Ammonia decomposition catalyst and method for producing same, and method for producing hydrogen gas

By supporting ruthenium and rare earth oxides on a metal oxide carrier with optimized ratios and distributions, the catalyst addresses low temperature activity issues, enhancing ammonia decomposition efficiency and reducing costs.

JP7586219B2Active Publication Date: 2024-11-19RESONAC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023061899
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-26
Filing Date
2023-04-06
Publication Date
2024-11-19
Estimated Expiration
2039-03-11

AI Technical Summary

Technical Problem

Existing ammonia decomposition catalysts, such as those described in Patent Documents 1 to 3, lack sufficient activity at low temperatures, leading to high costs due to the use of expensive rare earth oxides.

Method used

A catalyst is developed by supporting ruthenium and a rare earth oxide on a metal oxide carrier, with specific ratios and distributions to enhance catalytic activity, including an eggshell type support for ruthenium to improve efficiency.

Benefits of technology

The catalyst achieves high activity in ammonia decomposition at low temperatures, reducing costs by minimizing the use of expensive rare earth metals and promoting efficient hydrogen gas production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586219000001
    Figure 0007586219000001
  • Figure 0007586219000002
    Figure 0007586219000002
Patent Text Reader

Abstract

To provide: an ammonia decomposition catalyst which can exhibit a high activity even at a lower temperature in an ammonia decomposition reaction; a method for producing the ammonia decomposition catalyst; and a method for producing a hydrogen gas using the ammonia decomposition catalyst.SOLUTION: An ammonia decomposition catalyst in which ruthenium and a rare earth oxide are carried on a carrier composed of a metal oxide other than the rare earth oxide and the content of the rare earth oxide is 0.1 to 30.0 mass% can be produced through step 1 and step 2, wherein the step 1 comprises allowing the rare earth oxide to be carried on the carrier and step 2 comprises allowing the ruthenium to be carried on the carrier produced in step 1 and having the rare earth oxide carried thereon. A hydrogen gas can be produced by decomposing ammonia using the ammonia decomposition catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ammonia decomposition catalyst that promotes a reaction for decomposing ammonia into hydrogen gas and nitrogen gas, a method for producing the same, and a method for producing hydrogen gas using the ammonia catalyst. [Background technology]

[0002] Hydrogen produces water when burned and does not produce carbon dioxide, a greenhouse gas, like common fossil fuels, so it has attracted attention as a clean energy source, and fuel cells that use hydrogen as fuel have been put to practical use in recent years. However, hydrogen is very light in gaseous state, making it difficult to transport, and a large amount of energy is required to liquefy it, resulting in high transportation costs.

[0003] To address this issue, a technology is known in which ammonia, which contains 1.5 molecules of hydrogen per molecule, is used as a hydrogen carrier, hydrogen gas and nitrogen gas are generated by catalytic decomposition of ammonia, and this hydrogen gas is extracted and used as an energy source. In order to generate hydrogen gas more efficiently, research and development is being conducted on catalysts that promote the decomposition reaction of ammonia at low temperatures below 600°C.

[0004] For example, Patent Document 1 describes an ammonia decomposition catalyst in which ruthenium is supported on an inorganic support such as α-alumina. Furthermore, Patent Document 2 describes that the ammonia decomposition rate can be improved by supporting ruthenium and an alkali metal or alkaline earth metal as a promoter on a support such as alumina. Furthermore, Patent Document 3 describes an ammonia decomposition catalyst that contains ruthenium and a rare earth oxide such as cerium oxide, and further contains 1 to 50 parts by mass of a refractory inorganic oxide such as aluminum oxide per 100 parts by mass of the rare earth oxide. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-84910 [Patent Document 2] JP 2011-78888 A [Patent Document 3] JP 2013-237045 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the catalysts described in the above Patent Documents 1 to 3 do not have sufficient activity in decomposing ammonia at low temperatures. In addition, as described in Patent Document 3, when the content of rare earth oxide is increased in order to increase the catalytic activity, the catalyst becomes expensive, which is a problem in that the cost of decomposing ammonia increases.

[0007] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide an ammonia decomposition catalyst that exhibits high activity even at low temperatures in an ammonia decomposition reaction, a method for producing the same, and a method for producing hydrogen gas using the ammonia decomposition catalyst. [Means for solving the problem]

[0008] The present invention is based on the discovery that in a catalyst containing ruthenium as an active metal, by supporting a rare earth oxide in addition to ruthenium on a carrier, the catalytic activity in an ammonia decomposition reaction is improved.

[0009] That is, the present invention provides the following [1] to

[16] . [1] An ammonia decomposition catalyst, in which ruthenium and a rare earth oxide are supported on a support made of a metal oxide other than a rare earth oxide, and the content of the rare earth oxide is 0.1 to 30.0 mass %. [2] The ammonia decomposition catalyst according to the above [1], wherein the metal oxide is at least one selected from the group consisting of alumina, zirconia and titania. [3] The ammonia decomposition catalyst according to the above [1] or [2], wherein the metal oxide is alumina. [4] The ammonia decomposition catalyst according to the above [2] or [3], wherein the alumina is alpha alumina. [5] The ammonia decomposition catalyst according to any one of the above [1] to [4], wherein the rare earth oxide is at least one selected from the group consisting of lanthanum oxide, cerium oxide, neodymium oxide and samarium oxide. [6] The ammonia decomposition catalyst according to any one of the above [1] to [5], wherein the rare earth oxide is neodymium oxide. [7] The ammonia decomposition catalyst according to any one of the above [1] to [6], wherein the ruthenium content is 0.1 to 10.0 mass %. [8] The ammonia decomposition catalyst according to any one of the above [1] to [7], wherein the support further supports one or more metals selected from alkali metals and alkaline earth metals. [9] The ammonia decomposition catalyst according to the above [8], wherein the content of the metal is 0.1 to 10.0 moles per mole of the ruthenium.

