Surface treatment method for aluminum or magnesium material
By incorporating a humidification step before steam treatment, the method accelerates the formation of a thick, homogeneous anticorrosive film on aluminum and magnesium materials, addressing the inefficiencies of conventional steam treatment methods and enhancing corrosion resistance and productivity.
Patent Information
- Application Number
- JP2020016740
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-04
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-02-04
AI Technical Summary
Conventional steam treatment methods for aluminum and magnesium materials are time-consuming, limiting productivity, and require long times to form thick anticorrosive films, which are essential for improved corrosion resistance.
A surface treatment method involving a humidification step followed by steam treatment, where moisture is applied to the base material before steam exposure, significantly enhancing the growth rate of the anticorrosive film, allowing for efficient formation in a shorter time.
The method enables the formation of a thick, homogeneous anticorrosive film in a shorter time, improving corrosion resistance and productivity while maintaining environmental compatibility.
Smart Images

Figure 0007587802000004 
Figure 0007587802000005 
Figure 0007587802000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface treatment method for a substrate made of an aluminum material or a magnesium material, and more particularly to a method for forming an anticorrosive coating by bringing water vapor into contact with the surface of a substrate made of an aluminum material or a magnesium material, which is capable of forming an anticorrosive coating having excellent corrosion resistance in a shorter time than conventional methods. [Background technology]
[0002] Since aluminum and magnesium materials are lightweight, they are widely used in automobiles, aircraft, and other general industrial fields to reduce the weight of various parts, and the range of their application is expanding. In particular, in the fields of automobiles and aerospace equipment, various members made of aluminum and magnesium materials are widely used as substitutes for steel materials in order to improve fuel efficiency through weight reduction.
[0003] Corrosion resistance is one of the concerns when aluminum and magnesium materials are used for the above-mentioned purposes. When aluminum is left in the air, a natural oxide film is generated and the aluminum is passivated. However, since the thickness of this natural oxide film is about several nanometers, it is easily corroded in an extremely humid, acidic or alkaline environment. On the other hand, magnesium is a very active metal, and the surface is easily corroded by oxidation in the usage environment. Therefore, surface treatment methods for improving the corrosion resistance of these alloy materials have been studied. Currently, chemical conversion treatments such as anodizing, plating, zinc phosphate treatment, and chromate treatment are known depending on the usage environment (for example, Patent Document 1). In these various chemical conversion treatments, a corrosion-resistant film is formed on the alloy surface by contacting or immersing the alloy material to be treated in a treatment solution containing an acid or alkali such as H2SO4 or heavy metal ions such as Cr.
[0004] The above-mentioned surface treatment techniques such as chemical conversion treatment have problems of increased costs for procuring unique treatment liquids and treating waste liquids, and problems of environmental burden. Therefore, surface treatment techniques using water vapor have been attracting attention as a surface treatment method with a smaller environmental burden than the above-mentioned chemical conversion treatment. The present inventors have also disclosed a water vapor treatment in which water vapor in a predetermined temperature range is brought into contact with the surface of an alloy in order to improve the corrosion resistance of aluminum and magnesium materials (for example, Patent Document 2 and Patent Document 3). This water vapor treatment is a surface treatment technique in which a film mainly composed of hydroxides of each metal is formed on the surface of a substrate made of an aluminum or magnesium material, and the corrosion resistance is improved by the anticorrosive effect of the film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-112521 [Patent Document 2] International Publication No. 2017 / 135363 [Patent Document 3] JP 2014-125639 A Summary of the Invention [Problem to be solved by the invention]
[0006] Steam treatment of aluminum and magnesium materials is safer and more environmentally friendly than conventional chemical conversion treatments in terms of waste liquid treatment, and can relatively easily impart corrosion resistance to alloy materials by forming an anticorrosive film. In addition, in steam treatment, a film is formed by the direct reaction of steam with the substrate surface, so a uniform film with good adhesion can be formed. Furthermore, a film that can be formed with high conformity to the substrate shape can be formed, making it effective as a surface treatment for substrates with complex shapes.
[0007] However, in consideration of the above-mentioned trend toward expanding the range of application of aluminum and magnesium materials, there are also areas in which steam treatment should be improved. One of the areas in which steam treatment can be improved is shortening the treatment time. The corrosion resistance of a material on which a corrosion-resistant film is formed is greatly affected by the thickness of the film. In order to ensure corrosion resistance even with steam treatment, it is necessary to form a thick corrosion-resistant film. In this regard, steam treatment is a treatment method that requires a relatively long time to form a corrosion-resistant film, and products that use this treatment have inferior productivity. Therefore, there is a need for improvements in steam treatment to efficiently form a thick corrosion-resistant film in a short time.
