Copper foil laminate film and electronic device including same
The copper foil laminate film with a fluorine-containing base material and a tie layer with high metal-oxygen bond dissociation energy addresses dielectric and adhesive strength issues, enhancing performance at high frequencies and temperatures.
Patent Information
- Application Number
- JP2022201354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-20
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Existing copper foil laminate films face challenges with deteriorating dielectric properties at high frequencies, coatability, and adhesive strength between the substrate and copper foil, particularly at room temperature and high temperatures.
A copper foil laminate film comprising a fluorine-containing base material with a tie layer having a metal-oxygen bond dissociation energy of 400 kJ/mol or more, a copper layer, and specific thicknesses for the tie and copper layers, enhancing dielectric properties and adhesive strength.
The laminate film exhibits improved dielectric properties, coatability, and excellent adhesive strength at high frequencies, ensuring stable bonding between the substrate and copper foil.
Smart Images

Figure 0007587566000002 
Figure 0007587566000003 
Figure 0007587566000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a copper foil laminate film and an electronic device including the same. [Background technology]
[0002] A copper foil laminate film is a laminate of a substrate and a conductive copper foil. The use of the copper foil laminate film is increasing with the trend of miniaturization and weight reduction of electronic devices. Recently, with the development of 5G mobile communication devices, signal transmission speeds in the GHz band have become common. Due to such a trend toward higher signal frequencies, research is being conducted to improve the dielectric properties at high frequencies for substrates used in printed circuits or antenna elements. In response to such demands, a method of forming a coating layer on the substrate surface is used. However, the substrate on which such a coating layer is formed has reduced coatability of the substrate surface and room temperature adhesion and / or high temperature adhesion between the substrate and the copper foil. As a result, there is a tendency for pattern etching and chemical resistance under acid or base to decrease. Therefore, there is still a demand for a copper foil laminate film having improved dielectric properties at high frequencies, as well as coatability of the substrate surface and excellent room temperature and high temperature adhesion between the substrate and the copper foil. Summary of the Invention [Problem to be solved by the invention]
[0003] The problem to be solved by the present invention is to provide a copper foil laminated film having improved dielectric properties at high frequencies, as well as excellent coatability on the substrate surface and excellent room temperature and high temperature adhesion between the substrate and the copper foil.
[0004] Another problem to be solved by the present invention is to provide an electronic device including the copper foil laminate film. [Means for solving the problem]
[0005] According to one aspect, A fluorine-containing substrate; a tie layer disposed on the fluorine-containing substrate; a copper layer disposed on the tie layer; The tie layer is a metal layer or a metal alloy layer containing a metal having a metal-oxygen (MO) bond dissociation energy of 400 kJ / mol or more, The thickness of the tie layer is provided as a copper foil laminate film of 10 nm to 100 nm.
[0006] The water contact angle with the fluorine-containing substrate is also 120° or less.
[0007] The contact angle of diiodomethane with the fluorine-containing substrate is also 90° or less.
[0008] The surface energy of the fluorine-containing substrate is also 11 dyne / cm to 25 dyne / cm.
[0009] The fluorine content of the surface of the fluorine-containing substrate is also 60 atomic % to 75 atomic %.
[0010] The tie layer also includes one or more metals or metal alloys selected from W, Ti, Sn, Cr, Al, and Mo.
[0011] The tie layer further comprises Ni, the Ni content being 50 wt % or less.
[0012] The peel strength of the copper seed layer and the copper plating layer from the polyimide-based substrate having the fluorine layer disposed thereon, measured after leaving the substrate at room temperature (25° C.) for 3 days, is 0.65 kgf / cm or more.
[0013] The peel strength of the copper seed layer and the copper plating layer from the polyimide-based substrate having the fluorine layer thereon, measured after two or more heat treatments at a temperature of 150° C. or higher and leaving the substrate for one day, is 0.35 kgf / cm or more.
[0014] The thickness of the copper plating layer is also 12 μm or less.
[0015] According to another aspect, An electronic device is provided that includes the aforementioned copper foil laminate film.
[0016] The electronic element may also include an antenna element or an antenna cable. Effect of the Invention
[0017] A copper foil laminated film according to one embodiment includes a fluorine-containing substrate, a tie layer disposed on the fluorine-containing substrate, and a copper layer disposed on the tie layer. The tie layer is a metal layer or a metal alloy layer containing a metal having a metal-oxygen (MO) bond dissociation energy of 400 kJ / mol or more, and the thickness of the tie layer is 10 nm to 100 nm. The copper foil laminated film can have improved dielectric properties at high frequencies, as well as coatability on the substrate surface and excellent room temperature and high temperature adhesion between the substrate and the copper foil. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic cross-sectional view of a copper foil laminate film according to an embodiment. [Diagram 2] 1 is a schematic cross-sectional view of a double-sided copper foil laminate film according to another embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, a copper foil laminate film and an electronic device including the same will be described in detail with reference to the following examples and drawings. It will be obvious to those skilled in the art that the examples are merely presented to more specifically explain the present invention, and the scope of the present invention is not limited by the examples.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. In case of conflict, the present specification, including definitions, will control.
