Adhesive tape and method for manufacturing semiconductor wafer
The adhesive tape with controlled weight loss and peel strength properties addresses the issue of peeling at high temperatures by using specific polymers and crosslinking, ensuring reliable handling and easy removal post-processing.
Patent Information
- Application Number
- JP2020201957
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-06
- Filing Date
- 2020-12-04
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-12-04
AI Technical Summary
Adhesive tapes used in semiconductor processing peel off at high temperatures due to outgassing from the adhesive layer, compromising the handling and processing of wafers and chips.
The adhesive tape is formulated with specific weight loss and peel strength properties, using acrylic polymers obtained through living radical polymerization, silicone-based graft copolymers, and controlled crosslinking to minimize outgassing and maintain adhesion at high temperatures, allowing easy removal post-processing.
The adhesive tape maintains integrity during high-temperature processing and can be easily peeled off after completion, reducing adhesive residue and enhancing processing reliability.
Smart Images

Figure 0007587407000005 
Figure 0007587407000001 
Figure 0007587407000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive tape that is difficult to peel even at high temperatures during processing of an adherend and can be easily peeled off after the processing is completed. The present invention also relates to a method for producing a semiconductor wafer using the adhesive tape. [Background technology]
[0002] In the manufacturing process of semiconductor chips, adhesive tapes are used to facilitate the handling of wafers and semiconductor chips during processing and to prevent breakage. For example, when a thick-film wafer cut from a high-purity silicon single crystal is ground to a predetermined thickness to obtain a thin-film wafer, the grinding is performed after adhering an adhesive tape to the thick-film wafer. In addition, an adherend such as a wafer or a semiconductor chip is fixed to a support plate via an adhesive tape, and the adherend fixed to the support plate is sometimes subjected to a treatment.
[0003] Such adhesive tapes are required to have high enough adhesion to firmly fix adherends such as wafers and semiconductor chips during processing, and also to be able to be peeled off without damaging the adherends such as wafers and semiconductor chips after processing is completed (hereinafter, also referred to as "high adhesion and easy peeling"). As an adhesive tape that realizes high adhesion and easy peeling, Patent Document 1 discloses an adhesive tape that uses a photocurable adhesive that hardens and loses adhesive strength when irradiated with light such as ultraviolet light. By using a photocurable adhesive as the adhesive, the adherend can be reliably fixed during processing, and can be easily peeled off by irradiating with ultraviolet light or the like. Patent Document 2 discloses a removable adhesive in which a non-silicone adhesive contains a silicone graft copolymer having a functional group capable of crosslinking with the base polymer of the adhesive. Patent Document 2 describes that the removable property is improved by using a silicone graft copolymer that has an excellent effect of suppressing an increase in adhesive strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-32946 [Patent Document 2] Japanese Patent Application Publication No. 2-123182 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in recent years, there has been an increase in the use of adhesive tapes attached to adherends such as wafers and semiconductor chips, which are then subjected to treatments that involve heating at higher temperatures than before, specifically at temperatures as high as 250°C or higher. This has resulted in the problem that the adhesive tape peels off at such high temperatures. The present invention aims to provide an adhesive tape that is difficult to peel off even at high temperatures during processing of an adherend and can be easily peeled off after the processing is completed. Another object of the present invention is to provide a method for manufacturing a semiconductor wafer using the adhesive tape. [Means for solving the problem]
[0006] The present invention is an adhesive tape having an adhesive layer on at least one surface, the adhesive layer having a weight loss rate of 15% by weight or less after heating at 280°C for 1 hour, and the adhesive tape having a surface peel strength to glass of 15 to 50 N after heating at 150°C for 10 minutes with an application area of 10 mm x 10 mm. The present invention will be described in detail below.
[0007] The present inventors have found that at high temperatures of 250° C. or higher, outgassing originating from the adhesive polymer contained in the adhesive layer occurs at the interface with the adherend, and this outgassing causes the adhesive tape to peel off. As a result of investigations into how to suppress the peeling off of the adhesive tape caused by such outgassing, the present inventors have found that by adjusting the weight loss rate after heating of the adhesive layer and the surface peel strength measured by a specific method within specific ranges, it is possible to suppress the peeling off of the adhesive tape at high temperatures, and also to easily peel off the adhesive tape after the process is completed, which has led to the completion of the present invention.
[0008] The pressure-sensitive adhesive tape of the present invention has a pressure-sensitive adhesive layer on at least one surface. The pressure-sensitive adhesive tape of the present invention may have other layers as long as it has the pressure-sensitive adhesive layer. The pressure-sensitive adhesive tape of the present invention may be a support type having a substrate, or a non-support type having no substrate. When the pressure-sensitive adhesive tape of the present invention has a substrate, it is sufficient that the pressure-sensitive adhesive layer is present on at least one side of the substrate, and it may be a single-sided pressure-sensitive adhesive tape or a double-sided pressure-sensitive adhesive tape. When the pressure-sensitive adhesive tape of the present invention is a double-sided pressure-sensitive adhesive tape having a substrate, it is sufficient that the pressure-sensitive adhesive layer is present on at least one side of the substrate, and it may have a pressure-sensitive adhesive layer similar to the pressure-sensitive adhesive layer on the other side of the substrate, or it may have a pressure-sensitive adhesive layer having a composition and physical properties different from those of the pressure-sensitive adhesive layer on the other side of the substrate.
[0009] The pressure-sensitive adhesive layer of the pressure-sensitive adhesive tape of the present invention has an upper limit of the weight loss rate after heating at 280° C. for 1 hour of 15% by weight. If the weight loss rate after heating is 15% by weight or less, the amount of outgassing derived from the adhesive polymer contained in the adhesive layer is reduced, and the adhesive tape is less likely to peel off even at high temperatures. The preferred upper limit of the weight loss rate after heating is 12% by weight, and the more preferred upper limit is 10% by weight. The lower limit of the weight loss rate after heating is not particularly limited, and is preferably closer to 0% by weight, since the adhesive tape is less likely to peel off even at high temperatures. The weight loss rate after heating can be measured by the following method. The adhesive layer is peeled off from the substrate to obtain a measurement sample consisting of only the adhesive layer. The weight of the obtained measurement sample is measured. Under a nitrogen atmosphere (nitrogen flow, flow rate 50 mL / min), the measurement sample is heated from 25°C to 280°C at a heating rate of 10°C / min using a differential thermal and thermogravimetric simultaneous measurement device (e.g., Hitachi High-Tech Science Corporation, TG-DTA; STA7200), and heated for 1 hour after reaching 280°C. After cooling, the weight loss is measured, and the weight loss rate is calculated from the obtained weight loss and the weight before heating.
[0010] The method for adjusting the weight loss rate after heating to the above range is not particularly limited, and may be any method that adjusts the type, composition, physical properties, content, etc. of the adhesive polymer, release agent, crosslinking agent, etc. contained in the adhesive layer. Among these, a method using an acrylic polymer obtained by living radical polymerization or an acrylic polymer obtained by constant temperature free radical polymerization as the adhesive polymer is preferred. Specifically, examples of methods for reducing the weight loss rate after heating include a method for purifying the adhesive polymer by reprecipitation or the like to reduce the content of low molecular weight components and tin components described below, a method for increasing crosslinking by increasing the crosslinkable functional groups in the adhesive polymer or release agent, and a method for crosslinking at a higher density by increasing the content of the crosslinking agent.
[0011] The pressure-sensitive adhesive tape of the present invention has a surface peel strength from glass of 15N lower limit and 50N upper limit after heating at 150° C. for 10 minutes with an application area of 10 mm×10 mm. The surface peel strength is measured by attaching the pressure-sensitive adhesive layer (i.e., the pressure-sensitive adhesive layer whose weight loss rate after heating satisfies the above range) to glass. If the surface peel strength is 15N or more, the pressure-sensitive adhesive tape is difficult to peel off even at high temperatures. If the surface peel strength is 50N or less, the pressure-sensitive adhesive tape can be easily peeled off after the process is completed. The preferred lower limit of the surface peel strength is 20N, the preferred upper limit is 45N, the more preferred lower limit is 25N, and the more preferred upper limit is 40N. The surface peel strength can be measured by the following method. The adhesive tape is cut into 10 mm x 10 mm pieces. In an environment of room temperature 23°C and relative humidity 50%, the cut adhesive tape is attached to glass (e.g., Matsunami Glass Industrial Co., Ltd., large slide glass with white edge polishing No. 2) at a speed of 10 mm / sec using a 2 kg pressure rubber roller. Next, heat treatment is performed at 150°C for 10 minutes. After cooling, the surface peel strength (maximum load) of the adhesive tape against the glass is measured according to the method for measuring the surface peel strength of adhesive tape shown in Figure 1 below.
