Greaseproof Paper

The oil-resistant paper design with a polyvinyl alcohol intermediate layer and styrene-(meth)acrylic copolymer resin surface layer addresses the challenge of achieving both high oil resistance and air permeability, ensuring effective food preservation and flavor retention.

JP7587402B2Active Publication Date: 2024-11-20LINTEC CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020197171
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-27
Publication Date
2024-11-20
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Existing oil-resistant papers face challenges in achieving both high oil resistance and high air permeability, leading to issues such as damage to packaged foods and reduced flavor and preservability due to steam causing pulp fibers to break down, especially when reheated in a microwave.

Method used

An oil-resistant paper design comprising a paper base, an intermediate layer made of polyvinyl alcohol, and a surface layer containing a styrene-(meth)acrylic copolymer resin and a sizing agent, with specific adhesion amounts and compositions to maintain both oil resistance and air permeability.

Benefits of technology

The solution provides oil-resistant paper with high oil resistance and air permeability, preventing oil leakage and maintaining food flavor and preservability even under reheating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587402000003
    Figure 0007587402000003
  • Figure 0007587402000004
    Figure 0007587402000004
  • Figure 0007587402000005
    Figure 0007587402000005
Patent Text Reader

Abstract

To provide oil resistant paper having both high oil resistance and high gas permeability.SOLUTION: There is provided oil resistant paper 1 comprising a paper base material 10, an intermediate layer 20 and a surface layer 30, with the intermediate layer 20 being disposed at least on one surface of the paper base material 10, the surface layer 30 being disposed on the surface of the intermediate layer 20 opposite to the surface thereof whereon the paper base material 10 is disposed, the intermediate layer 20 containing polyvinyl alcohol, and the surface layer 30 containing a styrene-(meth)acrylate copolymer resin and a sizing agent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to greaseproof paper. [Background technology]

[0002] Greaseproof paper is widely used as wrapping paper or packaging containers for cooked foods such as fast food, fried foods, and baked foods that contain a lot of oil and moisture, as well as foods that contain a lot of fats and oils, such as chocolate, or as paper coverings for food trays, etc.

[0003] Generally, fluororesin-based oil-resistant agents are widely used as oil-resistant agents that impart oil resistance to paper, and for example, grease-resistant paper in which an oil-resistant layer is formed by coating a fluororesin-based oil-resistant agent on the surface of a paper substrate, and grease-resistant paper in which a fluororesin-based oil-resistant agent is internally added to a paper substrate are known. However, grease-resistant paper using a fluororesin-based oil-resistant agent is difficult to handle the inert gas generated from the oil-resistant agent during combustion, and there has been a demand for grease-resistant paper that does not contain a fluororesin-based oil-resistant agent.

[0004] For example, Patent Document 1 discloses an example of an grease-resistant paper that does not contain a fluororesin-based grease-resistant agent, which has an undercoat coating layer and a topcoat coating layer on at least one side of a paper base material, in which the undercoat coating layer contains oxidized starch and at least one of a fatty acid sizing agent and an alkyl ketene dimer, and the topcoat coating layer contains oxidized starch and at least one of a styrene-butadiene copolymer and a starch oxide.

[0005] Patent Document 2 discloses an grease-resistant paper having at least one oil-resistant layer mainly composed of an acrylic resin on at least one side of a paper support, in which the acrylic resin has a weight-average molecular weight of 50,000 to 2,000,000 and an acid value of 50 to 200 mg KOH. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2017-119921 A [Patent Document 2] JP 2012-067402 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, when using oil-resistant agents such as starch or acrylic resins, the paper base material is coated with the agent to prevent pinholes from forming in order to achieve the oil-resistant properties, resulting in insufficient air permeability, which makes it difficult for water vapor generated from the packaged food to escape from the oil-resistant paper to the outside, loosening the bonds of the pulp fibers that make up the oil-resistant paper. This leads to problems such as a decrease in oil resistance and a decrease in the flavor and shelf life of the food.

[0008] The level of oil resistance (oil resistance) of greaseproof paper is evaluated by an index called Kit value. Kit value is measured by JAPAN TAPPI Paper and Pulp Testing Method No. 41:2000. However, even if the greaseproof paper has a good Kit value measurement, it may not have sufficient oil resistance when actually used. When the inventors studied this phenomenon, they thought that one of the causes may be that when food or the like packaged in greaseproof paper is reheated in a microwave oven, the steam generated in the microwave oven loosens the bonds of the pulp fibers of the greaseproof paper, making it easier for the oil components contained in the food to penetrate through the front and back surfaces of the greaseproof paper.

[0009] As described above, greaseproof paper that has both high oil resistance and high air permeability at a practical level has not yet been developed, and there is still room for improvement in this regard.

[0010] The present invention has been made in view of the above circumstances, and has an object to provide an greaseproof paper that has both high oil resistance and high air permeability. [Means for solving the problem]

[0011] As a result of intensive research by the inventors in order to achieve the above-mentioned object, they discovered that an greaseproof paper comprising a paper base material, an intermediate layer and a surface layer, the intermediate layer being provided on at least one surface of the paper base material, the surface layer being provided on the surface of the intermediate layer opposite to the side on which the paper base material is provided, the intermediate layer containing polyvinyl alcohol, and the surface layer containing a styrene-(meth)acrylic copolymer resin and a sizing agent, and thus completed the present invention.

[0012] That is, the present invention is as follows.