[0021] Although methods and materials similar or equivalent to those described herein can also be used in the practice or testing of the present invention, suitable methods and materials are described herein.
[0022] As used herein, the term "comprises" means that it does not exclude other elements, but also includes other elements, unless specifically stated to the contrary.
[0023] As used herein, the term "and / or" means any and all combinations of one or more of the associated listed items. As used herein, the term "or" means "and / or." As used herein, the phrase "at least one" or "one or more" preceding an element may be used to indicate that the entire list of elements may be supplemented, and not that each of the elements listed above may be supplemented individually.
[0024] In this specification, the term "polyimide-based substrate" is meant to include "polyimide substrate" and "polyimide-containing derivative substrate."
[0025] In this specification, when an element is referred to as being disposed "on" another element, the element may be disposed directly on the other element, or there may be intervening elements between the elements, whereas when an element is referred to as being disposed "directly on" another element, there are no intervening elements.
[0026] In electronic devices, antenna elements are generally manufactured by laminating a metal layer, such as a copper foil, onto a substrate, through which electrical current flows according to radio signals.
[0027] Losses occurring in relation to signal reception of an antenna may include losses due to the dielectric constant of the substrate, and signal losses physically occurring due to electrical resistance when a radio signal, i.e., an electrical signal, flows through a metal layer. In a radio signal having a high frequency band, the electrical flow of the radio signal is more concentrated on the surface of the metal layer than in a radio signal having a relatively low frequency band. In addition, in a laminated copper foil laminate film, physical stress is generated in the copper foil in the bent region of the antenna element, causing cracks on the surface. As a result, transmission losses may occur. To solve such problems, a method of applying a substance that improves the dielectric properties on the substrate surface has been adopted. However, such a method has a problem in that the coating property of the substrate surface and the adhesive strength between the substrate and the copper foil are reduced.
[0028] Taking note of such a point, the inventors of the present invention propose the following copper foil laminate film.
[0029] According to one embodiment, the copper foil laminate film includes a fluorine-containing substrate, a tie layer disposed on the fluorine-containing substrate, and a copper layer disposed on the tie layer, the tie layer being a metal layer or metal alloy layer containing a metal having a metal-oxygen (MO) bond dissociation energy of 400 kJ / mol or more, and the thickness of the tie layer is 10 nm to 100 nm.
[0030] In this specification, the term "fluorine-containing substrate" refers to a substrate containing fluorine, specifically, a substrate containing a resin containing fluorine atoms. In this case, the fluorine-containing substrate may be a substrate itself containing a resin containing fluorine atoms, or may contain a resin containing fluorine atoms together with other resins in the substrate, or may be formed by surface-treating or coating the substrate surface with a resin containing fluorine atoms. Examples of the case where a resin containing fluorine atoms is contained in the substrate together with other resins include a case where a resin containing fluorine atoms is mixed with a polyimide resin to form a substrate, a case where a resin containing fluorine atoms is coated on the surface of an organic or inorganic particle contained in the substrate, or a resin containing fluorine atoms is mixed and contained in the organic or inorganic particle itself. Examples of the case where a resin containing fluorine atoms is surface-treated or coated on the substrate surface include a case where a resin containing fluorine atoms is surface-treated or coated on one or both sides of the substrate. The copper layer may be formed by a layer arranged in the order of a copper seed layer and a copper plating layer.
[0031] The copper foil laminate film may have excellent room temperature and high temperature adhesion between the fluorine-containing substrate and the copper seed layer and the copper plating layer while improving the coatability of the substrate surface along with improved dielectric properties at high frequencies.
[0032] Fig. 1 is a schematic cross-sectional view of a copper foil laminate film 10 according to an embodiment. Fig. 2 is a schematic cross-sectional view of a double-sided copper foil laminate film 20 according to an embodiment.
[0033] 1, a copper foil laminate film 10 according to one embodiment includes a polyimide substrate 1 having a fluorine layer 5 disposed thereon as a fluorine-containing substrate, and a tie layer 2, a copper seed layer 3, and a copper plating layer 4 disposed in that order on the upper surface of the polyimide substrate 1 having the fluorine layer 5 disposed thereon. Referring to FIG. 2, a copper foil laminate film 20 according to another embodiment includes a polyimide substrate 11 having a fluorine layer 15 disposed thereon as a fluorine-containing substrate, a first surface 21 having a tie layer 12, a copper seed layer 13, and a copper plating layer 14 disposed in that order on the upper surface of the polyimide substrate 11 having the fluorine layer 15 disposed thereon, and a second surface 22 having a tie layer 12', a copper seed layer 13', and a copper plating layer 14' disposed in that order on the lower surface of the polyimide substrate 11 having a fluorine layer 15' disposed thereon as a fluorine-containing substrate.
