Solid fuel and its manufacturing method

A solid fuel with biomass char and inorganic binder addresses the strength issues of organic binders in high-temperature environments, offering stability in furnaces and reducing costs.

JP7584687B1Active Publication Date: 2024-11-15NIPPON STEEL & SUMIKIN ENGINEERING CO LTD +1

Patent Information

Application Number
JP2024008115
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-11-15
Estimated Expiration
2044-01-23

AI Technical Summary

Technical Problem

Existing carbon-containing molded products used as fuels face challenges with organic binders being expensive and lacking strength in high-temperature environments.

Method used

A solid fuel composed of biomass char with a fixed carbon content of 85% by mass or more and an inorganic binder with a CaO content of 50% by mass or more, which maintains strength in high-temperature environments.

Benefits of technology

The solid fuel provides sufficient strength in high-temperature environments, reducing the need for organic binders and enhancing stability in furnaces like gasification melting furnaces and cupolas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584687000001_ABST
    Figure 0007584687000001_ABST
Patent Text Reader

Abstract

To provide a solid fuel having sufficient strength in a high-temperature environment and a method for producing the same. [Solution] A solid fuel is provided that contains biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis and an inorganic binder having a CaO content of 50% by mass or more in a dry state.A method for producing a solid fuel is provided that includes a step of kneading and molding a molding raw material that contains biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis, an inorganic binder having a CaO content of 50% by mass or more in a dry state, and water to obtain a solid fuel.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid fuel and a method for producing the same. [Background technology]

[0002] As a means of reducing CO2 emissions to combat global warming, technological development is underway to use biomass instead of existing fossil fuels. Patent Document 1 proposes adding a binder to biomass charcoal, forming it, and then dry distilling it to obtain a carbon-containing molded product, instead of the coke used in waste melting treatment facilities. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2006-57082 A Summary of the Invention [Problem to be solved by the invention]

[0004] In Patent Document 1, when a carbon-containing molded product is used as a fuel, an organic binder is preferable. However, organic binders are generally expensive and have difficulty in maintaining their strength in a high-temperature environment. Therefore, the present disclosure provides a solid fuel having sufficient strength in a high-temperature environment and a method for producing the same. [Means for solving the problem]

[0005] One aspect of the present disclosure provides a solid fuel comprising a biomass char having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis and an inorganic binder having a CaO content of 50% by mass or more in a dry state. Since the solid fuel comprises a biomass char having a fixed carbon content of 85% by mass or more and an inorganic binder, the solid fuel has sufficient strength in a high-temperature environment.

[0006] One aspect of the present disclosure provides a method for producing a solid fuel, comprising a step of kneading and forming a forming raw material containing biomass carbide having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis, an inorganic binder having a CaO content of 50% by mass or more in a dry state, and water. This production method has sufficient strength in a high-temperature environment because it uses biomass carbide having a fixed carbon content of 85% by mass or more and an inorganic binder. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a solid fuel having sufficient strength in a high-temperature environment and a method for producing the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of an example of a gasification melting furnace and a waste melting treatment facility equipped with the same. [Diagram 2] FIG. 2 is a diagram for explaining a method for measuring hot strength and cold strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, exemplary embodiments of the present disclosure will be described with reference to the drawings. The following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following embodiments.

[0010] A solid fuel according to one embodiment includes biomass charcoal having a fixed carbon content of 88% by mass or more on an anhydrous ash-free basis, and an inorganic binder having a CaO content of 50% by mass or more in a dry state.

[0011] In this specification, biomass refers to biological resources other than fossil fuels. Examples of biomass include waste materials such as thinned wood, pruned branches, waste wood, bark chips, other wood, bamboo, grass, coconut shells, palm oil residue, vegetables, fruits, food residues, and sludge. Biomass may be wood-based biomass such as thinned wood, pruned branches, waste wood, bark chips, and other wood. Biomass carbonized material can be obtained by dry distilling such biomass.

