Method for producing conductive polymer dispersion and method for producing conductive film

A controlled dispersion process with specific polymer ratios and viscosity maintains the stability of conductive polymer dispersions, ensuring consistent conductivity in formed layers despite prolonged storage.

JP7586668B2Active Publication Date: 2024-11-19SHIN ETSU POLYMER CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020140071
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-21
Publication Date
2024-11-19
Estimated Expiration
2040-08-21

AI Technical Summary

Technical Problem

Conductive polymer dispersions containing π-conjugated conductive polymers, such as PEDOT-PSS, suffer from poor dispersion stability when water-soluble organic solvents are added, leading to reduced conductivity and dispersibility over time, which affects the quality of the conductive layers formed.

Method used

A conductive polymer dispersion is formulated with a specific mass ratio of π-conjugated conductive polymer to polyanion (1:2 to 1:5) and controlled viscosity (35 to 45 cP) and particle size (<500 nm), using a controlled dispersion process at 14°C to 25°C to maintain stability.

Benefits of technology

The method enhances the dispersion stability of the conductive polymer dispersion, ensuring good conductivity in the formed conductive layers even after prolonged storage, with minimal changes in surface resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586668000001
    Figure 0007586668000001
  • Figure 0007586668000002
    Figure 0007586668000002
  • Figure 0007586668000003
    Figure 0007586668000003
Patent Text Reader

Abstract

To provide a conductive polymer dispersion having improved stability after dispersion treatment and a method for producing the same.SOLUTION: There is provided a conductive polymer dispersion which contains a conductive composite containing a π conjugated conductive polymer and a polyanion and water, wherein the mass ratio of the π conjugated conductive polymer and the polyanion is (1:2) to (1:5), the polyanion has a weight average molecular weight Mw of 200000 or more and 1000000 or less and the viscosity at 25°C when the concentration of the conductive composite to the total mass of the conductive polymer dispersion is adjusted to 1.3 mass% is 35 cP or more and 45 cP or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive polymer dispersion containing a π-conjugated conductive polymer and a method for producing the same, a paint, and a conductive film and a method for producing the same. [Background technology]

[0002] As a paint for forming a conductive layer, a conductive polymer dispersion containing a conductive complex in which a π-conjugated conductive polymer is doped with a polyanion may be used. For example, poly(3,4-ethylenedioxythiophene), a π-conjugated conductive polymer, is difficult to disperse in water, but by doping it with polystyrene sulfonic acid to form PEDOT-PSS, the dispersibility in water is improved. Patent Document 1 discloses a technique for improving the hydrophilicity of a conductive complex and improving its reactivity to an epoxy compound by dispersing the conductive complex in water and leaving it for 180 days or more. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-31013 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the method of Patent Document 1, the conductive complex is reacted with an epoxy compound, and then dissolved in an organic solvent to form a paint, thereby improving the wettability of the hydrophobic film substrate. When the conductive complex is not hydrophobized by reacting with an epoxy compound, a water-soluble organic solvent such as alcohol is usually added to the conductive polymer dispersion to improve the wettability of the conductive complex to the film substrate. However, the dispersion stability of the conductive complex in the paint to which the water-soluble organic solvent is added is not necessarily high, and the dispersibility may decrease several tens of hours after the addition of the water-soluble organic solvent. The conductivity of the conductive layer formed by applying the paint with reduced dispersibility also decreases. For this reason, it is required to maintain the dispersibility of the conductive complex in the paint after the paint is obtained by adding a water-soluble organic solvent to the conductive polymer dispersion that has been subjected to a dispersion treatment.

[0005] Therefore, the present inventors have intensively investigated a method for obtaining a conductive polymer dispersion in which the dispersibility of the conductive complex is improved by devising a dispersion treatment at the conductive polymer dispersion stage prior to preparation of a paint, and a method for producing a conductive polymer dispersion in which the decrease in dispersibility of the conductive complex over time is suppressed even after a water-soluble organic solvent is added to form a paint, and have completed the present invention.

[0006] The present invention provides a conductive polymer dispersion having improved stability after dispersion treatment and a method for producing the same. Also provided are a paint containing the conductive polymer dispersion, and a conductive film using the conductive polymer dispersion or the paint and a method for producing the same. [Means for solving the problem]

[0007] [1] A conductive polymer dispersion comprising water and a conductive complex containing a π-conjugated conductive polymer and a polyanion, wherein the mass ratio of the π-conjugated conductive polymer to the polyanion is from (1:2) to (1:5), and the weight-average molecular weight Mw of the polyanion is from 200,000 to 1,000,000, and wherein the conductive polymer dispersion has a viscosity of from 35 cP to 45 cP at 25° C. when the concentration of the conductive complex relative to the total mass of the conductive polymer dispersion is adjusted to 1.3 mass %. [2] The conductive polymer dispersion according to [1], wherein the conductive complex has a particle size of less than 500 nm at 25° C. when the concentration of the conductive complex is adjusted to 0.13% by mass. [3] The conductive polymer dispersion according to [1] or [2], wherein the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrenesulfonic acid. [4] A coating material comprising the conductive polymer dispersion liquid according to any one of [1] to [3] and a water-soluble organic solvent. [5] The paint according to [4], wherein the water-soluble organic solvent contains at least one of methanol and isopropanol. [6] A method for producing a conductive polymer dispersion, comprising: polymerizing a monomer that forms a π-conjugated conductive polymer in a reaction liquid containing a polyanion, and water, to obtain a conductive polymer dispersion containing a conductive complex containing the π-conjugated conductive polymer and the polyanion, and water; and then dispersing the conductive polymer dispersion, wherein, in the dispersion treatment, the conductive complex is dispersed so that the viscosity at 25° C. is 35 cP or more and 45 cP or less when the concentration of the conductive complex is adjusted to 1.3 mass % relative to the total mass of the obtained conductive polymer dispersion. [7] The method for producing a conductive polymer dispersion according to [6], further comprising adjusting the liquid temperature of the conductive polymer dispersion during the dispersion treatment to 14° C. or higher and 25° C. or lower. [8] A method for producing a conductive polymer dispersion according to [6] or [7], comprising the steps of: retaining the conductive polymer dispersion before the dispersion treatment in a first container adjusted to a temperature of 14° C. or higher and 25° C. or lower; gradually introducing the conductive polymer dispersion from the first container into a disperser body to carry out the dispersion treatment; and sequentially leading the conductive polymer dispersion after the dispersion treatment from the disperser body to a second container adjusted to a temperature of 14° C. or higher and 25° C. or lower and collecting the conductive polymer dispersion. [9] A method for producing a conductive film, comprising applying the conductive polymer dispersion according to any one of [1] to [3], or the coating material according to [4] or [5] to at least one surface of a film substrate.

[10] A conductive film comprising a conductive layer formed on at least one surface of a film substrate, the conductive layer being composed of the conductive polymer dispersion according to any one of [1] to [3], or a cured layer of the coating material according to [4] or [5]. Effect of the Invention

[0008] In the conductive polymer dispersion of the present invention, the viscosity when measured under predetermined conditions falls within a specific range, and thus the dispersion stability is improved. According to the method for producing a conductive polymer dispersion of the present invention, a conductive polymer dispersion having improved dispersion stability as described above can be easily produced. According to the coating material of the present invention, the dispersion stability of the conductive complex is improved, so that a conductive layer having good conductivity can be formed even after the coating material is prepared and left to stand for one day or more. According to the method for producing a conductive film of the present invention, a conductive film having a conductive layer with good conductivity can be easily formed.

[0009] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."