[0034] The fluorine-containing substrates constituting the copper foil laminate films 10, 20 are the polyimide substrates 1, 11 with the fluorine layers 5, 15, 15', the tie layers 2, 12, 12', the copper seed layers 3, 13, 13' and the copper plating layers 4, 14, 14'.
[0035] <Polyimide-based substrate 1, 11 having fluorine layer 5, 15, 15' as fluorine-containing substrate>
[0036] The fluorine-containing substrate of the copper foil laminated film 10 according to an embodiment is also the polyimide-based substrate 1, 11 on which the fluorine layers 5, 15, 15' are disposed.
[0037] The polyimide-based substrates 1 and 11 are also modified polyimide (m-PI) substrates. The modified polyimide substrate is a resin substrate in which the number of highly polar substituents has been reduced. When a wireless signal is passed through a circuit, a change occurs in the electric field around the circuit. If such an electric field change approaches the relaxation time of the polarization in the resin substrate, a delay occurs in the electric displacement. At this time, molecular friction occurs inside the resin substrate, generating heat, which affects the dielectric properties. Therefore, a modified polyimide substrate in which the number of highly polar substituents has been reduced is used as the substrate.
[0038] A fluorine layer 5, 15, 15' may be disposed on one or both sides of the polyimide-based substrate 1, 11. The fluorine layer 5, 15, 15' may contain one or more fluorine resins selected from polytetrafluoroethylene (PTFE), perfluoroalkoxy (PFA), fluorinated ethylene propylene (FEP), chlorotrifluoroethylene (CTFE), tetrafluoroethylene / chlorotrifluoroethylene (TFE / CTFE), ethylene chlorotrifluoroethylene (ECTFE) and polyvinylidene fluoride (PVDF). For example, the fluorine layer 5, 15, 15' may be perfluoroalkoxy (PFA).
[0039] The thickness of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is arranged is 25 μm to 100 μm. For example, the thickness of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is 25 μm to 90 μm, 25 μm to 80 μm, 25 μm to 70 μm, 25 μm to 60 μm, or 25 μm to 50 μm. The thickness of the fluorine layer 5, 15, 15' is 50% or less based on the 100% thickness of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is arranged. If the thickness of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is less than 25 μm, the productivity decreases during the production of the copper foil laminate film 10, 20, and if it exceeds 100 μm, the thickness cannot be reduced.
[0040] The water contact angle of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is provided is 120° or less. For example, the water contact angle of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is provided is 107° to 120°.
[0041] The diiodomethane contact angle of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed is also 90° or less. For example, the diiodomethane contact angle of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed is also 77° to 90°.
[0042] The surface energy of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed is also 11 dyne / cm to 25 dyne / cm.
[0043] When the ranges of the water contact angle, diiodomethane contact angle and surface energy of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed are satisfied, the thickness deviation of the fluorine layer 5, 15, 15' disposed on both sides of the polyimide-based substrate 1, 11 can be kept to ±10% or less by ensuring appropriate coating properties, and curling can be suppressed. As a result, a stable copper seed layer 3, 13, 13' and copper plating layer 4, 14, 14' can be formed on the surface of the polyimide-based substrate 1, 11.
[0044] The fluorine content of the surface of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed is 60 atomic % to 75 atomic %. Within this fluorine content range, the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed may have a low dielectric constant, low dielectric loss, and low transmission loss. The polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed has a dielectric constant (D k ), and a dielectric loss (D f For example, the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is provided may have a dielectric constant (D k ), and a dielectric loss (D f ).
[0045] The coefficient of thermal expansion (CTE) of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed is 25 ppm / ° C. or less. For example, the coefficient of thermal expansion (CTE) of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed is 0.01 ppm / ° C. to 25 ppm / ° C. When the polyimide-based substrate 1, 11 having the fluorine layer 5, 15, 15' with such a coefficient of thermal expansion (CTE) is used together with the copper foil including the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' to produce the copper foil laminate film 10, 20, the difference between the coefficient of thermal expansion (CTE) (16 to 20 ppm) of the copper layer formed by the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' and the coefficient of thermal expansion (CTE) of the substrate is not large, so there is little residual stress, no warping, and no problems of twisting and warping due to shrinkage.
[0046] If necessary, before arranging the tie layer 2, 12, 12' described below, the polyimide base material 1, 11 having the fluorine layer 5, 15, 15' arranged thereon can be irradiated with an ion beam obtained by ionizing the reactive gas itself, to perform surface treatment of the polyimide base material 1, 11 having the fluorine layer 5, 15, 15' arranged thereon. As a result, functional groups such as -OH, -CHO, and -COOH are generated on the surface of the fluorine layer 5, 15, 15', and a copper foil laminate film 10, 20 having excellent adhesive strength between the polyimide base material 1, 11 and the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' described below at room temperature and high temperature can be provided.
