0080] <Final pickling process> The final pickling step S8 is a step in which the steel strip after the nitric acid electrolysis step S7 is immersed in a pickling solution such as a mixture of nitric acid and hydrofluoric acid. In the final pickling step S8, the inner oxides that peeled off in the nitric acid electrolysis step S7 are removed. As a result, a 93 μm thick oxide film is formed on the surface of the steel strip. 2 It is possible to improve the brightness by removing more than necessary Al / Si-based oxides while securing 10 or more Al / Si-based oxides per unit area.
[0081] As described above, in the conventional technology, a finishing step such as polishing or forming a plating layer is further performed as a finishing step to improve red scale resistance. However, such a finishing step requires the introduction of a new device for the finishing step, which increases the manufacturing cost. From this viewpoint, there is a demand for a manufacturing method for manufacturing a ferritic stainless steel having excellent red scale resistance without increasing the manufacturing cost.
[0082] In the above-described manufacturing method according to this embodiment, since equipment commonly used in pickling processes can be used in the nitric acid electrolysis process S7 and the final pickling process S8, a ferritic stainless steel with excellent red scale resistance can be realized without increasing manufacturing costs.
[0083] <Manufacturing method for exhaust gas parts> The exhaust gas component according to this embodiment is obtained by processing the above-mentioned ferritic stainless steel according to this embodiment into a predetermined component shape by a known processing method.
[0084] <Example> Examples of the present invention are described below. First, using the components shown in Table 1 below as raw materials, the steps up to the final annealing step S6 of the above-mentioned manufacturing method were all carried out under the same conditions, followed by the nitric acid electrolysis step S7 for the electrolysis time shown in Table 2, and then the final pickling step S8, to produce ferritic stainless steel.
[0085] In this example, the composition of each stainless steel shown in Table 1 is shown in mass %. The balance other than each component shown in Table 1 is Fe and impurities. The underlines in Table 1 indicate that the range of each component contained in each stainless steel according to the comparative example of the present invention is outside the range of the present invention.
[0086] [Table 1]
[0087] As shown in Table 1, ferritic stainless steels produced so that their chemical compositions were within the range of the present invention were designated as steel types A1 to A10. Ferritic stainless steels produced so that their chemical compositions were outside the range of the present invention were designated as steel types B1 to B3.
[0088] Table 2 shows the conditions used to manufacture steel materials No. 1 to 46 using steel types A1 to A10 and steel types B1 to B3, and the evaluation results of each steel material. The conditions used to manufacture each steel material shown in Table 2 are as follows.
[0089] · Atmosphere of the melting furnace in the pretreatment step S1: Vacuum · Mass of the slab pieces produced in the pretreatment step S1: 30 kg · Heating temperature of the slab pieces in the pretreatment step S1: 1230 °C · Heating time of the slab pieces in the pretreatment step S1: 2 hours · Plate thickness after the hot rolling step S2: 4 mm · Annealing step S3 not performed · Pickling solution used in the first pickling step S4: Nitrofluoric acid solution (aqueous solution with fluoride acid concentration: 30 g / L and nitric acid concentration: 100 g / L) · Liquid temperature in the first pickling step S4: 40 - 50 °C · Plate thickness after the cold rolling step S5: 1.5 mm · Annealing temperature in the final annealing step S6: 900 - 1100 °C (changed according to the alloy composition) · Annealing time in the final annealing step S6: 60 seconds · Annealing atmosphere in the final annealing step S6: Air · Nitric acid concentration in the nitric acid electrolysis step S7: 150 g / L · Liquid temperature in the nitric acid electrolysis step S7: 50 - 70 °C · Current density in the nitric acid electrolysis step S7: 150 mA / cm 2 · Electrolysis time in the nitric acid electrolysis step S7: 30 - 180 seconds (shown in Table 2) · Pickling solution used in the final pickling step S8: Nitrofluoric acid solution (aqueous solution with fluoride acid concentration: 20 g / L and nitric acid concentration: 70 - 80 g / L) · Liquid temperature in the final pickling step S8: 40 - 50 °C
[0090]
Table 2
[0091] For steel materials No.1 - 46, the number of Al / Si - based oxides was measured by the method described in detail below. The measurement results are shown in Table 2.
