Thermoplastic resin composition, method for producing same, molded article containing same, and method for producing molded article
Patent Information
- Application Number
- JP2021559222
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-18
- Filing Date
- 2020-07-07
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-07-07
AI Technical Summary
【0018】 本発明によれば、従来と比較して同等以上の機械的物性を有しながらも、毒性が低減されたクロムフリーのエッチング液を用いためっき工程時に熱サイクル特性、めっき密着力及び外観品質がいずれも優れた熱可塑性樹脂組成物、その製造方法、それを含む成形品及び成形品の製造方法を提供する効果がある。
Smart Images

Figure 0007587519000001 
Figure 0007587519000002
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0129852, filed on October 18, 2019, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a thermoplastic resin composition, a production method thereof, a molded article containing the same, and a production method for the molded article; more specifically, the present invention relates to a thermoplastic resin composition which has mechanical properties equivalent to or better than those of conventional compositions, while being excellent in thermal cycle properties, plating adhesion, and appearance quality, a production method thereof, a molded article containing the same, and a production method for the molded article. [Background technology]
[0003] ABS-based resins, represented by acrylonitrile-butadiene-styrene (ABS), are used in a variety of applications, including automotive products, electronic products, and office equipment, due to the rigidity and chemical resistance of acrylonitrile, and the processability, mechanical strength, and beautiful appearance of butadiene and styrene.
[0004] Existing ABS resins require an etching process to improve plating adhesion in the wet plating process and prevent unplated areas.
[0005] However, the etching solutions used in conventional etching of ABS resins generally contain hexavalent chromium (Cr) in chromic anhydride to provide a physical bond between the plating layer and the base layer. 6+ ), which is designated as a Class 1 carcinogen and has caused adverse effects on workers.
[0006] In addition, in order to safely treat the etching solution as wastewater, a complicated treatment process must be carried out, such as reducing hexavalent chromium to trivalent chromium, neutralizing it, and precipitating it.
[0007] In order to solve these problems, efforts have been made recently to develop less toxic plating processes, and in particular to develop new chromium-free etching solutions for use in less toxic plating processes.
[0008] However, in the process of using a new chrome-free etching solution with reduced toxicity instead of using the existing etching solution, the low reactivity and instability of the new etching solution resulted in reduced plating adhesion and thermal cycle characteristics, resulting in plating reliability that did not meet general standards and, in severe cases, non-plating.
[0009] As a solution to solve this problem, a method of increasing the rubber content of the ABS resin has been proposed, but this may result in a decrease in moldability and a decrease in thermal cycle resistance due to an increase in the linear expansion coefficient. Another solution proposed is to increase the temperature and time of the etching solution during the plating process, but this increases the overall process time and is therefore not efficient in terms of process costs.
[0010] Therefore, there is a pressing need for the development of a thermoplastic resin that has excellent plating adhesion and thermal cycle properties in a toxicity-reducing plating process, does not produce unplated areas, and does not deteriorate in processability, mechanical properties, and appearance properties. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Korean Patent Publication No. 10-2013-0006551 Summary of the Invention [Problem to be solved by the invention]
[0012] In order to solve the above problems of the conventional technology, the present invention aims to provide a thermoplastic resin composition that has mechanical properties equal to or better than those of conventional products and is excellent in thermal cycle characteristics, plating adhesion, and appearance quality during a plating process using a chromium-free etching solution with reduced toxicity, and a manufacturing method thereof, a molded article containing the same, and a manufacturing method of the molded article.
[0013] The above and other objects of the present invention can be achieved by the present invention described below. [Means for solving the problem]
[0014] In order to achieve the above object, the present invention provides a thermoplastic resin composition comprising: (A-1) 17 to 49% by weight of a base resin including an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an alkyl acrylate rubber with an average particle size of 0.05 μm to 0.2 μm and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an average particle size of more than 0.2 μm and not more than 0.7 μm, in a weight ratio of 1:1.5 to 1:4; and (B) 51 to 83% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 200,000 g / mol.
[0015] The present invention also provides a method for producing a thermoplastic resin composition, comprising the steps of kneading and extruding 17 to 49% by weight of a base resin containing (A-1) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an alkyl acrylate rubber with an average particle size of 0.05 μm to 0.2 μm and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an average particle size of more than 0.2 μm and not more than 0.7 μm, in a weight ratio of 1:1.5 to 1:4; and (B) 51 to 83% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 200,000 g / mol.
[0016] The present invention also provides a molded article comprising the thermoplastic resin composition described herein.