[0012] FIG. 1 is a diagram showing a schematic diagram of a method for measuring the surface peel strength of an adhesive tape. Under an environment of room temperature 23°C and relative humidity 50%, one side of a double-sided adhesive tape 3 for measurement (product name #560, manufactured by Sekisui Chemical Co., Ltd., or equivalent) is attached to the back side of an adhesive tape 1 attached to a glass 2. The glass 2 is fixed so that the side to which the adhesive tape 1 and the double-sided adhesive tape 3 for measurement are attached faces upward, and the other side of the double-sided adhesive tape 3 for measurement is attached and fixed to a jig 4 of a tensile tester. A tensile test is performed in the 90° direction (arrow direction in the figure) at a peel speed of 300 mm / min using a tensile tester (AG-IS, manufactured by Shimadzu Corporation, or equivalent) to measure the surface peel strength. The surface peel strength means the maximum peel strength during the evaluation measurement.
[0013] The method for adjusting the surface peel strength to the above range is not particularly limited, and may be any method that adjusts the type, composition, physical properties, content, etc. of the adhesive polymer, release agent, crosslinking agent, polymerization initiator, etc. contained in the adhesive layer. Among these, a method using an acrylic polymer obtained by living radical polymerization or an acrylic polymer obtained by constant temperature free radical polymerization as the adhesive polymer, a method using a silicone-based graft copolymer as the release agent, a method adjusting the content of the silicone-based graft copolymer to a specific range, etc. are preferred. Specifically, examples of the method for increasing the surface peel strength include a method for reducing the content of the silicone-based graft copolymer described below, a method for reducing the weight average molecular weight of the adhesive polymer, a method for reducing the content of the polymerization initiator, a method for reducing the content of the crosslinking agent, etc. Examples of the method for decreasing the surface peel strength include a method for increasing the content of the silicone-based graft copolymer described below, a method for increasing the weight average molecular weight of the adhesive polymer, a method for increasing the content of the crosslinking agent, etc.
[0014] The tin content of the adhesive layer of the adhesive tape of the present invention is not particularly limited, but the preferred upper limit in terms of tin is 0.05% by weight. The tin content in the adhesive layer is mainly derived from a catalyst used in producing an acrylic polymer when the adhesive polymer contained in the adhesive layer is an acrylic polymer and / or a catalyst used in introducing a radically polymerizable unsaturated bond to the side chain of the acrylic polymer, which will be described later. If the tin content is 0.05% by weight or less, the tin component acts as a catalyst at high temperatures to decompose the alkyl ester portion of the acrylic polymer, which can be suppressed from becoming outgassed, so that the adhesive tape becomes more difficult to peel even at high temperatures. A more preferred upper limit of the tin content is 0.03% by weight. The lower limit of the tin content is not particularly limited, and the closer to 0% by weight, the more difficult the adhesive tape becomes to peel even at high temperatures, which is preferable. The tin content can be measured using an ICP optical emission spectrometer (Agilent, 5110 ICP-OES or an equivalent).
[0015] The method for adjusting the tin component content to the above range is not particularly limited, but examples include, when the adhesive polymer contained in the adhesive layer is an acrylic polymer, a method for adjusting the amount of catalyst added when producing the acrylic polymer, and a method for purifying the adhesive polymer by reprecipitation or the like.
[0016] The pressure-sensitive adhesive layer is not particularly limited as long as the post-heat weight loss rate and the surface peel strength can be adjusted within the above ranges, but it preferably contains an adhesive polymer, a silicone-based graft copolymer, a crosslinking agent, and a polymerization initiator.
[0017] The adhesive polymer is not particularly limited in the content of components having a molecular weight of 50,000 or less as measured by gel permeation chromatography (hereinafter also referred to as "low molecular weight components"), but a preferred upper limit of the total amount of the adhesive polymer is 10% by weight. If the content of the low molecular weight components is 10% by weight or less, the amount of outgassing originating from the adhesive polymer is further reduced, and the adhesive tape becomes less likely to peel even at high temperatures. A more preferred upper limit of the content of the low molecular weight components is 5% by weight. The lower limit of the content of the low molecular weight components is not particularly limited, and is preferably closer to 0% by weight, since the adhesive tape becomes less likely to peel even at high temperatures. The method for adjusting the content of the low molecular weight component to the above range is not particularly limited, and it is sufficient to adjust the type, composition, physical properties, content, etc. of the adhesive polymer. Among them, a method using an acrylic polymer obtained by living radical polymerization or an acrylic polymer obtained by constant temperature free radical polymerization as the adhesive polymer is preferred.
[0018] The weight average molecular weight of the adhesive polymer is not particularly limited, but the preferred lower limit is 500,000, and the preferred upper limit is 1,500,000. If the weight average molecular weight is within the above range, the flexibility of the adhesive layer is increased, and the adhesion to the adherend is improved, so that the adhesive tape is less likely to peel off even at high temperatures. The more preferred lower limit of the weight average molecular weight is 800,000, and the more preferred upper limit is 1,200,000. The weight average molecular weight can be adjusted to fall within the above range by adjusting, for example, the composition of the adhesive polymer, the polymerization method, the polymerization conditions, and the like.
[0019] The content and weight average molecular weight of the low molecular weight component can be measured by the following method. The solution of the adhesive polymer is filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm). The obtained filtrate is fed to a gel permeation chromatograph (e.g., Waters 2690 Separations Model) and GPC measurement is performed under the conditions of tetrahydrofuran as the mobile phase solvent, a sample flow rate of 1 ml / min, and a column temperature of 40°C. The polystyrene-equivalent molecular weight of the adhesive polymer is measured to determine the content and weight average molecular weight of low molecular weight components. For example, a GPC KF-806L (Showa Denko KK) is used as the column, and a differential refractometer is used as the detector. The content of low molecular weight components can be calculated from the integral ratio of each molecular weight in the GPC chart obtained by the measurement.
[0020] The adhesive polymer preferably has a polar functional group. When the adhesive polymer has the polar functional group, the silicone graft copolymer described below has a functional group that can be crosslinked with the adhesive polymer, and the silicone graft copolymer is bonded to the adhesive polymer via a crosslinking agent. This can further reduce the contamination of the adherend caused by the silicone graft copolymer bleeding out. The polar functional group is not particularly limited, and examples thereof include a carboxyl group, a hydroxyl group, a glycidyl group, an amide group, a nitrile group, etc. Among these, a carboxyl group and a hydroxyl group are preferred, and a carboxyl group is more preferred.
[0021] The adhesive polymer preferably has a radically polymerizable unsaturated bond in the molecule. Since the adhesive polymer has the radically polymerizable unsaturated bond, the adhesive layer hardens in the presence of a polymerization initiator by stimuli such as heat and light, the elastic modulus increases, and the adhesive strength decreases, so that the adhesive tape can be peeled off more easily after the process is completed, and adhesive residue can be further suppressed. Also, since the adhesive polymer has the radically polymerizable unsaturated bond, the polarity of the crosslinking point is lower than when it has other polymerizable functional groups, and the crosslinking density increases when the adhesive layer hardens, so that the elastic modulus of the adhesive layer increases, and the adhesive tape can be peeled off more easily after the process is completed, and adhesive residue can be further suppressed.
[0022] The method for introducing the radically polymerizable unsaturated bond into the adhesive polymer is not particularly limited, and examples thereof include a method of using a monomer having a radically polymerizable unsaturated bond when synthesizing the adhesive polymer, and a method of reacting a compound having a radically polymerizable unsaturated bond with a precursor polymer of the adhesive polymer.