[0008] The present invention has been made under the above-mentioned background, and an object of the present invention is to provide a surface treatment method capable of efficiently forming an anticorrosive coating on a substrate made of an aluminum or magnesium material in a short period of time. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems and have found that by subjecting a substrate to a humidified state by supplying water in advance, followed by a water vapor treatment, the growth rate of a corrosion-resistant coating is significantly increased, and a corrosion-resistant coating can be efficiently formed in a short period of time.
[0010] That is, the present invention provides a surface treatment method for forming an anticorrosive coating on at least a part of the surface of a substrate made of an aluminum material or a magnesium material, the surface treatment method comprising a humidification step of supplying moisture to at least a part of the surface of the substrate, and a water vapor treatment step of contacting the substrate after the humidification step with water vapor to form an anticorrosive coating on at least a part of the surface of the substrate. Details of the treatment steps of the surface treatment method according to the present invention will be described below.
[0011] I. Base material The subject of the surface treatment method according to the present invention is a substrate made of an aluminum material or a magnesium material. In the present invention, the shape of the substrate is not particularly limited, and any shape such as a plate shape or a tube shape can be applied. There is also no limitation on the dimensions of the substrate. The meanings of aluminum material and magnesium material are as follows.
[0012] I-1.Aluminum materials The aluminum material is aluminum or an aluminum alloy containing aluminum as a main component. The additive elements that are alloyed with aluminum in the aluminum alloy include at least one of zinc (Zn), magnesium (Mg), silicon (Si), copper (Cu), manganese (Mn), lithium (Li), iron (Fe), nickel (Ni), silver (Ag), zirconium (Zr), and chromium (Cr). The aluminum alloy substrate of the present invention is preferably an aluminum alloy containing 0.1% by mass or more and less than 50% by mass of these additive elements in total.
[0013] Specific examples of aluminum alloys include various aluminum alloys specified by the International Aluminum Alloy Name. For example, various precipitation hardening aluminum alloys such as 2000 series Al-Cu alloys, 4000 series Al-Si alloys, 5000 series Al-Mg alloys, 6000 series Al-Mg-Si alloys, 7000 series Al-Zn-Mg alloys or Al-Zn-Mg-Cu alloys are suitable. However, the present invention is not limited to these standardized alloys, and alloys of a wide range of compositions can be used.
[0014] I-2. Magnesium materials The magnesium material constituting the substrate is magnesium or a magnesium alloy containing magnesium as the main component. The additive elements that are alloyed with magnesium in the magnesium alloy include aluminum (Al), zinc (Zn), calcium (Ca), manganese (Mn), zirconium (Zr), and rare earth elements (scandium (Sc), yttrium (Y), lanthanoids), etc. Many of the magnesium alloys in practical use contain aluminum as an additive element.
[0015] The content of the additive elements in the magnesium alloy is preferably 1% by mass or more and 15% by mass or less for aluminum. As for the other additive elements, the content of zinc is preferably more than 0% by mass and 5% by mass or less. The content of calcium is preferably more than 0% by mass and 5% by mass or less, and the content of manganese is preferably more than 0% by mass and 5% by mass or less. Furthermore, the content of zirconium is preferably more than 0% by mass and 5% by mass or less, and the content of rare earth elements is preferably more than 0% by mass and 5% by mass or less.
[0016] As specific examples of the magnesium alloys described above, alloys specified by ASTM standards can be applied. For example, AZ alloys (AZ31, AZ61, AZ91) containing aluminum and zinc as additive elements, AZX alloys (AZX311, AZX611, AZX612, AZX615, AZX6112, AZX711, AZX811, AZX911, AZX1001) containing aluminum, zinc, and calcium as additive elements, and AMX alloys (AMX301, AMX601, AMX701, AMX801, AMX901, AMX1001) containing aluminum, manganese, and calcium as additive elements can be suitably applied to the present invention.
[0017] When the substrate made of the above-described aluminum or magnesium material is subjected to the surface treatment method according to the present invention, it may be pretreated by washing and drying as appropriate. For aluminum or magnesium alloys having age hardening properties based on their composition, solution heat treatment and, if necessary, ageing heat treatment may be performed before the surface treatment.
