Polyester film and its manufacturing method

A polyester film with controlled crystallinity and improved tear resistance is achieved through a low-temperature stretching process, addressing breakage issues during manufacturing and winding.

JP7584560B2Active Publication Date: 2024-11-15MICROWORKS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023073404
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-28
Filing Date
2023-04-27
Publication Date
2024-11-15
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The rapid crystallization of polycyclohexylene dimethylene terephthalate (PCT) during the stretching process of polyester film manufacturing leads to easy breakage and winding issues, making it difficult to control the degree of crystallinity and resulting in film breakage.

Method used

A polyester film with controlled crystallinity of 36% or less, achieved through a manufacturing process involving low-temperature stretching and preheating, using a composition of polycyclohexylene dimethylene terephthalate resin with specific molecular ratios and additives, and controlled stretching ratios and temperatures.

Benefits of technology

The film exhibits improved tear resistance and breakage resistance, suitable for various applications due to its low crystallinity and controlled manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584560000002
    Figure 0007584560000002
  • Figure 0007584560000001
    Figure 0007584560000001
Patent Text Reader

Abstract

To provide a polyester film having improved breakage resistance and a method for producing the same.SOLUTION: There are provided: a polyester film containing a polycyclohexylenedimethylene terephthalate resin, wherein the crystallinity measured by differential scanning calorimetry is 36% or less, the tear strength in the machine direction is 250 kg / cm or more and 350 kg / cm or less, the tear strength in the width direction is 300 kg / cm or more and 400 kg / cm or less and the tear strength is measured according to ASTM D1004; and a method for producing the same.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiments relate to a polyester film having improved break resistance and a method for producing the same. [Background technology]

[0002] In the manufacturing process of polyester film, the stretching process is carried out at a temperature above the glass transition temperature (Tg). However, polycyclohexylene dimethylene terephthalate (PCT), a type of polyester, crystallizes very quickly, so it is not easy to adjust the crystallinity when used as a film. As a result, problems can arise where the film breaks easily when stretched due to the rapid crystallization, or when wound onto a roll.

[0003] Therefore, in the production of PCT films, it is necessary to devise an improved method for controlling the crystallinity and ensuring the breakage resistance.

[0004] The above-mentioned background art is technical information that the inventor possessed for the purpose of deriving the embodiments or that he / she acquired in the process of deriving the embodiments, and is not necessarily publicly known art that was disclosed to the general public prior to the filing of the present application.

[0005] Related prior art includes "Polyester film, method for producing polyester film, polarizing plate, and image display device" disclosed in International Publication No. WO2015 / 046122. Summary of the Invention [Problem to be solved by the invention]

[0006] It is an object of the embodiments to provide a polyester film having improved resistance to breakage.

[0007] Another object of the present embodiment is to provide a method for manufacturing a polyester film that minimizes the occurrence of breakage. [Means for solving the problem]

[0008] In order to achieve the above object, the polyester film according to the embodiment has: Contains polycyclohexylene dimethylene terephthalate resin, The crystallinity as measured by a differential scanning calorimeter is 36% or less; The tear strength in the machine direction is 240 kg / cm or more and 350 kg / cm or less, The tear strength in the width direction is 280 kg / cm or more and 400 kg / cm or less, The tear strength may be measured according to ASTM D1004.

[0009] In one embodiment, the polyester film comprises: The crystallinity is 33% or less, The tear strength in the machine direction is 280 kg / cm or more, The tear strength in the width direction may be 307 kg / cm or more.

[0010] In one embodiment, the polyester film may have a thickness of 10 μm to 500 μm.

[0011] In one embodiment, the polycyclohexylene dimethylene terephthalate resin includes a repeating unit derived from a dicarboxylic acid compound and a repeating unit derived from a diol compound, The repeating unit derived from the dicarboxylic acid compound contains 80 mol % to 100 mol % of a terephthalic acid residue and 0 mol % to 20 mol % of an isophthalic acid residue, The repeating units derived from the diol compound may contain 85 mol % to 100 mol % of cyclohexanedimethanol residues.