[0023] Specific examples of the adhesive polymer include acrylic polymers, silicone polymers, urethane polymers, rubber polymers, etc. Among them, acrylic polymers are preferred because they have excellent heat resistance and weather resistance, are applicable to a wide range of adherends, and the weight loss rate after heating and the surface peel strength can be easily adjusted to the above ranges.
[0024] When the adhesive polymer is the acrylic polymer, in order to have the polar functional group, the acrylic polymer preferably has a constituent unit derived from a monomer having the polar functional group. When the polar functional group is a carboxyl group, examples of the monomer having a carboxyl group include (meth)acrylic acid. When the polar functional group is a hydroxyl group, examples of the monomer having a hydroxyl group include (meth)acrylic acid esters having a hydroxyl group such as 4-hydroxybutyl (meth)acrylate and 2-hydroxyethyl (meth)acrylate. When the polar functional group is a glycidyl group, examples of the monomer having a glycidyl group include glycidyl (meth)acrylate. When the polar functional group is an amide group, examples of the monomer having an amide group include hydroxyethyl acrylamide, isopropyl acrylamide, and dimethylaminopropyl acrylamide. When the polar functional group is a nitrile group, examples of the monomer having a nitrile group include acrylonitrile. These monomers having a polar functional group may be used alone or in combination of two or more.
[0025] When the acrylic polymer has a constituent unit derived from the monomer having a carboxyl group, its content is not particularly limited, but the preferred lower limit is 0.1% by weight, and the preferred upper limit is 10% by weight. If the content is 0.1% by weight or more, the acrylic polymer can be sufficiently bonded to the silicone graft copolymer via the crosslinking agent, so that the contamination of the adherend can be further reduced. If the content is 10% by weight or less, the pressure-sensitive adhesive layer does not become too hard, and adhesive residue can be further suppressed.
[0026] When the acrylic polymer has a constituent unit derived from the monomer having a hydroxyl group, its content is not particularly limited, but the preferred lower limit is 0.1% by weight, and the preferred upper limit is 30% by weight. If the content is 0.1% by weight or more, the acrylic polymer can be sufficiently bonded to the silicone graft copolymer via the crosslinking agent, so that contamination of the adherend can be further reduced. If the content is 30% by weight or less, the adhesive tape becomes more difficult to peel off even at high temperatures.
[0027] The acrylic polymer may have a constituent unit derived from another radical polymerizable monomer in addition to the constituent unit derived from the monomer having a polar functional group. Examples of the other radical polymerizable monomer include (meth)acrylic acid esters and vinyl compounds.
[0028] The (meth)acrylic acid ester is not particularly limited, and examples thereof include (meth)acrylic acid alkyl esters. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isomyristyl (meth)acrylate, and stearyl (meth)acrylate. Examples of the (meth)acrylic acid ester include cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and polypropylene glycol mono(meth)acrylate. These (meth)acrylic acid esters may be used alone or in combination of two or more kinds.
[0029] The vinyl compound is not particularly limited, and examples thereof include styrene, vinyl acetate, etc. These vinyl compounds may be used alone or in combination of two or more kinds.
[0030] When the adhesive polymer is the acrylic polymer, in order to have the radically polymerizable unsaturated bond, it is preferable to react a compound having a functional group that reacts with the polar functional group and a radically polymerizable unsaturated bond (hereinafter, also referred to as a "functional group-containing unsaturated compound") with the polar functional group present in the acrylic polymer. If all of the polar functional groups present in the acrylic polymer react with the functional group-containing unsaturated compound, the acrylic polymer will no longer have polar functional groups, and therefore it is necessary to adjust the reactivity by appropriately adjusting the type of the functional group-containing unsaturated compound, reaction conditions, etc.
[0031] The functional group-containing unsaturated compound is not particularly limited and can be appropriately selected depending on the polar functional group present in the acrylic polymer. When the polar functional group present in the acrylic polymer is a carboxyl group, a compound having an epoxy group and a radically polymerizable unsaturated bond, a compound having an isocyanate group and a radically polymerizable unsaturated bond, etc. are used. When the polar functional group present in the acrylic polymer is a hydroxyl group, a compound having an isocyanate group and a radically polymerizable unsaturated bond, etc. are used. When the polar functional group present in the acrylic polymer is an epoxy group, a compound having a carboxyl group and a radically polymerizable unsaturated bond, a compound having an amide group and a radically polymerizable unsaturated bond, etc. are used. When the polar functional group present in the acrylic polymer is an amino group, a compound having an epoxy group and a radically polymerizable unsaturated bond, etc. are used.
[0032] The acrylic polymer is obtained by copolymerizing the monomer mixture. To obtain the acrylic polymer by copolymerizing the monomer mixture, the monomer mixture may be subjected to a radical reaction in the presence of a polymerization initiator. As a method for radically reacting the monomer mixture, that is, a polymerization method, a conventionally known method is used, and examples of the method include solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, and bulk polymerization. Examples of the reaction method when the monomer mixture is radically reacted include living radical polymerization and free radical polymerization.
[0033] The acrylic polymer is preferably an acrylic polymer obtained by living radical polymerization (hereinafter, also referred to as "living radically polymerized acrylic polymer"). Living radical polymerization is a polymerization in which molecular chains grow without being hindered by side reactions such as termination reactions or chain transfer reactions. In living radical polymerization, the reaction proceeds without deactivating the growing terminal radicals and without generating new radical species during the reaction. During the reaction, all molecular chains are polymerized while reacting with monomers uniformly, and the composition of all molecular chains approaches uniformity. Therefore, living radical polymerization can obtain a polymer having a more uniform molecular weight and composition than free radical polymerization, and can suppress the generation of low molecular weight components, making it easier to adjust the weight loss rate after heating to the above range. In addition, if the generation of low molecular weight components can be suppressed, the cohesive strength of the pressure-sensitive adhesive layer increases, and the surface peel strength can also be easily adjusted to the above range. As a result, the pressure-sensitive adhesive tape becomes more difficult to peel even at high temperatures.
[0034] On the other hand, in free radical polymerization, radical species are continuously generated during the reaction and added to the monomer, and the polymerization proceeds. Therefore, in free radical polymerization, molecular chains are generated in which the growing terminal radicals are deactivated during the reaction, and molecular chains are generated that grow due to new radical species generated during the reaction. Therefore, free radical polymerization results in a polymer with a non-uniform composition compared to living radical polymerization, and also includes polymers with relatively low molecular weights.
[0035] In the living radical polymerization, various polymerization methods may be adopted. For example, iron, ruthenium or copper catalyst and halogen-based initiator may be used (ATRP), TEMPO may be used, or an organic tellurium polymerization initiator may be used. Among them, it is preferable to use an organic tellurium polymerization initiator. Unlike other living radical polymerizations, living radical polymerization using an organic tellurium polymerization initiator can obtain a polymer having a uniform molecular weight and composition by polymerizing radical polymerizable monomers having polar functional groups such as hydroxyl groups and carboxyl groups with the same initiator without protecting any of them. Therefore, radical polymerizable monomers having polar functional groups can be easily copolymerized.