[0013] (1) The grease-resistant paper includes a paper base material, an intermediate layer, and a surface layer, the intermediate layer being provided on at least one surface of the paper base material, the surface layer being provided on the surface of the intermediate layer opposite to the side on which the paper base material is provided, the intermediate layer containing polyvinyl alcohol, and the surface layer containing a styrene-(meth)acrylic copolymer resin and a sizing agent. (2) The grease-resistant paper according to (1), wherein the sizing agent includes at least one selected from the group consisting of olefin-based sizing agents, rosin-based sizing agents, and alkyl ketene dimer-based sizing agents. (3) The dry adhesion amount of the polyvinyl alcohol in the intermediate layer is 0.2 to 0.6 g / m 2 The grease-resistant paper according to (1) or (2) is characterized in that (4) The grease-resistant paper according to (1) or (2), wherein the intermediate layer is provided on both sides of the paper base material. (5) The intermediate layer is provided on both sides of the paper base material, and the total dry adhesion amount of the polyvinyl alcohol in the intermediate layer on both sides is 0.4 to 1.2 g / m 2 The grease-resistant paper according to (4) is as described above. (6) The grease-resistant paper according to (4) or (5), wherein the surface layer is provided on both sides of the paper base material via the intermediate layer. (7) The dry adhesion amount of the styrene-(meth)acrylic copolymer resin in the surface layer is 1.2 to 3.6 g / m per one side of the paper base material. 2 The greaseproof paper according to any one of (1) to (6), (8) The greaseproof paper according to any one of (1) to (7), wherein the content of the sizing agent in the surface layer is 25 to 75 mass % in terms of solid content. (9) The greaseproof paper according to any one of (1) to (8), wherein the greaseproof paper has an Oken air permeability of 2000 to 80000 seconds according to the JAPAN TAPPI paper pulp testing method. Effect of the Invention

[0014] According to the present invention, it is possible to provide greaseproof paper having both high oil resistance and high air permeability. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view of the greaseproof paper according to the first embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of the greaseproof paper according to the second embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view of the greaseproof paper according to the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content. The present invention can be carried out by appropriately modifying it within the scope of its gist.

[0017] In the drawings, the same elements are given the same reference numerals, and duplicated explanations are omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.

[0018] In addition, in this specification, unless otherwise specified, "(meth)acrylic" includes methacryl and acrylic. For example, (meth)acrylic means methacryl, acrylic, or both.

[0019] FIG. 1 is a schematic cross-sectional view of the greaseproof paper according to the first embodiment.

[0020] The grease-resistant paper 1 according to this embodiment includes a paper base material 10, an intermediate layer 20, and a surface layer 30. The intermediate layer 20 is provided on at least one surface of the paper base material 10, and the surface layer 30 is provided on the surface of the intermediate layer 20 opposite to the side on which the intermediate layer 20 is provided. The intermediate layer 20 contains polyvinyl alcohol, and the surface layer 30 contains a styrene-(meth)acrylic copolymer resin and a sizing agent. That is, the grease-resistant paper 1 has a structure in which the paper base material 10, the intermediate layer 20, and the surface layer 30 are laminated in this order. For example, when the grease-resistant paper 1 is used for food packaging bags, the surface layer 30 is the layer that comes into contact with the food to be stored, and when the grease-resistant paper 1 is processed into a packaging bag, it becomes the inner surface of the bag.

[0021] According to this embodiment, it is possible to obtain a greaseproof paper having both high oil resistance and high air permeability. In a particularly preferred embodiment, even if the greaseproof paper 1 is a greaseproof paper that does not substantially contain a fluororesin, it can exhibit such high oil resistance and high air permeability. Therefore, the greaseproof paper 1 can be suitably used as wrapping paper or wrapping containers for cooked foods such as fast food, fried foods, and baked foods that contain a lot of oil and moisture, and foods that contain a lot of fats and oils such as chocolate, or paper mats such as food trays. Furthermore, it can be suitably used as a non-fluororesin greaseproof paper 1.

[0022] Each component will be described below.

[0023] (Middle class)

[0024] By providing the intermediate layer 20, the coating liquid that will become the surface layer 30 during production can be controlled so that it remains uniformly on the surface of the paper base material 10, and even if the surface layer 30 has a low adhesion amount, it can exhibit sufficient oil resistance. Furthermore, by reducing the total adhesion amount of the surface layer 30 and the intermediate layer 20, it is possible to make the texture of the greaseproof paper 1 closer to that of normal paper. Furthermore, the intermediate layer 20 of the greaseproof paper 1 contains polyvinyl alcohol. By including polyvinyl alcohol in the intermediate layer 20, it is possible to impart excellent oil resistance and moisture permeability to the greaseproof paper.

[0025] Examples of the polyvinyl alcohol used in the intermediate layer 20 include unmodified polyvinyl alcohol and modified polyvinyl alcohol, which include fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol, respectively. Examples of the modified polyvinyl alcohol that can be used include α-olefin modified polyvinyl alcohol, cation modified polyvinyl alcohol, anion modified polyvinyl alcohol, silanol modified polyvinyl alcohol, acetoacetyl modified polyvinyl alcohol, mercapto modified polyvinyl alcohol, etc.

[0026] From the viewpoint of exerting a barrier property sufficient to prevent the surface layer coating liquid (coating liquid constituting the surface layer 30) applied to the surface of the intermediate layer 20 from penetrating to the paper substrate 10, the saponification degree of polyvinyl alcohol, expressed as the molar ratio of saponified ester groups to the ester groups present before saponification, is preferably 80 to 100%. Furthermore, from the viewpoint of imparting appropriate air permeability so as not to trap water vapor derived from food inside the grease-resistant paper bag, the saponification degree is more preferably 90% or more, even more preferably 95% or more, and even more preferably 98% or more.