[0012] In order to achieve the above object, a method for producing a polyester film according to an embodiment includes: A sheet forming step of melting and extruding a film-making composition comprising a polycyclohexylene dimethylene terephthalate resin to form a sheet; a MD stretching step of stretching the extruded sheet in the machine direction; and a TD stretching step in which the sheet subjected to the MD stretching step is stretched in the width direction and heat-set to produce a polyester film. The MD stretching step includes a preheating process of preheating the extruded sheet, and an MD stretching process of stretching the preheated sheet in the machine direction, The temperature of the preheating process is 80°C to 87°C. The stretching temperature in the MD stretching process is 80°C to 89°C, The MD stretching step includes a heating process of applying heat to the extruded sheet via an infrared heater, The polyester film is The crystallinity as measured by a differential scanning calorimeter is 36% or less; The tear strength in the machine direction is 240 kg / cm or more and 350 kg / cm or less, The tear strength in the width direction is 280 kg / cm or more and 400 kg / cm or less, The tear strength may be measured according to ASTM D1004.

[0013] In an embodiment, the composition for preparing a film may further include an electrostatic agent and an antioxidant.

[0014] In one embodiment, the stretching temperature in the TD stretching step may be 100°C to 125°C.

[0015] In one embodiment, the heat setting temperature in the TD stretching step may be 200°C to 250°C.

[0016] In one embodiment, the MD stretching step has a machine direction stretching ratio of 2.5 times to 3.5 times; The stretching ratio in the transverse direction in the TD stretching step may be 3.3 times to 4.5 times.

[0017] In one embodiment, the infrared heater in the heating process is an upper heater spaced a predetermined distance from an upper portion of the sheet, and a lower heater spaced a predetermined distance from a lower portion of the sheet, The surface temperature of the upper heater is 450°C to 800°C. The surface temperature of the lower heater may be 350°C to 700°C. Effect of the Invention

[0018] The polyester film according to the embodiment has a relatively low crystallinity and excellent break resistance, and therefore has the advantage of being applicable in various fields.

[0019] The method for producing a polyester film according to the embodiment may produce a polyester film having low crystallinity and excellent break resistance through low-temperature stretching and preheating in the machine direction. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram related to the tear strength metrics of the experimental examples. BEST MODE FOR CARRYING OUT THEINVENTION

[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS One or more exemplary embodiments will now be described in detail with reference to the accompanying drawings in order to enable those of ordinary skill in the art to easily make and use the present invention. However, the exemplary embodiments may be embodied in many different forms and are not limited to the embodiments set forth herein. Like reference numerals are used throughout the specification to refer to like parts.

[0022] In this specification, when a certain configuration "includes" another configuration, this does not mean to exclude the other configurations, unless specifically stated to the contrary, but rather means that the other configurations may also be included.

[0023] In this specification, when a certain component is said to be "connected" to another component, this includes not only the case where the component is "directly connected" but also the case where the component is "connected via another component between them."

[0024] In this specification, the term "B is located on A" means that B is located on A in direct contact therewith, or that B is located on A with another layer located therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.

[0025] As used herein, the term "combinations thereof" contained in a Markush form expression means a mixture or combination of one or more selected from the group of components set forth in the Markush form expression, and is meant to include one or more selected from the group of components.

[0026] In this specification, the phrase "A and / or B" means "A, B, or A and B."

[0027] In this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from each other, unless otherwise specified.

[0028] In this specification, the term "singular" is to be construed as including the singular or plural as the context requires, unless otherwise specified.

[0029] Polyester Film In order to achieve the above object, the polyester film according to the embodiment has Contains polycyclohexylenedimethylene terephthalate resin, The crystallinity as measured by a differential scanning calorimeter is 36% or less; The machine direction (MD) tear strength is 240 kg / cm or more and 350 kg / cm or less, The tear strength in the transverse direction (TD) is 280 kg / cm or more and 400 kg / cm or less, The tear strength is measured in accordance with ASTM D1004.

[0030] The polycyclohexylenedimethylene terephthalate (PCT) resin of the polyester film may be a copolymer of a dicarboxylic acid compound and a diol compound, and may contain residues and repeating units derived therefrom.

[0031] The polyester film may contain terephthalic acid residues in an amount of 80 mol% or more, or 90 mol% or more, or 100 mol% or less, or 99 mol% or less, and may contain isophthalic acid residues in an amount of 20 mol% or less, or 10 mol% or less, or 0 mol% or more, 1 mol% or more, or 2 mol% or more, based on 100 mol% of the total repeating units derived from dicarboxylic acid compounds.