[0018] II. Supplying moisture to the substrate (humidification process) The surface treatment method according to the present invention includes a new pretreatment step in comparison with the conventional surface treatment method using steam treatment of a substrate made of an aluminum material or a magnesium material. Specifically, a humidification step of supplying moisture to the substrate surface is added before the steam treatment. From the study of the present inventors, by contacting the substrate in a moisture-supplied state with steam, the growth rate of the anticorrosive film is significantly improved, and a homogeneous anticorrosive film can be formed in a short time. The reason why the growth of the anticorrosive film on the substrate to which moisture has been applied is thus accelerated is not clear. However, the present inventors consider that the reason is due to the water film on the substrate surface formed by the supply of moisture. In the present invention, the dissolution of metal ions derived from the substrate into the water film is promoted, and the reaction between the metal ions and hydroxide ions derived from the steam occurs quickly, accelerating the film growth.
[0019] There is no particular limitation on the method of supplying moisture to the surface of the substrate. Examples of the moisture supplying method include a process of immersing the substrate in a treatment liquid containing water. Such a moistening process by immersion is completed by immersing the entire or part of the substrate in the treatment liquid and then lifting the substrate. The immersion time is not particularly determined. The necessary area of the substrate may be immersed in the treatment liquid and immediately lifted, or it may be immersed for 1 second to about 3 minutes and then lifted.
[0020] The humidification step can also be carried out by spraying or dripping a treatment liquid containing water onto the substrate. In these cases, the amount of water sprayed or dripped onto the substrate is not particularly limited. For example, 2 It is sufficient to apply about 50 μL to 5 mL of processing solution per spot.
[0021] In these humidifying steps, moisture may be supplied to the entire surface of the substrate, or may be supplied partially, or to one or both surfaces.
[0022] The processing liquid, which is the moisture supplied in the humidification step, essentially contains water. The processing liquid may be substantially composed of water, in which case industrial water or tap water can be used, but it is preferable to use pure water. When using pure water, it is preferable to use ion-exchanged water, distilled water, or ultrapure water with an electric conductivity of 1 mS / m or less.
[0023] The treatment liquid in the humidification step can be the same as the aqueous solution containing water or an appropriate salt, which is the source of water vapor to be brought into contact with the substrate in the subsequent water vapor treatment step. The aqueous solution in this case will be described in detail later, but an aqueous solution containing at least one of carbonates, nitrates, sulfates, and fluorides can be used. In particular, when a method of immersing the substrate in a treatment liquid is adopted as the humidification step, the substrate is immersed in the treatment liquid, and then the treatment liquid is heated to produce water vapor, thereby enabling water vapor treatment. The technique of using a common treatment liquid and water vapor source in the humidification step can simplify the structure of the surface treatment device compared to the case where they are prepared separately.
[0024] However, even if the same water or aqueous solution as the water vapor source can be used, the treatment liquid supplied to the substrate in the humidification step must not be in a vapor state. If the treatment liquid is in a vapor state, the formation of a coating will start, and the object of the present invention cannot be achieved. In other words, the treatment liquid supplied to the substrate in the humidification step is preferably at a temperature of 5°C or higher and 95°C or lower.
[0025] III. Steam treatment process As described above, by carrying out the steam treatment in which the substrate that has undergone the moisture supplying step is brought into contact with steam, a corrosion-resistant film is formed on at least a part of the substrate surface. The temperature of the steam brought into contact with the substrate in the steam treatment step for forming the corrosion-resistant film is preferably 100°C or higher and 350°C or lower. If the temperature of the steam exceeds 350°C, the corrosion-resistant film may become porous or crack. If the temperature of the steam is lower than 100°C, the rate at which the corrosion-resistant film is formed decreases, and the corrosion-resistant film is not formed sufficiently. The temperature of the steam is more preferably 130°C to 250°C. In addition, the treatment time of the steam treatment is preferably 0.1 hours or higher. If it is less than 0.1 hours, it is difficult to form a corrosion-resistant film of sufficient thickness even if the humidification treatment of the present invention is performed. There is no particular need to limit the upper limit, but in consideration of the purpose of shortening the time for forming the corrosion-resistant film and improving productivity, it is preferably 5 hours or lower, and more preferably 2 hours or lower.