[0027] From the viewpoints of coatability and barrier property, the degree of polymerization of polyvinyl alcohol is preferably in the range of 200 to 8000. The lower limit of the degree of polymerization is more preferably 300 or more, further preferably 400 or more, and even more preferably 500 or more. The upper limit of the degree of polymerization is more preferably 2500 or less, further preferably 2000 or less, and even more preferably 1800 or less.

[0028] From the viewpoint of further improving the barrier properties of the intermediate layer 20 and the air permeability of the greaseproof paper, it is preferable that the intermediate layer 20 is made of only polyvinyl alcohol. Here, "only" means that nothing other than the component is actively added or mixed, and does not exclude the inevitable inclusion or mixing. In this case, polyvinyl alcohol can be diluted with water to adjust the concentration and viscosity to a level suitable for the coating method. Note that other additives such as dispersants, defoamers, and colorants can also be appropriately selected and used in the intermediate layer 20 as necessary, within a range that does not impair the effects of this embodiment.

[0029] The dry adhesion amount of polyvinyl alcohol in the intermediate layer 20 is 0.2 to 0.6 g / m 2 It is preferable that the dry adhesion amount is 0.25 g / m. For example, when the intermediate layer 20 is provided only on one side of the paper base material 10, the dry adhesion amount is the dry adhesion amount per one side of the paper base material 10. Also, for example, when the intermediate layer 20 and the intermediate layer 40 are provided on both sides of the paper base material 10 with the same area (see FIG. 2, for example), the dry adhesion amount is 1 / 2 the total dry adhesion amount of the intermediate layer 20 and the intermediate layer 40. The lower limit of this dry adhesion amount is 0.25 g / m. 2 More preferably, it is 0.3 g / m or more. 2 The upper limit of the dry coating weight is 0.55 g / m or more. 2 More preferably, it is 0.5 g / m or less. 2 It is even more preferable that:

[0030] (Surface layer)

[0031] The surface layer 30 contains a styrene-(meth)acrylic copolymer resin and a sizing agent. The combination of a styrene-(meth)acrylic resin with high barrier properties and a sizing agent contributes to maintaining both oil resistance and moisture permeability at a high level. The styrene-(meth)acrylic resin means a styrene-acrylic resin, a styrene-methacrylic resin, or both.

[0032] When used as wrapping paper or packaging containers for foods that contain a lot of fat and oil, such as fast food, fried foods, and baked foods that contain a lot of oil and moisture, or foods that contain a lot of fat, such as chocolate, or as paper linings such as food trays, the foods are heated in a microwave oven. In such practical environments, there is a problem that the oil resistance and air permeability of the greaseproof paper cannot be maintained at a practical level.

[0033] The inventors of the present invention have studied this problem and found that when the pulp fibers are bonded to each other by coating the surface of the paper base material 10 with a highly film-forming styrene-(meth)acrylic copolymer resin, the oil resistance of the paper is improved, but the water vapor generated in the microwave oven is trapped, degrading the flavor and texture of the food. When the amount of the styrene-(meth)acrylic copolymer resin coating is reduced, the fibers of the paper base material 10 are loosened by the water vapor generated in the microwave oven, and the oil resistance of the oil-resistant paper is insufficient. Therefore, it was thought that such a problem could not be solved by controlling the film-forming properties of the styrene-(meth)acrylic copolymer resin. As a result of further intensive research based on this idea, it was unexpectedly possible to improve the moisture permeability without reducing the barrier properties of the surface layer by blending polyvinyl alcohol in the intermediate layer 20 and using not only the styrene-(meth)acrylic copolymer resin but also a sizing agent in the surface layer 30. It is believed that this makes it possible to maintain high levels of oil resistance, air permeability, and even moisture permeability in practical environments (however, the action of this embodiment is not limited to these).

[0034] Styrene-(meth)acrylic copolymer resin has high barrier properties and excellent water resistance, and also has an effect of improving the oil resistance of the intermediate layer 20. There are no particular limitations on the styrene-(meth)acrylic copolymer resin, and any known resin can be used.

[0035] Examples of the constituent monomers of the styrene-(meth)acrylic copolymer resin include copolymers containing at least a styrene-based monomer and a (meth)acrylic monomer. In addition, other monomers copolymerizable with the constituent monomer components of the styrene-(meth)acrylic copolymer resin can be used in combination as necessary, so long as the monomer composition of the copolymer resin is satisfied. In the styrene-(meth)acrylic copolymer resin, the ratio of the styrene-based monomer and the (meth)acrylic monomer in the constituent monomers is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and even more preferably 90 mol% or more, and even more preferably is a copolymer of only these two monomers. The term "substantially" used here does not exclude so-called unavoidably contained or mixed components.

[0036] The styrene-based monomer is not particularly limited, and examples thereof include styrene, α-methylstyrene, β-methylstyrene, 2,4-dimethylstyrene, α-ethylstyrene, α-butylstyrene, 4-methoxystyrene, vinyltoluene, and the like.

[0037] The (meth)acrylic monomer is not particularly limited, and examples thereof include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, and n-butyl (meth)acrylate; (meth)acrylic acid ester derivatives such as 3-ethoxypropyl acrylate, 3-ethoxybutyl acrylate, and hydroxyethyl methacrylate; aryl acrylates and aralkyl acrylates such as phenyl acrylate and benzyl acrylate; and monoacrylic acid esters of polyhydric alcohols such as diethylene glycol, triethylene glycol, and glycerin.

[0038] The weight average molecular weight of the styrene-(meth)acrylic copolymer resin is preferably 10,000 to 5,000,000. The lower limit of this weight average molecular weight is more preferably 50,000 or more, and even more preferably 200,000 or more. The upper limit of this weight average molecular weight is more preferably 2,000,000 or less, and even more preferably 800,000 or less. Within such a range, it is possible to achieve a balance between oil resistance and air permeability at an even higher level.