[0010] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <<Conductive polymer dispersion>> A first aspect of the present invention is a conductive polymer dispersion comprising a conductive complex containing a π-conjugated conductive polymer and a polyanion, and water, wherein the mass ratio of the π-conjugated conductive polymer:the polyanion is from (1:2) to (1:5), and the weight-average molecular weight Mw of the polyanion is from 200,000 to 1,000,000, and wherein the viscosity at 25° C. is from 35 cP to 45 cP when the concentration of the conductive complex is adjusted to 1.3 mass %.

[0012] <π-conjugated conductive polymers> The π-conjugated conductive polymer is not particularly limited as long as it has the effect of the present invention and is an organic polymer whose main chain is composed of a π-conjugated system, and examples thereof include polypyrrole-based conductive polymers, polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyphenylene-based conductive polymers, polyphenylenevinylene-based conductive polymers, polyaniline-based conductive polymers, polyacene-based conductive polymers, polythiophenevinylene-based conductive polymers, and copolymers thereof. From the viewpoint of stability in air, polypyrrole-based conductive polymers, polythiophenes, and polyaniline-based conductive polymers are preferred, and from the viewpoint of transparency, polythiophene-based conductive polymers are more preferred.

[0013] Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Examples of polypyrrole-based conductive polymers include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole). Examples of polyaniline-based conductive polymers include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid). Among the above-mentioned π-conjugated conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferable from the viewpoints of conductivity, transparency, and heat resistance. The conductive composite may contain one type of π-conjugated conductive polymer, or two or more types of polymers.

[0014] <Polyanion> A polyanion is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of the polyanion functions as a dopant for a π-conjugated conductive polymer, improving the conductivity of the π-conjugated conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. These may be homopolymers or copolymers of two or more kinds. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The conductive complex may be composed of one type of polyanion or two or more types of polyanions.

[0015] The weight-average molecular weight Mw of the polyanion is 200,000 to 1,000,000, preferably 300,000 to 1,000,000, more preferably 400,000 to 1,000,000, even more preferably 500,000 to 1,000,000, even more preferably 600,000 to 1,000,000, even more preferably 700,000 to 1,000,000, particularly preferably 800,000 to 1,000,000, and most preferably 900,000 to 1,000,000. Here, the weight-average molecular weight Mw is the average molecular weight based on mass (which may be called mass-average molecular weight) measured by gel permeation chromatography using pullulan of known weight-average molecular weight as a standard substance. When the weight average molecular weight Mw is within the above preferred range, the dispersion stability of the conductive composite in the conductive polymer dispersion of this embodiment and in the coating material of the second embodiment described below is further improved.

[0016] A conductive complex is formed by doping a polyanion into a π-conjugated conductive polymer. However, in the polyanion, some anion groups are not doped into the π-conjugated conductive polymer, and there are excess anion groups that are not involved in the doping. Since these excess anion groups are hydrophilic groups, the conductive complex has high water dispersibility and low organic solvent dispersibility. When the number of all anionic groups in the polyanion is taken as 100 mol %, the excess anionic groups are preferably from 30 mol % to 90 mol %, more preferably from 45 mol % to 75 mol %.

[0017] The content ratio of the π-conjugated conductive polymer to the polyanion in the conductive composite is, on a mass basis, from (1:2) to (1:5), preferably from (1:2) to (1:4.5), more preferably from (1:2) to (1:4), and even more preferably from (1:2) to (1:3). When the content is at least the lower limit of the above range, the doping effect of the polyanion is sufficiently exhibited, and the dispersion stability of the conductive composite is further improved. When the content is equal to or less than the upper limit of the above range, a conductive layer having excellent conductivity can be formed.

[0018] The content of the conductive complex relative to the total mass of the conductive polymer dispersion of this embodiment is, for example, preferably 0.1 mass% or more and 20 mass% or less, more preferably 0.2 mass% or more and 10 mass% or less, even more preferably 0.3 mass% or more and 10.0 mass% or less, and particularly preferably 1.0 mass% or more and 5.0 mass% or less. When the content is within the above range, the dispersion stability of the conductive composite is further improved.

[0019] The conductive polymer dispersion of this embodiment has a viscosity at 25° C. of 35 cP or more and 45 cP or less when the concentration of the conductive complex relative to the total mass of the conductive polymer dispersion is adjusted to 1.3 mass %. In measuring the viscosity, the conductive polymer dispersion preferably contains only ion-exchanged water as a dispersion medium, and preferably does not contain any additives other than the conductive complex. The viscosity was measured at 25° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer). The above viscosity range is preferably 35 to 45 cP, and more preferably 38 to 42 cP. When the viscosity is within these suitable ranges, the dispersion stability of the conductive composite is further improved.

[0020] The particle size of the conductive polymer dispersion of this embodiment at 25° C. is preferably less than 500 nm, more preferably 300 nm to 480 nm, more preferably 350 nm to 460 nm, and even more preferably 380 nm to 440 nm, when the concentration of the conductive complex relative to the total mass of the conductive polymer dispersion is adjusted to 0.13 mass %. Within these preferred ranges, the dispersion stability of the conductive complex is further improved. In measuring the particle size, the conductive polymer dispersion preferably contains only ion-exchanged water as a dispersion medium, and preferably does not contain any additives other than the conductive complex. The particle size is determined as a cumulant average particle size measured by dynamic light scattering.

[0021] ≪Paint≫ A second aspect of the present invention is a coating material comprising the conductive polymer dispersion of the first aspect and a water-soluble organic solvent. In the coating material of this aspect, the conductive complex is in a dispersed state.

[0022] The coating material of this embodiment contains water and a water-soluble organic solvent. The mixture of water and the water-soluble organic solvent is sometimes called an aqueous dispersion medium.

[0023] A water-soluble organic solvent is an organic solvent that dissolves in an amount of 1 g or more in 100 g of water at 20°C. Examples of the water-soluble organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, nitrogen atom-containing solvents, and ester-based solvents. Examples of alcohol-based solvents include methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 2-methyl-2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, allyl alcohol, ethylene glycol, propylene glycol, propylene glycol monomethyl ether, and ethylene glycol monomethyl ether. Examples of the ether solvent include diethyl ether, dimethyl ether, propylene glycol dialkyl ether, and diethylene glycol diethyl ether. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the nitrogen atom-containing solvent include N-methylpyrrolidone, dimethylacetamide, and dimethylformamide. The water-soluble organic solvent may be contained alone or in combination of two or more kinds. In order to improve the coatability of the coating material of this embodiment onto the film substrate, the water-soluble organic solvent is preferably an alcohol-based solvent or a ketone-based solvent, and more preferably an alcohol-based solvent.

[0024] The content of the water-soluble organic solvent relative to the total mass of the aqueous dispersion medium is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The content of the water-soluble organic solvent is preferably 90% by mass or less. When the content is within the above preferred range, the wettability of the conductive composite to the film substrate can be improved while suppressing deterioration over time of the dispersion stability of the conductive composite in the coating material of this embodiment.

[0025] The water content relative to the total mass of the aqueous dispersion medium is preferably from 10% by mass to 50% by mass, more preferably from 20% by mass to 40% by mass, and even more preferably from 25% by mass to 35% by mass. When the content is within the above preferred range, the wettability of the conductive composite to the film substrate can be improved while suppressing deterioration over time of the dispersion stability of the conductive composite in the coating material of this embodiment.

[0026] The content of the conductive complex relative to the total mass of the paint of this embodiment is, for example, preferably from 0.001 mass% to 1 mass%, more preferably from 0.005 mass% to 0.2 mass%, even more preferably from 0.01 mass% to 0.1 mass%, and particularly preferably from 0.03 mass% to 0.05 mass%. When the content is within the above preferred range, a decrease in the dispersion stability of the conductive composite in the coating material of this embodiment can be suppressed, and a conductive layer with good conductivity can be formed by applying the coating material to a film substrate.

