Sensor element of NOx sensor and method for manufacturing the sensor element of NOx sensor
A two-layer measurement electrode structure in NOx sensors with specific volume and thickness ratios addresses the issue of oxide evaporation and excess oxygen, maintaining high sensitivity over time.
Patent Information
- Application Number
- JP2022002294
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-22
- Filing Date
- 2022-01-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-01-11
AI Technical Summary
The formation of oxides such as PtO, PtO2, and RhO2 at the measurement electrode in NOx sensors reduces catalytic reactivity, leading to a decrease in NOx sensitivity due to evaporation of these oxides and the presence of excess oxygen that cannot be absorbed into the solid electrolyte.
A limiting current type NOx sensor with a two-layer measurement electrode structure, where the lower layer consists of a noble metal and solid electrolyte without pores and the upper layer contains a mixture of noble metal, solid electrolyte, and pores, along with specific volume and thickness ratios, to minimize the exposure of the noble metal to excess oxygen.
The two-layer structure effectively suppresses the deterioration of the measurement electrode, maintaining high NOx sensitivity even after continuous use by reducing the evaporation of oxides and minimizing the impact of excess oxygen.
Smart Images

Figure 0007588103000003 
Figure 0007588103000004 
Figure 0007588103000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a sensor element of a limiting current type NOx sensor, and in particular to the configuration of a measurement electrode of the sensor element. [Background technology]
[0002] Conventionally, NOx sensors in which a sensor element is formed using an oxygen ion conductive solid electrolyte ceramic such as zirconia (ZrO2) as a substrate have been known as devices for measuring the concentration of NOx in measured gases such as combustion gases and exhaust gases in internal combustion engines such as automobile engines (see, for example, Patent Documents 1 and 2).
[0003] The sensor element of the NOx sensor (NOx sensor element) is equipped with various electrodes (pump electrode, measurement electrode, reference electrode, etc.). These electrodes are porous cermet electrodes made of a composite material of catalytic precious metal and electrolyte zirconia, and have a porous structure including many pores. The catalytic precious metals used are Pt and Pt with small amounts of other substances (e.g. Rh and other precious metals, etc.). The NOx sensor element is used in a state heated to a relatively high sensor element operating temperature (600°C to 900°C) in order to utilize the catalytic reaction of the catalytic precious metal used in the electrodes and the oxygen ion conductivity of the zirconia used in the substrate during its operation.
[0004] Measurement gases such as engine exhaust gases usually contain O2. Therefore, in the NOx sensors disclosed in Patent Documents 1 and 2, O2 in the measurement gas introduced into the NOx sensor element is removed (separated from NOx) by an electrochemical pump cell provided in the NOx sensor element, and NOx is decomposed into O2 and N2 by a catalytic reaction in the measurement electrode, and the NOx concentration in the measurement gas is measured based on the magnitude of the oxygen ion current flowing through the measurement pump cell at that time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 2885336 [Patent Document 2] International Publication No. 2019 / 188613 Summary of the Invention [Problem to be solved by the invention]
[0006] When the measurement electrode is exposed to O2, the Pt or Pt / Rh of the electrode reacts with O2 to produce oxides such as PtO, PtO2, and RhO2. When the precious metal of the electrode is reduced due to the production of such oxides, the catalytic reactivity of the measurement electrode decreases. In addition, these oxides have a lower vapor pressure than Pt, so they tend to evaporate at lower temperatures than Pt. Such evaporation reduces the three-phase interface of catalyst / electrolyte / pores and the two-phase interface of catalyst / electrolyte in the measurement electrode, which also reduces the catalytic reactivity of the measurement electrode.
[0007] As mentioned above, the measured gas that reaches the measuring electrode has had oxygen removed in advance, but a small amount of oxygen still remains in the measured gas. Also, O2 produced by the decomposition of NOx may not be ionized quickly and may remain near the measuring electrode.
[0008] Therefore, when the NOx sensor is used continuously, the sensitivity to NOx gradually decreases due to a decrease in the catalytic reactivity at the measurement electrode.
[0009] To explain the mass transfer in the vicinity of the measurement electrode during measurement in more detail, first, O2 and NOx in the measurement gas that reaches the measurement electrode move through the pores of the measurement electrode (this is called the mass transfer process). When these O2 and NOx come into contact with the catalyst metal in the pores, Pt, the main component of the catalyst metal, decomposes NO into N2 and O2, and furthermore, removes electrons from O2 to generate oxygen ions. The generated oxygen ions are taken up from Pt into zirconia, the solid electrolyte, at the catalyst / electrolyte two-phase interface, and move through the zirconia due to the potential difference generated between the measurement electrode and the external electrode when a voltage is applied from an external power source (this is called the charge transfer process).
[0010] However, if there are oxygen ions that cannot be absorbed from the catalytic metal into the zirconia during this process, as well as oxygen before ionization (collectively referred to as excess oxygen), the catalytic metal, which is mainly Pt, will be oxidized by the excess oxygen inside and on the surface of the electrode, producing PtO, PtO2, etc. These oxides will then gradually evaporate.
[0011] The inventors of the present invention believed that by reducing the excess oxygen that cannot be absorbed by zirconia, it would be possible to suppress the evaporation of oxides from the measurement electrode and thereby prevent a decrease in the sensitivity of the NOx sensor, and after extensive research, they came up with the present invention.
[0012] In addition, Patent Document 2 focuses on the fact that impurities present in the electrode further lower the evaporation temperature of the oxide during oxidation of Pt in the measurement electrode, and discloses an embodiment in which the evaporation of the oxide is suppressed by providing a gettering layer that getter the impurities. However, Patent Document 2 does not disclose or suggest anything about suppressing the evaporation of the oxide by reducing excess oxygen.
[0013] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a NOx sensor in which the decrease in sensitivity caused by oxidation of the measurement electrode is suppressed even when the sensor is used continuously. [Means for solving the problem]
[0014] In order to solve the above problems, a first aspect of the present invention is a sensor element of a limiting current type NOx sensor, comprising a base portion made of an oxygen ion conductive solid electrolyte; The oxygen concentration was adjusted in advance. The gas to be measured is introduced For measurement An internal cavity; For measurement It is arranged facing the internal void. measurement An electrode and the For measurement a pump electrode disposed outside the internal cavity; measurement and a portion existing between the electrode and the outer pump electrode. A pump current proportional to the concentration of NOx contained in the measurement gas flows. R measurement A pump cell, measurement The electrode is characterized in that it comprises an upper layer consisting of a precious metal, the solid electrolyte, and pores, and a lower layer consisting of the precious metal and the solid electrolyte, and the volume ratio of the solid electrolyte in the lower layer is greater than the volume ratio of the solid electrolyte in the upper layer.
[0016] In addition, the present invention 2 The embodiment is 1 of A sensor element of a NOx sensor according to the present invention is characterized in that the volume ratio of the solid electrolyte in the upper layer is 20% to 40%, and the volume ratio of the solid electrolyte in the lower layer is 50% to 60%.
[0017] In addition, the present invention 3 The first aspect is or No. 2 attitude Like The sensor element of the NOx sensor is characterized in that the thickness ratio of the upper layer to the lower layer is in the range of 95:5 to 10:90.
[0018] In addition, the present invention 4 The embodiment is 3 The sensor element of the NOx sensor according to the above aspect is characterized in that a thickness ratio of the upper layer to the lower layer is in a range of 90:10 to 30:70.
[0019] In addition, the present invention5 The embodiment is a sensor element of a limiting current type NOx sensor, comprising a base portion made of an oxygen ion conductive solid electrolyte; The oxygen concentration was adjusted in advance. The gas to be measured is introduced For measurement an internal cavity; For measurement In the portion defining the internal space, For measurement It is arranged facing the internal void. measurement An electrode and the For measurement a pump electrode disposed outside the internal cavity; measurement and a portion existing between the electrode and the outer pump electrode. A pump current proportional to the concentration of NOx contained in the measurement gas flows. R measurement A pump cell, measurement The electrode is composed of a precious metal, the solid electrolyte, and pores. measurement The boundary with the electrode and the measurement The boundary between the region where the pores are present and the region where the pores are not present in the electrode is different, a boundary between the base portion and the measurement electrode is a lowermost end of a region in the measurement electrode where the precious metal is present, and a boundary between a region in the measurement electrode where the pores are present and a region in which the pores are not present is a lowermost end of a region in which the pores are present, The volume ratio of the solid electrolyte is larger in the region where the pores are not present than in the region where the pores are present. a ratio of the distance from the upper end of the measuring electrode to the lowermost end of the region in which the pores exist to the distance from the lowermost end of the region in which the precious metal exists to the lowermost end of the region in which the pores exist is in the range of 95:5 to 10:90. It is characterized by:
[0022] In addition, the present invention 6 The embodiment is 5 The sensor element of the NOx sensor according to the embodiment is characterized in that the ratio of the distance from the upper end of the measurement electrode to the lowermost end of the region in which the pores exist and the distance from the lowermost end of the region in which the precious metal exists to the lowermost end of the region in which the pores exist is in the range of 90:10 to 30:70.