[0039] The glass transition point of the styrene-(meth)acrylic copolymer resin is preferably −50 to 100° C. The lower limit of the glass transition point is more preferably −30° C. or higher, and even more preferably −20° C. or higher. The upper limit of the glass transition point is more preferably 30° C. or lower, and even more preferably 10° C. or lower. Within the above range, the oil resistance is excellent.

[0040] The dry adhesion amount of the styrene-(meth)acrylic copolymer resin in the surface layer 30 is 1.2 to 3.6 g / m per one side of the paper base material 10. 2 The lower limit of the dry coating weight is preferably 1.5 g / m 2 More preferably, it is 2.0 g / m or more. 2 The upper limit of the dry coating weight is 3.0 g / m or more. 2More preferably, it is 2.5 g / m or less. 2 If the dry adhesion amount of the styrene-(meth)acrylic copolymer resin is within this range, condensation is unlikely to occur even when food is heated in a microwave oven or the like, while maintaining a higher level of oil resistance and practical oil resistance.

[0041] The sizing agent can impart a sufficient level of oil resistance to the surface layer 30. Examples of the sizing agent include olefin-based sizing agents, rosin-based sizing agents, acrylic-based sizing agents, polyacrylamide-based sizing agents, styrene-maleic acid-based sizing agents, acrylic copolymer-based sizing agents, acrylic emulsion-based sizing agents, olefin-maleic acid resin-based sizing agents, urethane-based sizing agents, AKD (alkyl ketene dimer)·ASA (alkenyl succinic anhydride)-based sizing agents, and petroleum resin-based sizing agents. Among these, it is preferable to include at least one selected from the group consisting of olefin-based sizing agents, rosin-based sizing agents, and alkyl ketene dimer-based sizing agents. The ionic nature of the sizing agent may be any of cationic, anionic, and nonionic, but anionic is preferred.

[0042] The content of the sizing agent in the surface layer 30 is preferably 25 to 75 mass % in terms of solid content. The lower limit of this content is more preferably 35 mass % or more, and even more preferably 40 mass % or more. The upper limit of this content is more preferably 65 mass % or less, and even more preferably 60 mass % or less.

[0043] The content ratio of the sizing agent to the styrene-(meth)acrylic copolymer resin in the surface layer 30 (sizing agent / styrene-(meth)acrylic copolymer) is not particularly limited, but is preferably, for example, 25 to 75 mass%. The lower limit of this ratio is more preferably 35 mass% or more, and even more preferably 40 mass% or more. The upper limit of this ratio is more preferably 65 mass% or less, and even more preferably 60 mass% or less.

[0044] Other additives such as a dispersant, an antifoaming agent, and a colorant may be appropriately selected and used as necessary in the surface layer 30 within a range that does not impair the effects of the present embodiment. In addition, it is preferable that the surface layer 30 does not contain a fluorine-based resin.

[0045] According to this embodiment, the surface layer 30 may be a single layer, or may be a multi-layer structure of two or more layers.

[0046] Furthermore, according to this embodiment, in addition to the intermediate layer 20 and the surface layer 30, other functional layers (e.g., a printing layer, a print-receiving layer, an adhesive layer for bag-making processing) may be provided. For example, a functional layer such as a printing layer or a cover layer may be provided on the surface of the surface layer 30. For example, when used as a food packaging bag, a printing layer may not be provided on the inner surface that comes into contact with the food, but a printing layer may be provided on the outer surface.

[0047] (Paper base material)

[0048] The paper substrate 10 is not particularly limited and can be appropriately selected depending on the application, and examples thereof include bleached or unbleached kraft paper (acidic paper or neutral paper), fine paper, medium quality paper, lightly coated paper, coated paper, liner, semi-glassine paper, glassine paper, one-sided gloss paper, parchment paper, white paperboard, etc. Among these, glassine paper is preferable from the viewpoint of oil resistance.

[0049] Examples of the pulp constituting the paper base material 10 include wood pulp, non-wood pulp, waste paper pulp, and synthetic fiber pulp. Examples of wood pulp include chemical pulp and mechanical pulp of softwood and hardwood. Examples of non-wood pulp include kenaf pulp, bagasse pulp, rag pulp, linen pulp, hemp pulp, paper mulberry pulp, mitsumata pulp, gampi pulp, straw pulp, and bamboo pulp. Examples of waste paper pulp include magazine waste paper, flyer waste paper, colored waste paper, newspaper waste paper, Kent waste paper, white waste paper, coated waste paper, photocopy waste paper, and broke waste paper. Examples of synthetic fiber pulp include rayon resin, vinylon resin, polyolefin resin, polyester resin, acrylic resin, polyamide resin, polyparaphenylene resin, and polyurethane resin.

[0050] Among these, it is preferable to contain chemical pulp such as hardwood bleached kraft pulp (LBKP), softwood bleached kraft pulp (NBKP), hardwood bleached sulfite pulp (LBSP), and softwood bleached sulfite pulp (NBSP).

[0051] Other additives such as sizing agents (alkyl ketene dimers, alkenyl succinic anhydrides, higher fatty acids, petroleum resins, rosin, etc.), paper strength agents (starch, polyacrylamide, polyamidoamine-epichlorohydrin, etc.), retention aids, drainage aids, aluminum sulfate, pH adjusters, defoamers, pitch control agents, slime control agents, etc. may be appropriately selected and used in the paper base material 10 as needed, so long as they do not impair the effects of this embodiment.