[10] The ammonia decomposition catalyst according to any one of the above [1] to [9], wherein the ruthenium is supported in an eggshell form.

[11] The ammonia decomposition catalyst according to the above

[10] , wherein the eggshell type has a shell portion, which is a distribution region of ruthenium, having a thickness of 10 to 300 μm.

[12] The ammonia decomposition catalyst according to the above

[11] , wherein a concentration of ruthenium in the shell portion is 0.1 to 15.0 mass % relative to 100 mass % of the constituent atoms of the shell portion.

[0010]

[13] A method for producing the ammonia decomposition catalyst according to any one of the above [1] to

[12] , comprising: step 1 of supporting a rare earth oxide on the support; and step 2 of supporting the ruthenium on the support supporting the rare earth oxide obtained in step 1.

[14] The method for producing an ammonia decomposition catalyst according to the above

[13] , wherein the step 2 comprises a step of immersing the support on which the rare earth oxide is supported in an aqueous solution of a ruthenium salt and then contacting the support with a basic aqueous solution.

[15] A method for producing an ammonia decomposition catalyst according to the above item

[13] or

[14] , further comprising a step of supporting one or more metals selected from alkali metals and alkaline earth metals on the support carrying the rare earth oxide obtained in step 1, or on the support carrying the rare earth oxide and ruthenium obtained in step 2.

[16] A method for producing hydrogen gas, comprising decomposing ammonia in the presence of the ammonia decomposition catalyst according to any one of the above [1] to

[12] to produce hydrogen gas. Effect of the Invention

[0011] According to the present invention, it is possible to provide an ammonia decomposition catalyst having improved catalytic activity in an ammonia decomposition reaction. Therefore, by using the ammonia decomposition catalyst of the present invention, it is possible to promote the ammonia decomposition reaction even at low temperatures, and it becomes possible to produce hydrogen gas at low cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the ammonia decomposition catalyst and its production method, as well as the method for producing hydrogen gas using the ammonia decomposition catalyst of the present invention will be described in detail. [Ammonia decomposition catalyst] The ammonia decomposition catalyst of the present invention (hereinafter also simply referred to as "catalyst") is characterized in that ruthenium and a rare earth oxide are supported on a carrier made of a metal oxide other than a rare earth oxide, and the content of the rare earth oxide is 0.1 to 30.0 mass %. The catalyst of the present invention exhibits high activity even at low temperatures in an ammonia decomposition reaction while reducing the amount of expensive rare earth metal used, and by using this catalyst, ammonia can be decomposed at low cost.

[0013] (Carrier) The support in the present invention is for supporting ruthenium and a rare earth oxide, and is made of a metal oxide other than a rare earth oxide. The metal oxide may be a metal oxide used as a general catalyst carrier. Examples of the metal oxide include alumina, silica, titania, zirconia, magnesia, iron oxide, zinc oxide, and tin oxide. The metal oxide may be used alone or in combination of two or more. Among these, alumina, zirconia, or titania is preferred, and alumina is more preferred. The type of alumina is not particularly limited, and examples include α-alumina, θ-alumina, and γ-alumina, and α-alumina is preferred. Since α-alumina has a smaller specific surface area than other types of alumina, the carrier surface can be covered even with a small amount of rare earth oxide supported on the carrier, and high catalytic activity can be maintained in the ammonia decomposition reaction.

[0014] Here, α-alumina refers to a crystal phase of alumina with a corundum type crystal structure, θ-alumina refers to a monoclinic crystal system, and γ-alumina refers to a defective spinel type crystal structure. The presence of the metal oxide in the catalyst can be confirmed by powder X-ray diffraction analysis (XRD).

[0015] The carrier is the main component contained in the largest amount among the components of the catalyst of the present invention, and the content in the components is preferably greater than the amount of the rare earth oxide to be supported, and is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 65% ​​by mass or more. The upper limit of the content of the carrier is not particularly limited, but is preferably 99% by mass or less, more preferably 97% by mass or less, taking into consideration the amount of ruthenium to be supported, etc. The content of the carrier can be determined by analyzing the component composition of the catalyst as described in the Examples below, and can also be estimated by calculation from the amounts of other components charged in the catalyst.

[0016] From the viewpoint of preventing a decrease in catalytic activity due to diffusion of ammonia gas within the pores, the support preferably has an average pore size of 5 nm or more, more preferably 8 to 200 nm, and further preferably 10 to 180 nm. The average pore diameter can be determined by a gas adsorption method, and is determined from the total pore volume and BET specific surface area measured by a specific surface area pore distribution measurement device. The average pore diameter in this specification is a value determined by the measurement method described in the examples described later.

[0017] The shape and size of the carrier are appropriately determined depending on the specifications of the device in which the ammonia decomposition reaction is carried out, the operating conditions, etc. The shape is, for example, powder, granule, sphere, pellet, etc. The size is, from the viewpoint of the pressure loss of the ammonia gas to be decomposed and the contact area with the catalyst, a particle size of 1 μm to 3 mm, more preferably 2 μm to 2.5 mm, and further preferably 3 μm to 2.5 mm. In the present specification, the particle size of the carrier is determined as the volume average particle size D50 using a laser diffraction particle size distribution analyzer. The values ​​in the following examples are catalog values.

[0018] (Rare Earth Oxides) Examples of rare earth oxides supported on the carrier include yttrium oxide, lanthanum oxide, cerium oxide, neodymium oxide, samarium oxide, gadolinium oxide, and ytterbium oxide. The rare earth oxides may be used alone or in combination of two or more. Among these, from the viewpoint of improving catalytic activity, those having a basicity of more than 600 μmol / g at 500° C. are preferred, specifically, lanthanum oxide, cerium oxide, neodymium oxide, or samarium oxide are preferred, and neodymium oxide is more preferred. The basicity can be measured by a temperature programmed desorption method using carbon dioxide as an acid probe molecule. The basicity of the rare earth oxide can be determined by referring to, for example, the values ​​described in “Applied Catalysis A: General”, vol. 356, 2009, pp. 57-63.