[0023] In addition, the present invention 7 The embodiment is 5 or No. 6 attitude Like The sensor element of the NOx sensor is characterized in that the volume ratio of the solid electrolyte in the region where the pores are present is 20% to 40%, and the volume ratio of the solid electrolyte in the region where the pores are not present is 50% to 60%.
[0024] In addition, the present invention8 The embodiment of the present invention is a method for manufacturing a sensor element of a limiting current type NOx sensor, the sensor element comprising: a base portion made of an oxygen ion conductive solid electrolyte; at least one internal space into which a gas to be measured is introduced; an internal electrode disposed in a portion of the base portion that defines the at least one internal space so as to face the at least one internal space; an external-space pump electrode disposed in a location other than the at least one internal space; and at least one pump cell comprising a portion of the base portion that is present between the internal electrode and the external-space pump electrode. ,before The method includes a preparation step of preparing a plurality of green sheets containing an oxygen ion conductive solid electrolyte as a ceramic component, which is a constituent material of the sensor element; a pattern formation step of forming a predetermined pattern on each of the plurality of green sheets; a lamination step of laminating the plurality of green sheets on which the predetermined pattern is formed to obtain a laminate; a cutting step of cutting the laminate to obtain element bodies each corresponding to the sensor element; and a firing step of firing the element bodies to obtain the sensor element, wherein the pattern formation step includes an internal electrode film formation step of forming the internal electrode paste film at a predetermined formation position of an internal electrode formation green sheet, which is one of the plurality of green sheets, and the internal electrode film formation step includes At least one of a first application step of applying a solid electrolyte paste comprising the solid electrolyte and an organic component to the formation position where the solid electrolyte paste has been applied; , Takashi A metal, the solid electrolyte, and a pore-forming material The three components Organic ingredients and Mixed A second coating step of coating the three-component mixed paste in an overlapping manner, and pressing the coating film formed at the formation position by the second coating step. and causing a part of the noble metal particles and the pore-forming material particles to penetrate into the coating film of the solid electrolyte paste formed in the first coating step. and a pressing step for pressing the metal plate.
[0025] In addition, the present invention 9The embodiment of the present invention is a method for manufacturing a sensor element of a limiting current type NOx sensor, the sensor element comprising: a base portion made of an oxygen ion conductive solid electrolyte; at least one internal space into which a gas to be measured is introduced; an internal electrode disposed in a portion of the base portion that defines the at least one internal space so as to face the at least one internal space; an external-space pump electrode disposed in a location other than the at least one internal space; and at least one pump cell comprising a portion of the base portion that is present between the internal electrode and the external-space pump electrode. ,before The method includes a preparation step of preparing a plurality of green sheets containing an oxygen ion conductive solid electrolyte as a ceramic component, which is a constituent material of the sensor element; a pattern formation step of forming a predetermined pattern on each of the plurality of green sheets; a lamination step of laminating the plurality of green sheets on which the predetermined pattern is formed to obtain a laminate; a cutting step of cutting the laminate to obtain element bodies each corresponding to the sensor element; and a firing step of firing the element bodies to obtain the sensor element, wherein the pattern formation step includes an internal electrode film formation step of forming an internal electrode paste film at a predetermined formation position of an internal electrode formation green sheet, which is one of the plurality of green sheets, and the internal electrode film formation step includes forming a paste film at the formation position. At least one of the following is true: A metal and the solid electrolyte The two components Organic ingredients and Mixed A first application step of applying a two-component mixed paste, and a second application step of applying the noble metal, the solid electrolyte, and the pore-forming material to the formation position where the two-component mixed paste is applied. The three components Organic ingredients and Mixed A second coating step of coating the three-component mixed paste in an overlapping manner, and pressing the coating film formed at the formation position by the second coating step. and causing a part of the particles of the precious metal and the particles of the pore-forming material to penetrate into the coating film of the two-component mixed paste formed in the first coating step. and a pressing step for pressing the metal plate. Effect of the Invention
[0026] The first to third aspects of the present invention 9 According to the above, even if used continuously, Measurement electrode or A NOx sensor in which peeling of the internal electrode is suitably suppressed is realized.
[0027] Also, The present invention 1 or 9 According to this aspect, deterioration of the measurement electrode caused by the presence of excess oxygen that cannot be taken in the measurement electrode is preferably suppressed, thereby realizing a NOx sensor in which deterioration of measurement sensitivity is preferably suppressed even with continuous use. [Brief description of the drawings]
[0028] [Figure 1] 1 is a diagram illustrating an example of the configuration of a gas sensor 100. FIG. [Diagram 2] 1 is a model diagram showing a partial cross section of a measuring electrode 44 along the element thickness direction. [Diagram 3] 13 is a model diagram of a partial cross section of a measurement electrode 44Z having a three-phase mixed configuration throughout the electrode. FIG. [Figure 4] 3 is a diagram showing a process flow for manufacturing the sensor element 101. FIG. [Diagram 5] 11A to 11C are diagrams showing a procedure for forming a pattern that will ultimately become a measurement electrode 44. [Figure 6] 13 is a graph showing the results of a continuous drive test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] <Outline of gas sensor configuration> Fig. 1 is a diagram illustrating an example of the configuration of a gas sensor 100 according to this embodiment. The gas sensor 100 is a limiting current type NOx sensor that detects NOx and measures its concentration using a sensor element 101. The gas sensor 100 further includes a controller 110 that controls the operation of each component and determines the NOx concentration based on the NOx current flowing through the sensor element 101. Fig. 1 includes a vertical cross-sectional view of the sensor element 101 along the longitudinal direction.
[0030] The sensor element 101 is a flat (long plate-like) element having a structure in which six solid electrolyte layers, namely, a first substrate layer 1, a second substrate layer 2, a third substrate layer 3, a first solid electrolyte layer 4, a spacer layer 5, and a second solid electrolyte layer 6, each of which is made of zirconia (ZrO2) (e.g., yttria-stabilized zirconia (YSZ)) that is an oxygen ion conductive solid electrolyte, are stacked in this order from the bottom as viewed in the drawing. The solid electrolyte forming these six layers is dense and airtight. In the following, the upper surface of each of these six layers in FIG. 1 may be simply referred to as the upper surface, and the lower surface thereof may be simply referred to as the lower surface. The entire part of the sensor element 101 made of the solid electrolyte is collectively referred to as the base part.
[0031] The sensor element 101 is manufactured, for example, by laminating ceramic green sheets corresponding to each layer after carrying out predetermined processing and printing a circuit pattern thereon, and then firing the laminated sheets to integrate them.
[0032] At one tip of the sensor element 101, between the lower surface of the second solid electrolyte layer 6 and the upper surface of the first solid electrolyte layer 4, a first diffusion rate-controlling section 11 also serving as a gas inlet 10, a buffer space 12, a second diffusion rate-controlling section 13, a first internal void 20, a third diffusion rate-controlling section 30, a second internal void 40, a fourth diffusion rate-controlling section 60, and a third internal void 61 are formed adjacent to each other and communicated with each other in this order.
[0033] The buffer space 12, the first internal space 20, the second internal space 40, and the third internal space 61 are spaces (regions) inside the sensor element 101, the upper part of which is defined by the lower surface of the second solid electrolyte layer 6, the lower part by the upper surface of the first solid electrolyte layer 4, and the sides by the side surfaces of the spacer layer 5, and are provided by hollowing out the spacer layer 5. Similarly, the gas inlet 10 may be provided by hollowing out the spacer layer 5 at the tip surface (left end as viewed in the drawing) of the sensor element 101, separately from the first diffusion rate-controlling section 11. In this case, the first diffusion rate-controlling section 11 is formed adjacent to the inside of the gas inlet 10.
[0034] The first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, the third diffusion rate-controlling section 30, and the fourth diffusion rate-controlling section 60 are each provided as two horizontally elongated slits (with the opening having the longitudinal direction perpendicular to the drawing). The portion from the gas inlet 10 to the third internal space 61 is also referred to as a gas flow section.
[0035] Further, at a position farther from the tip side than the gas flow section, a reference gas introduction space 43 is provided between the upper surface of the third substrate layer 3 and the lower surface of the spacer layer 5, and at a position defined at the side by the side surface of the first solid electrolyte layer 4. Into the reference gas introduction space 43, for example, air is introduced as a reference gas when measuring the NOx concentration.
[0036] The air introducing layer 48 is a layer made of porous alumina, and a reference gas is introduced into the air introducing layer 48 through the reference gas introducing space 43. In addition, the air introducing layer 48 is formed so as to cover the reference electrode 42.
[0037] Reference electrode 42 is an electrode formed in a manner to be sandwiched between the upper surface of third substrate layer 3 and first solid electrolyte layer 4, and as described above, is surrounded by air introduction layer 48 which is connected to reference gas introduction space 43. In addition, as will be described later, it is possible to measure the oxygen concentration (oxygen partial pressure) in first internal space 20 and second internal space 40 using reference electrode 42.
[0038] In the gas flow section, the gas inlet 10 (first diffusion rate-controlling section 11) is a section that opens to the outside space, and the measurement gas is taken into the sensor element 101 from the outside space through the gas inlet 10.
[0039] The first diffusion rate-controlling portion 11 is a portion that imparts a predetermined diffusion resistance to the taken-in measurement gas.