[0012] The fixed carbon of biomass charcoal may be 85% by mass or more, 88% by mass or more, or 90% by mass or more on an anhydrous ash-free basis. Biomass charcoal with a high fixed carbon content has a low volatile content, and therefore has few components that volatilize even in high-temperature environments. Therefore, it is possible to sufficiently maintain strength even in high-temperature environments. The fixed carbon on an anhydrous ash-free basis can be calculated by converting the value of fixed carbon on an anhydrous basis measured in accordance with "8. Calculation method for fixed carbon mass fraction (%)" of JIS M 8812:2006 "Coals and cokes - Industrial analysis methods" into the value on an anhydrous ash-free basis.

[0013] The particle size of the biomass charcoal may be 10 mm or less, 2 mm or less, 0.5 to 2 mm, or 0.8 to 1.5 mm. If the particle size is too large, the adhesion between the particles of the biomass charcoal may decrease, resulting in a decrease in strength. If the particle size is too small, the contact area between the particles of the biomass charcoal may increase too much, resulting in a decrease in strength. The particle size of the biomass charcoal can be measured using a sieve. When sieved using a sieve with a mesh size of 2 mm, the particle size under the sieve is 2 mm or less.

[0014] The content of biomass char in the solid fuel is 50% by mass or more, and may be 60% by mass or more or 65% by mass or more. By increasing the content of biomass char, the calorific value of the solid fuel can be sufficiently increased. The content of biomass char in the solid fuel may be 90% by mass or less, 85% by mass or less, 80% by mass or less, or 75% by mass or less. Such a solid fuel can have higher strength in a high-temperature environment.

[0015] The inorganic binder is an inorganic substance that has the function of binding particles of biomass charcoal together. The inorganic binder has a CaO content of 50% by mass or more in a dry state. In a dry state, the CaO content in the inorganic binder may be 55% by mass or more, or 60% by mass or more. Such an inorganic binder can reduce the melting point of slag when used as a solid fuel in a gasification melting furnace or a cupola furnace. In these facilities, limestone may be used as an auxiliary material, and part or all of the limestone can be replaced by the inorganic binder CaO.

[0016] FIG. 1 shows a waste melting treatment facility 100 equipped with a coke-bed type melting furnace 40, which is an example of a gasification melting furnace. The solid fuel of this embodiment can replace the coke in such a melting furnace 40. The waste melting treatment facility 100 of FIG. 1 is equipped with a melting furnace 40 and a charging device 50 provided at the upper part of the melting furnace 40. The melting furnace 40 has a shaft section 42, a morning glory section 44 provided at the lower end of the shaft section 42, and a furnace bottom section 46 provided at the lower part of the morning glory section 44. From the shaft section 42 to the furnace bottom section 46, an upper stage tuyere 45 for the pyrolysis zone and a lower stage tuyere 47 for the combustion melting zone are provided in order from the top. The upper stage tuyere 45 and the lower stage tuyere 47 may each be provided in multiple stages.

[0017] The waste, solid fuel and auxiliary materials are charged into the melting furnace 40 by the charging device 50. Examples of the waste include general waste, industrial waste, incineration ash obtained by drying, incineration, crushing and other processes, and landfill waste containing soil and sand that is dug up after being buried in a landfill. The auxiliary materials may include at least one selected from limestone, iron ore, magnesia, periclase, kudoliite, jamonite, and the like. By using such auxiliary materials, the waste 48 can be sufficiently melted inside the melting furnace 40. Coal, coke, molded charcoal, and the like may be used together with the solid fuel of this embodiment.

[0018] Waste, solid fuel, and secondary materials are charged into the melting furnace 40 from the charging device 50. Oxygen or oxygen-enriched air is supplied from the lower tuyere 47, and air is supplied as a combustion support gas from the upper tuyere 45. The solid fuel charged into the melting furnace 40 is combusted by the oxygen or oxygen-enriched air supplied from the lower tuyere 47 and functions as a heat source. Waste 48 including secondary materials charged into the melting furnace 40 is heated to, for example, 1600°C or higher by the combustion of the solid fuel, and becomes pyrolysis residue 43. The pyrolysis residue 43 is combusted mainly by the air supplied from the upper tuyere 45.