[0032] The polyester film may contain cyclohexanedimethanol residues in an amount of 70 mol % or more, 80 mol % or more, or 90 mol % or more to 100 mol % or less, based on 100 mol % of all repeating units derived from diol compounds.

[0033] When the dicarboxylic acid compound-derived repeating units include terephthalic acid residues and isophthalic acid residues in the above amounts, the copolymer may have a relatively high melting point and low crystallization properties.

[0034] The repeating unit derived from the diol compound may include a repeating unit derived from the following compounds other than the repeating unit derived from the cyclohexanedimethanol, such as ethylene glycol, 1,3-propanediol, 1,2-octanediol, 1,3-octanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 2-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,1-dimethyl-1,5-pentanediol, and residues derived therefrom.

[0035] The polycyclohexylene dimethylene terephthalate resin may have a weight average molecular weight (Mw) of 30,000 g / mol to 50,000 g / mol, or 30,000 g / mol to 40,000 g / mol.

[0036] The polycyclohexylene dimethylene terephthalate resin may be used with a catalyst to improve the efficiency of the polymerization reaction.

[0037] The catalyst may be contained in an amount of 0.1 ppm to 500 ppm, or 0.5 ppm to 100 ppm, based on 100 parts by weight of polycyclohexylene dimethylene terephthalate.

[0038] The catalyst may be a titanium-based compound, an antimony-based compound, a germanium-based compound, an aluminum-based compound, or a mixture thereof. Exemplarily, the catalyst may be a titanium-based compound. The titanium-based compound may include titanium tetraisopropoxide.

[0039] An antioxidant may be added to the polymerization of the polycyclohexylene dimethylene terephthalate resin. The antioxidant may be added as necessary for the purpose of suppressing thermal oxidation at the temperature at which the esterification reaction proceeds. However, the antioxidant is generally applied in an appropriate amount. Adding an excessive amount of antioxidant during polymerization may slow down the reaction and may cause a decrease in the intrinsic viscosity of the produced resin. Antioxidants that affect the polymerization of the resin are consumed during the polymerization process and may be distinguished from antioxidants added during the subsequent production of a film.

[0040] The antioxidant may include a phenol-based antioxidant, a phosphorus-based antioxidant, a sulfur-based antioxidant, and the like.

[0041] The antioxidant may be contained in an amount of 0.01 part by weight to 1 part by weight based on 100 parts by weight of the polycyclohexylene dimethylene terephthalate.

[0042] When a film is manufactured using the polycyclohexylene dimethylene terephthalate resin, a static electricity applying agent may be applied. The static electricity applying agent may be an alkali metal salt, an alkaline earth metal salt, or the like, or may be a magnesium-based compound or a calcium-based compound, and for example, magnesium acetate, calcium acetate, or the like may be applied.

[0043] The electrostatic applying agent may contain a metal or metal ion in an amount (by weight) of 300 ppm to 1000 ppm based on 100 parts by weight of the polycyclohexylene dimethylene terephthalate resin.

[0044] In the polyester film, the machine direction (MD) is the longitudinal direction parallel to the direction of movement during the film production process, and the transverse direction (TD) is the direction perpendicular to the machine direction.

[0045] The polyester film may have a crystallinity of 36% or less, 34% or less, 33% or less, or 31.1% or less, as measured by a differential scanning calorimeter. The crystallinity may be 10% or more. The polyester film has such a crystallinity so that it is not easily broken when wound up or applied to a product. The measurement of the crystallinity using a differential scanning calorimeter may be performed by the method of the experimental example described below.

[0046] The polyester film may have a machine direction tear strength of 240 kg / cm or more, 250 kg / cm or more, 270 kg / cm or more, or 280 kg / cm or more, and may have a machine direction tear strength of 350 kg / cm or less, or 340 kg / cm or less.

[0047] The polyester film may have a tear strength in the width direction of 280 kg / cm or more, 290 kg / cm or more, 300 kg / cm or more, 307 kg / cm or more, or 331 kg / cm or more. The tear strength in the width direction may be 400 kg / cm or less, or 390 kg / cm or less.