[0052] The basis weight of the paper base material 10 is 20 to 150 g / m 2 The lower limit of the basis weight is preferably 25 g / m 2 More preferably, it is 30 g / m or more. 2 More preferably, it is 35 g / m or more. 2 It is even more preferable that the basis weight is 80 g / m or more. 2 More preferably, it is 70 g / m or less. 2More preferably, it is 60 g / m or less. 2 It is even more preferable that the basis weight is not more than 100%. This basis weight is a value measured based on the basis weight testing method of JIS P 8124: 2011. If the lower limit of the basis weight is within this range, the strength of the greaseproof paper is further improved, and if the upper limit of the basis weight is within this range, the cost is not high.

[0053] The thickness of the paper substrate 10 is preferably 20 to 150 μm. The lower limit of the thickness is more preferably 25 μm or more, even more preferably 30 μm or more, and even more preferably 35 μm or more. The upper limit of the thickness is more preferably 80 μm or less, even more preferably 70 μm or less, and even more preferably 60 μm or less.

[0054] The paper base material 10 can be manufactured by a known method. For example, softwood pulp and hardwood pulp are dispersed in water in a predetermined mass ratio, and the pulp is beaten to a predetermined degree by a beater to obtain a pulp slurry. Then, additives and the like are added to the obtained pulp slurry as desired. The prepared slurry is made into paper using a known papermaking machine such as a Fourdrinier papermaking machine, a cylinder papermaking machine, or a twin-wire papermaking machine to obtain the paper base material 10. The papermaking method is not particularly limited, and either acidic papermaking or neutral papermaking can be selected.

[0055] A preferred method for forming the intermediate layer 20 is an external addition method in which the intermediate layer 20 is applied and / or impregnated after the paper substrate 10 is made. For example, the intermediate layer 20 can be formed by preparing a coating liquid for forming the intermediate layer 20 as an aqueous dispersion having a solid content concentration of 0.01 to 30% by mass, and applying the coating liquid to one side or both sides of the paper substrate 10 using a coating machine such as a bar coater, die coater, gravure coater, roll coater, blade coater, air knife coater, or size press coater. An air knife coater or size press coater is preferred because it is easy to localize the components of the intermediate layer 20 near the surface of the paper substrate 10.

[0056] The method for forming the surface layer 30 is preferably an external addition method, similar to the intermediate layer 20. For example, the coating liquid for forming the surface layer 30 is made into an aqueous dispersion having a solid content concentration of 0.01 to 10% by mass, and the surface layer 30 can be formed on the surface having at least the intermediate layer 20 using a coating machine such as a bar coater, die coater, gravure coater, roll coater, blade coater, air knife coater, or size press coater. A bar coater or air knife coater is preferred because it is easy to form a uniform coating film.

[0057] After coating, the greaseproof paper may be subjected to a calendering process using a calendering device such as a machine calender, a heat calender, a super calender, or a soft calender.

[0058] The thickness of the greaseproof paper 1 is preferably 20 to 150 μm. The lower limit of this thickness is more preferably 30 μm or more, even more preferably 35 μm or more, and even more preferably 40 μm or more. The upper limit of this thickness is more preferably 100 μm or less, even more preferably 80 μm or less, and even more preferably 70 μm or less. If the thickness is within this range, sufficient strength and oil resistance can be imparted to the paper for use as a base material for food packaging.

[0059] (Oil resistance) The oil resistance of the greaseproof paper, measured on the surface of the surface layer 30 in accordance with JAPAN TAPPI Paper and Pulp Testing Method No. 41:2000, is preferably 5 or more. If the greaseproof paper 1 having the configuration of this embodiment has a kit value of 5 or more, it can exhibit sufficient oil resistance (particularly practical oil resistance) as an greaseproof paper used in a standard environment.

[0060] (Practical oil resistance) In this embodiment, practical oil resistance refers to the resistance to oil stains that appear when edible oil actually used is dropped onto the surface layer of the greaseproof paper and penetrates from the surface layer to the inside. A specific method for evaluating practical oil resistance is as described in the examples described later.

[0061] (Condensation prevention) In this embodiment, the condensation suppression property indicates the degree of grease resistance when the greaseproof paper is exposed to high humidity. For example, when food such as French fries is placed in a bag made of greaseproof paper and the food is reheated in a microwave oven, the water vapor generated from the food condenses, loosening the bonds of the pulp of the greaseproof paper, and the oil in the food is likely to leak out of the bag. In other words, it can be said that a greaseproof paper with high condensation suppression property that allows water vapor to pass from the inside of the bag to the outside is excellent in the resistance to oil passing through. A specific method for evaluating the condensation suppression property is as described in the examples described later.

[0062] (Air permeability) The air permeability of the greaseproof paper 1, measured on the surface of the surface layer 30, is preferably 2000 to 100000 seconds or less, as measured by the Oken air permeability according to JAPAN TAPPI Paper and Pulp Testing Method No. 5-2:2000. The upper limit is more preferably 80000 seconds or less, more preferably 70000 seconds or less, and even more preferably 60000 seconds or less. The lower limit is more preferably 3000 seconds or more, more preferably 5000 seconds or more, and even more preferably 10000 seconds or more. According to this embodiment, the Oken air permeability can be set to the above upper limit or less, so that the air permeability of the greaseproof paper is high enough to withstand practical use, and the deterioration of the flavor and storage stability of food can be effectively prevented.

[0063] FIG. 2 is a schematic cross-sectional view of the greaseproof paper according to the second embodiment.