[0019] The pyrolysis gas generated in the melting furnace 40 rises up the shaft 42 and is introduced into the combustion chamber through an exhaust gas pipe 52 connected to the bottom of the charging device 50. The combustion exhaust gas is burned as combustible gas, and the waste heat is recovered in a boiler. The exhaust gas then has its temperature adjusted in a cooling tower, passes through a dust collector and a catalytic reaction tower, and is discharged from a chimney.

[0020] Inside the melting furnace 40, a temperature gradient is generated by the combustion of solid fuel and the like. Specifically, the melting furnace 40 has, from top to bottom, a drying / preparation zone 40a, a pyrolysis zone 40b, and a combustion / melting zone 40c. The secondary materials introduced into the melting furnace 40 from the charging device 50 reach the drying / preparation zone 40a, the pyrolysis zone 40b, and the combustion / melting zone 40c, in that order, together with the waste and solid fuel. CaO and the like contained in the inorganic binder of the solid fuel reach the combustion / melting zone 40c.

[0021] The combustible matter in the waste 48 and the biomass charcoal contained in the solid fuel are gasified and rise inside the melting furnace 40, and are introduced into the combustion chamber via the exhaust gas pipe 52. Meanwhile, the ash becomes molten slag via the pyrolysis residue 43. The CaO and silica source contained in the inorganic binder function as a melting point adjuster and a basicity adjuster for the molten slag. The molten slag, whose melting point and basicity have been adjusted, flows down the coke packed layer 41 at the furnace bottom 46 and is discharged from the slag outlet 49.

[0022] The maximum temperature of the melting furnace 40 may be, for example, 1600°C or more in the combustion / melting zone 40c. The solid fuel charged from the charging device 50 has sufficient strength in a high-temperature environment, so it can maintain its shape for a while after being introduced into the melting furnace 40. During this time, the solid fuel is prevented from being pulverized, and the inorganic binder is prevented from scattering. As a result, CaO contained in the inorganic binder of the solid fuel functions sufficiently as a melting point adjuster and a basicity adjuster for the molten slag. The composition of the solid fuel charged from the charging device 50 and the amount of auxiliary materials may be adjusted so that the basicity (CaO / SiO2) of the molten slag discharged from the slag discharge port 49 of the melting furnace 40 is, for example, 0.7 to 1.0. As a result, molten slag with excellent fluidity is discharged from the slag discharge port 49.

[0023] The molten slag may be discharged from the slag discharge port 49 continuously (continuous slag discharge) or intermittently (intermittent slag discharge). The interval between slag discharges during intermittent slag discharge may be, for example, 30 minutes or more, or 1 hour or more. The molten slag discharged from the slag discharge port 49 may be introduced, for example, into a water granulation tank containing cooling water and granulated there.

[0024] In a cupola furnace, the solid fuel of this embodiment can be used instead of coke piled up in the furnace body. From above the solid fuel piled up to a certain height, metals such as pig iron and scrap steel and solid fuel are charged at a predetermined ratio. The solid fuel is burned while air is sent from a tuyere provided at the bottom of the furnace body, and the metals are melted by the combustion heat. The metals are melted in a melting zone in the center of the furnace body and discharged from a tapping port at the bottom. Since the solid fuel has sufficient strength in a high-temperature environment, a bed can be stably formed in the furnace body. Since CaO contained in the solid fuel functions as a melting point adjuster, the amount of auxiliary materials such as limestone used can be reduced.

[0025] The inorganic binder may contain Portland cement as specified in JIS R 5210:2009. Such a solid fuel can have a sufficiently high strength in a high-temperature environment and can sufficiently reduce the production cost. Examples of Portland cement include ordinary Portland cement, high-early-strength Portland cement, ultra-high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, and sulfate-resistant Portland cement. The CaO content in Portland cement can be measured in accordance with JIS R 5202:2010 "Chemical Analysis of Cement". When the inorganic binder contains Portland cement, the hot strength of the solid fuel can be sufficiently increased.