[0027] <Binder components> The coating material of this embodiment may contain a binder component. The binder component is a resin other than the π-conjugated conductive polymer and the polyanion or a precursor thereof, and is a thermoplastic resin, or a curable monomer or oligomer that is cured when the conductive layer is formed. The thermoplastic resin becomes the binder resin as it is, and the curable monomer or oligomer becomes the resin formed by curing becomes the binder resin. The binder component may be one type only, or two or more types may be included.

[0028] Specific examples of binder resins derived from binder components include acrylic resins (acrylic compounds), polyester resins, polyurethane resins, polyimide resins, polyether resins, melamine resins, and silicones. The binder resin contained in the coating material of this embodiment is preferably a water-dispersible resin, more preferably a water-dispersible emulsion resin. The water-dispersible resin is an emulsion resin or a water-soluble resin.

[0029] Specific examples of water-dispersible emulsion resins include acrylic resins (acrylic compounds), polyester resins, polyurethane resins, polyimide resins, melamine resins, etc., which are emulsionized with an emulsifier. Among them, polyester emulsions are preferred because the strength of the coating film formed by applying the coating material of this embodiment to a film substrate is high. In particular, when applying the coating material to a polyester film substrate, polyester emulsions are preferred because the adhesion of the coating film to the film substrate is high.

[0030] Specific examples of the water-soluble resin include acrylic resin (acrylic compound), polyester resin, polyurethane resin, polyimide resin, and melamine resin, which have an acid group such as a carboxy group or a sulfo group or a salt thereof. Here, the water-soluble resin is preferably one that dissolves in an amount of 1 g or more, preferably 5 g or more, and more preferably 10 g or more in 100 g of distilled water at 25° C.

[0031] The acid group, such as a carboxy group or a sulfo group, contained in the water-dispersible resin may form a salt with a cation, such as a sodium ion or a potassium ion.

[0032] The curable monomer or oligomer may be a thermosetting monomer or oligomer, or a photocurable monomer or oligomer. Here, the oligomer refers to a polymer having a mass average molecular weight of less than 10,000. Note that a polymer having a mass average molecular weight of more than 10,000 does not have curability. Examples of the curable monomer include an acrylic monomer (acrylic compound), an epoxy monomer, an organosiloxane, etc. Examples of the curable oligomer include an acrylic oligomer (acrylic compound), an epoxy oligomer, a silicone oligomer (curable silicone), etc. When an acrylic monomer or an acrylic oligomer is used as the binder component, it can be easily cured by heating or light irradiation. When an organosiloxane or a silicone oligomer is used as the binder component, it is possible to impart releasability (non-adhesiveness) to the conductive layer.

[0033] When the composition contains a curable monomer or oligomer, it is preferable to further contain a curing catalyst. For example, when the composition contains a thermosetting monomer or oligomer, it is preferable to contain a thermal polymerization initiator that generates radicals by heating, and when the composition contains a photocurable monomer or oligomer, it is preferable to contain a photopolymerization initiator that generates radicals by light irradiation. In addition, when the composition contains an organosiloxane or silicone oligomer, it is preferable to contain a platinum catalyst for curing.

[0034] The content of the binder component in the coating material of this embodiment is preferably from 100 to 20,000 parts by mass, and more preferably from 100 to 5,000 parts by mass, relative to 100 parts by mass of the conductive composite. When the content is equal to or greater than the lower limit of the above range, the film formability and film strength can be improved when the coating material of this embodiment is applied to a film substrate. When the content is equal to or less than the upper limit of the above range, a decrease in electrical conductivity due to a decrease in the content ratio of the conductive complex can be suppressed.

[0035] (Other additives) The coating material of this embodiment may contain other known additives. Examples of the additives that can be used include surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, and ultraviolet absorbing agents. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having a vinyl group or an amino group. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers. When the coating material of this embodiment contains the above-mentioned additives, the content ratio is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the conductive composite.

[0036] The coating material of this embodiment can be produced by appropriately adding water, a water-soluble organic solvent, a binder component, other additives, and the like to the conductive polymer dispersion of the first embodiment, and mixing them in a conventional manner.

[0037] <Method for producing conductive polymer dispersion> A third aspect of the present invention is a method for producing a conductive polymer dispersion, the method comprising: polymerizing a monomer that forms a π-conjugated conductive polymer in a reaction liquid containing the monomer, a polyanion, and water to obtain a conductive polymer dispersion containing a conductive complex containing the π-conjugated conductive polymer and the polyanion, and water, and then dispersing the conductive polymer dispersion, wherein, in the dispersion treatment, the conductive complex is dispersed so that the viscosity at 25° C. is 35 cP or more and 45 cP or less when the concentration of the conductive complex is adjusted to 1.3 mass % relative to the total mass of the obtained conductive polymer dispersion.

[0038] An aqueous solution (the reaction solution) containing the monomer and the polyanion at a specific content ratio is prepared, and the monomer is polymerized to form a π-conjugated conductive polymer. In the reaction solution, the polyanion is naturally doped into the π-conjugated conductive polymer, and a conductive complex consisting of the π-conjugated conductive polymer and the polyanion is formed. The content ratio (mass basis) of the π-conjugated conductive polymer:polyanion contained in the formed conductive complex is the same as the ratio of the content of the monomer and the content of the polyanion contained in the aqueous solution immediately before the start of polymerization. In other words, the content ratio of the monomer and the polyanion blended in the reaction solution is reflected in the content ratio of the π-conjugated conductive polymer and the polyanion in the formed conductive complex.

[0039] The content ratio of the monomer to the polyanion in the reaction solution immediately before the start of polymerization is (1:2) to (1:5) on a mass basis, preferably (1:2) to (1:4.5), more preferably (1:2) to (1:4), and even more preferably (1:2) to (1:3). When the content is within the above range, the conductive polymer dispersion liquid of the first embodiment described above can be easily formed.

[0040] A catalyst may be added to the reaction solution. The catalyst is not particularly limited as long as it polymerizes the monomer, and examples thereof include transition metal compounds such as ferric chloride, ferric sulfate, ferric nitrate, and cupric chloride. Among them, it is preferable to use a catalyst containing iron, since the polymerization of the monomer proceeds stably at room temperature. It is preferable to contain an oxidizing agent together with the catalyst. The oxidizing agent can return the reduced catalyst to its original oxidized state. Examples of the oxidizing agent include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate.

[0041] The content of the monomer contained in the reaction liquid immediately before the start of polymerization is, for example, preferably 0.1 mass % or more and 20 mass % or less, more preferably 0.2 mass % or more and 10 mass % or less, and even more preferably 0.3 mass % or more and 5 mass % or less, relative to the total mass of the reaction liquid. When the amount is within the above range, the polymerization reaction can proceed stably, so that the formation of a complex with the polyanion present in the reaction system proceeds stably, and a conductive complex with good conductivity can be easily obtained.

[0042] The content of the catalyst in the reaction liquid immediately before the start of polymerization is, for example, preferably 0.001 mass % or more and 2 mass % or less, more preferably 0.005 mass % or more and 1 mass % or less, and even more preferably 0.01 mass % or more and 0.5 mass % or less, relative to the total mass of the reaction liquid. When the amount is within the above range, the polymerization reaction can proceed stably, so that the formation of a complex with the polyanion present in the reaction system proceeds stably, and a conductive complex with good conductivity can be easily obtained.

[0043] The content of the polyanion in the reaction liquid immediately before the start of polymerization is preferably set based on the content ratio relative to the monomer.