[0019] The content of the rare earth oxide in the catalyst of the present invention is 0.1 to 30.0 mass%, preferably 1.0 to 30.0 mass%, more preferably 3.0 to 29.0 mass%, further preferably 8.0 to 28.0 mass%, and particularly preferably 13.0 to 27.0 mass%. If the content is 0.1 mass% or more, it is sufficient to cover the support, and the catalytic activity in the ammonia decomposition reaction can be improved. Also, if the content is 30.0 mass% or less, the specific surface area of ​​the support due to the coating with the rare earth oxide is not significantly reduced, and the reduction in catalytic activity is suppressed. The content of the rare earth oxide in the catalyst is preferably 0.3 to 20.0 mass%, more preferably 0.5 to 10.0 mass%, when the metal oxide of the carrier is α-alumina, preferably 10.0 to 25.0 mass%, more preferably 12.0 to 21.0 mass%, when the metal oxide is θ-alumina, and preferably 10.0 to 30.0 mass%, more preferably 14.0 to 28.0 mass%, when the metal oxide is γ-alumina.

[0020] From the viewpoint of making the rare earth oxide easily contribute to the ammonia decomposition reaction, it is preferable that the rare earth oxide is distributed only on the surface of the support. When the impregnation method described below is used as the catalyst preparation method, the rare earth oxide is supported so as to cover the surface of the carrier. Therefore, unlike catalysts with high component uniformity such as those obtained by coprecipitation methods, the rare earth oxide is present substantially only on the surface of the carrier.

[0021] (ruthenium) Ruthenium is the metal species of the active component of the ammonia decomposition catalyst of the present invention, and is supported on the support together with a rare earth oxide. By supporting ruthenium in such a manner, the catalytic activity in the ammonia decomposition reaction can be improved. The content of ruthenium in the catalyst is an amount that provides sufficiently high catalytic activity and takes into consideration the cost of ammonia decomposition, and is preferably 0.1 to 10.0 mass%, more preferably 0.5 to 8.0 mass%, and even more preferably 1.0 to 7.0 mass%. The presence of metallic ruthenium in the catalyst can be confirmed by a transmission electron microscope (TEM).

[0022] Typical examples of the manner in which the active component of the catalyst is supported include uniform, eggshell, egg yoke, and egg white types. The uniform type is a mode in which the active component is uniformly distributed on the support. The eggshell type is also called the outer layer support type, and is a mode in which the active component is distributed in a predetermined thickness from the surface of the support to the inside, like an egg shell. The egg yoke type is a mode in which the active component is distributed in the core of the support, like an egg yolk. The egg white type is a mode in which the active component is distributed within a predetermined depth range inside the support surface, like an egg white.

[0023] In the catalyst of the present invention, the supporting form of ruthenium, which is an active component, may be any of the above-mentioned forms. However, from the viewpoint of suppressing the diffusion of ammonia gas into the pores of the support from becoming the reaction rate-limiting factor, the eggshell form is preferred. The eggshell catalyst has a region in which ruthenium is distributed at a predetermined concentration from the surface of the carrier to the inside, i.e., a shell portion, and the thickness of the shell portion is preferably 10 to 300 μm, more preferably 20 to 250 μm, and even more preferably 50 to 200 μm. Even if ruthenium is contained in a portion other than the shell portion, it is unlikely to contribute to the ammonia decomposition reaction, so it is preferable that ruthenium is not contained in a portion other than the shell portion, i.e., in a region inside the shell portion. The concentration of ruthenium in the shell portion is preferably 0.1 to 15.0 mass %, more preferably 0.5 to 10.0 mass %, and even more preferably 1.0 to 8.0 mass %, relative to 100 mass % of the constituent atoms of the shell portion.

[0024] The thickness of the shell part of the eggshell catalyst and the concentration of ruthenium in the shell part can be determined by measuring the cross section of the catalyst using an electron probe microanalyzer (EPMA) or a scanning electron microscope / energy dispersive X-ray spectrometer (SEM / EDX). In the present invention, the values ​​are determined by the measurement method described in the examples below.

[0025] (Alkaline metals and alkaline earth metals) The support may further support one or more metals selected from alkali metals and alkaline earth metals. These metals act as promoters for further accelerating the ammonia decomposition reaction in the catalyst of the present invention. Examples of the alkali metal include sodium, potassium, and cesium. Examples of the alkaline earth metal include calcium and barium. These metals may be used alone or in combination of two or more. Among these, sodium, potassium, or cesium is preferred, and potassium is more preferred.

[0026] When the catalyst contains the metal, the content of the metal is preferably 0.1 to 10.0 mol, more preferably 0.2 to 8.0 mol, and further preferably 0.5 to 5.0 mol, per mol of the ruthenium.

[0027] The composition of the catalyst can be determined by a general analysis method for metals, metal oxides, and metal salts. For example, an aqueous solution in which the catalyst is completely dissolved using an acid or base can be prepared, and each metal element can be quantitatively analyzed using an ICP (inductively coupled plasma) emission spectrometer. As a simple method, the remaining components in a container used for supporting a specific substance can be dissolved, the metal elements can be quantified by ICP emission spectrometer, and the composition of the catalyst can be determined from the difference between the amount of the metal elements contained in the raw material for supporting. The composition of the catalyst in the present invention is a value determined by the analysis method described in the examples described below.

[0028] [Method of manufacturing ammonia decomposition catalyst] The catalyst can be produced by a production method including step 1 of supporting the rare earth oxide on the support, and step 2 of supporting the ruthenium on the support supporting the rare earth oxide obtained in step 1.