[0026] The inorganic binder may contain components other than Portland cement. Examples of the components include clay and sodium silicate. Examples of the clay include bentonite (montmorillonite) and kaolin. When the inorganic binder contains multiple types of components, the content of CaO in the inorganic binder as a whole may be within the above range.

[0027] The content of the inorganic binder in the solid fuel may be 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more. Such a solid fuel has higher strength in a high-temperature environment. The content of the inorganic binder in the solid fuel may be 45% by mass or less, 40% by mass or less, or 35% by mass or less. By reducing the content of the inorganic binder, the content of the biomass charcoal can be increased, thereby sufficiently increasing the calorific value of the solid fuel.

[0028] The solid fuel may contain components other than the biomass charcoal and the inorganic binder. Examples of such components include coke powder and an organic binder. When the solid fuel contains coke powder, the coke powder can be effectively used as a heat source. Examples of organic binders include polyvinyl alcohol, carboxymethyl cellulose, and starch. When the solid fuel contains an organic binder, the cold strength of the solid fuel (molded body) can be increased. This can improve the handleability immediately after molding.

[0029] The solid fuel is a compact obtained by compression molding. There is no limit to the size of each compact, and it can be, for example, 1 to 800 cm. 3 , 3~600cm 3 , or 50~200cm 3 When solid fuel of such a size is used as fuel for a gasification melting furnace and a cupola, a suitable fire grate can be formed, and the combustion condition in the furnace can be sufficiently stable.

[0030] The hot strength of the solid fuel is preferably 300N or more, more preferably 500N or more, further preferably 800N or more, and particularly preferably 1000N or more. Such a solid fuel can maintain a sufficiently high strength in a high-temperature environment. For example, when used as a solid fuel for a gasification melting furnace and a cupola, a suitable fire grate can be formed to sufficiently stabilize the combustion state in the furnace.

[0031] The hot strength and cold strength in this specification are measured by the following procedure. The solid fuel is heated in air at 1000°C for 30 minutes using an electric furnace. Then, it is cooled to room temperature (about 20°C) in a nitrogen atmosphere. When the solid fuel is cylindrical, after cooling, the solid fuel (sample 10) is placed on a measurement table 20 as shown in FIG. 2, and a load is applied in the direction of the arrow (radial direction). The load at which cracks or breaks occur in the sample 10 is taken as the hot strength (N). A solid fuel with high hot strength has sufficiently high strength in a high-temperature environment. Alternatively, a load is applied as shown in FIG. 2 to another sample 10 without heating using an electric furnace, and the load at which cracks or breaks occur in the sample 10 is taken as the cold strength (N).

[0032] Since the solid fuel of this embodiment contains biomass carbide, it is possible to reduce the consumption of fossil fuels and reduce carbon dioxide emissions. By using it as fuel for gasification melting furnaces and cupolas, it is possible to adjust the melting point of slag. In addition, it is possible to reduce the amount of limestone used as a secondary material.

[0033] A method for producing a solid fuel according to one embodiment includes a dry distillation step of dry distilling and carbonizing biomass to obtain a biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis, a crushing step of crushing the biomass charcoal, a molding step of kneading and molding a molding raw material containing the crushed biomass charcoal, an inorganic binder having a CaO content of 50% by mass or more in a dry state, and water, and a curing step of curing the molded body. The solid fuel obtained by this manufacturing method may be the solid fuel described in the above embodiment. Therefore, the contents described for the solid fuel are also applicable to this manufacturing method.

[0034] The carbonization step may be performed by heating the biomass to a carbonization temperature of 200°C or higher in an oxygen-free atmosphere. The ease with which carbonization of biomass proceeds varies depending on the species of tree and the part of the tree. Regardless of the species of biomass and the part of the tree, from the viewpoint of stably and smoothly proceeding with carbonization, the carbonization may be performed by heating the biomass to 250°C or higher, or may be performed by heating to 320°C or higher. From the viewpoint of increasing the yield of the carbon material, the carbonization step may be performed by heating the biomass to 900°C or lower, or 700°C or lower. That is, an example of the carbonization temperature is 200 to 900°C.