[0044] The weight average molecular weight Mw of the polyanion contained in the reaction solution is preferably 200,000 or more and 1,000,000 or less. In other words, it is preferable that the weight average molecular weight of the polyanion does not change in the reaction solution. As a method for synthesizing a polyanion with a specific weight-average molecular weight Mw, for example, the weight-average molecular weight Mw can be adjusted by adjusting the amount of oxidizing agent added to polymerize the monomers constituting the polyanion, as shown in the examples described below. Specifically, by increasing the concentration of the oxidizing agent, the weight-average molecular weight of the polyanion formed by polymerization of the monomers can be reduced. By this method, for example, polystyrene sulfonic acid with a weight-average molecular weight Mw of 100,000 to 1,200,000 can be obtained.

[0045] By the above method, a conductive polymer dispersion is obtained which contains a conductive complex containing a π-conjugated conductive polymer and a polyanion, and water, in which the mass ratio of the π-conjugated conductive polymer:the polyanion is (1:2) to (1:5), and the weight average molecular weight Mw of the polyanion is 200,000 or more and 1,000,000 or less.

[0046] Next, the conductive polymer dispersion liquid is dispersed using a disperser, whereby the conductive polymer dispersion of the first embodiment can be easily obtained.

[0047] An example of a disperser used in this embodiment is a disperser that takes a portion of the dispersed sample from a holding tank (first container) that stores the dispersed sample, sends it to the disperser body, disperses it, and then collects it in another tank (collection tank; second container).

[0048] In the method for producing a conductive polymer dispersion of this embodiment, by controlling the temperature of the conductive polymer dispersion to be subjected to the dispersion treatment, it becomes easy to obtain a conductive polymer dispersion having a desired viscosity and particle size.

[0049] From the viewpoint of obtaining a conductive polymer dispersion having the viscosity and particle size described in the first embodiment, the liquid temperature (inlet temperature) of the conductive polymer dispersion to be subjected to dispersion treatment, the liquid temperature of the conductive polymer dispersion during dispersion, and the liquid temperature (outlet temperature) of the conductive polymer dispersion discharged from the main body of the disperser (the center where the dispersed sample is stirred) are preferably adjusted to 14° C. or more and 25° C. or less, and more preferably adjusted to 15° C. or more and 20° C. In this case, the temperature of the dispersed sample stored in the collection kiln after dispersion treatment (inside kiln solution temperature) is also preferably adjusted to 14° C. or more and 25° C. or less, and more preferably adjusted to 15° C. or more and 20° C. or less.

[0050] When the conductive polymer dispersion is dispersed using a disperser at the above-mentioned temperature setting, the time of the dispersion treatment is not particularly limited, and the dispersion treatment may be repeated while monitoring the viscosity and particle size of the dispersed conductive polymer dispersion until the desired viscosity and particle size are achieved.

[0051] Since the temperature control of the conductive polymer dispersion during and before and after dispersion is facilitated as described above, the dispersion treatment in this embodiment is preferably carried out as follows: That is, it is preferable to hold the conductive polymer dispersion before the dispersion treatment in a first container adjusted to 14° C. or higher and 25° C. or lower, gradually introduce the conductive polymer dispersion from the first container into a disperser body to carry out the dispersion treatment, and sequentially lead the conductive polymer dispersion after the dispersion treatment from the disperser body to a second container adjusted to 14° C. or higher and 25° C. or lower and collect it. The conductive polymer dispersion liquid held in the first container is fed little by little into the disperser body to be dispersed, and the conductive polymer dispersion liquid after dispersion processing is collected little by little from the disperser body into the second container, so that the liquid temperature and the degree of dispersion during the dispersion processing can be controlled more reliably. Note that, if one dispersion processing (one pass) is insufficient, the dispersion processing may be carried out again in the same manner.

[0052] By the above method, the conductive polymer dispersion of the first embodiment can be obtained. Since the dispersion liquid after completion of the dispersion treatment is the conductive polymer dispersion liquid of the first embodiment, the dispersion medium of the conductive polymer dispersion liquid to be subjected to the dispersion treatment is preferably water or an aqueous dispersion medium, as described above, and more preferably water.

[0053] The content of the conductive complex relative to the total mass of the conductive polymer dispersion to be subjected to the dispersion treatment is preferably from 0.01 to 10 mass%, more preferably from 0.1 to 5 mass%, and even more preferably from 0.5 to 2 mass%.

[0054] It is preferable to remove the catalyst and oxidizing agent added to the reaction liquid from the conductive polymer dispersion to be subjected to the dispersion treatment before the dispersion treatment. Examples of the removal method include a method of contacting the conductive polymer dispersion with an ion exchange resin to adsorb the catalyst and oxidizing agent to the ion exchange resin, and a method of ultrafiltrating the conductive polymer dispersion to replace the dispersion medium and remove the catalyst and oxidizing agent. Among these, the method using an ion exchange resin is preferable because it is simple. It is preferable to use a cation exchange resin and an anion exchange resin in combination as the ion exchange resin.

[0055] <Conductive film and manufacturing method thereof> A third aspect of the present invention is a method for producing a conductive film, comprising a step of applying the conductive polymer dispersion of the first aspect or the coating material of the second aspect to at least one surface of a film substrate to form a coating film.

[0056] A fourth aspect of the present invention is a conductive film comprising a film substrate and a conductive layer formed on at least one surface thereof, the conductive layer being made of the conductive polymer dispersion of the first aspect or a cured layer of the coating material of the second aspect. The conductive film of this aspect can be produced by the production method of the third aspect.

[0057] (Conductive film) The conductive layer of the conductive film of this embodiment contains a conductive complex containing a π-conjugated conductive polymer and a polyanion. When the conductive polymer dispersion applied to the film substrate contains a binder component, the conductive layer contains the binder component or a cured product of the binder component. The average thickness of the conductive layer is preferably 10 nm to 20,000 nm, more preferably 20 nm to 10,000 nm, and even more preferably 30 nm to 5,000 nm. When the average thickness of the conductive layer is equal to or greater than the lower limit, the conductive layer exhibits excellent conductivity, and when the average thickness is equal to or less than the upper limit, the conductive layer is difficult to peel off from the film substrate. The average thickness of the conductive layer is calculated by measuring the thickness at any ten points and averaging the measured values.

[0058] Examples of the film substrate used in the production method of this embodiment include plastic films and paper. Examples of the resin for film substrate constituting the plastic film include ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, cellulose acetate propionate, etc. Among these resins for film substrate, polyethylene terephthalate and cellulose triacetate are preferred because they are inexpensive and have excellent mechanical strength. The resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. Furthermore, the film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesion of the conductive layer formed from the conductive polymer dispersion.

[0059] The average thickness of the film substrate is preferably 10 μm or more and 500 μm or less, and more preferably 20 μm or more and 200 μm or less. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The thickness of the film substrate is determined by measuring the thickness at any ten points and averaging the measured values.