[0029] (Process 1) In step 1, a rare earth oxide is supported on the support made of a metal oxide other than a rare earth oxide. This step can be carried out using a general catalyst preparation method for supporting a metal oxide. For example, an impregnation method can be used in which a solution of a rare earth compound is impregnated into the support, followed by drying and calcination.

[0030] The rare earth compound is a precursor of a rare earth oxide, and is not particularly limited, and examples thereof include salts such as nitrates, carbonates, and chlorides. Water-soluble nitrates are preferred.

[0031] The specific method of the impregnation method is not particularly limited, and can be, for example, a pore filling method, an evaporation to dryness method, or the like. For example, when an aqueous solution of rare earth nitrate is used, first, the amount of rare earth nitrate corresponding to the amount of rare earth oxide to be supported is determined based on the constituent rare earth metals. In the pore filling method, the above-mentioned amount of rare earth nitrate is dissolved in water with a water content equal to or less than the water absorption of the carrier measured in advance to prepare an aqueous solution, and the entire amount of this aqueous solution is impregnated into the carrier and then dried. The water absorption of the carrier is calculated by subtracting the mass of the dried carrier from the mass of the carrier that has absorbed water. The mass of the carrier that has absorbed water is the mass of the carrier that has been thoroughly immersed in water, and then the water (supernatant) attached to the surface of the carrier is separated using a sieve, filter paper, etc. In the evaporation to dryness method, the above-mentioned amount of rare earth nitrate is dissolved in a predetermined amount of water to prepare an aqueous solution, and the entire amount of this aqueous solution is added to the support while heating to evaporate the water, thereby supporting the rare earth oxide precursor on the support.

[0032] Alternatively, a method can be used in which a support is impregnated with an aqueous solution of a rare earth nitrate or a rare earth chloride, etc., and then a basic aqueous solution is added to form a water-insoluble rare earth hydroxide, which is then calcined to support the rare earth oxide on the support.

[0033] In the above impregnation method, drying and calcination can be carried out under general conditions used in catalyst preparation methods. The drying method is not particularly limited as long as the liquid can be sufficiently evaporated as a pretreatment for calcination. For example, when the carrier is impregnated with an aqueous solution, the carrier can be dried by heating the carrier in an air atmosphere at normal pressure to 80 to 130°C, preferably 90 to 120°C, more preferably 100 to 110°C. The calcination method is not particularly limited as long as the rare earth oxide precursor can be oxidized to the rare earth oxide. For example, when a rare earth nitrate is used, the rare earth oxide can be obtained by pyrolyzing the rare earth nitrate by calcination at 450 to 800°C, preferably 470 to 700°C, more preferably 480 to 600°C, under normal pressure.

[0034] (Process 2) In step 2, ruthenium is supported on the support carrying the rare earth oxide obtained in step 1. This step can be carried out using a general method for preparing a catalyst for supporting a metal. For example, a ruthenium compound solution is impregnated into the carrier carrying the rare earth oxide, followed by drying and reduction, whereby an ammonia decomposition catalyst carrying rare earth oxide and ruthenium, in which the ruthenium is uniformly supported, can be prepared. Alternatively, for example, the support carrying the rare earth oxide may be impregnated with an aqueous solution of a ruthenium salt such as ruthenium chloride or ruthenium nitrosyl nitrate, and then contacted with a basic aqueous solution such as an aqueous solution of sodium carbonate, sodium metasilicate, potassium carbonate, barium hydroxide, etc. This support is dried to support water-insoluble ruthenium oxide on the surface of the support carrying the rare earth oxide, and then reduced to prepare an ammonia decomposition catalyst carrying rare earth oxide and ruthenium, in which the ruthenium is supported in an eggshell form.

[0035] The ruthenium compound is a precursor of the ruthenium to be supported, and is not particularly limited, but for example, a water-soluble salt such as ruthenium chloride, a compound having an organic ligand such as tris(acetylacetonato)ruthenium, etc. can be used. A water-soluble salt is preferable, and ruthenium chloride is more preferable.

[0036] The drying method can be the same as the drying method in step 1 above. The reduction method is not particularly limited, and examples thereof include gas phase reduction using a gas containing a reducing gas such as hydrogen gas or ammonia gas, and liquid phase reduction using a solution containing a reducing agent such as sodium borohydride. In the case of gas phase reduction, the temperature is preferably 200° C. or higher, more preferably 200 to 600° C., and further preferably 250 to 550° C. The reduction time is not particularly limited, but is preferably 1 to 24 hours, more preferably 1 to 10 hours, and further preferably 1.5 to 5 hours. From the viewpoint of sufficient reaction progress, it is also preferable to increase the reduction temperature stepwise. The above-mentioned gas phase reduction may be carried out, for example, in a state where the mixture is filled in an ammonia decomposition apparatus before the ammonia decomposition reaction is carried out.

[0037] (Supporting of alkali metals and / or alkaline earth metals) When preparing a catalyst in which ruthenium and rare earth oxides and further an alkali metal and / or an alkaline earth metal are supported on the support, a step of supporting an alkali metal and / or an alkaline earth metal is carried out in addition to the steps 1 and 2. This step can also be carried out by using a general method for preparing a catalyst by supporting a metal, for example, by impregnating the support with a solution of an alkali metal salt and / or an alkaline earth metal salt, drying the resultant, and then reducing the resultant. The drying method can be the same as the drying method in step 1 above. The reduction can be carried out under the same conditions as in step 2 above.