[0035] In the carbonization step, the time for heating to the above temperature range may be 20 minutes or more, or may be 30 minutes or more, from the viewpoint of sufficiently carbonizing the biomass. In the carbonization step, the time for heating to the above temperature range may be 3 hours or less, or may be 2 hours or less, from the viewpoint of improving the productivity of the biomass charcoal. The fixed carbon of the biomass charcoal can be adjusted by changing the carbonization temperature and the carbonization time.

[0036] In the pulverization step, the particle size of the biomass charcoal is adjusted. The pulverization may be performed using a pulverizing mill. The particle size of the biomass charcoal may be adjusted to the above-mentioned range. By performing the pulverization step after the carbonization step, the pulverization can be performed smoothly.

[0037] In the molding step, biomass charcoal, inorganic binder, water, and other optional components are mixed and kneaded to prepare a molding raw material. The optional components include coke powder, organic binder, and inorganic substances different from the inorganic binder. In the molding raw material, the mass ratio of water to the inorganic binder may be 0.5 or more, 0.7 or more, or 1.0 or more. This allows the strength of the solid fuel to be sufficiently high. From the same viewpoint, the mass ratio of water to the inorganic binder may be 3.0 or less, 2.5 or less, or 2.0 or less. From the same viewpoint, the mass ratio of water to the total of the biomass charcoal and the inorganic binder may be 15 to 65%, 20 to 60%, or 25 to 55%. This allows the inorganic binder to be sufficiently hardened even if the biomass charcoal absorbs a part of the water. After kneading, the molding raw material is molded to obtain a molded body. For molding, a normal molding machine such as a uniaxial pressure molding machine or a briquette roll can be used.

[0038] In the curing step, the inorganic binder contained in the compact is hardened to obtain a solid fuel. Appropriate curing conditions may be selected depending on the type of inorganic binder. For example, when the inorganic binder is Portland cement, curing may be performed by holding at 20 to 50°C for 4 hours or more, 6 hours or more, 10 hours or more, or 24 hours or more.

[0039] After the curing step, a drying step may be performed in an atmosphere having a higher temperature than that in the curing step, whereby the moisture content in the inorganic binder can be reduced, and a solid fuel having higher strength can be obtained.

[0040] The solid fuel obtained by the manufacturing method of this embodiment has sufficient strength in a high-temperature environment. Therefore, it is useful as fuel for a gasification melting furnace or a cupola, for example. In this case, the melting point of the slag can be adjusted. Also, the amount of limestone used as a secondary material can be reduced. Also, since biomass carbide is used, the consumption of fossil fuels can be reduced, and carbon dioxide emissions can be reduced.

[0041] Although the exemplary embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments. The application of the solid fuel is not limited to the gasification melting furnace and the cupola. The present disclosure includes the following embodiments.

[0042] [1] A solid fuel comprising: biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis; and an inorganic binder having a CaO content of 50% by mass or more in a dry state. [2] The solid fuel according to [1], wherein the content of the biomass carbonized material is 50% by mass or more, and the content of the inorganic binder is 15% by mass or more. [3] A solid fuel according to [1] or [2], having a hot strength of 1000 N or more when measured after heating in air at 1000°C for 30 minutes and then cooling. [4] The solid fuel according to any one of [1] to [3], wherein the inorganic binder contains Portland cement. [5] The solid fuel according to any one of [1] to [4], wherein the particle size of the biomass carbonized material is 10 mm or less. [6] The solid fuel according to any one of [1] to [5], further comprising at least one selected from the group consisting of carboxymethyl cellulose, polyvinyl alcohol, starch, sodium silicate, and clay. [7] The solid fuel according to any one of [1] to [6], further comprising coke powder. [8] A solid fuel according to any one of [1] to [7], which is for a gasification melting furnace or cupola and has a function of adjusting the melting point of slag. [9] A method for producing solid fuel, comprising a step of kneading and molding a raw material containing biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous ash-free basis, an inorganic binder having a CaO content of 50% by mass or more in a dry state, and water.