[0036] The organotellurium polymerization initiator is not particularly limited as long as it is one that is generally used in living radical polymerization, and examples thereof include organotellurium compounds and organotelluride compounds. Examples of the organotellurium compound include (methyltellanyl-methyl)benzene, (1-methyltellanyl-ethyl)benzene, (2-methyltellanyl-propyl)benzene, 1-chloro-4-(methyltellanyl-methyl)benzene, 1-hydroxy-4-(methyltellanyl-methyl)benzene, 1-methoxy-4-(methyltellanyl-methyl)benzene, 1-amino-4-(methyltellanyl-methyl)benzene, 1-nitro-4-(methyltellanyl-methyl)benzene, 1-cyano-4-(methyltellanyl-methyl)benzene, 1-methylcarboxamide ... 1-phenylcarbonyl-4-(methyltellanyl-methyl)benzene, 1-methoxycarbonyl-4-(methyltellanyl-methyl)benzene, 1-phenoxycarbonyl-4-(methyltellanyl-methyl)benzene, 1-sulfonyl-4-(methyltellanyl-methyl)benzene, 1-trifluoromethyl-4-(methyltellanyl-methyl)benzene, 1-chloro-4-(1-methyltellanyl-ethyl)benzene, 1-hydroxy-4-(1-methyltellanyl-ethyl)benzene, 1-methoxy-4-(methyltellanyl-methyl)benzene, 1-phenylcarbonyl-4-(methyltellanyl-methyl)benzene, 1-methoxycarbonyl-4-(methyltellanyl-methyl)benzene, 1-phenoxycarbonyl-4-(methyltellanyl-methyl)benzene, 1-sulfonyl-4-(methyltellanyl-methyl)benzene, 1-trifluoromethyl-4-(methyltellanyl-methyl)benzene, 1-chloro-4-(1-methyltellanyl-ethyl)benzene, 1-hydroxy-4-(1-methyltellanyl-ethyl)benzene, 1-methyl-4-(1-methyltellanyl-ethyl)benzene, 1-amino-4-(1-methyltellanyl-ethyl)benzene, 1-nitro-4-(1-methyltellanyl-ethyl)benzene, 1-cyano-4-(1-methyltellanyl-ethyl)benzene, 1-methylcarbonyl-4-(1-methyltellanyl-ethyl)benzene, 1-phenylcarbonyl-4-(1-methyltellanyl-ethyl)benzene, 1-methoxycarbonyl-4-(1-methyltellanyl-ethyl)benzene, 1-phenoxycarbonyl-4-(1-methyltellanyl-ethyl)benzene 1-sulfonyl-4-(1-methyltellanyl-ethyl)benzene, 1-trifluoromethyl-4-(1-methyltellanyl-ethyl)benzene, 1-chloro-4-(2-methyltellanyl-propyl)benzene, 1-hydroxy-4-(2-methyltellanyl-propyl)benzene, 1-methoxy-4-(2-methyltellanyl-propyl)benzene, 1-amino-4-(2-methyltellanyl-propyl)benzene, 1-nitro-4-(2-methyltellanyl-propyl)benzene, 1-cyano-4-(2-methyltellanyl-propyl)benzene,1-Methylcarbonyl-4-(2-methyltellanyl-propyl)benzene, 1-phenylcarbonyl-4-(2-methyltellanyl-propyl)benzene, 1-methoxycarbonyl-4-(2-methyltellanyl-propyl)benzene, 1-phenoxycarbonyl-4-(2-methyltellanyl-propyl)benzene, 1-sulfonyl-4-(2-methyltellanyl-propyl)benzene, 1-trifluoromethyl-4-(2-methyltellanyl-propyl)benzene, 2-(methyltellanyl-methyl)pyridine, 2-(1- Examples of the organotellurium compounds include 2-(methyltellanyl-ethyl)pyridine, 2-(2-methyltellanyl-propyl)pyridine, 2-methyltellanyl-methyl ethanoate, 2-methyltellanyl-methyl propionate, 2-methyltellanyl-methyl 2-methylpropionate, 2-methyltellanyl-ethyl ethanoate, 2-methyltellanyl-ethyl propionate, 2-methyltellanyl-ethyl 2-methylpropionate, 2-methyltellanyl acetonitrile, 2-methyltellanyl propionitrile, and 2-methyl-2-methyltellanyl propionitrile. The methyltellanyl group in these organotellurium compounds may be an ethyltellanyl group, an n-propyltellanyl group, an isopropyltellanyl group, an n-butyltellanyl group, an isobutyltellanyl group, a t-butyltellanyl group, a phenyltellanyl group, and the like. These organotellurium compounds may be used alone or in combination of two or more kinds.
[0037] Examples of the organic telluride compound include dimethyl ditelluride, diethyl ditelluride, di-n-propyl ditelluride, diisopropyl ditelluride, dicyclopropyl ditelluride, di-n-butyl ditelluride, di-sec-butyl ditelluride, di-tert-butyl ditelluride, dicyclobutyl ditelluride, diphenyl ditelluride, bis-(p-methoxyphenyl) ditelluride, bis-(p-aminophenyl) ditelluride, bis-(p-nitrophenyl) ditelluride, bis-(p-cyanophenyl) ditelluride, bis-(p-sulfonylphenyl) ditelluride, dinaphthyl ditelluride, and dipyridyl ditelluride. These organic telluride compounds may be used alone or in combination of two or more. Among them, dimethyl ditelluride, diethyl ditelluride, di-n-propyl ditelluride, di-n-butyl ditelluride, and diphenyl ditelluride are preferred.
[0038] In addition to the above-mentioned organotellurium polymerization initiator, an azo compound may be used as a polymerization initiator for the purpose of accelerating the polymerization rate, within the scope of the invention. The azo compound is not particularly limited as long as it is generally used in radical polymerization. Examples of the azo compound include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 1,1-azobis(cyclohexane-1-carbonitrile), 1-[(1-cyano-1-methylethyl)azo]formamide, 4,4' -Azobis(4-cyanovaleric acid), dimethyl-2,2'-azobis(2-methylpropionate), dimethyl-1,1'-azobis(1-cyclohexanecarboxylate), 2,2'-azobis{2-methyl-N-[1,1'-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2 '-Azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2'-azobis(1-imino-1-pyrrolidino-2-methylpropane) dihydrochloride, 2,2'-azobis(2,4,4-trimethylpentane), etc. These azo compounds may be used alone or in combination of two or more.
[0039] The molecular weight distribution (Mw / Mn) of the living radical polymerization acrylic polymer is not particularly limited, but the preferred lower limit is 1.05, and the preferred upper limit is 2.5. If the molecular weight distribution (Mw / Mn) is within the above range, the weight loss rate after heating and the surface peel strength are easily adjusted to the above ranges, and the adhesive tape is more difficult to peel even at high temperatures. The more preferred lower limit of the molecular weight distribution (Mw / Mn) is 1.1, and the more preferred upper limit is 2.0.
[0040] The acrylic polymer may be an acrylic polymer obtained by constant temperature free radical polymerization (hereinafter, also referred to as "constant temperature free radical polymerized acrylic polymer"). As described above, free radical polymerization results in a non-uniform polymer composition compared to living radical polymerization, and also includes polymers with relatively low molecular weight. However, among free radical polymerization, constant temperature free radical polymerization can suppress the generation of low molecular weight components compared to boiling point free radical polymerization, so that the weight loss rate after heating and the surface peel strength can be easily adjusted to the above ranges, and the pressure-sensitive adhesive tape becomes more difficult to peel even at high temperatures.
[0041] When the monomer mixture is subjected to a radical reaction, a dispersion stabilizer may be used. Examples of the dispersion stabilizer include polyvinylpyrrolidone, polyvinyl alcohol, methyl cellulose, ethyl cellulose, poly(meth)acrylic acid, poly(meth)acrylic acid ester, and polyethylene glycol. When a polymerization solvent is used in the radical reaction of the monomer mixture, the polymerization solvent is not particularly limited. As the polymerization solvent, for example, a non-polar solvent such as hexane, cyclohexane, octane, toluene, xylene, etc., or a highly polar solvent such as water, methanol, ethanol, propanol, butanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, dioxane, N,N-dimethylformamide, etc., can be used. These polymerization solvents may be used alone or in combination of two or more kinds. In addition, the polymerization temperature is preferably 0 to 110°C from the viewpoint of the polymerization rate.
[0042] The silicone graft copolymer is a copolymer having a graft chain containing a siloxane bond. By containing the silicone-based graft copolymer in the pressure-sensitive adhesive layer, the silicone-based graft copolymer undergoes molecular migration and gathers on the surface of the pressure-sensitive adhesive layer, making the surface of the pressure-sensitive adhesive layer hydrophobic. This makes it difficult for the pressure-sensitive adhesive layer to interact with the adherend, making it easier to adjust the surface peel strength to the above range and reducing the adhesion increase of the pressure-sensitive adhesive layer due to heating, so that the pressure-sensitive adhesive tape can be peeled off more easily after the process is completed, and adhesive residue can be further reduced.