[0017] The present invention also provides a method for producing a molded article, comprising the steps of: injecting a thermoplastic resin composition described in this specification to obtain an injected article; etching the injected article with a chromium-free etchant; and plating the etched injected article. Effect of the Invention
[0018] According to the present invention, there is provided a thermoplastic resin composition which has mechanical properties equivalent to or better than those of conventional products, and which is excellent in thermal cycle characteristics, plating adhesion, and appearance quality during a plating process using a chromium-free etching solution with reduced toxicity, as well as a manufacturing method thereof, a molded article containing the same, and a manufacturing method thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The thermoplastic resin composition of the present invention, its production method, a molded article containing the same, and a method for producing the molded article will be described in detail below.
[0020] The inventors have confirmed that when an aromatic vinyl compound-vinyl cyan compound copolymer having a specific weight average molecular weight is mixed with two ASA resins having different rubber particle sizes and a specific weight ratio and applied to a toxicity reducing plating process, there is no deterioration in mechanical properties and no occurrence of unplated areas, and furthermore, plating adhesion and heat cycle properties are greatly improved. Based on this, they have further pursued research and have completed the present invention.
[0021] In the present invention, a reduced toxicity plating process refers to a plating process that includes the step of etching with a chromium-free etchant.
[0022] In the present invention, chromium-free means that no chromium-containing components are intentionally added to the etching solution.
[0023] The thermoplastic resin composition of the present invention is characterized by comprising: (A-1) 17 to 49% by weight of a base resin containing an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an average particle diameter of the alkyl acrylate rubber of 0.05 μm to 0.2 μm and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an average particle diameter of the alkyl acrylate rubber of more than 0.2 μm to 0.7 μm, in a weight ratio of 1:1.5 to 1:4; and (B) 51 to 83% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 200,000 g / mol. In this case, the thermoplastic resin composition has the advantages of having mechanical properties equal to or greater than those of conventional products, while also being excellent in heat cycle properties, plating adhesion, and appearance quality.
[0024] The thermoplastic resin composition of the present invention will be described in detail below with respect to each component.
[0025] As an example, the base resin of the present invention may include (A-1) an alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer in which the average particle diameter of the alkyl acrylate rubber is 0.05 μm to 0.2 μm, and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer in which the average particle diameter of the alkyl acrylate rubber is more than 0.2 μm to 0.7 μm, in a weight ratio of 1:1.5 to 1:4. In this case, there is an advantage that the mechanical properties are not deteriorated and the plating adhesion and heat cycle properties are improved in a chrome-free, low-toxicity plating process.
[0026] The (A-1) alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer can, for example, contain an alkyl acrylate rubber having an average particle size of 0.05 μm to 0.2 μm, preferably 0.07 to 0.2 μm, and more preferably 0.07 to 0.15 μm. Within this range, no swelling or cracking occurs in the plating film after a thermal cycle evaluation, and thus there are advantages in that the thermal cycle characteristics are excellent and the plating adhesion is remarkably excellent.
[0027] In the present invention, the average particle size is measured by a Dynamic Laser Light Scattering method using an Intensity Gaussian Distribution (Nicomp 380).
[0028] The (A-1) alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may, for example, contain 20 to 80% by weight of alkyl acrylate rubber, 10 to 70% by weight of aromatic vinyl compound, and 5 to 50% by weight of vinyl cyan compound. Within these ranges, there are advantages in that no swelling or cracking occurs in the plating film after a heat cycle evaluation, and that adhesion to the plating layer is excellent.
[0029] As another example, the (A-1) alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may contain 30 to 60% by weight of alkyl acrylate rubber, 20 to 50% by weight of aromatic vinyl compound, and 10 to 30% by weight of vinyl cyan compound. Within these ranges, no swelling or cracking occurs in the plating film after a heat cycle evaluation, and thus the effect of excellent heat cycle characteristics, excellent appearance quality, and excellent plating adhesion is achieved.
[0030] The alkyl acrylate rubber may be, for example, an acrylate rubber in which the alkyl group has 1 to 10 carbon atoms.
[0031] As a preferred example, the alkyl acrylate rubber may be one or more selected from the group consisting of methyl acrylate rubber, ethyl acrylate rubber, butyl acrylate rubber, and ethylhexyl acrylate rubber. In this case, there are advantages such as excellent inherent weather resistance and chemical resistance, as well as excellent appearance quality and plating adhesion.