[0064] The grease-resistant paper 2 according to this embodiment differs from the grease-resistant paper 1 shown in Fig. 1 in that intermediate layers 20, 40 are provided on both sides of the paper base material 10. Thus, according to this embodiment, the intermediate layer 20 (for example, on the inner side that encases food when used as a packaging bag for food, etc.) and the intermediate layer 40 (for example, on the outer side when used as a packaging bag for food, etc.) may be provided on both sides of the paper base material 10. This intermediate layer 40 can be formed by a method similar to the method for forming the intermediate layer 20 described above.

[0065] When the intermediate layers 20, 40 are provided on both sides of the paper base material 10, the total dry adhesion amount of polyvinyl alcohol in the intermediate layers 20, 40 on both sides of the paper base material 10 is 0.4 to 1.2 g / m 2 The total amount of dry adhesion is preferably 1 m 2 This refers to the total dry adhesion amount of polyvinyl alcohol on the entire paper base material 10, and refers to the dry adhesion amount on both sides. That is, in the case of the paper base material 10, it refers to the sum of the dry adhesion amount of polyvinyl alcohol on the intermediate layer 20 and the dry adhesion amount of polyvinyl alcohol on the intermediate layer 40. The lower limit of this total amount is 0.45 g / m 2 More preferably, it is 0.55 g / m or more. 2 More preferably, it is 0.6 g / m or more. 2 It is even more preferable that the total amount is equal to or more than 1.1 g / m. 2 More preferably, it is 1.0 g / m or less. 2 More preferably, it is 0.9 g / m or less. 2 Even more preferably, it is:

[0066] FIG. 3 is a schematic cross-sectional view of the greaseproof paper according to the third embodiment.

[0067] The grease-resistant paper 3 according to this embodiment differs from the grease-resistant paper 1 shown in Figure 1 in that intermediate layers 20, 40 are provided on both sides of the paper base material 10, and surface layers 30, 50 are also provided on both sides of the paper base material. In other words, the grease-resistant paper 3 is an embodiment in which a surface layer 50 is further provided on the surface of the intermediate layer 40 of the grease-resistant paper 2 shown in Figure 2.

[0068] In this manner, in this embodiment, the surface layers 30, 50 may be provided on both sides of the paper base material 10 via the intermediate layers 20, 40. For example, when used as a packaging bag for food or the like, the surface layer 30 becomes the inner side that encases the food, and the surface layer 50 becomes the outer side. The surface layer 50 can be formed by the same method as the method for forming the surface layer 30 described above. The material, dimensions, shape, etc. of the surface layer 50 may be the same as or different from the surface layer 30. EXAMPLES

[0069] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples. Note that % and parts represent mass % and mass parts unless otherwise specified.

[0070] <Example 1>

[0071] (Preparation of Paper Base Material 10)

[0072] Pulp consisting of 25% by mass of softwood bleached kraft pulp (NBKP) and 75% by mass of hardwood bleached kraft pulp (LBKP) was beaten to a degree of beating of 55°SR according to the Shopper-Rigler method, and dispersed in water to a pulp slurry concentration of approximately 2.7% by mass to obtain a pulp slurry.

[0073] To 100 parts by mass of pulp in this pulp slurry, 2.0 parts by mass of a sizing agent (manufactured by Arakawa Chemical Industries, Ltd., product name: Sizepine N-775), 1.0 part by mass of starch (manufactured by GSL Japan, Inc., product name: Geltron 245), 1.3 parts by mass of a wet strength agent (manufactured by Seiko PMC Corporation, product name: Shikiryoku WS-4020), and 4.0 parts by mass of aluminum sulfate (manufactured by Asahi Chemical Industries, Ltd., liquid aluminum sulfate) were added, and the slurry was spun to a thickness of 60 μm and a basis weight of 40 g / m using a Fourdrinier multi-cylinder papermaking machine. 2 The glassine paper was made into a paper base material 10.

[0074] (Formation of intermediate layers 20, 40)

[0075] On both sides of the obtained paper base material 10, a coating liquid for an intermediate layer (coating liquid for an intermediate layer) containing 4.0 parts by mass of modified polyvinyl alcohol (PVA, manufactured by Mitsubishi Chemical Corporation, product name: Gohsenol T-350, saponification degree 93 to 95 mol%) and 96.0 parts by mass of water was applied by a size press to a total amount (wet adhesion amount) of 20 g / m on both sides of the paper base material 10. 2 The total dry adhesion amount of polyvinyl alcohol on both sides was 0.8 g / m 2 (Dry adhesion on one side is 0.4g / m 2) was.

[0076] (Formation of surface layer 30)

[0077] Next, a coating liquid for the surface layer (coating liquid for the surface layer) containing 12 parts by mass of styrene-acrylic copolymer resin (manufactured by Henkel Japan, product name: AQUENCE EPIX BC-900F), 12 parts by mass of an olefin-based sizing agent (manufactured by Arakawa Chemical Industries, product name: POLYMARON LM-25S) as a sizing agent, and 76 parts by mass of water was applied in an amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-acrylic copolymer resin and the sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and greaseproof paper 2 (sample) having the structure shown in FIG.

[0078] <Example 2>

[0079] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0080] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0081] (Formation of surface layer 30) Next, a coating liquid for the surface layer containing 12 parts by mass of a styrene-acrylic copolymer resin (manufactured by Henkel Japan, product name: AQUENCE EPIX BC-900F), 12 parts by mass of an alkyl ketene dimer sizing agent (manufactured by Arakawa Chemical Industries, product name: SKS-L20) as a sizing agent, and 76 parts by mass of water was applied at a rate of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-acrylic copolymer resin and the sizing agent was 4.8 g / m 2Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and greaseproof paper 2 (sample) having the structure shown in FIG.