[0043] The silicone graft copolymer is not particularly limited, but preferably has a structural unit derived from a silicone macromonomer. The silicone macromonomer is not particularly limited as long as it is a monomer having a siloxane bond-containing group, and examples thereof include acrylic silicone macromonomers, styrene silicone macromonomers, etc. Among these, acrylic silicone macromonomers are preferred because of their excellent heat resistance and weather resistance, and acrylic silicone macromonomers having the structure shown in the following general formula (1) or (2) are more preferred.
[0044] [ka]
[0045] Here, R represents a (meth)acryloyl group-containing functional group, and X and Y each independently represent an integer of 0 or more. An example of R is a (meth)acryloyl group. Although there are no particular limitations on the upper limits of X and Y, X and Y are usually 5,000 or less, preferably 500 or less, and more preferably 200 or less.
[0046] The weight average molecular weight of the silicone macromonomer is not particularly limited, but the preferred lower limit is 500, and the preferred upper limit is 50,000. If the weight average molecular weight is within the above range, the hydrophobic surface layer formed by the silicone graft copolymer becomes thicker, so that the adhesion enhancement of the pressure-sensitive adhesive layer due to heating can be further reduced, and the pressure-sensitive adhesive tape can be more easily peeled off after the process is completed, and adhesive residue can be suppressed. The more preferred lower limit of the weight average molecular weight is 1,000, and the more preferred upper limit is 20,000.
[0047] The content of the structural unit derived from the silicone macromonomer is not particularly limited, but the preferred lower limit in the silicone graft copolymer is 1% by weight, and the preferred upper limit is 90% by weight. If the content is within the above range, the adhesion enhancement of the pressure-sensitive adhesive layer due to heating can be further reduced, and the pressure-sensitive adhesive tape can be more easily peeled off after the process is completed, and adhesive residue can be suppressed. The more preferred lower limit of the content is 5% by weight, the more preferred upper limit is 80% by weight, the even more preferred lower limit is 10% by weight, and the even more preferred upper limit is 60% by weight.
[0048] The silicone graft copolymer preferably has a functional group capable of crosslinking with the adhesive polymer. The silicone graft copolymer has a functional group capable of crosslinking with the adhesive polymer, and thus the silicone graft copolymer is bonded to the adhesive polymer via a crosslinking agent, thereby reducing contamination of the adherend caused by bleeding out of the silicone graft copolymer.
[0049] The functional group crosslinkable with the adhesive polymer may be present in the graft chain of the silicone-based graft copolymer, may be present in the main chain, or may be present in both the graft chain and the main chain. The functional group capable of crosslinking with the adhesive polymer is not particularly limited and is appropriately determined according to the functional group present in the adhesive polymer, and examples thereof include a carboxyl group, a hydroxyl group, a glycidyl group, an amide group, a nitrile group, etc. Among these, a carboxyl group and a hydroxyl group are preferred, and a carboxyl group is more preferred.
[0050] In order to have a functional group crosslinkable with the adhesive polymer, the silicone graft copolymer preferably has a constituent unit derived from a monomer having a functional group crosslinkable with the adhesive polymer. The monomer having a functional group capable of crosslinking with the above-mentioned adhesive polymer is not particularly limited, and a monomer similar to the monomer having a polar functional group as described above, which is used in the case of an acrylic polymer as the above-mentioned adhesive polymer, can be used.
[0051] The content of the constituent unit derived from the monomer having a functional group capable of crosslinking with the adhesive polymer is not particularly limited, but the preferred lower limit in the silicone-based graft copolymer is 1% by weight, and the preferred upper limit is 40% by weight. If the content is within the above range, the silicone-based graft copolymer can be sufficiently bonded to the adhesive polymer while the adhesive polymers can also form a sufficient crosslinked structure, so that the adhesive tape is less likely to peel off even at high temperatures, and the adhesive tape can be more easily peeled off after the process is completed. The more preferred lower limit of the content is 3% by weight, the more preferred upper limit is 30% by weight, the even more preferred upper limit is 20% by weight, and the even more preferred upper limit is 15% by weight.
[0052] In addition, the functional group that can be crosslinked with the adhesive polymer can be a radically polymerizable unsaturated bond.In this case, in order for the silicone-based graft copolymer to have the radically polymerizable unsaturated bond, it is preferable to react the functional group present in the silicone-based graft copolymer with the compound that has the functional group that reacts with the functional group and the radically polymerizable unsaturated bond.This compound is not particularly limited, and the same compound as the functional group-containing unsaturated compound as described above that is used in the case of the acrylic polymer as the adhesive polymer can be used.
[0053] The silicone graft copolymer may further have a constituent unit derived from a (meth)acrylic acid ester, a vinyl compound, a monomer having another polar functional group, or the like, in addition to the constituent unit derived from the silicone macromonomer and the constituent unit derived from a monomer having a functional group capable of crosslinking with the adhesive polymer. The (meth)acrylic acid ester and the vinyl compound are not particularly limited, and the same monomers as the (meth)acrylic acid esters used in the case of the acrylic polymer as the adhesive polymer can be used. Among them, 2-ethylhexyl acrylate is preferred because it can impart an appropriate adhesive strength.
[0054] The weight average molecular weight of the silicone graft copolymer is not particularly limited, but the preferred upper limit is 400,000. If the weight average molecular weight is 400,000 or less, the silicone graft copolymer is more likely to move within the adhesive layer and to gather on the surface of the adhesive layer, so that the adhesion of the adhesive layer caused by heating can be further reduced, and the adhesive tape can be more easily peeled off after the process is completed, and adhesive residue can be suppressed. The more preferred upper limit of the weight average molecular weight is 300,000, the even more preferred upper limit is 250,000, and the particularly preferred upper limit is 200,000, and it is usually 10,000 or more.
[0055] The method for producing the silicone-based graft copolymer is not particularly limited, and the silicone-based graft copolymer can be obtained by copolymerizing a monomer mixture. The method for obtaining the silicone-based graft copolymer by copolymerizing the monomer mixture is not particularly limited, and the same method as that for the acrylic polymer as the adhesive polymer can be used.
[0056] The content of the silicone graft copolymer is not particularly limited, but since the silicone graft copolymer tends to collect on the surface of the pressure-sensitive adhesive layer, it can be used in a smaller amount than conventional silicone compounds. The silicone graft copolymer content is preferably 0.1 parts by weight at its lower limit relative to 100 parts by weight of the adhesive polymer, and is preferably 10 parts by weight at its upper limit. If the content is 0.1 parts by weight or more, the surface peel strength can be easily adjusted to the above range, and the adhesion increase of the adhesive layer due to heating can be further reduced, so that the adhesive tape can be more easily peeled off after the process is completed, and adhesive residue can be suppressed. If the content is 10 parts by weight or less, the adhesive tape is more difficult to peel off even at high temperatures, and the opacity of the adhesive layer can be suppressed. The more preferred lower limit of the content is 0.5 parts by weight, the more preferred upper limit is 5 parts by weight, and the even more preferred lower limit is 1 part by weight.
[0057] By containing the crosslinking agent in the pressure-sensitive adhesive layer, the adhesive polymer is crosslinked, which makes it easier to adjust the cohesive strength of the pressure-sensitive adhesive layer and the surface peel strength to the above range, which makes it harder for the pressure-sensitive adhesive tape to peel off even at high temperatures, and makes it easier to peel the pressure-sensitive adhesive tape after the process is completed. In addition, when the silicone graft copolymer has a functional group capable of crosslinking with the adhesive polymer, the silicone graft copolymer is bonded to the adhesive polymer via the crosslinking agent by the pressure-sensitive adhesive layer containing the crosslinking agent, thereby reducing contamination of the adherend caused by the silicone graft copolymer bleeding out.
[0058] The crosslinking agent is not particularly limited, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among these, isocyanate-based crosslinking agents are preferred because they increase the cohesive strength of the pressure-sensitive adhesive layer.
[0059] The content of the crosslinking agent is not particularly limited, but from the viewpoint of achieving a more appropriate cohesive force and of sufficiently bonding the adhesive polymer and the silicone-based graft copolymer, a preferred lower limit relative to 100 parts by weight of the adhesive polymer is 0.01 parts by weight, a preferred upper limit is 1 part by weight, a more preferred lower limit is 0.1 parts by weight, and a more preferred upper limit is 0.5 parts by weight.