[0047] The surface treatment using an ion beam may use a reactive gas containing at least one selected from nitrogen (N2), oxygen (O2), argon (Ar), xenon (Xe) and helium (He). For example, the reactive gas may be oxygen (O2) or a mixed gas of argon-oxygen (Ar-O2) or argon-nitrogen (Ar-N2). In this case, the adhesive strength between the polyimide-based substrate 1, 11 having the fluorine layer 5, 15, 15' and the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' described below may be significantly improved at room temperature and high temperature.
[0048] In addition, when argon (Ar) is mixed as a reaction gas, the argon (Ar) may be contained in an amount of 0.1 volume % to 50 volume %, 0.1 volume % to 30 volume %, or 0.1 volume % to 25 volume % based on the total volume of the entire reaction gas. When argon (Ar) is mixed and used within the above volume range, the adhesion between the polyimide-based substrate 1, 11 having the fluorine layer 5, 15, 15' and the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' described below can be greatly improved at room temperature and high temperature.
[0049] The amount of the reactive gas injected is, for example, 1 sccm to 100 sccm (standard cubic centimeter per minute), 50 sccm to 100 sccm, or 60 sccm to 80 sccm. Within this range, the ion beam can be irradiated stably onto the surfaces of the polyimide-based substrates 1, 11 on which the fluorine layers 5, 15, 15' are disposed.
[0050] The dose of the ion beam is not limited, but is, for example, 1×10 ions / cm 2 or 1×10 17 ions / cm 2 Within this range, the effect of ion beam irradiation on the surface of the polyimide layer can be maximized.
[0051] Furthermore, the irradiation time of the ion beam is not limited, and can be appropriately adjusted depending on the purpose.
[0052] The ion beam may be applied via a roll-to-roll process. For example, the roll-to-roll process may be performed by applying an ion beam in the MD (machine direction) for 1 to 50 seconds to the surface of the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is continuously provided at 2 to 10 mpm (meters per minute). Within this range, the copper foil laminate film 10, 20 may have excellent room temperature and high temperature adhesive strength and excellent efficiency between the polyimide-based substrate 1, 11 and the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' described below.
[0053] The power for applying the ion beam is 0.1 kW to 5 kW, 0.1 kW to 3 kW, or 0.5 kW to 2 kW. Within this range, the adhesion between the polyimide-based substrate 1, 11 having the fluorine layer 5, 15, 15' and the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' described below can be significantly improved at room temperature and high temperature.
[0054] <Thailand Layer 2,12,12'> The tie layer 2, 12, 12' is disposed on the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed. The tie layer 2, 12, 12' also contains one or more metal elements selected from the metal elements of groups 4, 6, 13, and 14 of the periodic table. The tie layer 2, 12, 12' also contains one or more metals or alloys selected from the metal elements of groups 4, 6, 13, and 14 of the periodic table.
[0055] The tie layer 2, 12, 12' is also a metal layer or metal alloy layer containing a metal having a metal-oxygen (MO) bond dissociation energy of 400 kJ / mol or more. Metal elements having the above metal-oxygen (MO) bond dissociation energy have a relatively stable bond with oxygen. As a result, a stable metal oxide or alloy oxide is secured at the interface between the tie layer 2, 12, 12' and the fluorine layer 5, 15, 15', and the adhesion is improved, and the application of the tie layer 2, 12, 12' with high electrical conductivity can minimize transmission loss.
[0056] The tie layer 2, 12, 12' may also contain one or more metals or metal alloys selected from W, Ti, Sn, Cr, Al, and Mo. The above-mentioned metals or metal alloys have relatively stable bonds with oxygen and may have low transmission loss compared to a metal tie layer made of Ni alone, which has ferromagnetic properties, and therefore the electrical conductivity of the surface of the tie layer 2, 12, 12' may be improved.
[0057] The tie layer 2, 12, 12' further contains Ni, and the Ni content is 50 wt% or less. The tie layer 2, 12, 12' forms an alloy with Ni and a metal selected from the above-mentioned W, Ti, Sn, Cr, Al, and Mo, and the Ni content in the alloy is 50 wt% or less. If the Ni content exceeds 50 wt%, high transmission loss occurs, and the room temperature adhesive strength and high temperature adhesive strength between the polyimide-based substrate 1, 11 on which the fluorine layer 5, 15, 15' is disposed and the copper seed layer 3, 13, 13' and the copper plating layer 4, 14, 14' are reduced.
[0058] The thickness of the tie layer 2, 12, 12' is 10 nm to 100 nm. For example, the thickness of the tie layer 2, 12, 12' is 12 nm to 50 nm, or 12 nm to 40 nm. If the thickness of the tie layer 2, 12, 12' is less than 10 nm, the thickness is too thin to form a sufficient metal oxide or alloy oxide at the interface with the substrate, so that it may be difficult to ensure adhesion at room temperature and high temperature. If the thickness of the tie layer 2, 12, 12' is more than 100 nm, the tie layer 2, 12, 12' is not well etched in the etching process for forming a circuit, and remains, which induces circuit defects and reduces the room temperature adhesion.