[0038] The step of supporting an alkali metal and / or an alkaline earth metal on the support may be performed before or after the step 1, or after the step 2. It is preferably performed after the step 1 or 2. That is, it is preferable to further support an alkali metal and / or an alkaline earth metal on the support on which the rare earth oxide is supported obtained in the step 1, or on the support on which the rare earth oxide and ruthenium are supported obtained in the step 2. More preferably, an alkali metal and / or an alkaline earth metal is supported on the support having the rare earth oxide and ruthenium supported thereon obtained in step 2 above.

[0039] [Hydrogen gas production method] The method for producing hydrogen gas of the present invention involves decomposing ammonia to produce hydrogen gas in the presence of the above-mentioned ammonia decomposition catalyst of the present invention. By using the catalyst of the present invention, the ammonia decomposition reaction can be promoted even at low temperatures, and hydrogen gas can be produced at low cost.

[0040] The ammonia decomposition reaction is basically a reaction in which an ammonia-containing gas is contacted with a catalyst to generate 1.5 moles of hydrogen gas and 0.5 moles of nitrogen gas from 1 mole of ammonia. This reaction can be carried out in a general gas-solid phase contact reaction apparatus. The reaction method can be, for example, a batch type, a flow type, or the like, or a fixed bed type, a fluidized bed type, or the like, and is not particularly limited, but is preferably a flow type or a fixed bed type.

[0041] The reaction temperature for the ammonia decomposition reaction is preferably 300 to 700°C, more preferably 400 to 600°C, and further preferably 400 to 500°C, from the viewpoints of the ammonia decomposition rate, equipment costs, and the like. From the same viewpoint as above, the space velocity of the ammonia-containing gas in the reactor is 50 to 30,000 h -1 It is preferable that the temperature is 50 to 20,000 h. -1 , and more preferably 100 to 15,000 h -1 It is. The reaction pressure is not particularly limited, but the absolute pressure is preferably 0.1 to 0.6 MPa, more preferably 0.1 to 0.5 MPa, and further preferably 0.1 to 0.3 MPa.

[0042] The hydrogen gas produced by the ammonia decomposition reaction is separated from the nitrogen gas and treated to remove residual ammonia and other trace impurities using a known purification method. For example, methods that use an adsorbent such as zeolite or activated carbon and utilize the difference in gas adsorption characteristics depending on pressure and temperature include the pressure swing adsorption (PSA) method, which varies the pressure, and the thermal swing adsorption (TSA) method, which varies the temperature. In addition, a palladium alloy membrane permeation method, a cryogenic separation method, etc. can also be used.

[0043] The amount of gas produced in the decomposition reaction of ammonia can be determined by, for example, quantifying hydrogen gas with a gas component analyzer such as a gas chromatograph, or quantifying the amount of residual ammonia gas in the gas after the decomposition reaction with an infrared spectrophotometer, and calculating the amount of decomposed ammonia gas. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0045] [Analysis and evaluation method] Various analytical and evaluation methods used in the present examples are shown below.

[0046] (Metal oxide average pore size) For approximately 0.1 g of a metal oxide sample, the total pore volume was measured using a specific surface area pore distribution measuring device (Microtrack-Bell Corporation's "BELSORP-max", adsorption gas: nitrogen), and the average pore diameter was calculated from this and the specific surface area by the BET single point method.

[0047] (θ Amount of water absorbed by alumina) The mass m1 [g] of the dried θ-alumina sample dried at 110°C for 6 hours was measured. The dried sample was immersed in water for 2 hours to absorb water, and the surface water (supernatant) that was not absorbed by the carrier was removed using a stainless steel sieve (710 μm mesh size), and the mass m2 [g] of the absorbed sample was measured. The mass m1 [g] of the dried sample was subtracted from the mass m2 [g] of the absorbed sample to determine the absorbed volume, assuming the specific gravity of water to be 1 g / mL. This was then divided by the mass m1 of the dried sample to calculate the amount of absorbed water (per 1 g of carrier) [mL / g], {(m2-m1) [g] / 1 [g / mL]} / m1 [g].

[0048] (Catalyst composition) In preparing the catalyst, hydrochloric acid was added to each of the vessels used for supporting the rare earth oxide, the vessel used for supporting ruthenium, and the vessel used for supporting the alkali metal to dissolve the residues, and the metal elements in the residues were quantified using an ICP optical emission spectrometer (Shimadzu Corporation, "ICPS-8100"), and the component composition of the catalyst was calculated from the difference with the amount of each metal element contained in the raw materials used.

[0049] (Analysis of eggshell-type catalyst) The prepared eggshell-shaped catalyst was embedded in resin using an automatic hydraulic embedding machine, then ground with a polishing machine to prepare a catalyst particle cross-sectional sample, and the catalyst particle cross-section was observed and measured using a SEM / EDX (scanning electron microscope / energy dispersive X-ray spectroscopy) device to determine the thickness of the shell part and the concentration of ruthenium in the shell part or outside the shell part. The thickness of the shell part was determined as the distance on a straight line from the outer periphery to the center of the particle in the observed image of the catalyst particle cross-section where the concentration of ruthenium is 0.1 mass% or more relative to 100 mass% of the constituent atoms of the shell part. The measured values ​​of two selected catalyst particle samples of the eggshell-type catalyst obtained in Example 12 and Comparative Example 9 are shown as representative examples in Table 2 below. Table 2 also shows the measured values ​​of three selected catalyst particle samples of the uniform-type catalyst obtained in Comparative Example 8 for reference. As shown in Table 2, the shell thickness of each catalyst particle sample in Example 12 and Comparative Example 9 was 100 to 200 μm, so the ruthenium concentration in the shell was measured in the range of 0 to 100 μm deep from the particle surface. In addition, the ruthenium concentration in the part other than the shell was measured in the range of 200 μm deep from the particle surface to the center.