[10] The solid fuel described in [9], wherein the particle diameter of the biomass carbonized material is 10 mm or less.

[11] The method for producing a solid fuel according to [9] or

[10] , wherein the inorganic binder contains Portland cement.

[12] The method for producing a solid fuel according to any one of [9] to

[11] , wherein the hot strength of the solid fuel is 1000 N or more.

[13] The method for producing a solid fuel according to any one of [9] to

[12] , wherein the mass ratio of the water to the inorganic binder in the forming raw material is 0.5 or more.

[14] The method for producing a solid fuel according to any one of [9] to

[13] , wherein the forming raw material further contains at least one selected from the group consisting of carboxymethyl cellulose, polyvinyl alcohol, sodium silicate, and clay.

[15] The method for producing a solid fuel according to any one of [9] to

[14] , wherein the forming raw material further contains coke powder. EXAMPLES

[0043] The present disclosure will be described in more detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the following examples.

[0044] [Effect of fixed carbon in biomass charcoal] (Examples 1 to 4, Comparative Examples 1 to 4) Acacia and pine chips were prepared as biomass. Each chip was heated in an oxygen-free atmosphere in an electric furnace at about 700°C for 30 minutes for dry distillation, and then cooled under a nitrogen gas atmosphere. In this way, eight types of biomass charcoal with different fixed carbon contents were obtained. Each biomass charcoal was pulverized using a powder mill (CGOLDENWALL, model number: HC-2500) to adjust the particle size to 1 mm or less.

[0045] Proximate analysis of each biomass charcoal was carried out in accordance with JIS M 8812:2006 "Coals and cokes - Proximate analysis method". The results are shown in Table 1. The measurement results for fixed carbon and volatile matter are on an anhydrous and ash-free basis.

[0046] Each biomass charcoal, the particle size of which was adjusted to 1 mm or less, was mixed with commercially available high-early-strength Portland cement (manufactured by Tokuyama Corporation) in a mass ratio of 70:30, and water was added and mixed. The CaO content of the high-early-strength Portland cement was 65 mass%. At this time, the mass ratio of water to the high-early-strength Portland cement (water addition rate) was 1.1. After mixing, a cylindrical molded body (diameter x height = 50 mm x 50 mm) was produced using a uniaxial pressure molding machine. This molded body was cured at 40°C for one day to obtain a solid fuel.

[0047] The solid fuel was placed in an electric furnace and heated in air at 1000°C for 30 minutes. It was then cooled to about 20°C in a nitrogen atmosphere. This solid fuel (sample 10) was placed on a measurement table 20 as shown in Figure 2, and a load was applied in the direction of the arrow (radial direction) to measure the strength at the time when cracks or fractures occurred. The measurement results are shown in the "Hot strength" column of Table 1.

[0048] [Table 1]

[0049] As shown in Table 1, it was confirmed that solid fuel with high hot strength can be obtained by using biomass charcoal with a high fixed carbon content.

[0050] [Effect of inorganic binder content] (Examples 5 to 7) Solid fuels were prepared in the same manner as in Example 2, except that the blending ratio of each biomass charcoal to commercially available high-early-strength Portland cement was changed as shown in Table 2, and the hot strength of the solid fuels was measured. The results are shown in Table 2. For comparison, the results of Example 2 are also shown in Table 2.

[0051] (Examples 8 to 10) Solid fuels were prepared in the same manner as in Example 4, except that the blending ratio of each biomass charcoal to commercially available high-early-strength Portland cement was changed as shown in Table 2, and the hot strength of the solid fuels was measured. The results are shown in Table 2. Table 2 also shows the results of Example 4 for comparison.