[0082] <Example 3>

[0083] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0084] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0085] (Formation of surface layer 30) Next, a coating liquid for the surface layer containing 12 parts by mass of a styrene-acrylic copolymer resin (manufactured by Henkel Japan, product name: AQUENCE EPIX BC-900F), 12 parts by mass of a rosin-based sizing agent (manufactured by Arakawa Chemical Industries, product name: Size Pine N-775) as a sizing agent, and 76 parts by mass of water was applied at a coating amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-acrylic copolymer resin and the sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and greaseproof paper 2 (sample) having the structure shown in FIG.

[0086] <Example 4>

[0087] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0088] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0089] (Formation of surface layer 30) Next, a coating liquid for the surface layer containing 9 parts by mass of styrene-acrylic copolymer resin (manufactured by Henkel Japan, product name: AQUENCE EPIX BC-900F), 15 parts by mass of an olefin-based sizing agent (manufactured by Arakawa Chemical Industries, product name: POLYMARON LM-25S) as a sizing agent, and 76 parts by mass of water was applied at a coating amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-acrylic copolymer resin and the sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and greaseproof paper 2 (sample) having the structure shown in FIG.

[0090] <Example 5>

[0091] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0092] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0093] (Formation of surface layer 30) Next, a coating solution for the surface layer containing 15 parts by mass of styrene-acrylic copolymer resin (manufactured by Henkel Japan, product name: AQUENCE EPIX BC-900F), 9 parts by mass of an olefin-based sizing agent (manufactured by Arakawa Chemical Industries, product name: POLYMARON LM-25S) as a sizing agent, and 76 parts by mass of water was applied at a coating amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-acrylic copolymer resin and the sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and greaseproof paper 2 (sample) having the structure shown in FIG.

[0094] <Example 6>

[0095] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0096] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0097] (Formation of surface layer 30) Next, a coating solution for the surface layer containing 8 parts by mass of styrene-acrylic copolymer resin (Henkel Japan, product name: AQUENCE EPIX BC-900F), 8 parts by mass of an olefin-based sizing agent (Arakawa Chemical Industries, product name: POLYMARON LM-25S) as a sizing agent, and 84 parts by mass of water was applied at a coating amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-acrylic copolymer resin and the sizing agent was 3.2 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and greaseproof paper 2 (sample) having the structure shown in FIG.

[0098] <Comparative Example 1>

[0099] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0100] (Formation of surface layer 30) The obtained paper base material 10 was not subjected to size pressing, and the surface layer 30 was formed directly on the surface of the paper base material 10. Specifically, the surface layer coating liquid used in Example 1 was prepared. Then, without providing the intermediate layers 20 and 40, the surface layer coating liquid was applied in an amount of 20 g / m 2 The surface layer 30 was formed by applying the styrene-acrylic copolymer resin and the sizing agent to one side of the paper substrate 10 so that the total dry adhesion amount was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and a greaseproof paper (sample) was obtained.

[0101] <Comparative Example 2>

[0102] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0103] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0104] (Formation of surface layer 30) Next, the surface layer coating liquid was applied to one side of the intermediate layer 20 of the paper base material 10 in the same manner as in Example 1, except that the surface layer coating liquid was formulated without adding a sizing agent. The dry adhesion amount of the styrene-acrylic copolymer resin in this case was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and a greaseproof paper (sample) was obtained.

[0105] <Comparative Example 3>

[0106] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0107] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0108] (Formation of surface layer 30) Next, a coating solution for the surface layer containing 12 parts by mass of styrene-butadiene copolymer resin (manufactured by Nippon A&L Co., Ltd., product name: Latex SN-309R), 12 parts by mass of an olefin-based sizing agent (manufactured by Arakawa Chemical Industries Co., Ltd., product name: Polymeron LM-25S) as a sizing agent, and 76 parts by mass of water was applied in an amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the styrene-butadiene copolymer resin and the sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and a greaseproof paper (sample) was obtained.

[0109] <Comparative Example 4>

[0110] (Preparation of Paper Base Material 10) A paper base 10 was obtained in the same manner as in Example 1, except that no sizing agent was used in the formulation of the pulp slurry.

[0111] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0112] (Formation of surface layer 30) The surface layer coating liquid used in Comparative Example 3 was prepared and applied to one side of the intermediate layer 20 of the paper base material 10 in the same manner as in Comparative Example 3. The total dry adhesion amount of the styrene-butadiene copolymer resin and sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and an greaseproof paper (sample) was obtained.

[0113] <Comparative Example 5>

[0114] (Preparation of Paper Base Material 10) In the same manner as in Comparative Example 4, a paper base 10 was obtained.

[0115] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0116] (Formation of surface layer 30) Next, a surface layer coating liquid was prepared in the same manner as in Comparative Example 4, except that a surface layer coating liquid without the addition of a sizing agent was formulated, and this was applied to one side of the intermediate layer 20 of the paper base material 10. The dry adhesion amount of the styrene-butadiene copolymer resin at this time was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and an greaseproof paper (sample) was obtained.

[0117] <Comparative Example 6>

[0118] (Preparation of Paper Base Material 10) In the same manner as in Example 1, a paper base 10 was obtained.

[0119] (Formation of intermediate layers 20, 40) In the same manner as in Example 1, intermediate layers 20 and 40 were provided on both sides of the paper base material 10 .

[0120] (Formation of surface layer 30) Next, a surface layer coating solution containing no resin (see "Resin (a)" in Table 1) but 24 parts by mass of an olefin-based sizing agent (manufactured by Arakawa Chemical Industries, Ltd., product name: Polymaron LM-25S) as a sizing agent and 76 parts by mass of water was applied in an amount of 20 g / m using the air knife of the papermaking machine. 2 The total dry adhesion amount of the resin and sizing agent was 4.8 g / m 2 Thereafter, the paper was subjected to a calendaring process so that the thickness of the paper became 55 μm, and an greaseproof paper (sample) was obtained.