[0040] The buffer space 12 is a space provided for guiding the measurement gas introduced from the first diffusion rate-controlling portion 11 to the second diffusion rate-controlling portion 13 .
[0041] The second diffusion rate-controlling portion 13 is a portion that imparts a predetermined diffusion resistance to the measurement gas introduced from the buffer space 12 into the first internal space 20 .
[0042] When the measurement gas is introduced from the outside of the sensor element 101 into the first internal space 20, the measurement gas is suddenly taken into the sensor element 101 from the gas inlet 10 due to pressure fluctuations of the measurement gas in the external space (exhaust pressure pulsations if the measurement gas is automobile exhaust gas), but is not introduced directly into the first internal space 20, but is introduced into the first internal space 20 after the concentration fluctuations of the measurement gas are cancelled out through the first diffusion rate-controlling section 11, buffer space 12, and second diffusion rate-controlling section 13. As a result, the concentration fluctuations of the measurement gas introduced into the first internal space 20 become almost negligible.
[0043] The first internal space 20 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the second diffusion rate-controlling part 13. The oxygen partial pressure is adjusted by the operation of the main pump cell 21.
[0044] The main pump cell 21 is an electrochemical pump cell including an inner pump electrode 22 having a ceiling electrode portion 22a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the first internal space 20, an outer (outside the space) pump electrode 23 provided in a region corresponding to the ceiling electrode portion 22a on the upper surface of the second solid electrolyte layer 6 (one of the main surfaces of the sensor element 101) so as to be exposed to the external space, and the second solid electrolyte layer 6 sandwiched between these electrodes.
[0045] The inner pump electrode 22 is formed on the upper and lower solid electrolyte layers (the second solid electrolyte layer 6 and the first solid electrolyte layer 4) that partition the first internal space 20. Specifically, a ceiling electrode portion 22a is formed on the lower surface of the second solid electrolyte layer 6 that provides the ceiling surface of the first internal space 20, and a bottom electrode portion 22b is formed on the upper surface of the first solid electrolyte layer 4 that provides the bottom surface. The ceiling electrode portion 22a and the bottom electrode portion 22b are connected by conductive portions (not shown) provided on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side wall portions of the first internal space 20.
[0046] The ceiling electrode portion 22a and the bottom electrode portion 22b are provided in a rectangular shape in a plan view, however, an embodiment in which only the ceiling electrode portion 22a or only the bottom electrode portion 22b is provided may also be adopted.
[0047] The inner pump electrode 22 and the outer pump electrode 23 are formed as porous cermet electrodes. In particular, the inner pump electrode 22, which comes into contact with the measured gas, is formed using a material with a weakened ability to reduce the NOx component in the measured gas. For example, it is formed as a cermet electrode of Au-Pt alloy containing about 0.6 wt% to 1.4 wt% Au and ZrO2 with a porosity of 5% to 40%, and a thickness of 5 μm to 20 μm. The weight ratio of the Au-Pt alloy to ZrO2 may be about Pt:ZrO2=7.0:3.0 to 5.0:5.0.
[0048] On the other hand, the outer pump electrode 23 is formed as a cermet electrode of, for example, Pt or an alloy thereof and ZrO2, and has a rectangular shape in a plan view.
[0049] In the main pump cell 21, a desired pump voltage Vp0 is applied between the inner pump electrode 22 and the outer pump electrode 23 by the variable power supply 24, and a main pump current Ip0 is caused to flow in a positive or negative direction between the inner pump electrode 22 and the outer pump electrode 23, thereby making it possible to pump oxygen from the first inner space 20 out to the external space, or to pump oxygen from the external space into the first inner space 20. The pump voltage Vp0 applied between the inner pump electrode 22 and the outer pump electrode 23 in the main pump cell 21 is also referred to as a main pump voltage Vp0.
[0050] In addition, in order to detect the oxygen concentration (oxygen partial pressure) in the atmosphere in the first internal space 20, a main sensor cell 80, which is an electrochemical sensor cell, is configured by the inner pump electrode 22, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42.
[0051] By measuring the electromotive force V0 in the main sensor cell 80, the oxygen concentration (oxygen partial pressure) in the first internal space 20 can be determined.
[0052] Furthermore, the controller 110 controls the main pump current Ip0 by feedback-controlling the main pump voltage Vp0 so that the electromotive force V0 is constant, thereby keeping the oxygen concentration in the first inner space 20 at a predetermined constant value.
[0053] The third diffusion rate-controlling section 30 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the main pump cell 21 in the first internal space 20, and guides the measurement gas to the second internal space 40.
[0054] The second internal space 40 is provided as a space for further adjusting the oxygen partial pressure in the measurement gas introduced through the third diffusion-controlling part 30. The oxygen partial pressure is adjusted by the operation of the auxiliary pump cell 50. In the second internal space 40, the oxygen concentration of the measurement gas is adjusted with even higher accuracy.
[0055] In the second internal space 40, the oxygen concentration (oxygen partial pressure) is previously adjusted in the first internal space 20, and then the oxygen partial pressure of the measurement gas introduced through the third diffusion-controlling section 30 is further adjusted by the auxiliary pump cell 50.
[0056] The auxiliary pump cell 50 is an auxiliary electrochemical pump cell that is composed of an auxiliary pump electrode 51 having a ceiling electrode portion 51a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the second internal space 40, an outer pump electrode 23 (not limited to the outer pump electrode 23, but a sensor element 101 and an appropriate outer electrode will suffice), and the second solid electrolyte layer 6.
[0057] The auxiliary pump electrode 51 is disposed in the second internal space 40 in the same manner as the inner pump electrode 22 disposed in the first internal space 20. That is, a ceiling electrode portion 51a is formed on the second solid electrolyte layer 6 that provides the ceiling surface of the second internal space 40, and a bottom electrode portion 51b is formed on the first solid electrolyte layer 4 that provides the bottom surface of the second internal space 40. The ceiling electrode portion 51a and the bottom electrode portion 51b are rectangular in plan view, and are connected by conductive portions (not shown) provided on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side wall portions of the second internal space 40.
[0058] Like the inner pump electrode 22, the auxiliary pump electrode 51 is also made of a material with a reduced ability to reduce the NOx component in the measurement gas.
[0059] In the auxiliary pump cell 50, under the control of the controller 110, by applying a desired voltage (auxiliary pump voltage) Vp1 between the auxiliary pump electrode 51 and the outer pump electrode 23, it is possible to pump oxygen in the atmosphere within the second internal space 40 out to the external space or pump oxygen from the external space into the second internal space 40.
[0060] In addition, in order to control the oxygen partial pressure in the atmosphere in the second internal space 40, an auxiliary sensor cell 81, which is an electrochemical sensor cell, is formed by the auxiliary pump electrode 51, the reference electrode 42, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, and the third substrate layer 3.
[0061] The auxiliary pump cell 50 performs pumping using a variable power supply 52 whose voltage is controlled based on an electromotive force V1 corresponding to the oxygen partial pressure in the second internal space 40 detected by the auxiliary sensor cell 81. This allows the oxygen partial pressure in the atmosphere in the second internal space 40 to be controlled to a low partial pressure that does not substantially affect the measurement of NOx.
[0062] In addition, the auxiliary pump current Ip1 is used to control the electromotive force of the main sensor cell 80. Specifically, the auxiliary pump current Ip1 is input to the main sensor cell 80 as a control signal, and the electromotive force V0 is controlled to always keep a constant gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling part 30 into the second internal space 40. When used as a NOx sensor, the oxygen concentration in the second internal space 40 is kept at a constant value of about 0.001 ppm by the action of the main pump cell 21 and the auxiliary pump cell 50.
[0063] The fourth diffusion rate-controlling section 60 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the auxiliary pump cell 50 in the second internal space 40, and guides the measurement gas to the third internal space 61.
[0064] The third internal space 61 is provided as a space (measurement internal space) for performing processing related to the measurement of the nitrogen oxide (NOx) concentration in the measurement gas introduced through the fourth diffusion-controlling part 60. The NOx concentration is measured by operating the measurement pump cell 41 in the third internal space 61. Since the measurement gas, the oxygen concentration of which has been adjusted with high precision in the second internal space 40, is introduced into the third internal space 61, the gas sensor 100 can measure the NOx concentration with high precision.
[0065] The measurement pump cell 41 measures the NOx concentration in the measurement gas in the third internal space 61. The measurement pump cell 41 is an electrochemical pump cell including a measurement electrode 44 provided on the upper surface of the first solid electrolyte layer 4 facing the third internal space 61 and spaced apart from the third diffusion-controlling part 30, an outer pump electrode 23, the second solid electrolyte layer 6, a spacer layer 5, and the first solid electrolyte layer 4.
[0066] The measurement electrode 44 is a porous cermet electrode of a precious metal and a solid electrolyte. For example, it is formed as a cermet electrode of Pt or an alloy of Pt and another precious metal such as Rh, and ZrO2, which is a constituent material of the sensor element 101. The measurement electrode 44 also functions as a NOx reduction catalyst that reduces NOx present in the atmosphere in the third internal space 61.
[0067] In the measurement pump cell 41, under the control of the controller 110, oxygen produced by the decomposition of NOx in the atmosphere surrounding the measurement electrode 44 is pumped out, and the amount of oxygen produced can be detected as a pump current Ip2.