[0059] <Copper seed layers 3, 13, 13' and copper plating layers 4, 14, 14'> Copper seed layers 3, 13, 13' are disposed on the tie layers 2, 12, 12'. The copper seed layers 3, 13, 13' are also sputtered layers. The copper sputtered seed layers can have low transmission loss while maintaining the surface roughness of the polyimide-based substrates 1, 11 themselves on which the fluorine layers 5, 15, 15' are disposed. As the sputtering method, methods such as physical vapor deposition (PVD), chemical vapor deposition (CVD), low pressure chemical vapor deposition (LPCVD), and vacuum deposition can be used, but are not limited thereto, and all sputtering methods that can be used as the sputtering method can be used. For example, the physical vapor deposition (PVD) method can be used as the sputtering method.
[0060] The thickness of the copper seed layer 3, 13, 13' may be 800 Å to 4,000 Å. For example, the thickness of the copper seed layer 3, 13, 13' may be 850 Å to 3,500 Å, 900 Å to 3,000 Å, 950 Å to 2,500 Å, 1,000 Å to 2,000 Å, or 1,000 Å to 1,500 Å. If the copper seed layer 3, 13, 13' has a thickness in the above-mentioned range, electrical conductivity can be ensured during film formation, and low surface roughness (R z) while having low transmission loss.
[0061] The copper plating layers 4, 14, 14' are located on the copper seed layers 3, 13, 13'. The copper plating layers 4, 14, 14' may be formed by electroless plating or electrolytic plating. For example, the copper plating layers 4, 14, 14' may be formed by electrolytic plating.
[0062] The copper electroplating layer may be formed by any method available in the art. For example, a copper electroplating layer may be formed on one side of the copper seed layer 3, 13, 13' by electroplating with an electroplating solution based on copper sulfate and sulfuric acid. In addition, additives such as brighteners, levelers, correctors, or relaxers may be added to the electroplating solution for productivity and surface uniformity.
[0063] The thickness of the copper plating layer 4, 14, 14' may be 12 μm or less. For example, the thickness of the copper plating layer 4, 14, 14' may be 0.1 μm to 12.0 μm, 1.0 μm to 12.0 μm, 2.0 μm to 12.0 μm, 4.0 μm to 12.0 μm, or 6.0 μm to 12.0 μm.
[0064] <Copper foil laminate film 10, 20> The copper foil laminated film 10, 20 according to one embodiment includes a polyimide-based substrate 1, 11 having a fluorine layer 5, 15, 15' as a fluorine-containing substrate, and a tie layer 2, 12, 12' which is a metal layer or metal alloy layer containing a metal having a metal-oxygen (MO) bond dissociation energy of 400 kJ / mol or more on the polyimide-based substrate 1, 11 having the fluorine layer 5, 15, 15', and the thickness of the tie layer 2, 12, 12' is 10 nm to 100 nm. The copper foil laminated film 10, 20 may have improved dielectric properties at high frequencies, as well as coatability of the substrate surface and excellent room temperature and high temperature adhesion between the substrate and copper foil.
[0065] According to one embodiment, the copper foil laminate film 10, 20 has a peel strength of 0.65 kgf / cm or more of the copper seed layer and the copper plating layer from the polyimide-based substrate having the fluorine layer, measured after being left at room temperature (25°C) for three days.
[0066] According to an embodiment, the copper foil laminate film 10, 20 has a peel strength of 0.35 kgf / cm or more of the copper seed layer and the copper plating layer from the polyimide substrate having the fluorine layer, measured after two or more heat treatments at a temperature of 150° C. or more and leaving it for one day. For example, the copper foil laminate film 10, 20 has a peel strength of 0.35 kgf / cm or more of the copper seed layer and the copper plating layer from the polyimide substrate having the fluorine layer, measured after a first heat treatment at 150° C. for two hours, leaving it at room temperature for 30 minutes, a second heat treatment at 150° C. for two hours, and a third heat treatment at 240° C. for 10 minutes and leaving it at room temperature (25° C.) for one day.
[0067] <Electronic elements> An electronic device according to another embodiment also includes copper foil laminate films 10,20.
[0068] The electronic element may include an antenna element or an antenna cable. For example, the antenna element may be an antenna element for a mobile phone or a display. The electrical element may also include a circuit board such as a network server, an IOT (Internet of Things) home appliance for 5G, a radar, or a USB.