[0060] (Coating process) Examples of the method for applying the conductive polymer dispersion in the application step include application methods using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; spraying methods using a sprayer such as an air spray, an airless spray, or a rotor dampening; and immersion methods such as dipping. Among the above, a bar coater is often used because it allows easy application. The amount of the conductive polymer dispersion applied to the film substrate is not particularly limited, but is preferably 0.1 g / m2 in terms of solid content. 2 More than 10.0g / m 2 The following ranges are preferred:

[0061] (drying process) Examples of methods for drying the coating film include heat drying and vacuum drying. Heat drying can be performed using conventional methods such as hot air heating and infrared heating. When heat drying is used, the heating temperature is appropriately set depending on the dispersion medium used, and can be set to, for example, 50° C. or higher and 150° C. or lower. The heating temperature is the set temperature of the drying device. When the conductive polymer dispersion contains an active energy ray-curable binder component, the method may further include an active energy ray irradiation step of irradiating the dried conductive polymer coating film with active energy rays after the drying step. The active energy ray irradiation step can increase the rate of formation of the conductive layer, thereby improving the productivity of the conductive film. In the case where the active energy ray irradiation step is included, examples of the active energy ray used include ultraviolet rays, electron beams, visible light, etc. Examples of the light source of the ultraviolet ray that can be used include light sources such as ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arcs, xenon arcs, and metal halide lamps. The illuminance of ultraviolet light is 100mW / cm 2 Illuminance of 100mW / cm or more is preferable. 2If the radiation dose is less than 50 mJ / cm2, the active energy ray-curable binder component may not be cured sufficiently. 2 More than 50mJ / cm is preferable. 2 If the irradiance is less than 100 nm, crosslinking may not be sufficient. In this specification, the illuminance and the integrated light amount are values ​​measured using a Topcon UVR-T1 (industrial UV checker, photoreceiver: UD-T36, measurement wavelength range: 300 nm to 390 nm, peak sensitivity wavelength: about 355 nm). EXAMPLES

[0062] (Production Example 1) Production of polystyrene sulfonic acid 206 g of sodium styrenesulfonate was dissolved in 1000 ml of ion-exchanged water, and while stirring at 80° C., 1.14 g of an oxidizing agent solution of ammonium persulfate previously dissolved in 10 ml of water was added dropwise over 20 minutes, and the solution was stirred for 12 hours. 1000ml of sulfuric acid diluted to 10% by mass was added to the obtained sodium polystyrene sulfonate solution, and about 1000ml of the solvent from the obtained polystyrene sulfonic acid solution was removed by ultrafiltration. Next, 2000ml of ion-exchanged water was added to the remaining liquid, and about 2000ml of the solvent was removed by ultrafiltration to wash the polystyrene sulfonic acid with water. This washing operation was repeated three times. Water in the resulting solution was removed under reduced pressure to obtain colorless solid polystyrene sulfonic acid. The weight-average molecular weight Mw of the polystyrene sulfonate (PSS) obtained above was measured by gel permeation chromatography (GPC) using pullulan of known weight-average molecular weight as the standard substance, and was found to be 200,000. The weight-average molecular weight was measured using a Shimadzu Corporation high-performance liquid chromatograph Prominence, with 0.1% NaNO as the solvent. 3The analysis was performed using an aqueous solution, a Shodex OHpack SB-806M HQ column, a RID-20A detector, solvent temperature set to 40°C, flow rate set to 0.6 ml / min, 100 μl of sample injected, and a PSS concentration of 0.1% by mass in the sample, using the analysis software LabSolutions (Shimadzu Corporation). Next, 10 g of the obtained polystyrene sulfonic acid was dissolved in 90 g of ion-exchanged water to obtain a 10% by mass aqueous polystyrene sulfonic acid solution.

[0063] (Production Example 2) Production of polystyrene sulfonic acid A 10% by mass aqueous solution of polystyrene sulfonic acid having a weight average molecular weight of 500,000 was obtained in the same manner as in Production Example 1, except that 1.14 g of ammonium persulfate was changed to 0.86 g.

[0064] (Production Example 3) Production of polystyrene sulfonic acid A 10% by mass aqueous solution of polystyrene sulfonic acid having a weight average molecular weight of 1,000,000 was obtained in the same manner as in Production Example 1, except that 1.14 g of ammonium persulfate was changed to 0.57 g.

[0065] (Production Example 4) Production of polystyrene sulfonic acid A 10% by mass aqueous solution of polystyrene sulfonic acid having a weight average molecular weight of 100,000 was obtained in the same manner as in Production Example 1, except that 1.14 g of ammonium persulfate was changed to 1.71 g.

[0066] (Production Example 5) Production of polystyrene sulfonic acid A 10% by mass aqueous solution of polystyrene sulfonic acid having a weight average molecular weight of 1,200,000 was obtained in the same manner as in Production Example 1, except that 1.14 g of ammonium persulfate was changed to 0.29 g.

[0067] Example 1 0.5 g of 3,4-ethylenedioxythiophene, 1.5 g of the aqueous solution of polystyrene sulfonic acid having a weight average molecular weight of 200,000 of Production Example 1, and 89.5 g of ion-exchanged water were mixed. The resulting mixed solution was kept at 20°C and, while being stirred, an oxidant solution prepared by dissolving 0.03 g of ferric sulfate in 4.97 g of ion-exchanged water and a catalyst solution prepared by dissolving 1.1 g of ammonium persulfate in 8.9 g of ion-exchanged water were slowly added, and the resulting reaction solution was stirred for 24 hours to cause a reaction. By the above reaction, a conductive polymer dispersion liquid containing a conductive complex (PEDOT-PSS) containing poly(3,4-ethylenedioxythiophene) and polystyrenesulfonic acid, which are π-conjugated conductive polymers, and water as a dispersion medium was obtained. The conductive complex obtained here had a PEDOT:PSS (mass ratio) of 1:3.

[0068] To this conductive polymer dispersion, 13.2 g of Duolite C255LFH (Sumika Chemtex Corporation, cation exchange resin) and 13.2 g of Duolite A368S (Sumika Chemtex Corporation, anion exchange resin) were added, and the ion exchange resin was removed by filtration to obtain a conductive polymer dispersion from which the oxidizing agent and catalyst had been removed. The conductive complex concentration in the conductive polymer dispersion thus obtained was about 1.7% by mass.

[0069] The obtained conductive polymer dispersion was dispersed at a rotation speed of 10,000 rpm using a pipeline homogenizer (manufactured by Primix Corporation), which is a dispersing machine. At this time, the temperature inside the holding tank (dispersion sample temperature) in which the conductive polymer dispersion was stored before being supplied to the dispersing machine body was set to 14°C, and the cooling water temperature of the pipeline homogenizer (dispersing machine body) was set to 10°C, and a conductive polymer dispersion with an outlet temperature of 14°C was obtained. In the above dispersion, the conductive polymer dispersion charged in the holding tank (first container) was gradually supplied to the pipeline homogenizer (dispersing machine body) and dispersed, and then sequentially discharged from the pipeline homogenizer at the above outlet temperature and collected in a collection kiln (second container). During this dispersion process, the cooling water temperature of the holding tank and the collection kiln was set to 14°C, and the entire amount of the conductive polymer dispersion was dispersed while keeping the temperature of the conductive polymer dispersion at 14°C. The solid content (non-volatile components) of the conductive polymer dispersion obtained through one-pass dispersion treatment was measured, ion-exchanged water was added to adjust the solid content to 1.3 mass%, and the viscosity and particle size of the conductive polymer dispersion obtained were measured by the methods described below. The results are shown in Table 1A.

[0070] Next, 6.5 g of ion-exchanged water, 7.5 g of methanol, and 15 g of isopropanol were added to 1 g of the conductive polymer dispersion whose viscosity and particle size had been measured to obtain a coating material. The above coating material was applied onto a PET film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater #4, and dried at 100°C for 1 minute to obtain a conductive film. The surface resistance of the conductive film immediately after production was measured using the method described below. The results are shown in Table 1A. Next, the above coating material was left at 25°C for 24 hours, and then coated onto a PET film using a #4 bar coater and dried at 100°C for 1 minute to obtain a conductive film. Here, the surface resistance value of the conductive film immediately after production was measured by the method described below. The results are shown in Table 1A.

[0071] [Method of measuring viscosity] As described above, a conductive polymer dispersion with a concentration of 1.3% by mass in water as a dispersion medium was used as a sample, and measurements were made at 25°C using a tuning fork vibration viscometer (model number: SV-10, manufactured by A&D Corporation) in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer). 1 Pa s (pascal second) was calculated as 1000 cP (centipoise).