[0068] However, in this embodiment, the measurement electrode 44 has a two-layer structure consisting of an area where no pores exist and an area where pores exist, the details of which will be described later.
[0069] In order to detect the oxygen partial pressure around the measurement electrode 44, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the measurement electrode 44, and the reference electrode 42 constitute a measurement sensor cell 82, which is an electrochemical sensor cell. The variable power supply 46 is controlled based on an electromotive force V2 corresponding to the oxygen partial pressure around the measurement electrode 44, which is detected by the measurement sensor cell 82.
[0070] The NOx in the measurement gas introduced into the third internal space 61 is reduced by the measurement electrode 44 (2NO→N2+O2) to generate oxygen. The generated oxygen is then pumped by the measurement pump cell 41, and the voltage (measurement pump voltage) Vp2 of the variable power supply 46 is controlled so that the electromotive force V2 detected by the measurement sensor cell 82 is constant. Since the amount of oxygen generated around the measurement electrode 44 is proportional to the concentration of NOx in the measurement gas, the NOx concentration in the measurement gas is calculated using the pump current Ip2 in the measurement pump cell 41. Hereinafter, this pump current Ip2 is also referred to as the NOx current Ip2.
[0071] Furthermore, by combining the measurement electrode 44, the first solid electrolyte layer 4, the third substrate layer 3 and the reference electrode 42 to form an oxygen partial pressure detection means as an electrochemical sensor cell, it is possible to detect an electromotive force corresponding to the difference between the amount of oxygen generated by reduction of the NOx components in the atmosphere around the measurement electrode 44 and the amount of oxygen contained in the reference atmosphere, thereby making it possible to determine the concentration of the NOx components in the measured gas.
[0072] In addition, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the outer pump electrode 23, and the reference electrode 42 constitute an electrochemical sensor cell 83, and the electromotive force Vref obtained by this sensor cell 83 makes it possible to detect the oxygen partial pressure in the measurement gas outside the sensor.
[0073] The sensor element 101 further includes a heater portion 70 which serves to adjust the temperature of the sensor element 101 by heating it and keeping it warm, in order to increase the oxygen ion conductivity of the solid electrolyte constituting the base portion.
[0074] The heater section 70 mainly includes a heater electrode 71, a heater element 72, a heater lead 72a, a through hole 73, a heater insulating layer 74, and a heater resistance detection lead not shown in Fig. 1. The heater section 70, except for the heater electrode 71, is embedded in the base portion of the sensor element 101.
[0075] The heater electrode 71 is an electrode formed in a manner to be in contact with the lower surface of the first substrate layer 1 (the other main surface of the sensor element 101).
[0076] The heater element 72 is a resistance heating element provided between the second substrate layer 2 and the third substrate layer 3. The heater element 72 generates heat when power is supplied from a heater power source (not shown in FIG. 1) provided outside the sensor element 101 through the heater electrode 71, the through hole 73, and the heater lead 72a, which are current paths. The heater element 72 is made of Pt or is made of Pt as a main component. The heater element 72 is embedded in a predetermined range on the side of the sensor element 101 where the gas flow section is provided, so as to face the gas flow section in the element thickness direction. The heater element 72 is provided to have a thickness of about 10 μm to 20 μm.
[0077] In the sensor element 101, a current is passed through the heater element 72 via the heater electrode 71 to cause the heater element 72 to generate heat, thereby heating and keeping each part of the sensor element 101 at a predetermined temperature. Specifically, the sensor element 101 is heated so that the temperature of the solid electrolyte and the electrodes in the vicinity of the gas flow part becomes about 700°C to 900°C. This heating enhances the oxygen ion conductivity of the solid electrolyte constituting the base part in the sensor element 101. The heating temperature by the heater element 72 when the gas sensor 100 is used (when the sensor element 101 is driven) is referred to as the sensor element driving temperature.
[0078] The degree of heat generated by the heater element 72 (heater temperature) is grasped by the magnitude of the resistance value of the heater element 72 (heater resistance).
[0079] Although not shown in Fig. 1, a thermal shock resistant protective layer, which is a single-layer or multi-layer porous layer covering the sensor element 101, may be further provided on the outer periphery of a predetermined range on one tip side (left end side in the drawing) of the sensor element 101. The thermal shock resistant protective layer is provided for the purpose of preventing cracks from occurring in the sensor element 101 due to thermal shock caused by moisture contained in the measured gas adhering to and condensing on the sensor element 101 during use of the gas sensor 100, and for the purpose of preventing poisonous substances mixed in the measured gas from penetrating into the sensor element 101. A layered gap (gap layer) may be formed between the sensor element 101 and the thermal shock resistant protective layer.
[0080] <Detailed configuration of the measurement electrodes> Next, the configuration of the measurement electrode 44 provided in the sensor element 101 having the above-mentioned configuration will be described in more detail. Fig. 2 is a model diagram showing a partial cross section of the measurement electrode 44 along the element thickness direction. Note that dashed lines La and Lb shown in Fig. 2 are added for ease of understanding.
[0081] 2, the area below the dashed line La is the first solid electrolyte layer 4 made of a solid electrolyte (zirconia), and the measurement electrode 44 is provided on the first solid electrolyte layer 4. The area above the measurement electrode 44 is the third internal space 61 (more specifically, the part of the third internal space 61 that is not occupied by the measurement electrode 44, but hereinafter, for convenience, this will be simply referred to as the third internal space 61).
[0082] As described above, the measurement electrode 44 is a porous cermet electrode of a precious metal, for example, Pt or its alloy with Rh, and a solid electrolyte (zirconia). Therefore, as shown in FIG. 2, the measurement electrode 44 has a mixed configuration of a part made of a precious metal NM, which is white in the figure, a part made of a solid electrolyte SE, which is gray (or light gray), and a part made of pores CV, which is black (or dark gray). In FIG. 2, the first solid electrolyte layer 4 is also gray in the figure, just like the solid electrolyte SE. This corresponds to both being made of zirconia. In addition, the third internal space 61 is also black in the figure, just like the pores CV, which corresponds to both being spaces or voids.
[0083] However, the measurement electrode 44 according to this embodiment does not have a configuration in which three parts (phases), i.e., the precious metal NM, the solid electrolyte SE, and the pores CV, are randomly mixed throughout the electrode, but has a two-layer configuration consisting of a lower layer (also called a two-phase region) 44L in which only the precious metal NM and the solid electrolyte SE are randomly mixed and no pores CV exists, and an upper layer (also called a three-phase region) 44U in which the precious metal NM, the solid electrolyte SE, and the pores CV are randomly mixed. In FIG. 2, the boundary between the lower layer 44L and the upper layer 44U is indicated by a dashed line Lb.
[0084] From another perspective, the dashed line La indicates the lowermost end of the range in the thickness direction of the measurement electrode 44 where the precious metal NM is present, and the dashed line Lb indicates the lowermost end of the range in the thickness direction of the measurement electrode 44 where the pores CV are present. In yet another way of expressing it, the dashed line La can be said to be the boundary in the thickness direction of the measurement electrode 44 between the region in which the precious metal NM is present and the region in which the precious metal NM is not present, and the dashed line Lb can be said to be the boundary in the thickness direction of the measurement electrode 44 between the region in which the pores CV are present and the region in which the pores CV are not present.
[0085] In the following description, the portion of the solid electrolyte SE constituting the measurement electrode 44 that is continuous with the base portion made of the solid electrolyte of the sensor element 101 (the portion that continues to the base portion beyond the dashed line La) will be referred to as the continuous region RE. Furthermore, the portion of the continuous region RE that belongs to the lower layer 44L (the portion located between the dashed line La and the dashed line Lb) will be referred to as the lower continuous region REL, and the portion of the continuous region RE that belongs to the upper layer 44U (the portion located between the dashed line Lb and the third internal void 61) will be referred to as the upper continuous region REU.
[0086] 2 further illustrates, on the left side of the model diagram, the change in the average volume ratio of each portion of the measurement electrode 44 in the thickness direction. Here, the thickness of the entire measurement electrode 44 is t0, and the thickness of the lower layer 44L is t L The thickness of the upper layer 44U is t U It states that:
[0087] Although there is some local variation, on average, the volume ratio of the precious metal NM, the solid electrolyte SE, and the pores CV in the upper layer 44U is approximately 1 / 2 the thickness t U In contrast, in the lower layer 44L, the volume ratio of the pores CV is 0, while the volume ratio of the solid electrolyte SE is approximately constant throughout the thickness range, and the value is greater than that in the upper layer 44U. Note that, although the volume ratio of the precious metal NM is constant in the measurement electrode 44 in FIG. 2, this is not a required embodiment.
[0088] That is, the measurement electrode 44 of the sensor element 101 according to the present embodiment is provided as a porous cermet electrode in which the precious metal NM, the solid electrolyte SE, and the pores CV are mixed as a whole, but these three phases are actually mixed only in a region having a predetermined thickness t on the upper surface side of the electrode. U The upper layer 44U is provided with a predetermined thickness t L This range is characterized in that there are no pores CV and therefore the volume ratio of the solid electrolyte SE is greater than that of the upper layer 44U, forming a two-phase lower layer 44L.