[0052] [Table 2]

[0053] As shown in Table 2, it was confirmed that the hot strength could be increased by increasing the ratio of inorganic binder (high-early-strength Portland cement). By increasing the inorganic binder content in the solid fuel to 15 mass% or more, the hot strength of the solid fuel could be increased to 1000 N or more.

[0054] [Effect of particle size of biomass charcoal] (Examples 11 to 14) A solid fuel was produced in the same manner as in Example 2, except that the sieve used to sieve the biomass charcoal was changed and biomass charcoal having a particle size shown in Table 3 was used, and the hot strength of the solid fuel was measured. The results are shown in Table 3. For comparison, Table 3 also shows the results of Example 2.

[0055] (Examples 15 to 18) By varying the grinding time in the powder mill, biomass charcoal was prepared with the particle sizes shown in Table 3. Except for using biomass charcoal with such particle sizes, solid fuel was produced in the same manner as in Example 4, and the hot strength of the solid fuel was measured. The results are shown in Table 3. For comparison, the results of Example 4 are also shown in Table 3.

[0056] [Table 3]

[0057] As shown in Table 3, it was confirmed that the hot strength of the solid fuel can be adjusted by changing the particle size of the biomass charcoal. A solid fuel with the highest hot strength was obtained when the particle size of the biomass charcoal was 1 mm or less.

[0058] [Effect of water addition rate] (Examples 19 to 23) Solid fuel was prepared in the same manner as in Example 13, except that the mass ratio of water to high-early-strength Portland cement (water addition rate) was changed as shown in Table 4, and the hot strength of the solid fuel was measured. The results are shown in Table 4. Table 4 also shows the results of Example 13 for comparison.

[0059] (Examples 24 to 28) Solid fuel was prepared in the same manner as in Example 2, except that the mass ratio of water to high-early-strength Portland cement (water addition rate) was changed as shown in Table 4, and the hot strength of the solid fuel was measured. The results are shown in Table 4. Table 4 also shows the results of Example 2 for comparison.

[0060] [Table 4]

[0061] "Moisture" in Table 4 is the mass ratio of water to the total of biomass charcoal and high-early-strength Portland cement. As shown in Table 4, it was confirmed that the hot strength increases as the water addition rate increases to 1.1 and the moisture content increases to about 33 mass%.

[0062] [Effects of inorganic binder type and curing conditions] (Examples 29 to 31) Solid fuels were prepared in the same manner as in Example 2, except that the curing time of the compacts at 40°C was changed as shown in Table 5, and the hot strength of the solid fuels was measured. The results are shown in Table 5. For comparison, Table 5 also shows the results of Example 2.

[0063] (Examples 32 to 34) Solid fuel was prepared in the same manner as in Example 2, except that commercially available ordinary Portland cement (manufactured by Tokuyama Corporation) was used instead of high-early-strength Portland cement, and the curing time of the compact at 40°C was changed as shown in Table 5, and the hot strength of the solid fuel was measured. The results are shown in Table 5.

[0064] [Table 5]

[0065] The results in Table 5 confirm that even if the inorganic binder is ordinary Portland cement, if the curing time is extended, a solid fuel with sufficient strength in a high-temperature environment can be obtained.

[0066] [Effects of additives] (Examples 35 to 41) The following additives were prepared. All of them are commercially available products. Polyvinyl alcohol Carboxymethylcellulose ·starch Bentonite Kaolin Frog-eye clay ·Sodium silicate

[0067] The biomass charcoal used in Example 2 and commercially available high-early-strength Portland cement were blended in a mass ratio of 70:30, and water was added and kneaded. At this time, the above-mentioned additives were added in the addition ratios shown in Table 6. The addition ratios shown in Table 6 are mass ratios relative to the total of the biomass charcoal and high-early-strength Portland cement. The mass ratio of water to the high-early-strength Portland cement (water addition rate) was 1.1. A solid fuel was produced in the same manner as in Example 2 except that such forming raw materials were used, and the hot strength of the solid fuel was measured. The results are shown in Table 6. Example 2A in Table 6 is a solid fuel prepared in the same procedure as Example 2 without adding any additives.