[0060] When the adhesive layer contains the polymerization initiator, and the adhesive polymer has the radically polymerizable unsaturated bond, the adhesive layer hardens in the presence of the polymerization initiator due to stimuli such as heat and light, increasing the elastic modulus and decreasing the adhesive strength, so that the adhesive tape can be more easily peeled off after completion of the process and reducing adhesive residue. The polymerization initiator is not particularly limited, and examples thereof include photopolymerization initiators, thermal polymerization initiators, etc. Among them, thermal polymerization initiators are preferred because they can cure the pressure-sensitive adhesive layer by heat when the adherend is subjected to a heating treatment, eliminating the need for a separate step of curing the pressure-sensitive adhesive layer, and they can cure even when used on an adherend that does not transmit light.
[0061] The photopolymerization initiator is not particularly limited, and examples thereof include those that are activated by irradiation with light having a wavelength of 250 to 800 nm. Examples of such photopolymerization initiators include acetophenone derivative compounds, benzoin ether compounds, ketal derivative compounds, phosphine oxide derivative compounds, bis(η5-cyclopentadienyl)titanocene derivative compounds, benzophenone, Michler's ketone, chlorothioxanthone, dodecylthioxanthone, dimethylthioxanthone, diethylthioxanthone, α-hydroxycyclohexylphenylketone, 2-hydroxymethylphenylpropane, etc. Examples of the acetophenone derivative compounds include methoxyacetophenone. Examples of the benzoin ether compounds include benzoin propyl ether and benzoin isobutyl ether. Examples of the ketal derivative compounds include benzyl dimethyl ketal and acetophenone diethyl ketal. These photopolymerization initiators may be used alone or in combination of two or more.
[0062] The thermal polymerization initiator is not particularly limited, and examples thereof include those that decompose by heat to generate active radicals that initiate a polymerization reaction, such as dicumyl peroxide, di-t-butyl peroxide, t-butyl peroxybenzoyl, t-butyl hydroperoxide, benzoyl peroxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, paramenthane hydroperoxide, and di-t-butyl peroxide.
[0063] The content of the polymerization initiator is not particularly limited and is appropriately determined depending on the types of the adhesive polymer and the polymerization initiator, but a preferred lower limit relative to 100 parts by weight of the adhesive polymer is 0.1 parts by weight, a preferred upper limit is 10 parts by weight, a more preferred lower limit is 1 part by weight, and a more preferred upper limit is 8 parts by weight.
[0064] The pressure-sensitive adhesive layer may contain known additives such as inorganic fillers such as fumed silica, plasticizers, resins, surfactants, wax, fine particle fillers, antioxidants, and gas generating agents.
[0065] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but the preferred lower limit is 5 μm, and the preferred upper limit is 100 μm. If the thickness of the pressure-sensitive adhesive layer is within the above range, the pressure-sensitive adhesive tape can be attached to the adherend with sufficient adhesive strength, and adhesive residue can be suppressed after the process is completed. The more preferred lower limit of the thickness of the pressure-sensitive adhesive layer is 10 μm, and the more preferred upper limit is 60 μm.
[0066] When the pressure-sensitive adhesive tape of the present invention is a support type, the material constituting the substrate is not particularly limited, but is preferably a material having heat resistance. Examples of heat-resistant materials include polyethylene terephthalate, polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyphenylene ether, polybutylene terephthalate, ultra-high molecular weight polyethylene, syndiotactic polystyrene, polyarylate, polysulfone, polyether sulfone, polyphenylene sulfide, polyether ether ketone, polyimide, polyetherimide, fluororesin, and liquid crystal polymer. Among them, polyimide is preferable because of its excellent heat resistance.
[0067] The thickness of the substrate is not particularly limited, but the preferred lower limit is 15 μm, and the preferred upper limit is 250 μm. If the thickness of the substrate is within the above range, the adhesive tape can be made to have excellent handling properties. The more preferred lower limit of the thickness of the substrate is 25 μm, and the more preferred upper limit is 125 μm.
[0068] The method for producing the pressure-sensitive adhesive tape of the present invention is not particularly limited, and examples thereof include the following methods. First, a silicone-based graft copolymer, a crosslinking agent, a polymerization initiator, and other additives as necessary are added to a solution of an adhesive polymer and mixed to obtain an adhesive solution. Next, the adhesive solution is applied onto a release film and dried to form an adhesive layer. The obtained adhesive layer is laminated to a substrate to produce an adhesive tape.
[0069] The application of the pressure-sensitive adhesive tape of the present invention is not particularly limited, but it is preferably used in the manufacture of electronic components such as semiconductor chips, display devices (OLEDs, liquid crystal display devices, etc.) etc. More specifically, in the manufacture of electronic components, it is preferably used when temporarily fixing an adherend such as a wafer or semiconductor chip onto the pressure-sensitive adhesive tape, or temporarily fixing an adherend such as a wafer or semiconductor chip to a support plate via the pressure-sensitive adhesive tape, and then treating the temporarily fixed adherend. The adhesive tape of the present invention is difficult to peel off even at high temperatures during the processing of the adherend, but can be easily peeled off after the processing is completed, and therefore can be suitably used even when the adhesive tape is attached to an adherend such as a wafer or semiconductor chip and subjected to a treatment that involves heating at temperatures higher than conventional temperatures, specifically, for example, at temperatures as high as 250°C or higher.
[0070] The present invention also provides a method for manufacturing a semiconductor wafer using the adhesive tape of the present invention, the method comprising a temporary fixing step of temporarily fixing a semiconductor wafer onto the adhesive tape, a semiconductor wafer processing step of subjecting the surface of the semiconductor wafer to a treatment involving heating at 250°C or higher, and an adhesive tape peeling step of peeling the adhesive tape from the semiconductor wafer.
[0071] The above-mentioned treatment involving heating at 250° C. or higher is not particularly limited, and examples thereof include a reflow process, a sputtering process, a deposition process, an etching process, a chemical vapor deposition (CVD) process, a physical vapor deposition (PVD) process, a resist coating process, a patterning process, a molding process, etc. The upper limit of the temperature of the above-mentioned treatment involving heating at 250° C. or higher is not particularly limited, and is, for example, 350° C. The method for peeling the pressure-sensitive adhesive tape from the semiconductor wafer is not particularly limited, and examples thereof include peel peeling and laser peeling. Instead of the adhesive tape peeling step of peeling the adhesive tape from the semiconductor wafer, a semiconductor wafer peeling step of peeling the semiconductor wafer from the adhesive tape by needle pick-up or the like may be performed. Effect of the Invention
[0072] According to the present invention, it is possible to provide an adhesive tape that is difficult to peel even at high temperatures during processing of an adherend and can be easily peeled off after the processing is completed. Also, according to the present invention, it is possible to provide a method for manufacturing a semiconductor wafer using the adhesive tape. [Brief description of the drawings]
[0073] [Figure 1]FIG. 2 is a diagram showing a schematic diagram of a method for measuring surface peel strength of an adhesive tape. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0075] (Synthesis Example 1 (Synthesis of living radical polymerization acrylic polymer)) 6.38g (50mmol) of tellurium (40 mesh, metallic tellurium, Aldrich) was suspended in 50mL of tetrahydrofuran (THF), and 34.4mL (55mmol) of 1.6mol / L n-butyllithium / hexane solution (Aldrich) was slowly added dropwise at room temperature. The reaction solution was stirred until the metallic tellurium was completely consumed. 10.7g (55mmol) of ethyl-2-bromo-isobutyrate was added to the reaction solution at room temperature and stirred for 2 hours. After the reaction was completed, the solvent was concentrated under reduced pressure, followed by vacuum distillation to obtain ethyl 2-methyl-2-n-butyltellanyl-propionate as a yellow oil.