[0050] (Ammonia decomposition rate) The gas recovered after the ammonia decomposition reaction was passed through a Fourier transform infrared spectrophotometer (FT-IR spectrophotometer, manufactured by Thermo Fisher Scientific Co., Ltd.) and measured at a wave number of 3333 cm -1The absorption peak intensity was measured, and the residual ammonia concentration (x [%]) was obtained from a calibration curve using a standard gas (ammonia: manufactured by Taiyo Nippon Sanso Corporation, dilution gas: nitrogen), and the decomposition rate was calculated using the following formula. Ammonia decomposition rate [%] = {(100-x) / (100+x)} x 100 In addition, the only substances contained in the recovered gas other than ammonia were nitrogen gas and hydrogen gas produced by the decomposition of ammonia.

[0051] [Preparation of ammonia decomposition catalyst] Details of the raw materials used in the preparation of the ammonia decomposition catalysts in the following Examples and Comparative Examples are as follows. The particle size values ​​of the raw materials are catalog values. <Ruthenium raw material> Ruthenium chloride: Ruthenium(III) chloride hydrate (RuCl3·nH2O), manufactured by Furuya Metal Co., Ltd. <Rare earth oxide raw materials> Neodymium nitrate hexahydrate: Strem Chemicals Lanthanum nitrate: Strem Chemicals Cerium nitrate: Strem Chemicals Samarium nitrate: Strem Chemicals Cerium oxide: Manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., average pore diameter 7.4 nm, pore volume 0.21 mL / g, particle size 4 μm <Carrier (metal oxide)> γ-alumina (1): Sigma-Aldrich, average pore size 20 nm, pore volume 0.74 mL / g, particle size 0.5 mm Zirconia: Manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., average pore diameter 17 nm, pore volume 0.35 mL / g, particle size 4 μm Titania: Saint-Gobain, average pore size 28 nm, pore volume 0.3 mL / g, particle size 0.5 mm ·α alumina (1): Manufactured by Sasol, average pore diameter 170.5 nm, pore volume 0.1243 mL / g, particle size 1 mm θ-alumina: Sasol, average pore size 14 nm, pore volume 0.398 mL / g, particle size 1 mm, water absorption 0.4 mL / g α-alumina (2): Kanto Chemical Co., Ltd., particle size 42 nm γ-alumina (2): Sasol, average pore size 10.9 nm, pore volume 0.529 mL / g, particle size 1 mm <Metal (alkali metal) raw materials> Potassium carbonate: Wako Pure Chemical Industries, Ltd. Potassium nitrate: Wako Pure Chemical Industries, Ltd. Sodium carbonate: Wako Pure Chemical Industries, Ltd. Cesium carbonate: Wako Pure Chemical Industries, Ltd.

[0052] Example 1 2.10 g of gamma alumina (1) carrier was placed in an evaporating dish, and 9.6 mL of neodymium nitrate aqueous solution prepared using 2.11 g of neodymium nitrate hexahydrate was added dropwise with a Pasteur pipette in an amount of about 1 mL, while mixing with a spoon. The operation of drying was repeated until the entire amount was added, and a gamma alumina carrier (Nd(NO3)3 / gamma Al2O3) carrying neodymium nitrate was obtained. This carrier was dried at 100-110°C in an air atmosphere, and then calcined at 500°C for 2 hours to obtain a gamma alumina carrier (Nd2O3 / gamma Al2O3) carrying neodymium oxide. After cooling the support to room temperature, about 1 mL of ruthenium chloride aqueous solution (0.09 g of ruthenium content) was dropped with a Pasteur pipette while mixing with a spoon, and the operation of drying was repeated to add the entire amount, and then dried at 100 to 110 ° C in an air atmosphere to obtain an ammonia decomposition catalyst precursor (RuCl3 / Nd2O3 / γAl2O3) on which ruthenium chloride and neodymium oxide are supported. 3 mL of this precursor was filled into a flow-type fixed-bed reactor and reduced in a mixed gas flow of hydrogen gas and nitrogen gas at 300 ° C for 1 hour and further at 500 ° C for 1 hour to obtain a uniform-type ammonia decomposition catalyst (Ru / Nd2O3 / γAl2O3) on which ruthenium and neodymium oxide are supported on a γ-alumina support.

[0053] (Examples 2 to 6, Comparative Examples 1 to 4, 7 and 8) Each ammonia decomposition catalyst was prepared in the same manner as in Example 1, except that the raw materials were changed so as to obtain the component composition of each catalyst shown in Table 1 below.

[0054] Example 7 In Example 1, the amount of the γ-alumina (1) carrier was changed to 2.01 g, and the rest was the same as in Example 1 to prepare an ammonia decomposition catalyst (Ru / Nd2O3 / γAl2O3) carrying ruthenium and neodymium oxide. While mixing this catalyst with a spoon, about 1 mL of 3.7 mL of an aqueous solution of potassium carbonate 0.16 g (the amount of potassium content per mole of ruthenium is 2.6 moles) was dropped with a Pasteur pipette and dried. The entire amount was added by repeating the operation, and then dried at 100 to 110 ° C in an air atmosphere to obtain a potassium carbonate-treated ammonia decomposition catalyst precursor (K2CO3 / Ru / Nd2O3 / γAl2O3) in which potassium carbonate, ruthenium, and neodymium oxide were supported. 3 mL of this precursor was reduced in the same manner as in Example 1 to obtain a uniform potassium-treated ammonia decomposition catalyst (K / Ru / Nd2O3 / γAl2O3) in which potassium, ruthenium, and neodymium oxide were supported on a γ-alumina support.