[0069] The configuration and effects of the present invention will be described in more detail below through examples and comparative examples. However, it is self-evident that the examples are provided to more specifically explain the present invention, and the scope of the present invention is not limited to these examples. EXAMPLES
[0070] Example 1: Copper foil laminated film A copper foil laminated film 20 as shown in FIG. 2 was produced as follows. As a substrate, a polyimide film 11 (made of PI Advanced Materials) with fluorine coating layers 15, 15' of about 12.5 μm thickness on both sides (total thickness: 50 μm, dielectric constant (D k ):2.8, Dielectric loss (D f (CTE: ≦25 ppm / ° C.) was prepared. The first surface 21 of the polyimide film 11 on which the fluorine coating layer 15 was formed was subjected to ion beam treatment using an ion beam source in a roll-to-roll type sputtering device. The ion beam treatment was performed for 10 -6 The inert gas Ar was injected at 30 sccm under Torr pressure conditions, and the applied power was 1.0 kV. Then, on the upper surface of the ion beam-treated fluorine coating layer 15, a tie layer 12 was formed to a thickness of about 20 nm by physical vapor deposition (PVD) using molybdenum (Mo) with a purity of 99.995% (Mo-O bond dissociation energy: 400 kJ / mol). Then, on the upper surface of the tie layer 12, a copper seed layer 13 was formed to a thickness of about 100 nm by physical vapor deposition (PVD) using copper with a purity of 99.995%. Then, the second surface 22 of the polyimide film 11 on which the fluorine coating layer 15' was disposed was subjected to ion beam treatment in the same manner as described above, to form a tie layer 12' and a copper seed layer 13'. Then, on each of the copper seed layers 13 and 13', a copper plating layer was formed to a thickness of about 12 μm by electrolytic copper plating. The electrolytic copper plating solution used for electrolytic copper plating is Cu 2+ The solution used was 28 g / L of ZnO and 195 g / L of sulfuric acid, and contained 0.01 g / L of 3-N,N-dimethylaminodithiocarbamoyl-1-propanesulfonic acid and a correction agent (manufactured by Atotech) as a brightener. The electrolytic copper plating was performed at 34°C and a current density of 1.0 A / dm 2 Start at 2.86A / dm and gradually increase 2 A current was applied in steps up to 1000 V.
[0071] Example 2: Copper foil laminated film A copper foil laminate film was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed to a thickness of about 12 nm on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) with a purity of 99.995%.
[0072] Example 3: Copper foil laminated film A copper foil laminate film was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed to a thickness of about 25 nm on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) with a purity of 99.995%.
[0073] Example 4: Copper foil laminated film A copper foil laminate film was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed to a thickness of about 40 nm on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) with a purity of 99.995%.
[0074] Example 5: Copper foil laminated film A copper foil laminated film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using a weight ratio of molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) and nickel (Ni) (Ni-O bond dissociation energy: 360 kJ / mol) of 70:30 (purity: 99.9% or more) to a thickness of about 20 nm.
[0075] Example 6: Copper foil laminated film A copper foil laminated film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using a weight ratio of tungsten (W) (WO bond dissociation energy: 710 kJ / mol) and titanium (Ti) (Ti-O bond dissociation energy: 670 kJ / mol) of 90:10 (purity: 99.9% or more) to a thickness of about 20 nm.
[0076] Example 7: Copper foil laminated film A copper foil laminated film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using a weight ratio of molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) and titanium (Ti) (Ti-O bond dissociation energy: 670 kJ / mol) of 50:50 (purity: 99.9% or more) to a thickness of about 20 nm.
[0077] Example 8: Copper foil laminated film When the ion beam treatment is performed on the first surface 21 of the polyimide film 11 on which the fluorine coating layer 15 is disposed, using a roll-to-roll type sputtering device, the ion beam treatment is performed in a 10 -6 A copper foil laminated film 20 was produced in the same manner as in Example 5, except that the reaction gases Ar and O2 were injected at a flow rate (sccm) ratio of 30:9 under Torr pressure conditions and the applied power was 1.0 kV.
[0078] Example 9: Copper foil laminated film When the ion beam treatment is performed on the first surface 21 of the polyimide film 11 on which the fluorine coating layer 15 is disposed, using a roll-to-roll type sputtering device, the ion beam treatment is performed in a 10 -6 A copper foil laminated film 20 was produced in the same manner as in Example 5, except that the reaction gases Ar and N2 were injected at a flow rate (sccm) ratio of 30:9 under Torr pressure conditions and the applied power was 1.0 kV.
[0079] Example 10: Copper foil laminated film When the ion beam treatment is performed on the first surface 21 of the polyimide film 11 on which the fluorine coating layer 15 is disposed, using a roll-to-roll type sputtering device, the ion beam treatment is performed in a 10 -6 A copper foil laminated film 20 was manufactured in the same manner as in Example 3, except that the reaction gas O2 was injected at 9 sccm under Torr pressure conditions and the applied power was 1.0 kV.