[0121] <Evaluation method>

[0122] The physical properties of each of the obtained greaseproof papers were evaluated according to the methods described below.

[0123] (Air permeability) The air permeability of the greaseproof paper was measured on the surface of the surface layer 30 by Oken air permeability measurement in accordance with JAPAN TAPPI Paper and Pulp Testing Method No. 5-2:2000.

[0124] (moisture permeability) The moisture permeability was measured according to JIS Z 0208:1976.

[0125] (Oil resistance) The oil resistance of the greaseproof paper, with the surface of the surface layer 30 as the measuring surface, was measured in accordance with JAPAN TAPPI Paper and Pulp Testing Method No. 41:2000.

[0126] (Practical oil resistance) The surface of each of the obtained grease-resistant papers was used as a measurement surface, and edible oil (manufactured by Nisshin Oillio Co., Ltd., product name "Canola Oil") was dropped onto the measurement surface. After 30 minutes at room temperature, traces of edible oil penetration onto the measurement surface were visually confirmed. ○: Even after wiping the measurement surface, no traces of edible oil penetration were found. ×: Traces of edible oil penetration (oil stains) were observed on the measurement surface.

[0127] (Condensation prevention) Bag making Each of the obtained greaseproof papers was processed into a bag without a gusset, measuring 120 mm wide by 90 mm long, and both the left and right ends were glued together so that only the top end of the bag was open. ·Conditions and criteria for adding moisture After the bags were made, 70g of fried potatoes cooked in oil were placed in the paper sample. The bags were heated in a microwave oven at 500W for 30 seconds. After the heat treatment, the adhesion of droplets consisting of oil or water droplets to the inner surface of the bags was observed. If the droplets had disappeared after 30 minutes of storage at room temperature, it was determined that the droplets formed inside the bag were water droplets and that the water vapor permeability was poor. If the droplets remained, it was determined that the droplets formed inside the bag were oil and that there was no problem with the water vapor permeability. ○: There were no water droplets inside the bag. ×: Water droplets were found inside the bag.

[0128] The manufacturing conditions and evaluation results of each Example and Comparative Example are shown in Tables 1 and 2. Note that the "dry adhesion weight (both sides)" of the intermediate layer in the tables refers to the total dry adhesion weight of both the intermediate layer 20 and the intermediate layer 40 of the paper base material 10. The dry adhesion weight of one side of the intermediate layer 20 or the intermediate layer 40 is 1 / 2 this value. For example, when the "dry adhesion weight (both sides)" of the intermediate layer in Table 1 is 0.8 g / m 2 In this case, the total dry coating weight of both the intermediate layer 20 and the intermediate layer 40 is 0.8 g / m 2 and the dry coating weight of one side of the intermediate layer or intermediate layer 40 is 0.4 g / m 2 In addition, the "total ((a) + (b)) dry adhesion amount" of the surface layer in the table is the sum of the dry adhesion amounts of the resin (a) and the sizing agent (b).

[0129] [Table 1]

[0130] [Table 2]

[0131] From the above, it was confirmed that this example at least provides an greaseproof paper having both high oil resistance and high air permeability. Furthermore, it was also confirmed that such excellent effects can be obtained even with a non-fluorine resin-based greaseproof paper that does not contain a fluorine resin, as in this example. [Explanation of symbols]

[0132] 1,2,3: Greaseproof paper 10:Paper base material 20,40: Middle class 30,50: Surface layer

Claims

1. The greaseproof paper includes a paper base material, an intermediate layer, and a surface layer, The intermediate layer is provided on at least one surface of the paper base material, the surface layer is provided on a surface of the intermediate layer opposite to a surface on which the paper base material is provided, The intermediate layer contains polyvinyl alcohol, the surface layer contains a styrene-(meth)acrylic copolymer resin and a sizing agent, The content of the sizing agent in the surface layer is 25 to 75 mass% in terms of solid content. Greaseproof paper.

2. The sizing agent includes at least one selected from the group consisting of an olefin-based sizing agent, a rosin-based sizing agent, and an alkyl ketene dimer-based sizing agent.

2. The greaseproof paper according to claim 1.

3. The dry adhesion amount of the polyvinyl alcohol in the intermediate layer is 0.2 to 0.6 g / m 2 That is, 3. The greaseproof paper according to claim 1 or 2.

4. The intermediate layer is provided on both sides of the paper base material.

3. The greaseproof paper according to claim 1 or 2.

5. The intermediate layer is provided on both sides of the paper base material, The total dry adhesion amount of the polyvinyl alcohol in the intermediate layer on both sides is 0.4 to 1.2 g / m 2 That is, The greaseproof paper according to claim 4.

6. The surface layer is provided on both sides of the paper base material via the intermediate layer. The greaseproof paper according to claim 4 or 5.

7. The dry adhesion amount of the styrene-(meth)acrylic copolymer resin in the surface layer is 1.2 to 3.6 g / m per one side of the paper base material. 2That is, The greaseproof paper according to any one of claims 1 to 6.

8. The grease-resistant paper has an Oken air permeability of 2000 to 80000 seconds according to the JAPAN TAPPI paper pulp testing method. The greaseproof paper according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Oil-resistant paper

    JP2004019036A

  • Fibrous structure and package

    JP2004244729A

  • Water-resistant and oil-resistant paper

    JP2005082919A

  • Oilproof paper