[0072] [Method of measuring particle size] As mentioned above, a conductive polymer dispersion with a concentration of 1.3% by mass in water as the dispersion medium was diluted 10 times with distilled water to prepare a sample (i.e., a concentration of 0.13% by mass). The cumulant average particle size was measured at 25°C using the dynamic light scattering method (Zeta potential / particle size / molecular weight measurement system ELSZ-2000ZS, manufactured by Otsuka Electronics Co., Ltd.).

[0073] [Measurement of surface resistance] For the conductive films prepared in each example, the surface resistance value of the conductive layer was measured using a resistivity meter (Hiresta manufactured by Nitto Seiko Analytech Co., Ltd.) under the condition of an applied voltage of 10 V. In the table, "1.0E+09" means "1.0×10 9 " and so on.

[0074] Example 2 Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Example 1, except that in Example 1, the mass ratio of PEDOT:PSS was changed to 1:2 by using 10 g of the polystyrene sulfonic acid aqueous solution of Production Example 1 and 94.5 g of ion-exchanged water. The results are shown in Table 1A.

[0075] Example 3 Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Example 1, except that in Example 1, the mass ratio of PEDOT:PSS was changed to 1:5 by using 25 g of the polystyrene sulfonic acid aqueous solution of Production Example 1 and 79.5 g of ion-exchanged water. The results are shown in Table 1A.

[0076] Comparative Example 1 In Example 1, an attempt was made to prepare a conductive polymer dispersion in the same manner as in Example 1, except that the mass ratio of PEDOT:PSS was changed to 1:1 by using 5 g of the polystyrene sulfonic acid aqueous solution of Production Example 1 and 99.5 g of ion-exchanged water. However, since PEDOT-PSS could not be sufficiently dispersed and a coating material could not be prepared, the attempt was discontinued.

[0077] Comparative Example 2 Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Example 1, except that in Example 1, the mass ratio of PEDOT:PSS was changed to 1:7.5 by using 37.5 g of the polystyrene sulfonic acid aqueous solution of Production Example 1 and 67 g of ion-exchanged water. The results are shown in Table 1A.

[0078] <Summary of Results (1)> In the conductive polymer dispersions of Examples 1 to 3 according to the present invention, the mass ratio of PEDOT:PSS is 1:2 to 1:5, the weight average molecular weight Mw of PSS of PEDOT-PSS is in the range of 200,000 to 1,000,000, and the dispersion is performed at a predetermined temperature using a dispersing machine, so that the viscosity measured under a predetermined condition is 35 cP to 45 cP, and the particle size is less than 500 nm. Therefore, the dispersion stability of the conductive polymer dispersion is excellent, and the increase in the surface resistance value R1 of the conductive layer formed by applying the paint that has been left for 24 hours after preparation is reduced (R1 / R0) and suppressed to 4 times or less, compared with the surface resistance value R0 of the conductive layer formed by applying the paint immediately after preparation. In comparison, in Comparative Examples 7 to 9 described later, R1 / R0 increases by 12 times or more. In Comparative Example 1, the mass ratio of PEDOT:PSS was too low, so that PEDOT-PSS could not be sufficiently dispersed, and a conductive layer could not be formed. In Comparative Example 2, the mass ratio of PEDOT:PSS was too high, and therefore the conductive layer had such high resistance that the conductivity was not measurable.

[0079] (Examples 4 to 6, Comparative Examples 3 to 4) The cooling water temperature of the pipeline homogenizer was set to 15° C., a conductive polymer dispersion was obtained with an outlet temperature of 20° C., and the temperatures of the solutions in the holding tank and the collecting furnace were set to 20° C., and other than that, the tests were performed in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. The results are shown in Table 1A.

[0080] <Summary of Results (2)> In the conductive polymer dispersions of Examples 4 to 6 according to the present invention, the mass ratio of PEDOT:PSS is 1:2 to 1:5, the weight average molecular weight Mw of PSS of PEDOT-PSS is in the range of 200,000 to 1,000,000, and the dispersion is performed at a predetermined temperature using a dispersing machine, so that the viscosity measured under a predetermined condition is 35 cP to 45 cP, and the particle size is less than 500 nm. Therefore, the dispersion stability of the conductive polymer dispersion is excellent, and the increase in the surface resistance value R1 of the conductive layer formed by applying the paint that has been left for 24 hours after preparation is reduced (R1 / R0) and suppressed to 3 times or less, compared with the surface resistance value R0 of the conductive layer formed by applying the paint immediately after preparation. In comparison, in Comparative Examples 7 to 9 described later, R1 / R0 increases by 12 times or more. In Comparative Example 3, the mass ratio of PEDOT:PSS was too low, so that PEDOT-PSS could not be sufficiently dispersed, and a conductive layer could not be formed. In Comparative Example 4, the mass ratio of PEDOT:PSS was too high, and therefore the conductive layer had such high resistance that the conductivity was unmeasurable.

[0081] (Examples 7 to 9, Comparative Examples 5 to 6) The cooling water temperature of the pipeline homogenizer was set to 20° C., a conductive polymer dispersion was obtained with an outlet temperature of 25° C., and the temperatures of the solutions in the holding tank and the collecting kiln were set to 25° C., and other than that, the tests were performed in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. The results are shown in Table 1A.

[0082] <Summary of Results (3)> In the conductive polymer dispersions of Examples 7 to 9 according to the present invention, the mass ratio of PEDOT:PSS is 1:2 to 1:5, the weight average molecular weight Mw of PSS of PEDOT-PSS is in the range of 200,000 to 1,000,000, and the dispersion is performed at a predetermined temperature using a dispersing machine, so that the viscosity measured under a predetermined condition is 35 cP to 45 cP, and the particle size is less than 500 nm. Therefore, the dispersion stability of the conductive polymer dispersion is excellent, and the increase in the surface resistance value R1 of the conductive layer formed by applying the paint that has been left for 24 hours after preparation is reduced (R1 / R0) and suppressed to less than 2 times, compared with the surface resistance value R0 of the conductive layer formed by applying the paint immediately after preparation. In comparison, in Comparative Examples 7 to 9 described later, R1 / R0 increases by 12 times or more. In Comparative Example 5, the mass ratio of PEDOT:PSS was too low, so that PEDOT-PSS could not be sufficiently dispersed, and a conductive layer could not be formed. In Comparative Example 6, the mass ratio of PEDOT:PSS was too high, and therefore the conductive layer had such a high resistance that the conductivity was not measurable.

[0083] (Comparative Examples 7 to 11) The cooling water temperature of the pipeline homogenizer was set to 5° C., a conductive polymer dispersion was obtained with an outlet temperature of 10° C., and the temperatures of the solutions in the holding tank and the collecting kiln were set to 10° C., and the tests were carried out in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. The results are shown in Table 1A.

[0084] <Summary of Results (4)> In Comparative Examples 7 to 9, the viscosity measured under the specified conditions was less than 35 cP, which resulted in poor dispersion stability of the conductive polymer dispersion, and the increase (R1 / R0) in the surface resistance value R1 of the conductive layer formed by applying the coating material that had been left for 24 hours after preparation was greater than the surface resistance value R0 of the conductive layer formed by applying the coating material immediately after preparation, increasing by a factor of 12 or more. In Comparative Example 10, the mass ratio of PEDOT:PSS was too low, so that PEDOT-PSS could not be sufficiently dispersed, and a conductive layer could not be formed. In Comparative Example 11, the mass ratio of PEDOT:PSS was too high, and therefore the conductive layer had such a high resistance that the conductivity was not measurable.

[0085] [Table 1A]

[0086] (Comparative Examples 12 to 16) The cooling water temperature of the pipeline homogenizer was set to 25° C., a conductive polymer dispersion was obtained with an outlet temperature of 30° C., and the temperatures of the solutions in the holding tank and the collecting kiln were set to 30° C., and the tests were carried out in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. The results are shown in Table 1B.