[0026] The water vapor to be brought into contact with the substrate is generated by heating and vaporizing water. As the water used as the water vapor source, industrial water or tap water can be used, and pure water is preferably used. In addition, an aqueous solution containing an appropriate salt can also be used. When using pure water, it is preferable to use ion-exchanged water, distilled water, or ultrapure water with an electric conductivity of 1 mS / m or less. In addition, as the aqueous solution containing salt, the vapor of an aqueous solution of carbonate, nitrate, sulfate, or fluoride salt can be used. As these salts, salts of alkali metals (lithium, sodium, potassium, etc.) (sodium carbonate, sodium nitrate, etc.), salts of alkaline earth metals (calcium, strontium, barium, etc.) (calcium carbonate, calcium nitrate, etc.), salts of precious metals, salts of common metals, etc. can be used. An aqueous solution of one or a combination of these salts can be used.
[0027] The pressure of the steam is preferably in the range of 0.1 to 10 MPa. More preferably, the pressure is 0.2 to 5 MPa. When pressurized steam is applied, a two-phase equilibrium state of saturated steam and subcritical water is reached, which makes it possible to promote the reactivity for the formation of a corrosion-resistant film. By maintaining a constant pressure of the steam during treatment, a uniform corrosion-resistant film can be formed.
[0028] The method of contacting the substrate with water vapor is not particularly limited. The water vapor treatment may be performed by exposing the substrate to water vapor in a closed space such as a reactor or container. As a specific method, the substrate may be placed in a container together with water, and exposed to a water vapor atmosphere generated by controlling the temperature and pressure. Alternatively, the substrate may be treated by directly spraying water vapor onto the substrate.
[0029] The above steam treatment can not only form an anticorrosive film but also increase the hardness (strength) of the substrate depending on the type of aluminum or magnesium material used. This increase in hardness is due to age hardening caused by the heat of the steam when the substrate is a precipitation hardening alloy, which will be described later.
[0030] The humidification process and the steam treatment process described above need to be performed at least once, and may be performed repeatedly. By performing the processes repeatedly, a corrosion-resistant coating consisting of multiple coating layers can be formed. Furthermore, each process may be performed under different conditions. By performing the processes repeatedly and under different conditions, multiple corrosion-resistant coatings with different compositions can be formed.
[0031] IV. Formation of anticorrosive coating by steam treatment The above-mentioned water vapor treatment forms an anticorrosive coating on at least a part of the surface of the substrate made of an aluminum or magnesium material. The composition of the anticorrosive coating varies depending on the material constituting the substrate.
[0032] (a) Anticorrosive coating on aluminum materials When the substrate is an aluminum material, the anticorrosive coating formed by steam treatment essentially contains aluminum oxide hydroxide. Aluminum oxide hydroxide is also called boehmite and is an aluminum compound expressed as γ-AlO(OH) or simply AlO(OH). Aluminum oxide hydroxide has chemical stability and has a high anticorrosive effect. The composition of the anticorrosive coating essentially contains aluminum oxide hydroxide, and may be composed of only aluminum oxide hydroxide. However, the coating may contain substances other than aluminum oxide hydroxide. For example, it may contain trace amounts of additive elements of the aluminum alloy substrate or compounds thereof (intermetallic compounds, oxides, hydroxides, etc.). In addition, compounds (oxides, hydroxides, hydrates, salts) derived from components in the steam that comes into contact with the substrate to form the coating may also be included.
[0033] Furthermore, the prior art states that, in addition to aluminum hydroxide oxide, an Al-based layered double hydroxide (hereinafter sometimes referred to as LDH) is optionally included as a component of the corrosion protection film of an aluminum material by steam treatment. LDH is a compound in which a hydroxide of a divalent metal (M) derived from an additive element of an aluminum alloy is combined with a double hydroxide in which an ion of a trivalent metal, Al, is substituted for the divalent metal site, forming a layered structure, and is represented by the following chemical formula:
[0034] [ka] (In the formula, M1 is a divalent metal element, and is one of cobalt (Co), zinc (Zn), magnesium (Mg), copper (Cu), manganese (Mn), iron (Fe), nickel (Ni), chromium (Cr), cadmium (Cd), and calcium (Ca). The cation M1 2+ is a divalent metal ion. A is an anion. n- is a hydroxide ion (OH - ), carbonate ion (CO3 2- ), nitrate ion (NO3 - ), sulfate ion (SO4 2- ), fluorine ion (F -), chloride ion (Cl - ) or at least one of the following.
[0035] In the structural formula shown in Chemical Formula 1, [M1 2+ 1-x Al 3+ x (OH)2] is called the double hydroxide basic layer, and [A n- x / n The Al-based layered double hydroxide has a layered structure in which a negatively charged intermediate layer is sandwiched between the positively charged double hydroxide basic layers, and this structure is maintained in the corrosion protection film.