[0048] The polyester film has such tear strength in the machine direction and width direction, so that it does not easily break when wound up or applied to a product, and can ensure excellent durability.

[0049] The tear strength can be measured in accordance with ASTM D1004, and can be measured through the method of the experimental examples described below.

[0050] The thickness of the polyester film may be from 10 μm to 500 μm, or from 20 μm to 300 μm.

[0051] The polyester film has an advantage of being excellent in break resistance since it is produced through a specific low-temperature stretching process in the production method described below.

[0052] Manufacturing method of polyester film In order to achieve the above object, the present invention provides a method for producing a polyester film, comprising: A sheet forming step of melting and extruding a film-making composition comprising a polycyclohexylene dimethylene terephthalate resin to form a sheet; a MD stretching step of stretching the extruded sheet in the machine direction; and a TD stretching step in which the sheet subjected to the MD stretching step is stretched in the width direction and heat-set to produce a polyester film. The MD stretching step includes a preheating process of preheating the extruded sheet, and an MD stretching process of stretching the preheated sheet in the machine direction, The temperature of the preheating process is 80°C to 87°C. The stretching temperature in the MD stretching process is 80°C to 89°C, The MD stretching step may include a heating process of applying heat to the extruded sheet via an infrared heater.

[0053] The composition for producing the film in the sheet forming step may include an electrostatic agent and an antioxidant. The electrostatic agent and the antioxidant are the same as those described above for the polyester film, so a duplicate description will be omitted.

[0054] The composition for producing a film may be subjected to a drying treatment before being melted, and the drying may be performed at a temperature of 150°C or less, and may be performed at a temperature of 70°C to 148°C.

[0055] The film-producing composition may be dried so that the total moisture content is 100 ppm or less, or 50 ppm or less. If the drying process is performed at a temperature higher than 150° C., the resin itself may undergo an unintended color change.

[0056] The composition for producing a film may be in the form of chips, pellets, plates, etc., and may be in a form that can be easily added to the film production process and effectively mixed.

[0057] The polycyclohexylene dimethylene terephthalate resin of the film-producing composition can be produced by a conventional polymerization method, and for example, a method in which a polymerization reaction is carried out in the presence of a metal-containing catalyst such as titanium or antimony may be used.

[0058] The polycyclohexylene dimethylene terephthalate resin of the film-producing composition may be a copolymer of a dicarboxylic acid compound and a diol compound, as described above, and may contain repeating units derived therefrom.

[0059] The extrusion in the sheet forming step may be carried out at a temperature of 230°C to 300°C, or may be carried out at a temperature of 250°C to 290°C.

[0060] In the preheating process of the MD stretching step, the sheet may be heat-treated at a temperature of 80° C. to 87° C. for 0.5 seconds to 2 minutes, or may be heat-treated at a temperature of 80° C. to 86° C. for the same period as above.

[0061] In the MD stretching process of the MD stretching step, the sheet that has been preheated may be stretched in the machine direction by 2.5 to 3.5 times at a temperature of 80°C to 89°C, or may be stretched in the machine direction by the same magnification as above at a temperature of 80°C to 87°C or 80°C to 85°C.

[0062] The MD stretching step may include a process of performing a heat treatment using an infrared heater at a position 30 mm to 200 mm away from the upper and / or lower part of the unstretched sheet that has been preheated. The surface temperature of the infrared heater installed on the upper part of the unstretched sheet may be 450°C to 800°C, or 500°C to 700°C.

[0063] The MD stretching step can be performed through the preheating process and the MD stretching process so that the film produced meets the desired break resistance.

[0064] The stretching in the TD stretching step may be performed by stretching 3.3 to 4.5 times in the width direction at a temperature of 100°C to 125°C, or may be performed by stretching in the width direction at the same magnification as above at a temperature of 102°C to 115°C or 105°C to 112°C.

[0065] The TD stretching step may further include a preheating step before stretching. The preheating step may be performed at a temperature of 90°C to 108°C for 0.5 seconds to 5 minutes, or may be performed multiple times by increasing or decreasing the temperature by 0.1°C to 5°C.

[0066] The heat setting in the TD stretching step may be performed at a temperature of 200° C. to 250° C. for 5 to 600 seconds, or for 10 to 200 seconds.