[0032] The aromatic vinyl compound may be, for example, one or more selected from the group consisting of styrene, α-methylstyrene, 2,4-dimethylstyrene, vinyltoluene, t-butylstyrene, and chlorostyrene, and may be preferably styrene. In this case, the aromatic vinyl compound has the effect of being excellent in processability and mechanical properties.
[0033] The vinyl cyanide compound may be, for example, one or more selected from the group consisting of acrylonitrile, methacrylonitrile, and ethacrylonitrile, and may preferably contain acrylonitrile. In this case, the vinyl cyanide compound has the effect of providing excellent processability, impact resistance, and plating properties.
[0034] The (A-2) alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may, for example, contain an alkyl acrylate rubber having an average particle size of more than 0.2 μm and not more than 0.7 μm, preferably 0.25 to 0.6 μm, and more preferably 0.25 to 0.45 μm. Within this range, there are effects such as excellent thermal cycle characteristics, fluidity, impact resistance, and appearance quality.
[0035] The (A-2) alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may, for example, comprise 20 to 80% by weight of alkyl acrylate rubber, 10 to 70% by weight of aromatic vinyl compound, and 5 to 50% by weight of vinyl cyan compound. Within these ranges, no swelling or cracking of the plating film occurs after a heat cycle evaluation, and thus the composition has the advantages of excellent heat cycle properties, fluidity, and impact strength.
[0036] As another example, the (A-2) alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer may contain 40 to 60% by weight of alkyl acrylate rubber, 20 to 40% by weight of aromatic vinyl compound, and 10 to 30% by weight of vinyl cyan compound. Within this range, mechanical properties such as impact strength are improved, flowability is appropriate, so processability is excellent, and there are advantages in that no cracks occur in the plating film after thermal cycle evaluation.
[0037] The types of the alkyl acrylate rubber, aromatic vinyl compound, and vinyl cyan compound contained in the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (A-2) may be within the same range as the types of the alkyl acrylate rubber, aromatic vinyl compound, and vinyl cyan compound contained in the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (A-1) of the present invention.
[0038] The weight ratio of the alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer (A-1) to the alkyl acrylate-aromatic vinyl compound-vinyl cyanide compound graft copolymer (A-2) may be, for example, 1:1.5 to 1:4, preferably 1:1.6 to 1:3.5, and more preferably 1:1.65 to 1:3. Within this range, the fluidity is appropriate, resulting in excellent processability, and since no swelling or cracking of the plating film occurs after the evaluation of the thermal cycle, the thermal cycle characteristics are excellent, and the plating characteristics are improved. If the ratio exceeds the above range, the plating adhesion and thermal cycle characteristics are reduced, and if it is below the above range, problems occur such as reduced fluidity, impact resistance, and thermal cycle characteristics.
[0039] The base resin may be contained in an amount of, for example, 17 to 49% by weight, preferably 20 to 40% by weight, relative to 100% by weight of the thermoplastic resin. Within this range, there are advantages in that the mechanical properties, processability and plating adhesion are excellent, and in particular, the thermal cycle properties are remarkably excellent.
[0040] If the content of the base resin is less than the above range, mechanical properties such as impact strength, plating adhesion, and thermal cycle properties are significantly reduced, and if the content of the base resin is more than the above range, processability and thermal cycle properties are reduced.
[0041] The aromatic vinyl compound-vinyl cyan compound copolymer (B) of the present invention may have a weight average molecular weight of, for example, 50,000 to 200,000 g / mol, preferably 60,000 to 180,000 g / mol, and more preferably 70,000 to 150,000 g / mol. Within this range, the copolymer has an appropriate fluidity and is therefore easy to process, and has excellent mechanical properties such as impact resistance, while also having excellent plating adhesion.
[0042] In the present invention, unless otherwise specified, the weight average molecular weight can be measured by dissolving 1 g of the copolymer in tetrahydrofuran (THF) at a temperature of 40° C. and then using a gel permeation chromatography (GPC) filled with porous silica. At this time, the molecular weight is measured after calibration using polystyrene (PS) as a standard substance.
[0043] The (B) aromatic vinyl compound-vinyl cyan compound copolymer may be contained in an amount of, for example, 51 to 83% by weight, preferably 60 to 83% by weight, and more preferably 60 to 75% by weight, relative to 100% by weight of the thermoplastic resin. Within this range, the flowability is appropriate, making the resin easy to process, and the resin surface is sufficiently uneven during the etching process using a chrome-free etching solution, providing the advantages of excellent plating adhesion, appearance quality, and the like.