[0092] <Number of Al / Si - based oxides> The number of Al / Si oxides on the surface of the steel material was measured as follows. First, a scanning electron microscope (SEM) SU5000 (manufactured by Hitachi High-Technologies Corporation) was used to take SEM photographs of the surface of the steel material at a magnification of 10,000 times. The dimensions of one field of view were 8.34 μm vertical × 11.2 μm horizontal, and the area of one field of view was 93 μm. 2 In addition, elemental analysis of the oxide composition was performed using an energy dispersive X-ray spectroscopy (EDS) for electron microscopes (manufactured by Horiba, Ltd.) at an accelerating voltage of 15 kV and an analysis time of 60 seconds.
[0093] The captured SEM photographs were subjected to image analysis using the image analysis software “Photoshop (registered trademark)” (manufactured by Adobe Co., Ltd.) to calculate the number of oxides containing 5 mass% or more of Al or Si and having a diameter D of 0.1 μm or more and 2.0 μm or less, i.e., the number of Al / Si-based oxides.
[0094] The thickness of the passive film was measured by the method described above. Although not shown in the table, the thickness of the passive film was 2.0 to 8.0 nm.
[0095] 2A and 2B show examples of SEM photographs taken by the above method. As shown in FIG. 2A, the number of Al / Si-based oxides present on the surface of steel material No. 6, which is an example of the invention, was 10 or more per visual field. In contrast, as shown in FIG. 2B, the number of Al / Si-based oxides present on the surface of steel material No. 8, which is a comparative example, was less than 10 per visual field. In the SEM photograph of steel material No. 6, it appears that there are 30 or more oxides in one visual field. However, the number of oxides containing 5 mass% or more of Al or Si and having a diameter D of 0.1 μm or more and 2.0 μm or less, i.e., Al / Si-based oxides, was 19 per visual field.
[0096] As shown in Table 2, in the steel materials Nos. 1 to 3, 5 to 7, 9 to 11, 13 to 15, 17 to 19, 21 to 23, 25 to 27, 29 to 30, 32 to 33, 35, and 36, which were steel types A1 to A10 and had electrolysis times of 30 to 120 seconds, the number of Al / Si-based oxides having a diameter D of 0.1 μm or more and 2.0 μm or less was 93 μm. 2 There were more than 10 per person. On the other hand, in the steel materials Nos. 4, 8, 12, 16, 20, 24, 28, 31 and 34, which were electrolysis timed for 180 seconds, the number of Al / Si oxide particles was 93 μm. 2 There were less than 10 per
[0097] On the other hand, in the case of steel type B1 or B2, the number of Al / Si oxide particles was 93 μm in all of steel materials No. 37 to 42. 2 There were less than 10 per
[0098] In the case of steel type B3, steels No. 43 and No. 44, in which the electrolysis time was 40 to 60 seconds, had an Al / Si oxide particle size of 93 μm. 2 The number of Al / Si oxide particles was 93μm or more for steel No. 45 and No. 46, which were steel type B3 and had an electrolysis time of 120 to 180 seconds. 2 There were less than 10 per
[0099] <Oxidation increase (red scale resistance evaluation)> Furthermore, for steel materials Nos. 1 to 46, in order to evaluate the red scale resistance, the oxidation weight gain of the steel materials was measured as follows in accordance with JIS Z 2281:1993 (high temperature continuous oxidation test method for metallic materials). First, a test piece measuring 20 mm x 25 mm was cut from each steel material. The test piece was heated continuously for 100 hours at 600°C in an atmospheric environment with a water vapor concentration of 10 vol%, simulating the situation of burning petroleum fuel. The oxidation weight gain was calculated from the change in mass before and after the test. The standard for evaluating red scale resistance is an oxidation gain of 0.20 mg / cm 2 If the measured value was less than or equal to the above, it was determined that the sample had excellent red scale resistance.
[0100] As shown in Table 2, the number of Al / Si oxide particles was 93 μm for steel types A1 to A10. 2 Steel Nos. 1-3, 5-7, 9-11, 13-15, 17-19, 21-23, 25-27, 29-30, 32-33, 35, and 36, which had 10 or more particles per square meter, had an oxidation gain of 0.20 mg / cm 2 Therefore, it was shown that these steel materials have good red scale resistance.