[0067] The film that has undergone the TD stretching step may be subjected to a predetermined relaxation treatment in the longitudinal direction and / or the width direction. The temperature during relaxation may be 150°C to 250°C, and the relaxation rate may be 1% to 10%, or 3% to 7%.

[0068] The present invention will be described in more detail with reference to the following specific examples. The following examples are merely illustrative for the purpose of aiding understanding of the present invention, and are not intended to limit the scope of the present invention.

[0069] Example 1 A monomer mixture of 100 mol% cyclohexanedimethanol (CHDM) as a diol compound, and 96 mol% terephthalic acid (TPA) and 4 mol% isophthalic acid (IPA) as dicarboxylic acid compounds was added to a stirrer, and a titanium catalyst was added in an amount of 1 ppm based on 100 parts by weight of the mixture, and then an ester exchange reaction was carried out at 285°C.

[0070] The transesterified material was transferred to a separate reactor equipped with a vacuum facility and polymerized at 290° C. for 160 minutes to obtain polycyclohexylene dimethylene terephthalate (PCT) resin.

[0071] 98% by weight of the chips containing the PCT resin and 2% by weight of the chips containing an antioxidant and an electrostatic applying agent were processed into master batch chips and dried at a temperature of 140° C. The raw material was then put into an extruder, extruded into a sheet at a temperature of about 295° C., and cast onto a casting roll.

[0072] The extruded sheet was preheated at 80° C. for 10 seconds and then stretched 3.2 times in the machine direction (MD) at 80° C. When stretching in the machine direction, a heating process was added using infrared heaters installed at the top and bottom, each 80 mm away from the top and bottom of the film, with the surface temperature of the top heater being 500° C. and the surface temperature of the bottom heater being 400° C. Next, the sheet was stretched 3.5 times in the transverse direction (TD) at 110° C. The stretched sheet was then heat-set at 230° C. for about 30 seconds and relaxed to produce a PCT film with a thickness of 40 μm.

[0073] Example 2 In Example 1, the surface temperature of the upper heater was changed to 700° C. and the surface temperature of the lower heater was changed to 600° C. to prepare a PCT film.

[0074] Example 3 In Example 1, the preheating temperature before stretching in the machine direction and the stretching temperature were changed to 85° C. to prepare a PCT film.

[0075] Example 4 In Example 1, the surface temperature of the upper heater was changed to 700° C., the surface temperature of the lower heater was changed to 600° C., and the preheating temperature before stretching in the machine direction and the stretching temperature were changed to 85° C. to prepare a PCT film.

[0076] Comparative Example 1 In Example 1, the preheating temperature before stretching in the machine direction and the stretching temperature were changed to 95° C. to prepare a PCT film.

[0077] Comparative Example 2 In Example 1, the preheating temperature before stretching in the machine direction and the stretching temperature were changed to 95° C., the surface temperature of the upper heater was changed to 700° C., and the surface temperature of the lower heater was changed to 600° C., to prepare a PCT film.

[0078] Experimental Example 1 - Measurement of crystallinity The crystallinity of the films prepared in the examples and comparative examples was measured using a differential scanning calorimetry (DSC-Q2000, TA instruments). Specifically, 5 mg of the film obtained in each example and comparative example was placed in an aluminum pan, sealed after compression, and heated in a reactor from room temperature to 350°C at a rate of 10°C / min, cooled to -70°C, and then heated again to room temperature at a rate of 10°C / min. When the phase transition of the sample occurred, the degree of heat absorption and heat release was confirmed by the amount of current through a platinum resistor sensor in the reactor, and the crystallinity was calculated by applying the enthalpy to the following formula, and is shown in Table 1.

[0079] Crystallinity (%) = (△H / △HO) × 100% Here, ΔH is the heat of fusion of the produced PCT copolymer (J / g), and ΔHO is the heat of fusion of a PCT resin having 100% crystallinity.

[0080] Experimental Example 2 - Tear strength measurement From the films prepared in the examples and comparative examples, samples were prepared according to the ASTM D1004 standard. The shape of the sample was 101.6 mm x 19.0 mm in size and had a right-angled groove in the center, as shown in Figure 1. The tear strength of the sample was measured at a tensile speed of 100 mm / min using an Instron UTM4520 device, and the results are shown in Table 1.