[0044] The (B) aromatic vinyl compound-vinyl cyan compound copolymer may contain, for example, 20 to 40% by weight of the vinyl cyan compound and 60 to 80% by weight of the aromatic vinyl compound. Within this range, the copolymer has an excellent balance of overall physical properties such as mechanical properties, while also exhibiting excellent plating adhesion and thermal cycle properties.
[0045] As another example, the (B) aromatic vinyl compound-vinyl cyan compound copolymer may contain 23 to 37% by weight of the vinyl cyan compound and 63 to 77% by weight of the aromatic vinyl compound. Within this range, there are advantages in that the plating adhesion, heat cycle characteristics, and appearance quality are all excellent during a plating process using a chromium-free etching solution with reduced toxicity.
[0046] The (B) aromatic vinyl compound-vinyl cyan compound copolymer may be prepared by, for example, solution polymerization or bulk polymerization, and in this case, it has the effect of being excellent in heat resistance and fluidity.
[0047] The solution polymerization and bulk polymerization are not particularly limited as long as they are solution polymerization and bulk polymerization methods commonly used in the technical field to which the present invention pertains.
[0048] The thermoplastic resin composition of the present invention may be, for example, a chromium-free thermoplastic resin composition for an etching solution. In this case, since it does not contain chromic acid, which is a toxic substance, it is environmentally friendly; since sufficient irregularities are formed on the surface of the resin during the etching process, plating adhesion is improved; and since no blistering or cracking occurs in the plating film after evaluation of the thermal cycle, it has the advantages of having excellent appearance characteristics as well as excellent mechanical properties.
[0049] The chromium-free etching solution may be, for example, a solution containing permanganate and an organic or inorganic acid, and preferably potassium permanganate (KMnO 4 ) and phosphoric acid (H 3 PO 4 ) and sulfuric acid (H 2 SO 4 ) is a chrome-free etching solution containing one or more of the following: In this case, there is an advantage that sufficient unevenness is formed on the surface of the resin, improving the plating adhesion between the resin and the plating layer, and maintaining excellent appearance quality.
[0050] The chromium-free etching solution may be, for example, an etching solution containing 20 to 30 g / L of permanganate and 550 to 650 mL / L of phosphoric acid. Within this range, there are advantages in that uniform unevenness is formed overall, plating adhesion is improved, and the appearance quality of the molded product is excellent.
[0051] The thermoplastic resin composition may further include additives such as, for example, a heat stabilizer, an antioxidant, an impact modifier, a light stabilizer, a plasticizer, a lubricant, and an antistatic agent. In this case, the function of the additives can be realized without deteriorating the inherent basic physical properties of the thermoplastic resin composition of the present invention.
[0052] For example, the additive may be included in an amount of 0.1 to 5 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the total content of the base resin and the aromatic vinyl compound-vinyl cyan compound copolymer.
[0053] The thermoplastic resin composition of the present invention may have a melt index (220°C, 10 kg) of 14 to 36 g / 10 min, for example, and may preferably have a melt index of 15 to 33 g / 10 min, as measured in accordance with ASTM D1238. Within this range, the composition has excellent fluidity, and thus provides the advantage of being easily injection molded into various shapes.
[0054] The thermoplastic resin composition of the present invention has, for example, an Izod impact strength (6.4 mm, 23°C) of 15 kgf cm / cm as measured in accordance with ASTM D256. 2 Above, 15~36kgf・cm / cm 2 , or 15~31kgf·cm / cm 2 Within this range, the effect of excellent impact resistance is obtained.
[0055] The thermoplastic resin composition of the present invention may have a plating adhesion of, for example, 9 N / cm or more, 9 to 25 N / cm, or 9 to 15 N / cm. Within this range, the composition has the effect of providing excellent appearance quality after plating.
[0056] The method for producing the thermoplastic resin composition of the present invention will be described below.
[0057] The method for producing the thermoplastic resin composition of the present invention may, for example, include a step of kneading and extruding 17 to 49% by weight of a base resin including (A-1) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an average particle diameter of the alkyl acrylate rubber of 0.05 μm to 0.2 μm and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer having an average particle diameter of the alkyl acrylate rubber of more than 0.2 μm to 0.7 μm in a weight ratio of 1:1.5 to 1:4; and (B) 51 to 83% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 200,000 g / mol. In this case, the flowability is appropriate, so that the process is easy, and there is no deterioration in mechanical properties. In a plating process using a chrome-free etching solution with reduced toxicity, the plating adhesion, heat cycle properties, and appearance properties are all excellent.