[0101] On the other hand, even in the steel types A1 to A9, the number of Al / Si oxides is 93 μm 2 Steel Nos. 4, 8, 12, 16, 20, 24, 28, 31 and 34, which had less than 10 particles per cm, had an oxidation gain of 0.20 mg / cm. 2 Therefore, it was shown that these steels have low red scale resistance.
[0102] In addition, the steel type is B1 or B2, and the number of Al / Si oxide particles is 93 μm 2 Steel Nos. 37 to 42, which had less than 10 particles per cm, had an oxidation gain of 0.20 mg / cm 2 Therefore, it was shown that these steels have low red scale resistance.
[0103] In steel type B3, regardless of the number of Al / Si oxides, the oxidation mass gain was 0.20 mg / cm for all steels No. 43 to 46. 2 Therefore, these steels were shown to have low red scale resistance. It is presumed that steel type B3 had low red scale resistance because the Al content was as low as 0.001 mass%, even though the number of Al / Si oxide particles was 10 or more.
[0104] <Surface morphology after long-term testing> In order to evaluate the oxide morphology on the surface after the long-term test, the Cr, Si, and Al contents were measured at random locations on the test pieces of steel Nos. 1 to 4, 13 to 16, 32 to 34, and 37 to 39, among the test pieces evaluated for the above-mentioned oxidation weight gain (red scale resistance evaluation), using a glow discharge spectroscopy (GDS) (HORIBA GD-Profiler2). The analysis area was φ4 mm, and measurements were made at 2.5 nm intervals from the surface to a depth of 1.0 μm. The elements analyzed were all elements other than C and N contained in each steel at random locations and were measured. Other GDS measurement conditions were as follows: Gas replacement time: 200 seconds, Pre-sputtering time: 30 seconds, Background: 5 seconds, Depth: 1.01μm, Pressure: 600Pa, Output: 35W, Effective value: 8.75W, Module: 8V, Phase: 4V, Frequency: 100Hz Duty Cycle: 0.25. After the measurements, the contents of Cr, Al, and Si at the positions where they each showed a peak up to a depth of 1.0 μm were substituted into formula (2) to perform calculations and confirm whether they were satisfactory. The value of the left side of formula (2) ([Cr] + [Si] + [Al]) is shown in the table.
[0105] As shown in Table 2, the oxidation gain was 0.20 mg / cm 2 or less, and Nos. 1 to 3, 13 to 15, and 32 to 33, which had high red scale resistance, satisfied formula (2). On the other hand, the oxidation gain is 0.20 mg / cm 2 Moreover, Nos. 4, 16, 34 and 37 to 39, which had low red scale resistance, did not satisfy formula (2).
[0106] <lightness> In order to evaluate the design of the steel materials, the brightness of the surface of steel materials Nos. 1 to 46 was measured in the following manner. Using a spectrophotometer (model: CM-700d, manufactured by Konica Minolta), white calibration was performed at room temperature of 23°C, and then the lightness L * The evaluation criteria were: lightness L * A rating of 60 or higher was deemed to be of excellent design.
[0107] As shown in Table 2, the lightness L of steels No. 2-4, 6-8, 10-12, 14-16, 18-20, 22-24, 26-28, 29-31 and 33-34, which were steels A1-A10 and had electrolysis times of 60 seconds to 180 seconds, was * The results showed that these steel materials have good design properties.
[0108] On the other hand, in the steels A1 to A9, steels No. 1, 5, 9, 13, 17, 21, 25, and 32, in which the electrolysis time was 30 to 40 seconds, the lightness L * was less than 60.