[0080] Example 11: Copper foil laminated film When the ion beam treatment is performed on the first surface 21 of the polyimide film 11 on which the fluorine coating layer 15 is disposed, using a roll-to-roll type sputtering device, the ion beam treatment is performed in a 10 -6 A copper foil laminated film 20 was manufactured in the same manner as in Example 3, except that the reaction gas N2 was injected at 9 sccm under Torr pressure conditions and the applied power was 1.0 kV.
[0081] Comparative Example 1: Copper foil laminated film A copper foil laminate film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed to a thickness of about 20 nm on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using nickel (Ni) with a purity of 99.995% (Ni-O bond dissociation energy: 360 kJ / mol).
[0082] Comparative Example 2: Copper foil laminated film A copper foil laminated film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using nickel (Ni) (Ni-O bond dissociation energy: 360 kJ / mol) and chromium (Cr) (Cr-O bond dissociation energy: 480 kJ / mol) in a weight ratio of 80:20 (purity: 99.9% or more) to a thickness of about 20 nm.
[0083] Comparative Example 3: Copper foil laminated film A copper foil laminated film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using nickel (Ni) (Ni-O bond dissociation energy: 360 kJ / mol) and copper (Cu) (Cu-O bond dissociation energy: 280 kJ / mol) in a weight ratio of 65:35 (purity: 99.9% or more) to a thickness of about 20 nm.
[0084] Comparative Example 4: Copper foil laminated film A copper foil laminated film 20 was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using a weight ratio of molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) and nickel (Ni) (Ni-O bond dissociation energy: 360 kJ / mol) of 30:70 (purity: 99.9% or more) to a thickness of about 20 nm.
[0085] Comparative Example 5: Copper foil laminated film A copper foil laminate film was manufactured in the same manner as in Example 1, except that a tie layer 12 was formed to a thickness of about 8 nm on the upper surface of the ion beam treated fluorine coating layer 15 by physical vapor deposition (PVD) using molybdenum (Mo) (Mo-O bond dissociation energy: 400 kJ / mol) with a purity of 99.995%.
[0086] Comparative Example 6: Copper foil laminated film A copper foil laminated film was manufactured in the same manner as in Example 3, except that ion beam treatment was not performed on the first surface 21 and the second surface 22 of the polyimide film 11 having the fluorine coating layer 15 disposed thereon.
[0087] Evaluation example 1: Physical property evaluation The physical properties of the copper foil laminated films produced in Examples 1 to 11 and Comparative Examples 1 to 6 were evaluated using the following measurement methods, and the results are shown in Table 1 below.
[0088] (1) Water contact angle (deg), diiodomethane contact angle (deg), and surface energy (dyne / cm) of the substrate surface Deionized water and diiodomethane were dropped 10 times each on the polyimide film substrate surface having the fluorine coating layer of the copper foil laminate film manufactured in Example 5, Example 8 to Example 11, and Comparative Example 6 under an atmosphere of 25°C and 50 RH%, and the average values of the water contact angle and the diiodomethane contact angle were obtained using a contact angle meter (Drop Master 300 (manufactured by Kyowa Interface Science Co., Ltd.)). The surface energy was then obtained by substituting the values of the contact angles according to the Owens-Wendt-Rabel-Kaelble (OWRK) method.
[0089] (2) Fluorine content on the substrate surface: XPS analysis X-ray photoelectron spectroscopy (XPS) analysis was performed on the polyimide film having a fluorine coating layer that was surface-treated by an ion beam, and the polyimide film surface having a fluorine coating layer that was not surface-treated by an ion beam, of the copper foil laminated films manufactured in Examples 5, 10, and 11 and Comparative Example 6. The XPS analysis was performed using K-Alpha (manufactured by ThermoFisher).
[0090] (3) Room temperature adhesive strength (kgf / cm) The copper foil laminated films manufactured in Examples 1 to 7 and Comparative Examples 1 to 5 were cut to a predetermined size to prepare samples. A circuit pattern with a width of 3 mm was formed on the surface of the sample, and the surface opposite to the surface on which the circuit pattern was formed was etched. The sample was then left at room temperature (25°C) for 3 days, and then peeled at a pulling speed of 50 mm / min and an angle of 180° using a peel strength tester (AG-50NIS (Shimadzu Corporation)) to measure the peel strength of the copper seed layer and the copper plating layer relative to the polyimide film having the fluorine coating layer.
[0091] (4) High temperature adhesive strength (kgf / cm) The copper foil laminated films manufactured according to Examples 1 to 7 and Comparative Examples 1 to 5 were cut to a predetermined size to prepare samples. A circuit pattern with a width of 3 mm was formed on the surface of the sample, and the surface opposite to the surface on which the circuit pattern was formed was etched. The sample was then subjected to a first heat treatment at 150°C for 2 hours, and then left at room temperature for 30 minutes. The sample was then subjected to a second heat treatment at 150°C for 2 hours, and then a third heat treatment at 240°C for 10 minutes. Finally, the sample was left at room temperature (25°C) for 1 day, and then peeled at a pulling speed of 50 mm / min and an angle of 180° using a peel strength tester (AG-50NIS (Shimadzu Corporation)) to measure the peel strength of the copper seed layer and the copper plating layer with respect to the polyimide film with the fluorine coating layer.