[0087] <Summary of Results (5)> In Comparative Examples 12 to 14, the viscosity measured under the specified conditions exceeded 45 cP, and the particle size was 500 nm or more. Therefore, the dispersion stability of the conductive polymer dispersion was poor, and although it was possible to form a conductive layer by applying the paint immediately after preparation, the paint left for 24 hours after preparation had gelled PEDOT-PSS and the dispersion state had deteriorated, so the experiment was discontinued. In Comparative Example 15, the mass ratio of PEDOT:PSS was too low, so that PEDOT-PSS could not be sufficiently dispersed, and a conductive layer could not be formed. In Comparative Example 16, the mass ratio of PEDOT:PSS was too high, and therefore the conductive layer had such a high resistance that the conductivity was not measurable.

[0088] Example 10 Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Example 1, except that 15 g of the aqueous polystyrene sulfonic acid solution having a weight average molecular weight of 500,000 in Production Example 2 was used. The results are shown in Table 1B.

[0089] Example 11 The cooling water temperature of the pipeline homogenizer was set to 15° C., a conductive polymer dispersion was obtained with an outlet temperature of 20° C., and the temperatures of the solutions in the holding tank and the collecting furnace were set to 20° C., but the test was performed in the same manner as in Example 10. The results are shown in Table 1B.

[0090] Example 12 The cooling water temperature of the pipeline homogenizer was set to 20° C., a conductive polymer dispersion was obtained with an outlet temperature of 25° C., and the temperatures of the solutions in the holding tank and the collecting furnace were set to 25° C., but the same test was performed as in Example 10. The results are shown in Table 1B.

[0091] (Comparative Example 17) The cooling water temperature of the pipeline homogenizer was set to 5° C., a conductive polymer dispersion was obtained with an outlet temperature of 10° C., and the temperatures of the solutions in the holding tank and the collecting furnace were set to 10° C., but the same test was performed as in Example 10. The results are shown in Table 1B.

[0092] (Comparative Example 18) The cooling water temperature of the pipeline homogenizer was set to 25° C., a conductive polymer dispersion was obtained with an outlet temperature of 30° C., and the temperatures of the solutions in the holding tank and the collecting furnace were set to 30° C., but the same test was performed as in Example 10. The results are shown in Table 1B.

[0093] <Summary of Results (6)> In the conductive polymer dispersions of Examples 10 to 12 according to the present invention, the mass ratio of PEDOT:PSS is 1:2 to 1:5, the weight average molecular weight Mw of PSS of PEDOT-PSS is in the range of 200,000 to 1,000,000, and the dispersion is performed at a predetermined temperature using a dispersing machine, so that the viscosity measured under a predetermined condition is 35 cP to 45 cP, and the particle size is less than 500 nm. Therefore, the dispersion stability of the conductive polymer dispersion is excellent, and the increase (R1 / R0) in the surface resistance value R1 of the conductive layer formed by applying the paint that has been left for 24 hours after preparation is reduced and suppressed to 3 times or less, compared with the surface resistance value R0 of the conductive layer formed by applying the paint immediately after preparation. In Comparative Example 17, the viscosity measured under the specified conditions was less than 35 cP, which resulted in poor dispersion stability of the conductive polymer dispersion, and the increase (R1 / R0) in the surface resistance value R1 of the conductive layer formed by applying the coating material that had been left for 24 hours after preparation was 10 times higher than the surface resistance value R0 of the conductive layer formed by applying the coating material immediately after preparation. In Comparative Example 18, the viscosity measured under the specified conditions exceeded 45 cP, and the particle size was 500 nm or more. Therefore, the dispersion stability of the conductive polymer dispersion was poor, and although it was possible to form a conductive layer by applying the paint immediately after preparation, the paint left for 24 hours after preparation had gelled PEDOT-PSS and the dispersion state had deteriorated, so the experiment was discontinued.

[0094] (Examples 13 to 15, Comparative Examples 19 to 20) Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Examples 10 to 12 and Comparative Examples 17 to 18, except that the aqueous polystyrene sulfonic acid solution having a weight average molecular weight of 1,000,000 in Production Example 3 was used. The results are shown in Table 1B.

[0095] <Summary of Results (7)> In the conductive polymer dispersions of Examples 13 to 15 according to the present invention, the mass ratio of PEDOT:PSS is 1:2 to 1:5, the weight average molecular weight Mw of PSS of PEDOT-PSS is in the range of 200,000 to 1,000,000, and the dispersion is performed at a predetermined temperature using a dispersing machine, so that the viscosity measured under a predetermined condition is 35 cP to 45 cP, and the particle size is less than 500 nm. Therefore, the dispersion stability of the conductive polymer dispersion is excellent, and the increase in the surface resistance value R1 of the conductive layer formed by applying the paint that has been left for 24 hours after preparation is reduced (R1 / R0) and is suppressed to 1 time or less, compared with the surface resistance value R0 of the conductive layer formed by applying the paint immediately after preparation. In Comparative Example 19, the viscosity measured under the specified conditions was less than 35 cP, which resulted in poor dispersion stability of the conductive polymer dispersion, and the increase (R1 / R0) in the surface resistance value R1 of the conductive layer formed by applying the coating material that had been left for 24 hours after preparation was 10 times higher than the surface resistance value R0 of the conductive layer formed by applying the coating material immediately after preparation. In Comparative Example 20, the viscosity measured under the specified conditions exceeded 45 cP, and the particle size was 500 nm or more. Therefore, the dispersion stability of the conductive polymer dispersion was poor, and although it was possible to form a conductive layer by applying the paint immediately after preparation, the paint left for 24 hours after preparation had gelled PEDOT-PSS and the dispersion state had deteriorated, so the experiment was discontinued.

[0096] (Comparative Examples 21 to 23) Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Examples 10 to 12, except that the aqueous polystyrene sulfonic acid solution having a weight average molecular weight of 100,000 in Production Example 4 was used. The results are shown in Table 1B.

[0097] <Summary of Results (8)> In Comparative Examples 21 to 23, the viscosity measured under the specified conditions was less than 35 cP, which resulted in poor dispersion stability of the conductive polymer dispersion, and the increase (R1 / R0) in the surface resistance value R1 of the conductive layer formed by applying the coating material that had been left for 24 hours after preparation was 10 times or more higher than the surface resistance value R0 of the conductive layer formed by applying the coating material immediately after preparation.

[0098] (Comparative Examples 24 to 26) Conductive films were produced in two batches and their surface resistance values ​​were measured in the same manner as in Examples 10 to 12, except that the aqueous polystyrene sulfonic acid solution having a weight average molecular weight of 1.2 million in Production Example 5 was used. The results are shown in Table 1B.

[0099] <Summary of Results (9)> In Comparative Examples 24 to 26, the viscosity measured under the specified conditions exceeded 45 cP, and the particle size was 500 nm or more. Therefore, the dispersion stability of the conductive polymer dispersion was poor, and although it was possible to form a conductive layer by applying the paint immediately after preparation, after leaving it for 24 hours after dispersion, the PEDOT-PSS had gelled and the dispersion state had deteriorated, so the experiment was discontinued.