[0081] Experimental Example 3 - Breakability Measurement In the manufacturing process of the above Examples and Comparative Examples, the degree of breakage during stretching in the width direction was indicated as ◯ if good, and × if breakage was present. The breakage resistance during winding on a winder was measured on a scale of 10 points, with 0.5 points subtracted if breakage occurred for each winding cycle. The results are shown in Table 1.

[0082] [Table 1]

[0083] Referring to Table 1, it can be seen that the examples in which the machine direction preheating and stretching processes were performed at a relatively low temperature have low crystallinity and at the same time excellent tear strength in the machine direction and width direction, and also have good break resistance even when wound multiple times.

[0084] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention.

Claims

1. A composition comprising only polycyclohexylene dimethylene terephthalate resin as a resin, The crystallinity as measured by a differential scanning calorimeter is 36% or less; The machine direction tear strength is 240 kg / cm or more and 350 kg / cm or less, The tear strength in the width direction is 280 kg / cm or more and 400 kg / cm or less, The tear strength was measured according to ASTM D1004 for biaxially oriented polyester films.

2. The degree of crystallinity is 33% or less, The tear strength in the machine direction is 280 kg / cm or more, 2. The biaxially oriented polyester film according to claim 1, wherein the tear strength in the transverse direction is 307 kg / cm or more.

3. 2. The biaxially oriented polyester film according to claim 1, having a thickness of 10 μm to 500 μm.

4. The polycyclohexylene dimethylene terephthalate resin contains a repeating unit derived from a dicarboxylic acid compound and a repeating unit derived from a diol compound, The repeating unit derived from the dicarboxylic acid compound contains 80 mol % to 100 mol % of a terephthalic acid residue and 0 mol % to 20 mol % of an isophthalic acid residue, 2. The biaxially stretched polyester film according to claim 1, wherein the repeating units derived from the diol compound contain 85 mol % to 100 mol % of cyclohexanedimethanol residues.

5. A sheet forming step of melting and extruding a film-producing composition containing only polycyclohexylene dimethylene terephthalate resin as a resin to form a sheet; an MD stretching step of stretching the extruded sheet in a machine direction; and a TD stretching step in which the sheet subjected to the MD stretching step is stretched in the width direction and heat-set to produce a polyester film. The MD stretching step includes a preheating process of preheating the extruded sheet, and an MD stretching process of stretching the preheated sheet in a machine direction, The temperature of the preheating process is 80°C to 87°C. The stretching temperature during the MD stretching process is 80° C. to 89° C. The MD stretching step includes a heating process of applying heat to the extruded sheet via an infrared heater, The polyester film is The crystallinity as measured by a differential scanning calorimeter is 36% or less; The machine direction tear strength is 240 kg / cm or more and 350 kg / cm or less, The tear strength in the width direction is 280 kg / cm or more and 400 kg / cm or less, The tear strength was measured according to ASTM D1004, Method for producing biaxially oriented polyester film.

6. The method for producing a biaxially oriented polyester film according to claim 5 , wherein the composition for producing a film further comprises an electrostatic agent and an antioxidant.

7. The method for producing a biaxially oriented polyester film according to claim 5, wherein the stretching temperature in the TD stretching step is 100°C to 125°C.

8. The method for producing a biaxially oriented polyester film according to claim 5, wherein the heat setting temperature in the TD stretching step is 200°C to 250°C.

9. The machine direction stretch ratio of the MD stretching step is 2.5 times to 3.5 times; The method for producing a biaxially oriented polyester film according to claim 5, wherein the stretching ratio in the transverse direction in the TD stretching step is 3.3 times to 4.5 times.

10. The infrared heater in the heating process is an upper heater spaced a predetermined distance from an upper portion of the sheet, and a lower heater spaced a predetermined distance from a lower portion of the sheet, The surface temperature of the upper heater is 450°C to 800°C. The method for producing a biaxially oriented polyester film according to claim 5, wherein the surface temperature of the lower heater is 350°C to 700°C.

Citation Information

Patent Citations

  • Electrical insulating material and film for metallizing

    JP1990196833A

  • Biaxial oriented laminated film, film for laminated glass, and laminated glass

    JP2005186613A

  • Improved heat-resistant transparent semi-crystalline article

    JP2015507074A