[0058] As an example of the kneading, (A-1) the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer, (A-2) the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer, and (B) the aromatic vinyl compound-vinyl cyan compound copolymer may be added at once and kneaded.
[0059] The kneading and extrusion may be carried out, for example, using a single screw extruder, a twin screw extruder, or a Banbury mixer. It is preferable to carry out the kneading and extrusion using a twin screw extruder. In this case, the composition is uniformly dispersed, resulting in excellent compatibility.
[0060] The kneading and extrusion may be carried out under conditions where, for example, the screw rotation speed is 200 to 300 rpm, or 250 to 300 rpm, and the temperature is 200 to 300° C., 200 to 270° C., or 220 to 260° C. In this case, since the processing amount per unit time is appropriate, there is an effect of suppressing excessive breakage while having excellent process efficiency.
[0061] The following describes a molded article containing the thermoplastic resin composition of the present invention and a method for producing the same. In describing the molded article of the present invention and the method for producing the same, all of the contents of the thermoplastic resin composition described above are included, as is the method for producing the thermoplastic resin composition of the present invention.
[0062] The molded article of the present invention may, for example, contain the thermoplastic resin composition of the present invention, and the molded article has the advantages of being excellent in all of mechanical properties, plating properties, and thermal cycle properties.
[0063] As an example, the molded article may include a substrate layer and a plating layer. The substrate layer may be molded from the thermoplastic resin composition of the present invention. The plating layer is preferably formed containing one or more elements selected from the group consisting of copper, nickel, and chromium. In this case, there are advantages in that the adhesion between the substrate layer and the plating layer is excellent, and the mechanical properties and appearance quality are excellent.
[0064] The molded article may be, for example, a molded article made using a chromium-free etching solution. In this case, since it does not contain chromic acid, which is a toxic substance, it is environmentally friendly, and since no blistering or cracking occurs in the plating film after a thermal cycle evaluation, it has the advantages of being excellent in appearance characteristics, as well as excellent mechanical properties and plating characteristics.
[0065] As a preferred example, the chromium-free etching solution may be a solution containing a permanganate and an organic acid or an inorganic acid, and more preferably, potassium permanganate (KMnO 4 ) and phosphoric acid (H 3 PO 4In this case, there is an advantage that sufficient irregularities are formed on the surface of the resin, improving the plating adhesion between the resin and the plating layer, and resulting in excellent appearance quality.
[0066] The molded product may be, for example, a water faucet, an automobile interior material, or an automobile exterior material, which has advantages such as excellent plating properties, mechanical properties, and thermal cycle properties, and therefore is not easily damaged even when directly touched by human hands and can be used for a long period of time.
[0067] As a specific example, the water faucet may be a shower head or a water pipe.
[0068] As an example, a method for producing a molded product of the present invention may include the steps of injecting the thermoplastic resin composition of the present invention to obtain an injected product, etching the injected product using a chromium-free etching solution, and plating the etched injected product. In this case, a molded product having excellent plating adhesion can be obtained without deterioration of mechanical properties and thermal cycle properties.
[0069] The etching step is a process of melting the rubber portion in the thermoplastic resin to impart irregularities to the surface. The holes formed by the melting of the rubber through this process act as anchoring sites that provide a physical bond with the plating film, thereby improving plating adhesion and imparting polarity to the surface to prevent the occurrence of unplated areas during the subsequent plating process.
[0070] In the etching step, the etching time may be, for example, 2 to 15 minutes or 3 to 10 minutes, and the etching temperature may be, for example, 60 to 80°C or 65 to 75°C. Within these ranges, a molded product having excellent plating adhesion and thermal cycle properties can be obtained while reducing process costs.
[0071] The chromium-free etching solution contains all of the contents of the chromium-free etching solution for the thermoplastic resin composition of the present invention described above.
[0072] In a preferred embodiment, the chrome-free etching solution is a mixture of permanganate and phosphoric acid (H 3 PO 4 ) is a chrome-free etching solution.
[0073] For example, the method for manufacturing the molded product may include a degreasing step for removing oil, etc., from the injection product prior to the etching step.
[0074] The degreasing step may be, for example, a step of treating the injection product with a surfactant to remove oil, and the surfactant is not particularly limited as long as it is a surfactant generally used in a degreasing step in the technical field to which the present invention belongs.
[0075] The degreasing step may be carried out, for example, at 40 to 60° C. or 50 to 60° C. for 1 to 15 minutes or 3 to 8 minutes, and within this range, the degreasing efficiency is excellent.