[0089] In other words, in the measurement electrode 44, the boundary (dashed line La) between the base portion made of a solid electrolyte (more specifically, the first solid electrolyte layer 4) and the measurement electrode 44 is different from the boundary (dashed line Lb) between the area where the pores CV exist and the area where they do not exist.
[0090] For comparison, Fig. 3 is a model diagram of a partial cross section of a measurement electrode 44Z having a configuration in which three phases are randomly mixed throughout the electrode. The position of the measurement electrode 44Z in the sensor element is the same as that of the measurement electrode 44. In the measurement electrode 44Z shown in Fig. 3, the white parts in the drawing are the precious metal NM, the gray parts in the drawing are the solid electrolyte SE, and the black parts in the drawing are the pores CV.
[0091] 3 also illustrates the change in the average volume ratio of each portion of measurement electrode 44Z in the thickness direction on the left side of the model diagram, where the thickness of measurement electrode 44Z is set to t0, which is the same as the thickness of measurement electrode 44, and the average volume ratio of each phase is set to the same as the average volume ratio in upper layer 44U of measurement electrode 44.
[0092] Although there is some local variation, on average, the volume ratio of the precious metal NM, the solid electrolyte SE, and the pores CV in the measurement electrode 44Z is approximately constant throughout the range of the thickness t0 of the measurement electrode 44Z, as shown in FIG.
[0093] In addition, in the measurement electrode 44Z, the boundary between the area where the pores CV are present and the area where they are not present coincides with the boundary between the base portion made of a solid electrolyte (more specifically, the first solid electrolyte layer 4) and the measurement electrode 44Z.
[0094] The measurement electrode 44 and the measurement electrode 44Z have in common the process of mass transfer within the electrode. That is, NOx and a small amount of O2 contained in the measurement gas that reaches the measurement electrode 44 or 44Z arranged in the third internal space 61 from the outside of the element move through the air hole CV and come into contact with the precious metal NM as a catalyst. Pt, which is the main component of the precious metal NM, decomposes NOx to generate O2, and removes electrons from O2 to generate oxygen ions. The oxygen ions thus generated are taken up from Pt into the solid electrolyte SE at the two-phase interface between the precious metal NM and the solid electrolyte SE, and move within the sensor element 101 due to the potential difference generated between the measurement electrode 44 or 44Z and the outer pump electrode 23 in the measurement pump cell 41.
[0095] However, in the case of the measurement electrode 44Z having a three-phase configuration as a whole, the pores CV are present up to the vicinity of the first solid electrolyte layer 4 or adjacent to the first solid electrolyte layer 4, and the proportion of the interface between the solid electrolyte SE and the pores CV is relatively high, while the proportion of the interface between the precious metal NM and the solid electrolyte SE is relatively low. For this reason, excess oxygen that comes into contact with the precious metal but is not taken up by the solid electrolyte is likely to be generated, and therefore the precious metal, mainly Pt, is likely to be oxidized by the excess oxygen, causing deterioration of the measurement electrode.
[0096] In contrast, in the case of the measurement electrode 44, the pores CV through which oxygen flows are present only in the upper layer 44U, while the solid electrolyte SE present in the lower layer 44L is almost entirely the lower continuous region REL that continues from the base portion and is in contact only with the precious metal NM. Therefore, the ratio of the two-phase interface between the precious metal NM and the solid electrolyte SE is higher than in conventional gas sensors, and in particular, since the only interface present in the lower layer 44L is this two-phase interface, it is less likely that excess oxygen will come into contact with the precious metal NM and remain in the pores CV, causing deterioration of the measurement electrode 44.
[0097] That is, in the gas sensor 100 according to the present embodiment, deterioration of the measurement electrode 44 caused by the presence of excess oxygen is suitably suppressed. Therefore, even if the gas sensor 100 is used continuously, deterioration of the measurement sensitivity is suitably suppressed.
[0098] Preferably, the measurement electrode 44 has a thickness of 10 μm to 30 μm and a thickness ratio t U :t L In other words, the distance t from the top of the measuring electrode 44 to the bottom end (dashed line Lb) of the area in which the pores CV are present is in the range of 95:5 to 10:90. U and the distance t from the bottom of the measuring electrode 44 to the bottom of the area in which the pores CV exist. L This also means that the ratio of the two is in the range of 95:5 to 10:90.
[0099] The volume ratio of the solid electrolyte SE in the upper layer 44U is 20% to 40%, and the volume ratio of the solid electrolyte SE in the lower layer 44L is 50% to 60%.
[0100] In these cases, the rate of change from the initial value of the NOx current Ip2 when the gas sensor 100 is continuously used is suppressed to 6% or less. In other words, the deterioration of the measurement sensitivity when the gas sensor 100 is continuously used is suppressed to 6% or less.
[0101] More preferably, the thickness ratio t U :t L is in the range of 90:10 to 30:70. In this case, the rate of change of the NOx current Ip2 from the initial value when the gas sensor 100 is continuously used, i.e., the deterioration of the measurement sensitivity when the gas sensor 100 is continuously used, is suppressed to approximately 3% or less. In addition, a decrease in the pumping ability of the measurement pumping cell 41 caused by a small number of sites for ionizing the measurement gas, which may occur when the thickness ratio of the upper layer 44U is small and therefore the measurement electrode 44 has few pores, is also suppressed.
[0102] The configuration of the measurement electrode 44 in which the solid electrolyte continuing from the first solid electrolyte layer 4 penetrates into the precious metal portion exhibits a so-called anchor effect. Therefore, the configuration of the measurement electrode 44 employed in the gas sensor 100 according to this embodiment is also effective in preventing the measurement electrode 44 from peeling off.
[0103] <Example of identifying the boundary position> Next, an exemplary method for identifying the boundary positions (dashed lines La, Lb) when evaluating the boundary position between the area where the precious metal NM is present and the area where the precious metal NM is not present, which is also the lowest end of the range in which the precious metal NM is present in the thickness direction of the measurement electrode 44 having the configuration described above, and the boundary position between the area where the pore CV is present and the area where the pore CV is not present, which is also the lowest end of the range in which the pore CV is present, will be described.
[0104] First, a cross-sectional image of the measurement electrode 44 along the thickness direction as shown in Fig. 2 is captured by, for example, an SEM (scanning electron microscope). At that time, the imaging range is set so that the measurement electrode 44 is as horizontal as possible in the captured image and so that the entire range in the thickness direction of at least the lower layer 44L of the measurement electrode 44 and the vicinity of the boundary between the measurement electrode 44 and the first solid electrolyte layer 4 are included. From the viewpoint that it is necessary to clearly identify the interfaces of the three phases in the captured image, the imaging magnification is preferably about 500 times to 1000 times. In such a case, a cross-sectional image of a range of about 100 µm to 200 µm in the longitudinal direction of the element is obtained.
[0105] Next, the captured image data obtained is analyzed based on a known image processing method to identify the respective existence ranges (all pixels corresponding to each) of the precious metal NM, the solid electrolyte SE (and the first solid electrolyte layer 4), and the pores CV (and the third internal void 61). For example, when the captured image is an SEM image, it is possible to identify which phase each pixel of the captured image corresponds to based on the difference in brightness, etc.
[0106] Next, a coordinate point (pixel position) that gives the lowest end position of the precious metal NM in the captured image is identified based on the captured image data. In the case of Fig. 2, this corresponds to point A. Then, a straight line that passes through point A and is parallel to the left-right direction of the captured image corresponds to the dashed line La that indicates the lowest end of the existence range of the precious metal NM.
[0107] However, although the measurement electrode 44 is made as horizontal as possible during imaging, the measurement electrode 44 may be tilted to some extent in the obtained image. In consideration of this, the coordinate point of the lowest position (e.g., point A in FIG. 2) and the coordinate point located next lower (e.g., point B in FIG. 2) from the range of the precious metal NM in the image may be identified, the image may be corrected so that the straight line passing through points A and B is horizontal, and the straight line passing through points A and B in the corrected image may be taken as the dashed line La indicating the lowest end of the range of the presence of the precious metal NM.
[0108] After the dashed line La is specified, a coordinate point (pixel position) that gives the lowest end position of the pore CV in the captured image (after correction) is specified based on the captured image data. In the case of FIG. 2, this corresponds to point C. Then, a straight line that passes through point C and is parallel to the left and right direction of the captured image corresponds to dashed line Lb that indicates the lowest end of the existence range of the pore CV.
[0109] The distance between the dashed lines La and Lb thus determined is the thickness t L It is identified as:
[0110] Furthermore, in FIG. 2, point D is the highest position of the measurement electrode 44 (of the upper layer 44U), and the distance between the dashed line Lb and point D is the thickness t U It is identified as:
[0111] <Sensor element manufacturing process> Next, a process for manufacturing the sensor element 101 having the above-mentioned configuration and characteristics will be described. In this embodiment, a laminate made of green sheets (also called base tape) containing zirconia as a ceramic component is formed, and the laminate is cut and fired to manufacture the sensor element 101.
[0112] In the following, an example will be described in which a sensor element 101 consisting of six layers as shown in Fig. 1 is fabricated. In this case, six green sheets corresponding to the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6 are prepared. Fig. 4 is a diagram showing the process flow when fabricating the sensor element 101.