[0036] In the corrosion protection coating for aluminum materials according to the present invention, the LDH is included as an optional component and is not an essential component. The effect of improving corrosion resistance by steam treatment does not require the presence of LDH in the coating, and it is considered that the effect is achieved by the formation of aluminum oxide hydroxide alone.
[0037] (b) Anticorrosive coating on magnesium material When a corrosion-resistant film is formed on a substrate made of magnesium material by steam treatment, the corrosion-resistant film essentially contains magnesium hydroxide (Mg(OH)2). Magnesium hydroxide is also chemically stable and is useful as a corrosion-resistant film. The corrosion-resistant film may be composed of magnesium hydroxide alone. The corrosion-resistant film is mainly composed of magnesium hydroxide, but also allows various additive elements other than magnesium contained in the magnesium alloy substrate as inevitable impurities, such as magnesium oxide (MgO), magnesium carbonate (MgCO3), and magnesium oxide hydroxide (Mg5O(OH)8). In addition, the corrosion-resistant film may also contain compounds (oxides, hydroxides, hydrates, salts) derived from components in the steam that comes into contact with the substrate to form the corrosion-resistant film.
[0038] Furthermore, the anticorrosive coating for magnesium materials essentially contains magnesium hydroxide (Mg(OH)2) and may optionally contain Mg-Al-based layered double hydroxide (Mg-Al-based layered double hydroxide). Mg-Al-based layered double hydroxide is a hydroxide represented by the following chemical formula 2.
[0039] [ka] (Wherein, A is an anion n- is a hydroxide ion (OH - ), carbonate ion (CO3 2- ), nitrate ion (NO3 - ), sulfate ion (SO4 2- ), fluorine ion (F - ), chloride ion (Cl - ) or at least one of the following.
[0040] The Mg-Al layered double hydroxide is a metal ion (magnesium ion (Mg 2+ ) and aluminum ion (Al 3+ ) and anions supplied from the water vapor that comes into contact with the substrate during film formation (A n- )
[0041] In the corrosion protection coating for magnesium material according to the present invention, the above-mentioned Mg-Al-based layered double hydroxide is included as an optional component and is not an essential component. The effect of improving corrosion resistance by steam treatment can be achieved by the formation of magnesium oxide hydroxide alone.
[0042] The structure of the corrosion protection coating on the aluminum and magnesium materials described above can be examined based on the profile obtained by, for example, X-ray diffraction analysis (XRD). The amount of each component can also be estimated based on the peak intensity of each component.
[0043] The thickness of the anticorrosive coating formed by the surface treatment method according to the present invention is preferably 10 μm to 100 μm. A coating less than 10 μm has poor anticorrosive effect on the substrate, while a coating thicker than 100 μm may crack or peel due to stress or thermal shock, resulting in poor corrosion resistance. A coating thickness of 5 μm, which is the lower limit, requires a long time in conventional surface treatment methods, but can be achieved in a short time in the present invention. Effect of the Invention
[0044] INDUSTRIAL APPLICABILITY As described above, the present invention is capable of forming a thicker and more uniform anticorrosive coating on a substrate made of an aluminum or magnesium material in a shorter time than conventional methods, and is useful as a surface treatment method that improves corrosion resistance and has excellent productivity. [Brief description of the drawings]
[0045] [Figure 1] FIG. 1 is a diagram for explaining the configuration of a steam curing apparatus. [Diagram 2] 2 is a SEM photograph showing the surface morphology of the anticorrosive coating formed on the surface of a substrate made of the aluminum alloy of Example 1. [Diagram 3] 1 shows XRD profiles of the surfaces of aluminum alloy substrates on which anticorrosive coatings of Example 1 and Comparative Example 1 are formed. [Figure 4] 4 shows polarization curves of aluminum alloy substrates on which the anticorrosive coatings of Example 1 and Comparative Example 1 are formed. [Diagram 5] 4 is a SEM photograph showing the surface morphology of anticorrosive coatings formed on magnesium alloy substrates in Examples 3 and 4 and Comparative Examples 2 and 4. [Figure 6] SEM photographs showing cross sections of magnesium alloy substrates on which anticorrosive coatings of Example 4 and Comparative Example 4 were formed. [Figure 7] 4 shows XRD profiles of the surfaces of magnesium alloy substrates on which anticorrosive coatings of Examples 3 and 4 and Comparative Examples 3 and 4 are formed. [Figure 8] 4 shows polarization curves of magnesium alloy substrates on which anticorrosive coatings of Example 2 and Comparative Example 2 are formed. [Figure 9]4 shows polarization curves of magnesium alloy substrates on which anticorrosive coatings of Example 4 and Comparative Example 4 are formed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0046] First embodiment Hereinafter, an embodiment of the present invention will be described with examples and comparative examples. In this embodiment, a substrate made of an aluminum material (aluminum alloy), a 7000 series aluminum alloy, Al-5.6 mass % Zn-2.6 mass % Mg-Cu alloy (7075 alloy), was subjected to a surface treatment to form an anticorrosive coating.