[0076] The plating step may include, for example, a plating pretreatment step including one or more of a catalysis step and an activation step, and a plating step including one or more of a chemical plating step and an electroplating step.
[0077] The catalysis step may be, for example, a step of adsorbing into the metal anchor holes using a metal catalyst. The metal catalyst is not particularly limited as long as it is a metal catalyst that is commonly used in plating pretreatment in the technical field to which the present invention belongs, but is preferably a palladium-tin catalyst, in which case palladium is adsorbed into the anchor holes.
[0078] The catalysis step can be carried out, for example, at 20 to 40°C for 1 to 8 minutes, and preferably at 25 to 35°C for 1 to 5 minutes. Within this range, there is an effect of excellent adsorption efficiency of the metal into the anchor pores.
[0079] The activation step may be, for example, a step of activating the metal by treating it with an aqueous sulfuric acid solution. In this case, by removing metals other than the metal to be adsorbed in the anchor holes, it is possible to achieve a significant effect of activating the metal adsorbed in the anchor holes.
[0080] The activation step can be carried out, for example, at 45 to 65° C. for 1 to 10 minutes, and preferably at 50 to 60° C. for 1 to 5 minutes. Within this range, the activation effect is large.
[0081] The chemical plating may be, for example, electroless plating using a metal salt, and the metal salt may preferably be nickel sulfate.
[0082] The chemical plating can be carried out preferably at 20 to 40° C. for 1 to 20 minutes, more preferably at 25 to 35° C. for 1 to 10 minutes. Within this range, there is an advantage in that the electroless plating properties are excellent.
[0083] The electroplating may be, for example, one or more types of electroplating selected from the group consisting of copper electroplating, nickel electroplating, and chromium electroplating.
[0084] The copper electroplating may be performed using any copper salt commonly used in the field of the present invention, without any restrictions, but is preferably performed using copper sulfate.
[0085] The copper electroplating may be carried out, for example, at 15 to 35° C. for 20 to 60 minutes at 2 to 4 A / dm 2 Preferably, the heating can be performed at 20 to 30° C. for 30 to 40 minutes at 2.5 to 3.5 A / dm 2 This can be done.
[0086] The nickel electroplating may be carried out using any nickel salt commonly used in nickel electroplating in the technical field to which the present invention pertains, without any restrictions, but preferably, nickel sulfate is used.
[0087] The nickel electroplating may be carried out, for example, at 50 to 60° C. for 10 to 30 minutes at 2 to 4 A / dm 2 Preferably, the heating can be performed at 55 to 60° C. for 10 to 20 minutes at 2.5 to 3.5 A / dm 2 This can be done.
[0088] The chromium electroplating may be carried out using any chromium-based compound commonly used in the art for chromium electroplating, without any restrictions, but preferably chromic anhydride.
[0089] The chromium electroplating is preferably performed at 45 to 65° C. for 1 to 15 minutes at 10 to 20 A / dm 2 More preferably, the heating can be performed at 50 to 60° C. for 1 to 5 minutes at 13 to 18 A / dm 2 This can be done.
[0090] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical spirit of the present invention. Naturally, such changes and modifications also fall within the scope of the appended claims. EXAMPLES
[0091] The materials used in the following examples and comparative examples are as follows.
[0092] (A-1) Graft ASA resin (SA130, manufactured by LG Chem) in which the average particle size of acrylate rubber is 100 nm (A-2) Graft ASA resin (SA928, manufactured by LG Chem) in which the average particle size of acrylate rubber is 300 nm (B) SAN resin (95RF, manufactured by LG Chem) containing 30% by weight of vinyl cyanide compound and having a weight average molecular weight of 80,000 g / mol. (C) Grafted ABS resin (DP270E, manufactured by LG Chem)
[0093] Examples 1 to 4 and Comparative Examples 1 to 7 Each component was fed into a twin-screw extruder to have the composition and content shown in Table 1 below, and melted and kneaded at 230°C to prepare a pellet-shaped resin composition, which was then extruded to prepare specimens for measuring physical properties. Through extrusion, square specimens measuring 100mm x 100mm x 3mm and cap-shaped specimens measuring 150mm x 80mm x 3mm were prepared.
[0094] A plating film having a uniform thickness of 30 μm or more was formed on the prepared specimen by the following plating method.