[0076] In a glove box substituted with argon, 19 μL of the obtained 2-methyl-2-n-butyltellanyl-ethyl propionate, 8.8 mg of V-65 (2,2'-azobis(2,4-dimethylvaleronitrile), Fujifilm Wako Pure Chemical Industries, Ltd.), and 1 mL of ethyl acetate were added to a reaction vessel, and the reaction vessel was then sealed and removed from the glove box. Next, while flowing argon gas into the reaction vessel, a total of 100 g of the monomer mixture shown in Table 1 except for 2-methacryloyloxyethyl isocyanate (MOI) and 66.5 g of ethyl acetate as a polymerization solvent were added to the reaction vessel, and a polymerization reaction was carried out at 60 ° C. for 20 hours to obtain a polymer-containing solution. Into a reaction vessel, 10 ppm of hydroquinone was added relative to 100 parts by weight of the obtained polymer, and the mixture was heated to 60° C. Then, 8 parts by weight of 2-methacryloyloxyethyl isocyanate (MOI) was dropped into the reaction vessel over 60 minutes, and the mixture was further reacted at 60° C. for 120 minutes to obtain a solution containing a living radical polymerized acrylic polymer (Synthesis Example 1). The resulting solution containing the living radical polymerization acrylic polymer was diluted 50 times with tetrahydrofuran (THF). The resulting diluted solution was filtered through a filter (material: polytetrafluoroethylene, pore size: 0.2 μm). The resulting filtrate was fed to a gel permeation chromatograph (Waters, 2690 Separations Model) and subjected to GPC measurement under conditions of a sample flow rate of 1 mL / min and a column temperature of 40° C., to measure the polystyrene-equivalent molecular weight of the living radical polymerization acrylic polymer. This allowed the content of low molecular weight components, weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) to be determined. A GPC KF-806L (Showa Denko) was used as the column, and a differential refractometer was used as the detector.
[0077] (Synthesis Example 2 (Synthesis of acrylic polymer by living radical polymerization)) A living radically polymerized acrylic polymer was obtained in the same manner as in Synthesis Example 1, except that the amount of V-65 (2,2'-azobis(2,4-dimethylvaleronitrile), manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) added was changed to 20 mg.
[0078] (Synthesis Example 3 (Synthesis of living radical polymerization acrylic polymer)) A living radical polymerized acrylic polymer was obtained in the same manner as in Synthesis Example 1, except that the composition of the monomer mixture was changed as shown in Table 1.
[0079] (Synthesis Example 4 (Synthesis of acrylic polymer by constant temperature free radical polymerization)) A reactor equipped with a thermometer, a stirrer, and a cooling tube was prepared, and a total of 100 parts by weight of the monomer mixture shown in Table 1 except for 2-methacryloyloxyethyl isocyanate (MOI), 60 parts by weight of ethyl acetate, and 60 parts by weight of toluene were added to the reactor. The reactor was heated to 60°C. Then, 0.15 parts by weight of V-60 (2,2'-azobisisobutyronitrile) was added as a polymerization initiator to the reactor, and a polymerization reaction was carried out at 60°C for 8 hours to obtain a polymer-containing solution. 10 ppm of hydroquinone was added to the reaction vessel with respect to 100 parts by weight of the obtained polymer, and the reaction vessel was heated to 60°C. Then, 8 parts by weight of 2-methacryloyloxyethyl isocyanate (MOI) was dropped into the reaction vessel over 60 minutes, and the reaction was further carried out at 60°C for 120 minutes to obtain a solution containing a constant temperature free radical polymerization acrylic polymer (Synthesis Example 4). In the same manner as in Synthesis Example 1, the content of low molecular weight components, the weight average molecular weight (Mw) and the molecular weight distribution (Mw / Mn) were determined.
[0080] (Synthesis Example 5 (Synthesis of boiling point free radical polymerization acrylic polymer)) A reactor equipped with a thermometer, a stirrer, and a cooling tube was prepared, and a total of 100 parts by weight of the monomer mixture shown in Table 1 except for 2-methacryloyloxyethyl isocyanate (MOI) and 80 parts by weight of ethyl acetate were added to the reactor. The reactor was heated to start reflux. Next, 0.05 parts by weight of V-60 (2,2'-azobisisobutyronitrile, Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator to start polymerization under reflux. Next, 0.15 parts by weight of V-60 (2,2'-azobisisobutyronitrile, Fujifilm Wako Pure Chemical Industries, Ltd.) was added again 2 hours after the start of polymerization. The polymerization reaction was carried out under reflux for 8 hours from the start of polymerization to obtain a polymer-containing solution. Into a reaction vessel, 10 ppm of hydroquinone was added relative to 100 parts by weight of the obtained polymer, and the mixture was heated to 60° C. Then, 8 parts by weight of 2-methacryloyloxyethyl isocyanate (MOI) was dropped into the reaction vessel over 60 minutes, and the mixture was further reacted at 60° C. for 120 minutes to obtain a solution containing a boiling point free radical polymerization acrylic polymer (Synthesis Example 5). In the same manner as in Synthesis Example 1, the content of low molecular weight components, the weight average molecular weight (Mw) and the molecular weight distribution (Mw / Mn) were determined.
[0081] (Synthesis Examples 6 to 9 (Synthesis of living radical polymerization acrylic polymer)) A living radical polymerization acrylic polymer was obtained in the same manner as in Synthesis Example 1, except that a tin catalyst (dioctyltin dilaurate or dibutyltin dilaurate) shown in Table 1 was added to the reaction vessel before dropping 2-methacryloyloxyethyl isocyanate (MOI).
[0082] [Table 1]
[0083] 2EHA: 2-(ethylhexyl) acrylate AAc: acrylic acid 4HBA: 4-Hydroxybutyl acrylate MOI: 2-Methacryloyloxyethyl isocyanate
[0084] (Synthesis Example 10 (Synthesis of Silicone-Based Graft Copolymer)) A reactor equipped with a thermometer, a stirrer, and a cooling tube was prepared. A total of 100 parts by weight of the monomer mixture shown in Table 2 and 80 parts by weight of ethyl acetate were added to the reactor. The reactor was heated to start reflux. Next, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (V-60, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator to the reactor, and polymerization was started under reflux. Next, 2 hours after the start of polymerization, 2,2'-azobisisobutyronitrile (V-60, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added in 0.1 parts by weight increments to continue the polymerization reaction. Then, 7 hours after the start of polymerization, an ethyl acetate solution of a silicone-based graft copolymer (Synthesis Example 10) was obtained. In the same manner as in Synthesis Example 1, the weight average molecular weight (Mw) and the molecular weight distribution (Mw / Mn) were determined.
[0085] (Synthesis Examples 11 to 13, 15 (Synthesis of Silicone-Based Graft Copolymers)) A silicone-based graft copolymer was obtained in the same manner as in Synthesis Example 10, except that the composition of the monomer mixture was changed as shown in Table 2.
[0086] (Synthesis Example 14 (Synthesis of Silicone-Based Graft Copolymer)) A reaction vessel was charged with 10 ppm of hydroquinone per 100 parts by weight of the polymer obtained in Synthesis Example 13, and heated to 60° C. Then, 5 parts by weight of 2-methacryloyloxyethyl isocyanate (MOI) was dropped into the reaction vessel over 60 minutes, and the mixture was allowed to react at 60° C. for a further 120 minutes, yielding a solution containing a silicone-based graft copolymer (Synthesis Example 14).
[0087] [Table 2]
[0088] 2EHA: 2-(ethylhexyl) acrylate AAc: acrylic acid 4HBA: 4-Hydroxybutyl acrylate MOI: 2-Methacryloyloxyethyl isocyanate Silicone macromonomer: One-terminated methacryloyl-modified polydimethylsiloxane (Shin-Etsu Chemical Co., Ltd., weight average molecular weight 4600)
[0089] Example 1 (1) Manufacture of adhesive tapes Ethyl acetate was added to a solution containing a living radical polymerization acrylic polymer (Synthesis Example 1) per 100 parts by weight of nonvolatile content, and the mixture was stirred. A release agent, a thermal polymerization initiator, and a crosslinking agent were added as shown in Table 3, and the mixture was stirred to obtain an adhesive solution with a nonvolatile content of 30% by weight. The obtained adhesive solution was applied to a 25 μm-thick polyimide film, one side of which had been corona-treated, with a doctor knife so that the dried film would be 40 μm thick, and the coating solution was dried by heating at 110° C. for 5 minutes. The mixture was then left to stand at 40° C. for 3 days to cure, to obtain an adhesive tape.