[0109] (Additional Notes) The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
Claims
1. The chemical composition is: 0.05% by mass or more and 2.50% by mass or less of Si; 0.05% by mass or more and 1.50% by mass or less of Mn, 0.025% by weight or less of C, 0.040% by weight or less of P, 0.003% by weight or less of S; 0.025% by weight or less of N, 0.01% by mass or more and 0.50% by mass or less of Ni; 10.50% by mass or more and 25.00% by mass or less of Cr; 0.01% by mass or more and 1.80% by mass or less of Cu, 0.002% by mass or more and 0.200% by mass or less of Al; 0.001% by mass or more and 1.00% by mass or less of Nb, 0% by mass or more and 2.5% by mass or less of W; Mo, from 0% by mass to 3.00% by mass Ti, from 0% by mass to 0.500% by mass; B, 0% by mass or more and 0.0030% by mass or less of Ca, Hf of 0 mass% or more and 0.50 mass% or less, 0% by mass or more and 0.40% by mass or less of Zr; Sb, 0% by mass or more and 0.30% by mass or less of Co, Ta, from 0% by mass to 1.0% by mass 0% by mass or more and 1.00% by mass or less of Sn, Ga, from 0% by mass to 0.30% by mass; V, 0% by mass or more and 0.50% by mass or less; 0% by mass or more and 0.003% by mass or less of Mg, and REM: 0% by mass or more and 0.20% by mass or less The balance includes Fe and impurities, At least one of oxides containing 5 mass % or more of Al and oxides containing 5 mass % or more of Si is present on the surface, and the number of oxides having a diameter D represented by the following formula (1) of 0.1 μm or more and 2.0 μm or less among the oxides present on the surface in the observation field of view is 93 μm 2 There are 10 or more per Ferritic stainless steel. D=(Dmax+Dmin) / 2...(1) Here, in the formula (1), Dmax is the maximum diameter of the oxide on the surface, and Dmin is the minimum diameter of the oxide on the surface.
2. The surface is measured using a D65 light source in a diffuse illumination mode, receiving light at a direction of 8° to the normal to the surface, with a viewing angle of 10° and a measurement time of 1 second. * is 60 or more, The ferritic stainless steel according to claim 1.
3. The chemical composition is 0.01% by mass or more and 2.5% by mass or less of W; 0.01% by mass or more and 3.00% by mass or less of Mo; 0.001% by mass or more and 0.500% by mass or less of Ti; 0.0002% by mass or more and 0.0100% by mass or less of B; 0.0002% by mass or more and 0.0030% by mass or less of Ca; Hf of 0.001% by mass or more and 0.50% by mass or less, 0.01% by mass or more and 0.40% by mass or less of Zr; 0.005% by mass or more and 0.50% by mass or less of Sb; 0.01% by mass or more and 0.30% by mass or less of Co; Ta of 0.001% by mass or more and 1.0% by mass or less, 0.002% by mass or more and 1.00% by mass or less of Sn, 0.0002% by mass or more and 0.30% by mass or less of Ga; 0.01% by mass or more and 0.50% by mass or less of V; 0.0003% by mass or more and 0.003% by mass or less of Mg, and REM: 0.001% by mass or more and 0.20% by mass or less Contains one or more of the following: The ferritic stainless steel according to claim 1 or 2.
4. After being held in an atmosphere of 300 to 900 ° C. for 100 hours or more, in the range from the surface to 1.0 μm, the following formula (2) is satisfied, where the Cr content is [Cr], the Si content is [Si], and the Al content is [Al], in unit mass%, The ferritic stainless steel according to any one of claims 1 to 3. [Cr]+[Si]+[Al]≧18.0…(2)
5. In the range from the surface to 1.0 μm, when the Cr content is [Cr], the Si content is [Si], and the Al content is [Al], the following formula (2) is satisfied: Ferritic stainless steel. 36.7≧[Cr]+[Si]+[Al]≧18.0…(2)
6. An exhaust gas component comprising the ferritic stainless steel according to any one of claims 1 to 5.
Citation Information
Patent Citations
Ferritic stainless steel bright annealed material excellent in rust resistance and its production
JP1999050202A
Ferritic stainless steel for hydrocarbon fuel reformer
JP2003160842A
Ferritic stainless steel for alcohol-base fuel reformer apparatus
JP2003160844A
Al-PLATED STEEL SHEET FOR EXHAUST GAS PASSAGEWAY MEMBER OF MOTORCYCLE AND MEMBER
JP2009035755A
Ferritic stainless steel sheet for part of urea SCR system and method for production thereof