[0095] First, the surfactant was treated at 55 °C for 5 min to remove the oil, and then KMnO 4 The specimens were oxidized at 68°C for 10 minutes using a chromium-free etching solution containing 25 g / L chromium and 600 mL / L phosphoric acid. Palladium was then adsorbed into the anchor holes using a palladium-tin catalyst at 30°C for 2 minutes. An activation step was performed at 55°C for 2 minutes, followed by removal of the tin using an aqueous sulfuric acid solution and electroless plating with nickel sulfate at 30°C for 5 minutes. Electroplating was performed using copper, nickel and chromium after electroless plating, while copper electroplating using copper sulfate was performed at 25°C for 35 minutes at 3 A / dm 2 Chromium electroplating using chromic anhydride solution was performed at 55°C for 3 minutes and 15A / dm 2 So I went.
[0096] [Table 1] (In Table 1, the content of each component is expressed as weight percent based on the total content of (A-1), (A-2), (B) and (C).)
[0097] [Test example] The properties of the specimens prepared in Examples 1 to 4 and Comparative Examples 1 to 7 were measured by the following methods, and the results are shown in Table 2 below.
[0098] *Melt Index (g / 10 min): The melt index was measured at 220°C and 10 kg in accordance with the standard measurement ASTM D1238 using the prepared test specimen.
[0099] *Notched Izod Impact Strength, kgf cm / cm 2 ):Measurements were performed using 6.4 mm thick test pieces in accordance with standard measurement ASTM D256.
[0100] * Evaluation of plating adhesion: A 10mm wide scratch was made on the front of a plated square specimen measuring 100mm x 100mm x 3mm, and the specimen was peeled off vertically for 80mm using a push-pull gage. The average value of the measured values was shown.
[0101] *Thermal cycle characteristics: After carrying out the following steps (1) to (5) in a chamber using a cap-shaped test piece, the appearance of the plating film was visually observed and categorized as follows: ○ if no cracks or plating blistering occurred, × if even a partial crack or plating blistering occurred. (1) The temperature inside the chamber was maintained at -40°C for 60 minutes. (2) The temperature inside the chamber is raised to 90°C within one minute. (3) The temperature inside the chamber is maintained at 90°C for 60 minutes. (4) The temperature inside the chamber is cooled to -40°C within one minute. (5) Repeat steps (1) to (4) eight times.
[0102] *Appearance quality evaluation (evaluation of the presence or absence of unplated areas): The appearance of a cap-shaped test piece with dimensions of 150mm x 80mm x 3mm was visually observed, and if there were no unplated areas, it was categorized as 'no abnormality', and if there were even a few unplated areas, it was categorized as 'unplated'.
[0103] [Table 2]
[0104] As shown in Table 2, in the case of Examples 1 to 4 of the present invention, it was confirmed that mechanical properties such as impact strength were improved by including two types of ASA resins with different rubber particle sizes and a specific amount of SAN resin having a specific weight average molecular weight, and that suitable fluidity resulted in excellent processability, and improved plating adhesion, thermal cycle properties, and appearance quality. Furthermore, it was confirmed that the present invention significantly improved plating adhesion and thermal cycle properties without reducing mechanical properties and fluidity in a plating process using a chromium-free etching solution with reduced toxicity.
[0105] On the other hand, in the case of Comparative Example 1, which contains one ASA resin instead of two ASA resins with different average particle diameters of rubber, it was confirmed that the melt index and impact strength were reduced and that cracks occurred in the plating film after the thermal cycle evaluation, indicating that the thermal cycle characteristics were poor.In addition, in the case of Comparative Example 2, which is another example containing one ASA resin, it was confirmed that the plating adhesion was significantly reduced and blisters occurred in the plating film after the thermal cycle evaluation.
[0106] Furthermore, in the case of Comparative Example 3 containing only ABS resin, there was a problem of non-plating.
[0107] In addition, in the case of Comparative Example 4, in which the total content of two ASA resins having different average particle diameters of rubber was below the content range according to the present invention, mechanical properties such as impact strength decreased, plating adhesion was significantly decreased, and after a heat cycle evaluation, blisters occurred in the plating film, confirming poor plating characteristics. In the case of Comparative Example 5, in which the total content exceeded the content range according to the present invention, the melt index was not appropriate, so processability decreased, and cracks occurred in the plating film after a heat cycle evaluation, confirming poor thermal cycle characteristics.