[0100] [Table 1B]

[0101] Example 16 In the same manner as in Example 1, PEDOT-PSS was synthesized, and a conductive polymer dispersion liquid containing water as a dispersion medium was prepared. The conductive polymer dispersion liquid from which the oxidant and catalyst had been removed using an ion exchange resin was obtained. The obtained conductive polymer dispersion was dispersed using a NanoVeita (manufactured by Yoshida Kikai Kogyo Co., Ltd.). The NanoVeita is a homogenizer that uses the shear force of turbulence generated in a fluid by passing the fluid through a nozzle (micro-hole) at high speed and pressure to disperse fine particles in the fluid. The dispersion pressure at the nozzle was set to 150 MPa. The temperature inside the holding tank that stores the conductive polymer dispersion before it is supplied to the nozzle (dispersion sample temperature) was set to 14°C, the temperature of the cooling water around the nozzle (homogenizer cooling water temperature) was set to 10°C, and the outlet temperature of the conductive polymer dispersion discharged from the nozzle and the temperature inside the kiln that collects it (kiln solution temperature) were set to 14°C, and one-pass dispersion processing was performed. The solid content (non-volatile components) of the conductive polymer dispersion obtained through the dispersion treatment was measured, and ion-exchanged water was added to adjust the solid content to 1.3 mass %, and the viscosity and particle size of the conductive polymer dispersion obtained were measured by the above-mentioned method. The results are shown in Table 2. In addition, using the conductive polymer dispersion obtained through the dispersion treatment, a coating material was prepared in the same manner as in Example 1, and conductive films were produced in two batches, and their surface resistance values ​​were measured. The results are shown in Table 2.

[0102] (Example 17) The temperature inside the holding tank (dispersed sample temperature) was set to 20°C, the cooling water temperature around the nozzle of the Nanovater (homogenizer cooling water temperature) was set to 15°C, and the outlet temperature of the conductive polymer dispersion discharged from the nozzle and the temperature inside the kiln for collecting it (solution temperature inside the kiln) were set to 20°C. Except for this, a single-pass dispersion process was performed in the same manner as in Example 16. A conductive polymer dispersion was obtained and a paint was prepared, and conductive films were produced in two batches and their surface resistance values ​​were measured. The results are shown in Table 2.

[0103] (Example 18) The temperature inside the holding tank (dispersion sample temperature) was set to 25°C, the cooling water temperature around the nozzle of the Nanovater (homogenizer cooling water temperature) was set to 20°C, and the outlet temperature of the conductive polymer dispersion discharged from the nozzle and the temperature inside the kiln for collecting it (solution temperature inside the kiln) were set to 25°C. Except for this, a single-pass dispersion process was performed in the same manner as in Example 16. A conductive polymer dispersion was obtained and a paint was prepared, and conductive films were produced in two batches and their surface resistance values ​​were measured. The results are shown in Table 2.

[0104] (Comparative Example 27) The temperature inside the holding tank (dispersion sample temperature) was set to 10°C, the cooling water temperature around the nozzle of the Nanovater (homogenizer cooling water temperature) was set to 5°C, and the outlet temperature of the conductive polymer dispersion discharged from the nozzle and the temperature inside the kiln for collecting it (temperature of the solution inside the kiln) were set to 10°C. Except for this, a single-pass dispersion process was performed in the same manner as in Example 16. A conductive polymer dispersion was obtained and a paint was prepared, and conductive films were produced in two batches and their surface resistance values ​​were measured. The results are shown in Table 2.

[0105] (Comparative Example 28) The temperature inside the holding tank (dispersed sample temperature) was set to 30°C, the cooling water temperature around the nozzle of the Nanovater (homogenizer cooling water temperature) was set to 25°C, and the outlet temperature of the conductive polymer dispersion discharged from the nozzle and the temperature inside the kiln for collecting it (solution temperature inside the kiln) were set to 30°C. Except for this, a single-pass dispersion process was performed in the same manner as in Example 16. A conductive polymer dispersion was obtained and a paint was prepared, and conductive films were produced in two batches and their surface resistance values ​​were measured. The results are shown in Table 2.

[0106] <Summary of Results (10)> In the conductive polymer dispersions of Examples 16 to 18 according to the present invention, the mass ratio of PEDOT:PSS is 1:2 to 1:5, the weight average molecular weight Mw of PSS of PEDOT-PSS is in the range of 200,000 to 1,000,000, and the dispersion is performed at a predetermined temperature using a nanovater, so that the viscosity measured under a predetermined condition is 35 cP to 45 cP, and the particle size is less than 500 nm. Therefore, the dispersion stability of the conductive polymer dispersion is excellent, and the increase (R1 / R0) of the surface resistance value R1 of the conductive layer formed by applying the paint left for 24 hours after preparation is reduced and suppressed to 4 times or less, compared with the surface resistance value R0 of the conductive layer formed by applying the paint immediately after preparation. In Comparative Example 27, the viscosity measured under the specified conditions was less than 35 cP, which resulted in poor dispersion stability of the conductive polymer dispersion, and the increase (R1 / R0) in the surface resistance value R1 of the conductive layer formed by applying a coating material that had been left for 24 hours after preparation was 30 times higher than the surface resistance value R0 of the conductive layer formed by applying a coating material immediately after preparation. In Comparative Example 28, the viscosity measured under the specified conditions exceeded 45 cP, and the particle size was 500 nm or more. Therefore, the dispersion stability of the conductive polymer dispersion was poor, and although it was possible to form a conductive layer by applying the paint immediately after preparation, after leaving it for 24 hours after preparation, the PEDOT-PSS had gelled and the dispersion state had deteriorated, so the experiment was discontinued.

[0107] [Table 2]

Claims

1. a method for producing a conductive polymer dispersion comprising: polymerizing a monomer forming a π-conjugated conductive polymer in a reaction liquid containing the monomer, a polyanion, and water to obtain a conductive polymer dispersion containing a conductive complex containing the π-conjugated conductive polymer and the polyanion, and water; and then dispersing the conductive polymer dispersion, wherein, in the dispersion treatment, the conductive complex is dispersed so that a viscosity at 25° C. is 35 cP or more and 45 cP or less when a concentration of the conductive complex is adjusted to 1.3 mass % with respect to a total mass of the obtained conductive polymer dispersion, the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene) or the polyanion is polystyrenesulfonic acid; a mass ratio of the π-conjugated conductive polymer to the polyanion is from (1:2) to (1:5), and the weight average molecular weight Mw of the polyanion is from 200,000 to 1,000,000; the conductive polymer dispersion before the dispersion treatment is held in a first container adjusted to a temperature of 14° C. or higher and 25° C. or lower, the conductive polymer dispersion is gradually introduced from the first container into a dispersing machine main body, and a high-speed shear force is generated in the conductive polymer dispersion, thereby carrying out the dispersion treatment; The temperature of the conductive polymer dispersion liquid during the dispersion treatment is adjusted to 14° C. or more and 25° C. or less. the conductive polymer dispersion that has been subjected to the dispersion treatment is successively discharged from the disperser body into a second container adjusted to a temperature of 14° C. or higher and 25° C. or lower, and collected.

2. A method for producing a conductive polymer dispersion as described in claim 1, wherein when the concentration of the conductive complex in the conductive polymer dispersion that has undergone the dispersion treatment is adjusted to 0.13 mass %, the particle size at 25°C is less than 500 nm.

3. A step of producing the conductive polymer dispersion by the production method according to claim 1 or 2; A method for producing a conductive film, comprising: applying the conductive polymer dispersion or a coating material containing the conductive polymer dispersion and a water-soluble organic solvent to at least one surface of a film substrate.

Citation Information

Patent Citations

  • Method for preparing conducting polymer aqueous dispersion by conducting polymer solid

    CN102408574A

  • Method for preparing nano-sized PEDOT / PSS aqueous dispersion

    CN107082873A

  • High-solid-content PEDOT-PSS (poly(3,4-ethylenedioxythiophene) / polystyrene sulfonic acid) dispersion and preparation method thereof

    CN109734932A

  • Dispersion and film comprising electroconductive polymer, and optoelectronic device

    JP2005206839A

  • Manufacturing method of conductive polymer solution

    JP2008171761A