[0113] When manufacturing the sensor element 101, first, a blank sheet (not shown), which is a green sheet on which no pattern is formed, is prepared (step S1). When manufacturing the sensor element 101 consisting of six layers, six blank sheets are prepared corresponding to the respective layers.
[0114] The blank sheet has a plurality of sheet holes that are used for positioning during printing and lamination. The sheet holes are formed in advance by punching with a punching device at the blank sheet stage prior to pattern formation. When the corresponding layer is a green sheet that forms an internal space, the through-holes corresponding to the internal space are also formed in advance by a similar punching process. Moreover, the thicknesses of the blank sheets corresponding to the layers of the sensor element 101 do not all need to be the same.
[0115] When the blank sheets corresponding to each layer are prepared, a pattern printing and drying process is performed on each blank sheet (step S2). Specifically, patterns of various electrodes, patterns of the heater element 72 and the heater insulating layer 74, and patterns of internal wiring (not shown) are formed.
[0116] In addition, at the same time as printing the pattern, the application or placement of sublimable materials for forming the first diffusion rate-controlling portion 11, the second diffusion rate-controlling portion 13, and the third diffusion rate-controlling portion 30 is also performed.
[0117] Each pattern is printed by applying a pattern-forming paste prepared according to the characteristics required for each object to a blank sheet using a known screen printing technique. For drying after printing, known drying means can be used.
[0118] However, a method different from the conventional method is used for forming the pattern that will ultimately become the measurement electrode 44. This will be described later.
[0119] After the pattern printing on each blank sheet is completed, the printing and drying process of adhesive paste for laminating and bonding the green sheets corresponding to each layer is performed (step S3). A known screen printing technique can be used to print the adhesive paste, and a known drying method can be used for the drying process after printing.
[0120] Next, the green sheets coated with adhesive are stacked in a predetermined order and pressed under predetermined temperature and pressure conditions to form a laminate (step S4). Specifically, the green sheets to be stacked are stacked and held in a predetermined lamination jig (not shown) while being positioned by the sheet holes, and the lamination jig is heated and pressed by a lamination machine such as a known hydraulic press. The pressure, temperature, and time for heating and pressing depend on the lamination machine used, but appropriate conditions should be determined so that good lamination can be achieved.
[0121] When the laminate is obtained as described above, the laminate is subsequently cut at a plurality of locations to cut out individual units (referred to as element bodies) of the sensor elements 101 (step S5).
[0122] The cut-out element body is fired at a firing temperature of about 1300°C to 1500°C (step S6). In this way, the sensor element 101 is produced. That is, the sensor element 101 is produced by integrally firing the solid electrolyte layer and the electrodes. The firing temperature at this time is preferably 1200°C or higher and 1500°C or lower (for example, 1400°C). By integrally firing in this manner, each electrode in the sensor element 101 has sufficient adhesion strength.
[0123] The sensor element 101 thus obtained is accommodated in a predetermined housing and assembled into the main body of the gas sensor 100 (not shown).
[0124] <Method of forming measurement electrodes> As described above, in this embodiment, the measurement electrode 44 having the above-mentioned two-layer structure is provided on the sensor element 101. The formation of the measurement electrode 44 will be described.
[0125] 5 is a diagram showing a procedure for forming a pattern that will ultimately become the measurement electrode 44. There are two methods for forming the pattern that will become the measurement electrode 44: manufacturing method A and manufacturing method B.
[0126] In manufacturing method A, first, an electrolyte paste containing zirconia as a ceramic component, like the green sheet, is applied to the upper surface of the green sheet for forming the first solid electrolyte layer 4 at a position where the measurement electrode 44 is to be formed (step S21A). The electrolyte paste is a paste-like mixture of zirconia powder, which is a solid electrolyte, and a binder and other organic components.
[0127] Next, a three-component mixed paste is applied in a superimposed manner on the coating film formed by applying the electrolyte paste (step S22). Here, the three-component mixed paste is a paste-like mixture of a powder of a precious metal mainly composed of Pt, a powder of zirconia as a ceramic component, a powder of a pore-forming material which is a sublimable material for forming pores CV in the measurement electrode 44 to be finally formed, and a binder and other organic components.
[0128] After the application of the three-component mixed paste is completed, the paste coating film (paste double film) formed by overlapping the electrolyte paste and the three-component mixed paste is pressed by a predetermined pressing means (step S23). By this pressing, a part of the precious metal particles and the pore-forming material particles contained in the coating film of the three-component mixed paste penetrates into the coating film of the electrolyte paste.
[0129] Thereafter, when the element body is fired as described above, the paste double film is also fired, and the organic components are evaporated and the precious metal NM and the solid electrolyte SE are sintered. At this time, the solid electrolyte in the electrolyte paste is integrated with the solid electrolyte in the green sheet, and the part where the precious metal particles are embedded in the electrolyte paste becomes the lower layer 44L as the sintering progresses. On the other hand, in the applied part of the three-component mixed paste, the pore former is sublimated as the precious metal NM and the solid electrolyte SE are sintered, forming pores CV, and finally, an upper layer 44U in which the precious metal NM, the solid electrolyte SE, and the pores CV are mixed is obtained. As a result, a two-layered measuring electrode 44 is formed as shown in FIG. 2.
[0130] The coating thickness and coating area of the electrolyte paste and the three-component mixed paste may be set so that the thickness of the upper layer 44U and the lower layer 44L in the measurement electrode 44 finally formed and the planar area of the measurement electrode 44 are desired values while taking into account shrinkage due to firing and the intrusion of the precious metal particles and the pore-forming material particles due to pressing. For example, the relationship between the coating thickness and coating area of the electrolyte paste and the three-component mixed paste and the thickness of the upper layer 44U and the lower layer 44L in the measurement electrode 44 and the planar area of the measurement electrode 44 may be specified experimentally in advance. In addition, the mixing ratio of the precious metal powder, the zirconia powder as the solid electrolyte, and the pore-forming material powder in the three-component mixed paste may be set so that the volume ratio of the precious metal NM, the solid electrolyte SE, and the pores CV in the upper layer 44U (three-phase region) finally formed of the measurement electrode 44 is a desired value while taking into account the intrusion of the precious metal particles and the pore-forming material particles due to pressing.
[0131] On the other hand, in manufacturing method B, a two-component mixed paste is applied to the upper surface of a green sheet for forming the first solid electrolyte layer 4 at a position where the measurement electrode 44 is to be formed (step S21B). Here, the two-component mixed paste is a paste made by mixing a powder of a precious metal mainly composed of Pt, a powder of zirconia as a ceramic component, a binder and other organic components.
[0132] Thereafter, as in manufacturing method A, the three-component mixed paste is applied in a superimposed manner on the coating film formed by applying the two-component mixed paste (step S22), and further, the paste coating film (paste double film) formed by overlapping the two-component mixed paste and the three-component mixed paste is pressed by a predetermined pressing means (step S23).
[0133] In the case of manufacturing method B, too, some of the precious metal particles and pore-forming material particles contained in the coating film of the three-component mixed paste penetrate into the coating film of the two-component mixed paste by pressing.
[0134] Thereafter, when the element body is fired as described above, the paste double film is also fired, and the organic components are volatilized and the precious metal NM and the solid electrolyte SE are sintered. As a result, the applied portion of the two-component mixed paste becomes the lower layer. Meanwhile, in the applied portion of the three-component mixed paste, the pore-forming material is sublimated as the precious metal NM and the solid electrolyte SE are sintered, forming pores CV, and finally, an upper layer 44U in which the precious metal NM, the solid electrolyte SE, and the pores CV are mixed is obtained. In this case as well, a two-layered measuring electrode 44 as shown in FIG. 2 is formed as a result.
[0135] In the case of manufacturing method B as well, the coating thickness and coating area of the two-component mixed paste and the three-component mixed paste may be set so that the thickness of the upper layer 44U and the lower layer 44L in the finally formed measurement electrode 44 and the planar area of the measurement electrode 44 are desired values, while taking into account shrinkage due to firing and the infiltration of precious metal particles and pore-forming material particles due to pressing. The mixing ratio of the precious metal powder and the zirconia powder as the solid electrolyte in the two-component mixed paste may be set so that the volume ratio of the precious metal NM to the solid electrolyte SE in the finally formed lower layer 44L (two-phase region) of the measurement electrode 44 is a desired value, while taking into account the infiltration of precious metal particles and pore-forming material particles due to pressing. Similarly, the mixing ratio of the precious metal powder, the zirconia powder as the solid electrolyte, and the pore-forming material powder in the three-component mixed paste may be set so that the volume ratio of the precious metal NM, the solid electrolyte SE, and the pores CV in the upper layer 44U (three-phase region) of the measurement electrode 44 finally formed is a desired value, taking into account the penetration of the precious metal particles and the pore-forming material particles by pressing. As in the case of manufacturing method A, the relationship between these values may also be experimentally determined in advance.