[0092] [Table 1]
[0093] As shown in Table 1, the water contact angle and diiodomethane contact angle of the substrate surface of the copper foil laminate films prepared in Examples 5, 8 to 11 were 107.3° to 110.8° and 77.7° to 84.5°, respectively, which were lower than those of the substrate surface of the copper foil laminate film prepared in Comparative Example 6. The surface energy of the substrate surface of the copper foil laminate films prepared in Examples 5, 8 to 11 was 14.4 dyne / cm to 18.8 dyne / cm, which was higher than those of the substrate surface of the copper foil laminate film prepared in Comparative Example 6. The fluorine content of the substrate surface of the copper foil laminate films prepared in Examples 1 to 7 was 64.92 atomic % to 73.82 atomic %.
[0094] As a result, it was confirmed that the copper foil laminate films manufactured in Examples 5, 8 to 11 had suitable coatability on the substrate surface, and stable tie layers, copper seed layers and copper plating layers were formed on the substrate.
[0095] The room temperature adhesive strength of the copper foil laminate films produced in Examples 1 to 7 was 0.68 kgf / cm or more, which was higher than that of the copper foil laminate films produced in Comparative Examples 1 to 5. The high temperature adhesive strength of the copper foil laminate films produced in Examples 1, 5 to 7 was 0.35 kgf / cm or more, which was higher than that of the copper foil laminate film produced in Comparative Example 5.
[0096] The copper foil laminated films manufactured according to Examples 1 to 7 include a tie layer composed of a metal layer or a metal alloy layer containing a metal having a metal-oxygen (MO) bond dissociation energy of 400 kJ / mol or more, and the thickness of the tie layer is 10 nm to 50 nm. As a result, it can be confirmed that the room temperature adhesive strength is improved by reacting the tie layer with a functional group on the surface of the polyimide substrate film having a fluorine coating layer. In addition, it can be confirmed that the copper foil laminated films manufactured according to Examples 1, 5 to 7 also have improved high temperature adhesive strength for the same reason. As a result, it can be seen that the copper foil laminated films manufactured according to Examples 1 to 7 can be applied to the inside and / or outside of electronic devices such as miniaturized 5G mobile communication devices. [Explanation of symbols]
[0097] 1,11 Polyimide (film) substrate 2,12,12' Thai layer 3,13,13' Copper seed layer 4,14,14' Copper plating layer 5,15,15' Fluorine (coating) layer 10,20 Copper foil laminated film 21 Page 1 22 Side 2
Claims
1. A fluorine-containing substrate; a tie layer disposed on the fluorine-containing substrate; a copper layer disposed on the tie layer; the tie layer is a metal layer or a metal alloy layer containing a metal having a metal-oxygen (M-O) bond dissociation energy of 400 kJ / mol or more; the tie layer is one or more metals or metal alloys selected from the group consisting of W, Ti, Sn, Al, and Mo; The copper foil laminate film, wherein the thickness of the tie layer is 10 nm to 100 nm.
2. The copper foil laminate film according to claim 1 , wherein the fluorine-containing substrate has a water contact angle of 120° or less.
3. 2. The copper foil laminate film according to claim 1, wherein the contact angle of diiodomethane with the fluorine-containing substrate is 90° or less.
4. 2. The copper foil laminate film according to claim 1, wherein the surface energy of the fluorine-containing substrate is 11 dyne / cm to 25 dyne / cm.
5. 2. The copper foil laminate film according to claim 1, wherein the fluorine content of the surface of the fluorine-containing substrate is 60 atomic % to 75 atomic %.
6. 2. The copper foil laminate film according to claim 1, wherein the peel strength of the copper seed layer and the copper plating layer from the fluorine-containing substrate measured after standing at room temperature (25° C.) for 3 days is 0.65 kgf / cm or more.
7. 2. The copper foil laminate film according to claim 1, wherein the peel strength of the copper seed layer and the copper plating layer from the fluorine-containing substrate measured after two or more heat treatments at a temperature of 150° C. or higher and leaving the film for one day is 0.35 kgf / cm or more.
8. The copper foil laminate film according to claim 1 , wherein the copper layer comprises a copper seed layer and a copper plating layer, and the copper plating layer has a thickness of 12 μm or less.
9. An electronic device comprising the copper foil laminate film according to any one of claims 1 to 8.
10. 10. The electronic device of claim 9, comprising an antenna element or an antenna cable.
Citation Information
Patent Citations
Conductive laminated film
JP1994143491A
Adhesive-free flexible laminate and method for producing adhesive-free flexible laminate
JP2000508265A
Fluorocarbon resin film and laminate, and production method for thermally-pressed laminate