[0108] Furthermore, in the case of Comparative Example 6, in which the weight ratio of the ASA resin having an average particle size of the alkyl acrylate rubber of 0.05 to 0.2 μm and the ASA resin having an average particle size of the alkyl acrylate rubber of more than 0.2 μm and 0.7 μm or less is below the range of the present invention, it was confirmed that the melt index was significantly reduced and cracks occurred after the thermal cycle evaluation. Conversely, in the case of Comparative Example 7, in which the weight ratio exceeds the range of the present invention, it was confirmed that the plating adhesion was reduced and at the same time, blisters were generated after the thermal cycle evaluation, resulting in poor thermal cycle characteristics.
Claims
1. 17 to 49% by weight of a base resin containing (A-1) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer in which an aromatic vinyl compound and a vinyl cyan compound are grafted onto an alkyl acrylate rubber, the alkyl acrylate rubber having an average particle size of 0.05 μm to 0.15 μm, and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer in which an aromatic vinyl compound and a vinyl cyan compound are grafted onto an alkyl acrylate rubber, the alkyl acrylate rubber having an average particle size of more than 0.2 μm to 0.7 μm, in a weight ratio of 1:1.5 to 1:4; (B) 51 to 83% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer having a weight average molecular weight of 50,000 to 80,000 g / mol, a thermoplastic resin composition used to obtain a molded article having a plating layer by injecting a thermoplastic resin composition into an injection product, etching the injection product with a chromium-free etching solution, and plating the etched injection product; A thermoplastic resin composition, characterized in that a molded article having the plating layer has a plating adhesion of 9 N / cm or more.
2. The thermoplastic resin composition according to claim 1, wherein the alkyl acrylate rubbers of the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (A-1) and the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (A-2) each independently have an alkyl group having 1 to 10 carbon atoms.
3. The thermoplastic resin composition according to claim 1 or 2, wherein the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (A-1) and the alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer (A-2) independently contain 20 to 80% by weight of an alkyl acrylate rubber, 10 to 70% by weight of an aromatic vinyl compound, and 5 to 50% by weight of a vinyl cyan compound.
4. The thermoplastic resin composition according to any one of claims 1 to 3, characterized in that the (B) aromatic vinyl compound-vinyl cyan compound copolymer contains 20 to 40% by weight of a vinyl cyan compound and 60 to 80% by weight of an aromatic vinyl compound.
5. The thermoplastic resin composition according to any one of claims 1 to 4, characterized in that the melt index (220 ° C, 10 kg) measured in accordance with ASTM D1238 is 14 to 36 g / 10 min.
6. Impact strength measured according to ASTM D256 is 15 kgf cm / cm 2 The thermoplastic resin composition according to any one of claims 1 to 5, characterized in that
7. A method for producing a thermoplastic resin composition, comprising the steps of kneading and extruding 17 to 49% by weight of a base resin including (A-1) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer in which an aromatic vinyl compound and a vinyl cyan compound are grafted onto an alkyl acrylate rubber, the alkyl acrylate rubber having an average particle size of 0.05 μm to 0.15 μm, and (A-2) an alkyl acrylate-aromatic vinyl compound-vinyl cyan compound graft copolymer in which an aromatic vinyl compound and a vinyl cyan compound are grafted onto an alkyl acrylate rubber, the alkyl acrylate rubber having an average particle size of more than 0.2 μm to 0.7 μm, in a weight ratio of 1:1.5 to 1:4; and (B) 51 to 83% by weight of an aromatic vinyl compound-vinyl cyan compound copolymer in which a weight average molecular weight is 50,000 to 80,000 g / mol, The thermoplastic resin composition is used to obtain a molded article having a plating layer by injecting the thermoplastic resin composition to obtain an injection product, etching the injection product with a chromium-free etching solution, and plating the etched injection product, The manufacturing method, wherein the molded article having the plating layer has a plating adhesion of 9 N / cm or more.
8. A molded article having a plating layer, comprising the thermoplastic resin composition according to any one of claims 1 to 6.
9. A step of injecting the thermoplastic resin composition according to any one of claims 1 to 6 to obtain an injected product; Etching the projectile using a chromium-free etchant; and plating the etched injected article.
Citation Information
Patent Citations
Thermoplastic resin composition, material for lighting fixture of vehicle and housing part for lighting fixture of vehicle
JP2007091970A
Method for metallizing plastic surface
JP2008031513A
Thermoplastic resin composition and method for producing the same
JP2008504387A
Graft Copolymer Composition and Thermoplastic ResinComposition the Same
KR1020060016165A
Thermoplastic resin composition with good mechanicalproperties, improved weatherability and less smoke andpolymer resin articles produced from the same