[0047] Example 1 An aluminum alloy plate (70 × 30 mm, 3.0 mm thick) was prepared as a substrate (sample), washed and dried. Then, pure water was applied to the surface of the substrate as a treatment liquid, with a thickness of 1 cm. 2 500 μL was sprayed per sample.
[0048] Next, a steam treatment was performed by contacting the moisture-supplied substrate with steam, and a corrosion-resistant film was formed on the substrate surface. For the steam treatment, a steam curing device shown in FIG. 1 was used. The steam curing device in FIG. 1 is a horizontal autoclave, and pure water (20 ml) serving as a steam source is poured into the lower part. The upper part of the device is designed to allow multiple samples (substrates) to be hung. For the steam treatment, the substrate was quickly set in the steam curing device after moisture was supplied, and the treatment was started. The steam treatment was performed at a temperature of 200° C., for a treatment time of 6 hours, and with a pressure of 1.0 MPa, while maintaining the temperature and pressure (Example 1).
[0049] Comparative Example 1 As a comparative example, the substrate after drying was subjected to a water vapor treatment without supplying water. The conditions for the water vapor treatment were the same as those in Example 1.
[0050] Various evaluations were carried out on the substrates of this embodiment and the comparative example produced by the above steps.
[0051] [Observation of the surface morphology of anticorrosive coating by SEM] The surface morphology of the anticorrosive coating was observed by a scanning electron microscope (SEM). Figure 2 is an SEM photograph (x30,000) showing the surface morphology of the anticorrosive coating formed after the steam treatment of the aluminum alloy substrates of Example 1 and Comparative Example 1. It can be seen from Figure 1 that the anticorrosive coating formed by the steam treatment after the supply of moisture in Example 1 uniformly and densely covers the substrate surface, even though the treatment time is the same as that of the anticorrosive coating of Comparative Example 1 where no moisture is supplied.
[0052] [Analysis by X-ray diffraction (XRD)] Next, the surfaces of the substrates on which the anticorrosive coatings of Example 1 and Comparative Example 1 were formed were analyzed by X-ray diffraction (XRD). X-ray diffraction (XRD) can identify the structure of the anticorrosive coating based on the obtained profile (X-ray diffraction pattern). XRD was measured using a Cu-Kα X-ray source at a voltage of 40 kV and a current of 30 mA.
[0053] Fig. 3 shows XRD profiles of the surfaces of the substrates on which the anticorrosive coatings of this embodiment and the comparative example are formed. Fig. 3 confirms that an anticorrosive coating containing aluminum oxide hydroxide (AlO(OH)) and an Al-based layered double hydroxide is formed on the surface of each substrate. However, the anticorrosive coating of Example 1 has stronger peak intensities of aluminum oxide hydroxide and Al-based layered double hydroxide compared to the anticorrosive coating of Comparative Example 1. In other words, it was confirmed that a thicker anticorrosive coating was formed in Example 1, in which moisture was supplied before the steam treatment, than in Comparative Example 1, even though the steam treatment time was the same.
[0054] [Polarization measurement] Next, the polarization curves were measured to evaluate the corrosion resistance of the substrates on which the anticorrosive coatings of Example 1 and Comparative Example 1 were formed. For the polarization measurement, a 5 wt% NaCl aqueous solution was used as the electrolyte, and after bubbling the solution with nitrogen before the measurement, the polarization curves were measured using a potentio / galvanostat (VersaSTAT4, manufactured by Princeton Applied Research).
[0055] FIG. 4 shows the polarization curves of the substrates on which the anticorrosive coatings of the present embodiment and the comparative example are formed. FIG. 4 also shows the polarization curves of an aluminum alloy (7075 alloy) substrate without the anticorrosive coating for comparison. From FIG. 4, it can be seen that Example 1, in which the anticorrosive coating was formed by steam treatment, exhibits a significant decrease in corrosion current density compared to the substrate without the anticorrosive coating, and the effect of improving corrosion resistance due to the anticorrosive coating is confirmed. Furthermore, when Example 1 and Comparative Example 1 are compared, it can be seen that Example 1 exhibits a decrease in corrosion current density and a noble corrosion potential. From this result, it can be seen that Example 1, in which moisture was supplied before steam treatment, exhibits improved corrosion resistance compared to Comparative Example 1, in which moisture was not supplied. It is believed that this improvement in corrosion resistance is due to the formation of a thick coating due to the moisture supply.