[0055] Example 8 2.81 g of the α-alumina (1) carrier was added to 0.35 mL of an aqueous solution of neodymium nitrate prepared using 0.27 g of neodymium nitrate hexahydrate, and the mixture was dried at 100-110°C in an air atmosphere and then calcined at 500°C for 2 hours to obtain an α-alumina carrier (Nd2O3 / αAl2O3) carrying neodymium oxide. After cooling this support to room temperature, it was added to 0.30 mL of ruthenium chloride aqueous solution (ruthenium content 0.09 g) and dried at 100 to 110°C in an air atmosphere to obtain an ammonia decomposition catalyst precursor (RuCl3 / Nd2O3 / αAl2O3) carrying ruthenium chloride and neodymium oxide. 3 mL of this precursor was reduced in the same manner as in Example 1 to obtain a uniform type ammonia decomposition catalyst (Ru / Nd2O3 / αAl2O3) carrying ruthenium and neodymium oxide on an α-alumina support.

[0056] Example 9 In Example 8, the amount of the α-alumina (1) carrier was changed to 2.67 g, and the amount of neodymium nitrate hexahydrate was changed to 0.63 g. The rest of the procedure was the same as in Example 8, and a uniform-type ammonia decomposition catalyst (Ru / Nd2O3 / αAl2O3) in which ruthenium and neodymium oxide were supported on the α-alumina carrier was obtained.

[0057] Example 10 2.46 g of the θ-alumina support was added to 0.88 mL of an aqueous solution of neodymium nitrate prepared using 1.17 g of neodymium nitrate hexahydrate, and the mixture was dried at 100 to 110°C in an air atmosphere and then calcined at 500°C for 2 hours to obtain a θ-alumina support (Nd2O3 / θAl2O3) carrying neodymium oxide. After cooling this support to room temperature, it was added to 0.80 mL of ruthenium chloride aqueous solution (ruthenium content 0.09 g) and dried at 100 to 110°C in an air atmosphere to obtain an ammonia decomposition catalyst precursor (RuCl3 / Nd2O3 / θAl2O3) supported with ruthenium chloride and neodymium oxide. 3 mL of this precursor was reduced in the same manner as in Example 1 to obtain a uniform type ammonia decomposition catalyst (Ru / Nd2O3 / θAl2O3) supported with ruthenium and neodymium oxide on a θ-alumina support.

[0058] Example 11 In the same manner as in Example 10, a θ-alumina support (Nd2O3 / θAl2O3) carrying neodymium oxide was obtained. After cooling the support to room temperature, 0.80 mL of ruthenium chloride aqueous solution (0.09 g of ruthenium content) was added, and 1.2 mL of sodium carbonate aqueous solution was added and left to stand overnight. Then, after removing the liquid using a Pasteur pipette, the mixture was washed with water and dried at 100 to 110 ° C in an air atmosphere to obtain an ammonia decomposition catalyst precursor (RuO2 / Nd2O3 / θAl2O3) in which ruthenium oxide and neodymium oxide are supported. 3 mL of this precursor was reduced in the same manner as in Example 1 to obtain an eggshell-type ammonia decomposition catalyst (Ru / Nd2O3 / θAl2O3) in which ruthenium and neodymium oxide are supported on a θ-alumina support.

[0059] Example 12 The amount of theta-alumina carrier was changed to 2.49 g, and the amount of neodymium nitrate hexahydrate was changed to 1.09 g. Except for this, the same procedure as in Example 11 was repeated to obtain a theta-alumina carrier (Nd2O3 / thetaAl2O3), and then an ammonia decomposition catalyst (Ru / Nd2O3 / thetaAl2O3) carrying ruthenium and neodymium oxide was obtained. This catalyst was added to 0.80 mL of an aqueous solution of 0.16 g of potassium carbonate (an amount such that the potassium content per mole of ruthenium was 2.6 moles) and dried at 100 to 110°C under an air atmosphere to obtain a potassium carbonate-treated ammonia decomposition catalyst (K2CO3 / Ru / Nd2O3 / θAl2O3) in which potassium carbonate, ruthenium, and neodymium oxide were supported. 3 mL of this catalyst was reduced in the same manner as in Example 1 to obtain an eggshell-type potassium-treated ammonia decomposition catalyst (K / Ru / Nd2O3 / θAl2O3) in which potassium, ruthenium, and neodymium oxide were supported on a θ-alumina carrier. The thickness of the shell of this catalyst was 100 to 200 μm (see Table 2 below).

[0060] Example 13 In Example 12, the operating procedure was changed so that potassium was supported before supporting ruthenium, and otherwise the same procedure was followed as in Example 12 to obtain an eggshell-type ammonia decomposition catalyst (Ru / K / Nd2O3 / θAl2O3) in which ruthenium, potassium, and neodymium oxide were supported on a θ-alumina support.

[0061] (Examples 14 to 18) Each eggshell-type ammonia decomposition catalyst was prepared in the same manner as in Example 12, except that the raw materials were changed so as to obtain the component composition of the catalyst shown in Table 1 below.

[0062] Comparative Example 5 2.91 g of cerium oxide, a rare earth oxide, was used as a support. 8.9 mL of ruthenium chloride aqueous solution (0.09 g of ruthenium content) was supported on this support in the same manner as in Example 1 to obtain an ammonia decomposition catalyst precursor (RuCl3 / CeO2) supported with ruthenium chloride. 3 mL of this precursor was loaded into a reactor and reduced in a mixed gas flow of hydrogen gas and nitrogen gas at 300°C for 1 hour and then at 500°C for 1 hour to obtain a uniform type ammonia decomposition catalyst (Ru / CeO2) supported with ruthenium on a cerium oxide support.

[0063] Comparative Example 6 In Comparative Example 5, the amount of cerium oxide added was changed to 2.43 g, and the rest was the same as in Comparative Example 5 to prepare an ammonia decomposition catalyst precursor (Ru / CeO2) carrying ruthenium. This precursor was mixed with 0.48 g of α-alumina (2) support to obtain an ammonia decomposition catalyst (Ru / CeO2+αAl2O3) consisting of a mixed powder of ruthenium-supported cerium oxide and α-alumina (2).