[0068] In each example, the strength of the molded body was also measured immediately after molding and before curing at 40° C. for one day. The strength measurement results are shown in Table 7 as "cold strength." The units of values ​​in Tables 6 and 7 are "N."

[0069] The cold strength is the strength measured immediately after forming without heat treatment. As in the case of the hot strength, the cold strength was measured by placing the formed body (sample 10) on a measuring table 20 as shown in Fig. 2, applying a load in the direction of the arrow (radial direction), and measuring the strength at the time when a crack or break occurs.

[0070] [Table 6]

[0071] [Table 7]

[0072] As shown in Table 6, the addition of additives did not result in a significant change in hot strength. On the other hand, as shown in Table 7, it was confirmed that the inclusion of additives can significantly improve cold strength. This improves handling until the inorganic binder hardens. In particular, it was found that the cold strength was particularly high when polyvinyl alcohol, a type of organic binder, was added. [Explanation of symbols]

[0073] 10...sample, 20...measurement table, 40...melting furnace, 40a...drying / preheating zone, 40b...pyrolysis zone, 40c...combustion / melting zone, 41...coke packed bed, 42...shaft section, 43...pyrolysis residue, 44...morning glory section, 45...upper tuyere, 46...furnace bottom, 47...lower tuyere, 48...waste, 49...slag discharge port, 50...charging device, 52...exhaust gas pipe, 100...waste melting treatment equipment.

Claims

1. A solid fuel for a gasification melting furnace or cupola, comprising: biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous and ash-free basis; and an inorganic binder having a CaO content of 50% by mass or more in a dry state.

2. The solid fuel according to claim 1 , wherein the content of the biomass charcoal is 50% by mass or more, and the content of the inorganic binder is 15% by mass or more.

3. 3. The solid fuel according to claim 1 or 2, which has a hot strength of 1000 N or more as measured after heating in air at 1000° C. for 30 minutes and cooling.

4. The solid fuel according to claim 1 or 2, wherein the inorganic binder comprises Portland cement.

5. The solid fuel according to claim 1 or 2, wherein the particle size of the biomass charcoal is 10 mm or less.

6. 3. The solid fuel according to claim 1 or 2, further comprising at least one selected from the group consisting of carboxymethyl cellulose, polyvinyl alcohol, starch, sodium silicate, and clay.

7. The solid fuel according to claim 1 or 2, further comprising coke breeze.

8. A solid fuel as described in claim 1 or 2, having a function of adjusting the melting point of slag.

9. A method for producing solid fuel for a gasification melting furnace or cupola, comprising a step of kneading and molding a raw material containing biomass charcoal having a fixed carbon content of 85% by mass or more on an anhydrous and ash-free basis, an inorganic binder having a CaO content of 50% by mass or more in a dry state, and water.

10. The method for producing a solid fuel according to claim 9, wherein the particle size of the biomass charcoal is 10 mm or less.

11. The method for producing a solid fuel according to claim 9 or 10, wherein the inorganic binder comprises Portland cement.

12. The method for producing a solid fuel according to claim 9 or 10, wherein the hot strength of the solid fuel is 1000 N or more.

13. The method for producing a solid fuel according to claim 9 or 10, wherein a mass ratio of the water to the inorganic binder in the forming raw material is 0.5 or more.

14. The method for producing a solid fuel according to claim 9 or 10, wherein the forming raw material further contains at least one selected from the group consisting of carboxymethyl cellulose, polyvinyl alcohol, starch, sodium silicate, and clay.

15. The method for producing a solid fuel according to claim 9 or 10, wherein the forming raw material further comprises coke fines.

Citation Information

Patent Citations

  • Solid fuel

    JP1990073892A

  • Solidified coal washing sludge for fuel

    JP1994166882A

  • Method for producing solid fuel from waste

    JP1998501569A

  • Production of waste-solidified fuel

    JP1999302673A

  • Facility for producing solid fuel

    JP2000096070A

Cited By

  • Formed coal and method for producing formed coal

    WO2026177178A1