[0056] Second embodiment In this embodiment, a substrate made of AZ31 alloy (Mg-3%Al-1%Zn) was used as the magnesium material (alloy), and a surface treatment was performed to form an anticorrosive coating on the substrate surface.
[0057] A magnesium alloy plate (70 × 30 mm, thickness 3.0 mm) was prepared as a substrate (sample), washed and dried. Then, pure water was applied to the surface of the substrate to a thickness of 1 cm as a treatment liquid. 2 100 μL was dropped per sample.
[0058] Next, the substrate to which moisture had been supplied was brought into contact with water vapor to perform water vapor treatment, thereby forming an anticorrosive film on the substrate surface. As in the first embodiment, the water vapor treatment was performed using the steam curing device shown in Fig. 1. The water vapor treatment was performed at a temperature of 140°C for a treatment time of 1 hour (Example 2), 3 hours (Example 3), and 5 hours (Example 4), while maintaining the temperature and pressure at 1 MPa.
[0059] Comparative Examples 2 to 4 As a comparative example, the dried substrate was subjected to steam treatment without supplying moisture. The conditions of the steam treatment were a steam temperature of 140°C and a treatment time of 1 hour (Comparative Example 2), 3 hours (Comparative Example 3), and 5 hours (Comparative Example 4).
[0060] Various evaluations were carried out on the substrates of this embodiment and the comparative example produced by the above steps.
[0061] [Observation of the surface morphology of anticorrosive coating by SEM] Fig. 5 is an SEM photograph (x5000) showing the surface morphology of the anticorrosive coating formed on the surface of the magnesium alloy substrate after each water vapor treatment time. As can be seen from Fig. 5, the anticorrosive coating of the comparative example has many microcracks on its surface, and is therefore considered to have insufficient corrosion resistance. In contrast, the anticorrosive coating of the present embodiment covers the substrate surface homogeneously and densely, as compared to the comparative example with the same treatment time, and it can be confirmed that the coating is formed stably.
[0062] Next, the substrate on which the anticorrosive coating was formed was cut perpendicular to the anticorrosive coating, and the cross section was polished and then observed by SEM to measure the film thickness. Fig. 6 is an SEM photograph (x5000) showing the cross section of the substrate on which the anticorrosive coating of Example 4 and Comparative Example 4 (steam treatment time: 5 hours) was formed. From Fig. 6, it can be seen that the anticorrosive coating of Example 4 (film thickness 12.5 µm) is thicker than that of Comparative Example 4 (film thickness 8 µm) at the same treatment time. From this observation result, it was confirmed that the humidification process by supplying moisture accelerates the film formation speed during steam treatment.
[0063] [Analysis by X-ray diffraction (XRD)] Next, the surfaces of the substrates on which the anticorrosive coatings of this embodiment and the comparative example were formed were analyzed by X-ray diffraction (XRD). Fig. 7 shows XRD profiles of the substrates on which the anticorrosive coatings of Example 3 (treatment time 3 hours), Example 4 (treatment time 5 hours), Comparative Example 3 (treatment time 3 hours), and Comparative Example 4 (treatment time 5 hours) were formed. From Fig. 7, it was confirmed that an anticorrosive coating containing magnesium hydroxide and Mg-Al-based layered double hydroxide was formed on the surface of each substrate. In Examples 3 and 4, the peak intensity of the Mg-Al-based layered double hydroxide was strong.
[0064] [Polarization measurement] Next, the polarization curves of the substrates on which the anticorrosive coatings according to the present embodiment and the comparative example were formed were measured to evaluate their corrosion resistance. FIG. 8 shows the polarization curves of the substrates on which the anticorrosive coatings of Example 2 (treatment time 1 hour) and Comparative Example 2 (treatment time 1 hour) were formed. FIG. 9 shows the polarization curves of the substrates on which the anticorrosive coatings of Example 4 (treatment time 5 hours) and Comparative Example 4 (treatment time 5 hours) were formed. FIG. 8 also shows the polarization curve of a magnesium alloy (AZ31 alloy) substrate without steam treatment for comparison. From FIG. 8, the substrates on which the anticorrosive coatings were formed by the steam treatment showed a significant decrease in corrosion current density compared to the substrates that were not subjected to the steam treatment, confirming the effect of improving the corrosion resistance by the anticorrosive coating.