[0136] As described above, according to this embodiment, the measurement electrode of the sensor element of the limiting current type gas sensor is provided as a porous cermet electrode as a whole, but by adopting a two-layer structure consisting of a lower layer containing only precious metal and solid electrolyte and no pores, and an upper layer containing a mixture of precious metal, solid electrolyte, and pores, deterioration of the measurement electrode caused by the presence of excess oxygen that cannot be taken in the measurement electrode is suitably suppressed. This realizes a gas sensor in which deterioration of measurement sensitivity is suitably suppressed even with continuous use.
[0137] <Modification> The two-layer structure of a region without pores and a region with pores, which is adopted for the measurement electrode 44 in the above-mentioned embodiment, may be applied to the inner pump electrode 22 and the auxiliary pump electrode 51, which are provided as a cermet of Au-Pt alloy and ZrO2 like the measurement electrode 44. In such a case, the effect of suppressing peeling due to the anchor effect can be obtained for these electrodes as well. Such inner pump electrode 22 and the auxiliary pump electrode 51 can also be formed by the same process as the measurement electrode 44.
[0138] In the above embodiment, two methods, manufacturing method A and manufacturing method B, are shown as methods for forming the pattern that becomes the measurement electrode 44. However, an alternative method, manufacturing method C, may also be adopted.
[0139] In manufacturing method C, the electrolyte paste used in manufacturing method A, the two-component mixed paste used in manufacturing method B, and the three-component mixed paste used in manufacturing methods A and B are applied in this order to the upper surface of a green sheet for forming first solid electrolyte layer 4 at the position where measurement electrode 44 is to be formed, and then pressed with a predetermined pressing means.
[0140] In the case of manufacturing method C, the coating thickness and coating area of the electrolyte paste, the two-component mixed paste, and the three-component mixed paste may be set so that the thickness of the upper layer 44U and the lower layer 44L in the finally formed measurement electrode 44 and the planar area of the measurement electrode 44 are desired values, while taking into account shrinkage due to firing and the infiltration of precious metal particles and pore-forming material particles due to pressing. The mixing ratio of the precious metal powder and the zirconia powder as the solid electrolyte in the two-component mixed paste may be set so that the volume ratio of the precious metal NM to the solid electrolyte SE in the finally formed lower layer 44L (two-phase region) of the measurement electrode 44 is a desired value, while taking into account the infiltration of precious metal particles and pore-forming material particles due to pressing. Similarly, the mixing ratio of the precious metal powder, the zirconia powder as the solid electrolyte, and the pore-forming material powder in the three-component mixed paste may be set so that the volume ratio of the precious metal NM, the solid electrolyte SE, and the pores CV in the upper layer 44U (three-phase region) of the measurement electrode 44 finally formed is a desired value, while taking into account the penetration of the precious metal particles and the pore-forming material particles by pressing. As in the cases of Manufacturing Methods A and B, the relationship between these values may also be experimentally determined in advance. EXAMPLES
[0141] As examples, six types of gas sensors 100 (Examples 1 to 6) were produced using different manufacturing conditions for the measurement electrode 44. The volume ratio of each phase (noble metal, solid electrolyte, and pores) in the upper layer 44U and the lower layer 44L of the measurement electrode 44 and the thickness ratio t U :t L In addition, a continuous drive test in the atmosphere was conducted to evaluate the degree of deterioration of the measurement electrodes due to continuous use.
[0142] In forming the measurement electrode 44, the manufacturing method was changed to two levels, manufacturing method A and manufacturing method B, and for each manufacturing method, the weight ratio of the precious metal powder, the solid electrolyte powder, and the pore former in the three-component mixed paste for mainly forming the upper layer 44U was changed to two levels. One type of electrolyte paste was used for manufacturing method A, and one type of two-component mixed paste was used for manufacturing method B.
[0143] As a conventional example, a gas sensor was also fabricated having a measurement electrode 44Z formed entirely from a three-component mixed paste (hereinafter, this fabrication method will be referred to as the conventional method). In the same manner as in the gas sensor of the embodiment, the volume ratio of each phase (noble metal, solid electrolyte, and pores) of the measurement electrode 44Z was evaluated, and a continuous drive test in the atmosphere was performed.
[0144] Table 1 shows a list of the weight ratios (component ratios) of the precious metal powder, solid electrolyte powder, and pore-forming material in the pastes used to fabricate the measurement electrodes 44 of Examples 1 to 6 and the conventional measurement electrode 44Z.
[0145] [Table 1]
[0146] In Table 1, the column "for forming upper layer" shows the weight ratio of the three-component mixed paste, and the column "for forming lower layer" shows the weight ratio of the electrolyte paste and the two-component mixed paste.
[0147] As shown in Table 1, when the weight ratios of the precious metal powder, solid electrolyte powder, and pore former used in the three-component mixed paste are a, b, and c, respectively, and the weight ratios of the precious metal powder and solid electrolyte powder used in the two-component mixed paste are d and e, respectively, the three-component mixed paste was either a:b:c=10:2:1 (Example 1, Example 4, Example 6) or a:b:c=30:10:1 (Example 2, Example 3, Example 5). In addition, for the two-component mixed paste, the value when the mixing ratio c of the pore former in the three-component mixed paste is 1 is (c:)d:e=(1:)5:1 (Example 4, Example 5, Example 6). Furthermore, for the solid electrolyte powder contained in the electrolyte paste, when the ratio to the mixing ratio c of the pore former in the three-component mixed paste is conveniently represented as e, it is c:e=1:10 (Example 1, Example 2, Example 3).
[0148] In Examples 1 to 3 in which the measurement electrode 44 was formed by Manufacturing Method A, the target coating thickness of the electrolyte paste was 10 μm, and the target coating thickness of the three-component mixed paste was 15 μm.
[0149] In Examples 4 to 6 in which the measurement electrode 44 was formed by Manufacturing Method B, the target coating thickness of the two-component mixed paste was 5 μm, and the target coating thickness of the three-component mixed paste was 15 μm.
[0150] In the conventional example in which the measuring electrode 44Z was produced by the conventional method, the three-component mixed paste had a:b:c=10:2:1, and the target coating thickness of the three-component mixed paste was 15 μm.
[0151] The volume ratio of each phase in the upper layer 44U and the lower layer 44L of the measuring electrode 44 and the thickness ratio t U :t L The volume ratio in the measurement electrode 44Z of the conventional example is shown in the "upper layer" column for convenience.
[0152] [Table 2]
[0153] In Table 2, the volume ratios of the precious metal NM, solid electrolyte SE, and pores CV in the upper layer 44U are P1 (%), P2 (%), and P3 (%), respectively, and the volume ratios of the precious metal NM and solid electrolyte SE in the lower layer 44L are P4 (%) and P5 (%), respectively. P1 + P2 + P3 = P4 + P5 = 100 (%).
[0154] The volume ratio of each phase in the measurement electrode 44 and the measurement electrode 44Z was obtained by taking a cross-sectional SEM image of each electrode and performing known image processing on the cross-sectional SEM image. In summary, the cross-sectional SEM image was tri-valued so that the area where the precious metal NM was present was white, the area where the solid electrolyte SE was present was gray, and the area where the pores or internal voids were present was black, and the area ratio (cross-sectional area ratio) of each area was taken as the volume ratio.
[0155] In addition, the thickness ratio t U :t L is the thickness t of the upper layer 44U based on a cross-sectional SEM image of the measurement electrode 44. U and the thickness t of the lower layer 44L L This was done by identifying the following:
[0156] The results shown in Table 2 indicate that in all of Examples 1 to 6, the measurement electrode 44 has a two-layer structure consisting of an upper layer 44U and a lower layer 44L.
[0157] Looking more specifically, in Examples 1, 4, and 6, in which the manufacturing methods of the measurement electrode 44 are different but the weight ratio a:b:c in the three-component mixed paste is common at 10:2:1, the values of P1, P2, P3, P4, and P5 were the same. Among these, the volume ratio of the precious metal NM in the upper layer 44U and the lower layer 44L was P1=P4=40%. In addition, the volume ratio of the solid electrolyte SE in the upper layer 44U was 20%, while the value P5 in the lower layer 44L was 60%, which was larger than that.
[0158] In contrast, in Examples 2, 3, and 5, in which the manufacturing methods of the measurement electrode 44 were different but the weight ratio a:b:c in the three-component mixed paste was common at 30:10:1, the values of P1, P2, and P3 were the same, but the values of P4 and P5 differed by 5% between Examples 2, 3, and 5. That is, in all of Examples 2, 3, and 5, the value of the volume ratio P1 of the precious metal NM in the upper layer 44U was 45%, and the value of the volume ratio P2 of the solid electrolyte SE was 40%, while the value of the volume ratio P4 of the precious metal NM in the lower layer 44L was 45% in Examples 2 and 3, and 40% in Example 5. Correspondingly, the value of the volume ratio P5 of the solid electrolyte SE was 55% in Examples 2 and 3, and 60% in Example 5.
[0159] However, in all Examples, the volume ratio of the solid electrolyte SE in the lower layer 44L was higher than the volume ratio of the solid electrolyte SE in the upper layer 44U. Specifically, the volume ratio of the solid electrolyte SE in the upper layer 44U was within a range of 20% to 40%, and the volume ratio of the solid electrolyte SE in the lower layer 44L was within a range of 50% to 60%.