[0090] (2) Measurement of weight loss rate after heating After obtaining a measurement sample consisting of only the adhesive layer, the weight was measured. Under a nitrogen atmosphere (nitrogen flow, flow rate 50 mL / min), the measurement sample was heated from 25°C to 280°C at a heating rate of 10°C / min using a simultaneous differential thermal and thermogravimetric analyzer (Hitachi High-Tech Science Corporation, TG-DTA; STA7200), and heated for 1 hour after reaching 280°C. After cooling, the weight loss was measured, and the weight loss rate was calculated from the obtained weight loss and the weight before heating.
[0091] (3) Measurement of surface peel strength The adhesive tape was cut into 10 mm x 10 mm pieces. Under an environment of room temperature 23°C and relative humidity 50%, the cut adhesive tape was attached to glass (large slide glass with white edge polished No. 2, manufactured by Matsunami Glass Industry Co., Ltd.) at a speed of 10 mm / sec using a 2 kg pressure rubber roller. Then, a heat treatment was performed at 150°C for 10 minutes. After cooling, the surface peel strength of the adhesive tape against the glass was measured according to the method for measuring the surface peel strength of an adhesive tape shown in Figure 1 below.
[0092] FIG. 1 is a diagram showing a schematic diagram of a method for measuring the surface peel strength of an adhesive tape. Under an environment of room temperature 23°C and relative humidity 50%, one side of a double-sided adhesive tape 3 for measurement (#560, manufactured by Sekisui Chemical Co., Ltd.) was attached to the back side of an adhesive tape 1 attached to a glass 2. The glass 2 was fixed so that the side to which the adhesive tape 1 and the double-sided adhesive tape 3 for measurement were attached faced upward, and the other side of the double-sided adhesive tape 3 for measurement was attached and fixed to a jig 4 of a tensile tester. A tensile test was performed in the 90° direction (arrow direction in the figure) at a peel speed of 300 mm / min using a tensile tester (AG-IS, manufactured by Shimadzu Corporation) to measure the surface peel strength. The surface peel strength means the maximum peel strength during the evaluation measurement. As the double-sided adhesive tape 3 for measurement, #560 manufactured by Sekisui Chemical Co., Ltd. was used.
[0093] (4) Measurement of tin content The adhesive layer of the adhesive tape was fed to an ICP optical emission spectrometer (Agilent, 5110 ICP-OES) for measurement, and the tin content in the adhesive layer was measured.
[0094] (Examples 2 to 14, Comparative Examples 1 to 6) Except for changing the composition of the adhesive layer as shown in Table 3, the same procedure as in Example 1 was carried out to obtain an adhesive tape. In Examples 11 and 12, since the adhesive layer was a photocurable type, in the measurement of the surface peel strength, an ultra-high pressure mercury lamp was irradiated from the glass side at 20 mW / cm before the heat treatment. 2 The light was irradiated for 150 seconds at an intensity of 1.
[0095] <Evaluation> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Table 3.
[0096] (1) Evaluation of adhesive tape peeling at high temperature (280℃) The adhesive tape was cut to a width of 25 mm. Under an environment of room temperature 23°C and relative humidity 50%, the cut adhesive tape was attached to glass (large slide glass, white edge polished No. 2, manufactured by Matsunami Glass Industry Co., Ltd.) at a speed of 10 mm / sec using a 2 kg pressure rubber roller. Next, a heat treatment was performed at 150°C for 10 minutes. Then, a heat treatment was performed once at 280°C for 60 minutes. After cooling, the state of the adhesive tape was visually observed. If the adhesive tape peeled off within 10 minutes, it was marked with ×, if the adhesive tape peeled off within 10 to 60 minutes, it was marked with ◯, and if the adhesive tape did not peel off even after 60 minutes, it was marked with ⊚.
[0097] (2) Evaluation of initial adhesive strength The adhesive tape was cut to a width of 25 mm. Under an environment of room temperature of 23°C and relative humidity of 50%, the cut adhesive tape was attached to glass (large slide glass with white edge polish No. 2, manufactured by Matsunami Glass Industry Co., Ltd.) at a speed of 10 mm / sec using a 2 kg pressure rubber roller. After leaving it for 30 minutes, the adhesive tape was peeled off at a speed of 300 mm / min in accordance with JIS Z0237:2009 to measure the 180-degree peel strength.
[0098] (3) Evaluation of adhesive strength after heating The adhesive tape was cut to a width of 25 mm. Under an environment of room temperature 23°C and relative humidity 50%, the cut adhesive tape was attached to glass (large slide glass with white edge polish No. 2, manufactured by Matsunami Glass Industry Co., Ltd.) at a speed of 10 mm / sec using a 2 kg pressure rubber roller. Next, a heat treatment was performed once at 280°C for 60 minutes. After cooling, the adhesive tape was peeled off at a speed of 300 mm / min according to JIS Z0237:2009 to measure the 180-degree peel strength. When the adhesive strength after heating was 1.0 N / inch or more, it was indicated as ○, and when it was less than 1.0 N / inch, it was indicated as ◎.
[0099] [Table 3]
[0100] Silicone diacrylate: EBECRYL350 (manufactured by Daicel Allnex) Thermal polymerization initiator: Perbutyl O (NOF Corporation) Photopolymerization initiator: Omnirad369 (IGM Resins) Isocyanate-based crosslinking agent: Coronate L (manufactured by Nippon Polyurethane Co., Ltd.) [Industrial Applicability]
[0101] According to the present invention, it is possible to provide an adhesive tape that is difficult to peel even at high temperatures during processing of an adherend and can be easily peeled off after the processing is completed. Also, according to the present invention, it is possible to provide a method for manufacturing a semiconductor wafer using the adhesive tape. [Explanation of symbols]
[0102] 1 adhesive tape 2. Glass 3 Double-sided adhesive tape for measurement 4. Jig
Claims
1. An adhesive tape having an adhesive layer on at least one surface, the pressure-sensitive adhesive layer contains a pressure-sensitive adhesive polymer, a silicone-based graft copolymer, a crosslinking agent, and a polymerization initiator, and has a weight loss rate of 15% by weight or less after heating at 280° C. for 1 hour; The adhesive polymer is an acrylic polymer having a radically polymerizable unsaturated bond in the molecule, the silicone-based graft copolymer has a functional group capable of crosslinking with the adhesive polymer, The adhesive tape has a surface peel strength of 15 to 50 N after heating at 150° C. for 10 minutes with an application area of 10 mm×10 mm. An adhesive tape characterized by:
2. 2. The adhesive tape according to claim 1, wherein the content of components having a molecular weight of 50,000 or less as measured by gel permeation chromatography in the adhesive polymer is 10% by weight or less of the total amount of the adhesive polymer.
3. 3. The adhesive tape according to claim 1, wherein the adhesive layer has a tin content of 0.05% by weight or less calculated as tin.
4. 4. The adhesive tape according to claim 1, wherein the adhesive polymer has a weight average molecular weight of 500,000 or more.
5. 5. The pressure-sensitive adhesive tape according to claim 1, wherein the silicone graft copolymer contains 1 to 40% by weight of a structural unit derived from a monomer having a functional group capable of crosslinking with the pressure-sensitive adhesive polymer.
6. 6. The adhesive tape according to claim 1, wherein the content of said silicone graft copolymer is 0.1 to 10 parts by weight based on 100 parts by weight of said adhesive polymer.
7. A method for producing a semiconductor wafer using the adhesive tape according to claim 1, 2, 3, 4, 5 or 6, comprising the steps of: a temporary fixing step of temporarily fixing a semiconductor wafer on the adhesive tape; a semiconductor wafer processing step of subjecting a surface of the semiconductor wafer to a heating process at 250° C. or higher; and an adhesive tape peeling step of peeling the adhesive tape from the semiconductor wafer. A method for manufacturing a semiconductor wafer comprising the steps of:
Citation Information
Patent Citations
Pressure-sensitive adhesive composition
JP1987288676A
Re-releasing-type tack agent
JP1990123182A
Releasable tacky adhesive polymer
JP1993032946A
Adhesive composition and adhesive sheet
JP2003073629A
Ionizing radiation-curable re-releasable adhesive composition
JP2010132755A