[0065] Moreover, comparing Example 2 with Comparative Example 2, it is found that in Example 2, the corrosion current density decreases and the corrosion potential becomes nobler. Example 2 and Comparative Example 2 are samples formed by steam treatment for one hour, and the difference between the two is clear even in the short time of one hour. The usefulness of supplying moisture before steam treatment can be confirmed.
[0066] 9, it can be seen that the five-hour water vapor treatment reduced the corrosion current density in both Example 4 and Comparative Example 4, and the corrosion resistance improved due to the growth of the coating. Moreover, Example 4, in which moisture was supplied before the water vapor treatment, showed a further reduction in corrosion current density and a noble corrosion potential compared to Comparative Example 4, in which only the water vapor treatment was performed, confirming that a coating with higher corrosion resistance was formed.
[0067] Third embodiment In this embodiment, an aluminum alloy substrate is used, and moisture is supplied in the humidifying step by immersing the substrate in the treatment liquid, and then a water vapor treatment is performed to form an anticorrosive coating.
[0068] In this embodiment, a rotating mechanism equipped with a motor was added to the hanging part of the sample in the steam curing apparatus of FIG. 1 so that the sample could be raised and lowered. Then, as in the first embodiment, an aluminum alloy (7075 alloy) substrate was washed, dried, and set in the apparatus. After that, the substrate was lowered to immerse the entire substrate in the treatment liquid (pure water) at the bottom of the apparatus, and then immediately raised to pull up the substrate and perform steam treatment. The conditions of the steam treatment were the same as in the first embodiment, with a temperature of 200°C, a treatment time of 6 hours, and a pressure of 1.0 MPa.
[0069] After the steam treatment according to this embodiment, the substrate on which the film was formed was taken out and its appearance was observed. The substrate surface had the same appearance as the aluminum alloy substrate of the first embodiment. When the substrate was subjected to XRD analysis, clear diffraction peaks of aluminum oxide hydroxide (AlO(OH)) and Al-based layered double hydroxide appeared, as in the first embodiment. This confirmed that immersion of the substrate in the treatment liquid was also an effective way of supplying moisture. [Industrial Applicability]
[0070] As described above, the present invention is capable of forming a thick and uniform anticorrosive coating on a substrate made of an aluminum alloy or magnesium alloy in a shorter time than before, and is useful as a surface treatment method that improves corrosion resistance and has excellent productivity. In addition, the present invention is expected to be applied as a surface treatment method for various aluminum and magnesium material members, the range of which is expanding.
Claims
1. A surface treatment method for forming an anticorrosive coating on at least a portion of a surface of a substrate made of a magnesium material, comprising: a humidifying step of supplying a treatment liquid made of pure water to at least a part of a surface of the substrate to humidify the substrate; and a water steam treatment step of contacting the substrate after the humidification step with water steam to form a corrosion protection film on at least a part of the surface of the substrate. The surface treatment method is characterized in that the anticorrosive coating formed by the water vapor treatment contains magnesium hydroxide (Mg(OH) 2 ) and, optionally, an Mg—Al-based layered double hydroxide represented by the following chemical formula 2. 【Chemistry 2】 (In the formula, the anion A n− is at least one of a hydroxide ion (OH − ), a carbonate ion (CO 3 2− ), a nitrate ion (NO 3 − ), a sulfate ion (SO 4 2− ), a fluorine ion (F − ), and a chloride ion (Cl − ).)
2. 2. The surface treatment method according to claim 1, wherein the humidifying step is a step of immersing the substrate in a treatment liquid comprising pure water.
3. 2. The surface treatment method according to claim 1, wherein the humidifying step is a step of spraying or dropping a treatment liquid consisting of pure water onto the substrate.
4. 4. The surface treatment method according to claim 1, wherein the water vapor treatment step is a treatment in which water vapor having a temperature of 100° C. to 350° C. is brought into contact with the base material.
Citation Information
Patent Citations
Pretreatment method for anode aluminum foil formation
CN107974701A
Aluminum part tightening bolt
JP1997112521A
Magnesium alloy material, and method of treating surface of magnesium alloy
JP2013023768A
High-corrosion-resistance magnesium-based material and production method thereof, and surface treatment method for magnesium-based material
JP2014125639A
Aluminum resin bonded body and method for producing same