[0064] Comparative Example 9 0.80 mL of ruthenium chloride aqueous solution (0.09 g of ruthenium content) was added to 2.91 g of the gamma alumina (2) carrier, and 2.4 mL of sodium carbonate aqueous solution was added and left to stand overnight. Then, after removing the liquid using a Pasteur pipette, the mixture was washed with water and dried at 100 to 110 °C in an air atmosphere to obtain an ammonia decomposition catalyst precursor (RuO2 / γAl2O3) supported by ruthenium oxide. 3 mL of this precursor was reduced in the same manner as in Example 1 to obtain an eggshell-type ammonia decomposition catalyst (Ru / γAl2O3) supported by ruthenium on a gamma alumina carrier. The thickness of the shell part of this catalyst was 100 to 200 μm (see Table 2 below).

[0065] [Ammonia decomposition reaction] Using each of the ammonia decomposition catalysts obtained in the above Examples and Comparative Examples, a cylindrical reactor (inner diameter 0.75 cm, length 40 cm for Examples 1 to 7 and Comparative Examples 1 to 5, inner diameter 1.1 cm, length 40 cm) of an ammonia decomposition apparatus (flow type / fixed bed type) was packed with 3 mL of catalyst, and the reaction mixture was heated at 0.1 MPa (atmospheric pressure) at a space velocity (SV) of 10,000 h -1 Ammonia was passed through the catalyst tube at a flow rate of 500 mL / min, the temperature of the lower end of the catalyst-packed section was set to 500° C., and an ammonia decomposition reaction was carried out to determine the ammonia decomposition rate. In Example 6 and Comparative Example 4, the temperature was set to 600° C. because the ammonia decomposition rate measurable by an infrared spectrophotometer was not reached at 500° C. In addition, in Examples 5 and 6 and Comparative Example 5, taking into consideration the difference in density from the ammonia decomposition catalyst in Example 1, the space velocity (SV) was adjusted to the values ​​shown in Table 1 so that the flow rate of ammonia per mass of ruthenium was approximately the same as in Example 1. The decomposition rate is an index showing the magnitude of the ammonia decomposition rate, that is, the degree of catalytic activity of the ammonia decomposition catalyst. The closer the decomposition rate is to 100%, the higher the catalytic activity of the ammonia decomposition catalyst. These results are shown in Table 1 together with the component compositions of the catalysts.

[0066] [Table 1]

[0067] [Table 2]

[0068] From the results shown in Table 1, it was found that when a catalyst in which ruthenium and 0.1 to 30.0 mass % of a rare earth oxide were supported on a support made of a metal oxide other than a rare earth oxide (Examples 1 to 18), high catalytic activity was exhibited in the ammonia decomposition reaction. Comparisons between Examples 1 to 4 and Comparative Examples 1 and 2, between Example 5 and Comparative Example 3, and between Example 6 and Comparative Example 4 show that the catalytic activity is improved by supporting a specified content of rare earth oxide. Furthermore, from a comparison between Example 7 and Example 1, and a comparison between Examples 12 to 18 and Example 11, it was confirmed that the catalytic activity was further improved by supporting an alkali metal. Furthermore, when an alkali metal was supported, the catalyst supported after ruthenium (Example 12) had higher catalytic activity than the catalyst supported earlier (Example 13). When α-alumina or θ-alumina was used as the support (Examples 8 to 10), it was found that sufficient catalytic activity could be obtained even if the amount of rare earth oxide supported was reduced. In particular, when α-alumina was used (Examples 8 and 9), sufficient catalytic activity could be maintained with a smaller amount of rare earth oxide supported. Furthermore, it was found that when an eggshell-type catalyst was used (Examples 11 to 18), the catalytic activity was improved.

Claims

1. Ruthenium and rare earth oxide are supported on a support made of a metal oxide other than a rare earth oxide, and the content of the rare earth oxide is 0.1 to 30.0 mass %, 1. An ammonia decomposition catalyst, wherein the rare earth oxide is neodymium oxide and the metal oxide is alumina.

2. 2. The ammonia decomposition catalyst of claim 1, wherein the alumina is alpha alumina.

3. The ammonia decomposition catalyst according to claim 2, wherein the content of the rare earth oxide is 0.3 to 20.0 mass %.

4. 2. The ammonia decomposition catalyst of claim 1, wherein the alumina is theta alumina.

5. The ammonia decomposition catalyst according to claim 4, wherein the content of the rare earth oxide is 10.0 to 25.0 mass %.

6. 2. The ammonia decomposition catalyst of claim 1, wherein the alumina is gamma alumina.

7. The ammonia decomposition catalyst according to claim 6, wherein the content of the rare earth oxide is 10.0 to 30.0 mass %.

8. The ammonia decomposition catalyst according to any one of claims 1 to 7, wherein the ruthenium content is 0.1 to 10.0 mass%.

9. The ammonia decomposition catalyst according to any one of claims 1 to 8, wherein the support further supports one or more metals selected from the group consisting of alkali metals and alkaline earth metals.

10. 10. The ammonia decomposition catalyst according to claim 9, wherein the content of the metal is 0.1 to 10.0 moles per mole of the ruthenium.

11. A method for producing hydrogen gas, comprising decomposing ammonia in the presence of the ammonia decomposition catalyst according to any one of claims 1 to 10 to produce hydrogen gas.

Citation Information

Patent Citations

  • Ruthenium-based catalyst for decomposing ammonia to prepare mixed H2-N2 gas and its prepn

    CN1506300A

  • Method for decomposing ammonia

    JP1996084910A

  • Ammonia decomposition catalyst and treatment of ammonia-containing waste gas

    JP2001009281A

  • Catalyst for decomposing ammonia

    JP2011078888A

  • Catalyst converting ammonia to nitrogen and hydrogen, method for manufacturing the catalyst, and method for converting ammonia using the catalyst