[0160] The volume ratios P1, P2, and P3 of the phases in the measurement electrode 44Z of the conventional example were the same as those in Examples 1 and 4, in which the three-component mixed pastes of the same weight ratios were used.
[0161] In addition, the thickness ratio t U :t L Regarding the value of t U In the examples 4 to 6 produced by the manufacturing method B, the value t U and value t L The relationship between the sizes of the two was different.
[0162] However, in all the examples, the thickness ratio t U :t L was in the range of 95:5 to 10:90.
[0163] The continuous drive test in air was performed by operating each gas sensor continuously for 3000 hours in an air atmosphere at 25±5°C, and measuring the NOx current value (also called NOx output) at the start of operation, after 1000 hours, after 2000 hours, and after 3000 hours. The rate of change in NOx current at each measurement timing, based on the NOx current value at the start of operation, was calculated as the NOx output change rate. The NOx output change rate is a value that serves as an index showing the degree of deterioration of the measurement electrode 44 or the measurement electrode 44Z.
[0164] Figure 6 is a graph showing the results of the continuous driving test, in which the horizontal axis represents the driving time and the vertical axis represents the rate of change in NOx output.
[0165] 6, in the conventional gas sensor, the NOx output changed significantly with the passage of operating time, and the NOx output change rate after 3000 hours was about 11.5%±3.5% when the variation was taken into account, whereas in the gas sensors of Examples 1 to 6, the NOx output change rate after 3000 hours was only about 6% at most. This means that in the gas sensors of Examples 1 to 6, the deterioration of the measurement electrode was suppressed even after 3000 hours.
[0166] In particular, in the gas sensors other than Example 3, the NOx output change rate after 3000 hours remained approximately 3% or less, and it is considered that the deterioration of the measuring electrode is more effectively suppressed in these gas sensors.
[0167] The results of the above continuous drive tests show that by providing the measurement electrode in the sensor element of a limiting current type gas sensor as a two-layer structure consisting of a lower layer having a two-phase structure of precious metal and solid electrolyte and an upper layer having a three-phase structure of precious metal, solid electrolyte, and pores, it is possible to suppress deterioration of the measurement electrode when the gas sensor is used continuously. [Explanation of symbols]
[0168] 1~3 1st~3rd substrate layer 4 First solid electrolyte layer 5 Spacer layer 6 Second solid electrolyte layer 10 Gas inlet 11 First diffusion-controlled section 12 Buffer space 13 Second diffusion-controlled section 20 1st internal void 21 Main pump cell 22 Inner pump electrode 23 Outer pump electrode 30 Third diffusion-controlled section 40 Second internal void 41 Measuring pump cell 42 Reference electrode 44 Measuring electrode 44L Lower layer (of the measuring electrode) 44U Upper layer (of measuring electrode) 50 Auxiliary pump cell 51 Auxiliary pump electrode 60 4th diffusion-controlled section 61 3rd internal void 70 Heater section 80 Main sensor cell 81 Auxiliary sensor cell 82 Measuring sensor cell 100 Gas Sensor 101 Sensor element CV pores Ip0 Main pump current Ip1 Auxiliary pump current Ip2 NOx current NM Precious metals SE solid electrolyte
Claims
1. A sensor element of a limiting current type NOx sensor, A base portion made of an oxygen ion conductive solid electrolyte; an internal space for measurement into which a gas to be measured, the oxygen concentration of which has been adjusted in advance, is introduced; a measurement pump cell including a measurement electrode disposed facing the measurement internal space, an outside-space pump electrode disposed at a location other than the measurement internal space, and a portion of the base portion that is present between the measurement electrode and the outside-space pump electrode, through which a pump current proportional to the concentration of NOx contained in the measurement gas flows; Equipped with The measuring electrode is an upper layer comprising a precious metal, the solid electrolyte and pores; a lower layer consisting of the precious metal and the solid electrolyte; Equipped with a volume ratio of the solid electrolyte in the lower layer is greater than a volume ratio of the solid electrolyte in the upper layer; A sensor element for a NOx sensor.
2. A sensor element for a NOx sensor according to claim 1, The volume ratio of the solid electrolyte in the upper layer is 20% to 40%, The volume ratio of the solid electrolyte in the lower layer is 50% to 60%. A sensor element for a NOx sensor.
3. A sensor element of a NOx sensor according to claim 1 or 2, the thickness ratio of the upper layer to the lower layer is in the range of 95:5 to 10:90; A sensor element for a NOx sensor.
4. A sensor element for a NOx sensor according to claim 3, the thickness ratio of the upper layer to the lower layer is in the range of 90:10 to 30:70; A sensor element for a NOx sensor.
5. A sensor element of a limiting current type NOx sensor, A base portion made of an oxygen ion conductive solid electrolyte; an internal space for measurement into which a gas to be measured, the oxygen concentration of which has been adjusted in advance, is introduced; a measurement pump cell including a measurement electrode disposed facing the measurement internal space in a portion of the base portion defining the measurement internal space, an outside-space pump electrode disposed in a location other than the measurement internal space, and a portion of the base portion present between the measurement electrode and the outside-space pump electrode, and through which a pump current proportional to the concentration of NOx contained in the measurement gas flows; Equipped with the measurement electrode is composed of a precious metal, the solid electrolyte, and pores; a boundary between the base portion and the measurement electrode is different from a boundary between a region in the measurement electrode where the pores are present and a region in the measurement electrode where the pores are not present; the boundary between the base portion and the measurement electrode is the lowest end of a region in the measurement electrode where the precious metal is present, a boundary between a region in which the pores are present and a region in which the pores are not present in the measurement electrode is a lowermost end of the region in which the pores are present; a volume ratio of the solid electrolyte is larger in the region where the pores are not present than in the region where the pores are present; The ratio of the distance from the upper end of the measurement electrode to the lowermost end of the region where the pores exist to the distance from the lowermost end of the region where the precious metal exists to the lowermost end of the region where the pores exist is in the range of 95:5 to 10:
90. A sensor element for a NOx sensor.
6. A sensor element for a NOx sensor according to claim 5, The ratio of the distance from the upper end of the measurement electrode to the lowermost end of the region where the pores exist to the distance from the lowermost end of the region where the precious metal exists to the lowermost end of the region where the pores exist is in the range of 90:10 to 30:
70. A sensor element for a NOx sensor.
7. A sensor element of a NOx sensor according to claim 5 or 6, the volume ratio of the solid electrolyte in the region where the pores are present is 20% to 40%; The volume ratio of the solid electrolyte in the region where no pores exist is 50% to 60%. A sensor element for a NOx sensor.
8. A method for manufacturing a sensor element of a limiting current type NOx sensor, comprising the steps of: The sensor element is A base portion made of an oxygen ion conductive solid electrolyte; At least one internal cavity into which a gas to be measured is introduced; at least one pump cell including an internal electrode disposed in a portion of the base portion defining the at least one internal cavity so as to face the at least one internal cavity, an outside-space pump electrode disposed in a location other than the at least one internal cavity, and a portion of the base portion present between the internal electrode and the outside-space pump electrode; comprising a preparation step of preparing a plurality of green sheets containing an oxygen ion conductive solid electrolyte as a ceramic component, which is a constituent material of the sensor element; a pattern forming step of forming a predetermined pattern on each of the plurality of green sheets; a lamination step of laminating the plurality of green sheets on which the predetermined pattern is formed to obtain a laminate; a cutting step of cutting the laminate to obtain element bodies each corresponding to the sensor element; a firing step of firing the element body to obtain the sensor element; Equipped with The pattern forming step includes: an internal electrode film forming step of forming an internal electrode paste film at a predetermined forming position of an internal electrode forming green sheet which is one of the plurality of green sheets; Equipped with The internal electrode film forming step includes: a first application step of applying a solid electrolyte paste containing the solid electrolyte and an organic component to at least one of the formation positions; a second application step of applying a three-component mixed paste obtained by mixing three components, namely, a precious metal, the solid electrolyte, and a pore-forming material, with an organic component, in a superimposed manner on the formation position where the solid electrolyte paste has been applied; a pressing step of pressing the coating film formed at the formation position by the second coating step, and causing the particles of the precious metal and a part of the particles of the pore-forming material to penetrate into the coating film of the solid electrolyte paste formed by the first coating step; A method for manufacturing a sensor element of a NOx sensor, comprising:
9. A method for manufacturing a sensor element of a limiting current type NOx sensor, comprising the steps of: The sensor element is A base portion made of an oxygen ion conductive solid electrolyte; At least one internal cavity into which a gas to be measured is introduced; at least one pump cell including an internal electrode disposed in a portion of the base portion defining the at least one internal cavity so as to face the at least one internal cavity, an outside-space pump electrode disposed in a location other than the at least one internal cavity, and a portion of the base portion present between the internal electrode and the outside-space pump electrode; comprising a preparation step of preparing a plurality of green sheets containing an oxygen ion conductive solid electrolyte as a ceramic component, which is a constituent material of the sensor element; a pattern forming step of forming a predetermined pattern on each of the plurality of green sheets; a lamination step of laminating the plurality of green sheets on which the predetermined pattern is formed to obtain a laminate; a cutting step of cutting the laminate to obtain element bodies each corresponding to the sensor element; a firing step of firing the element body to obtain the sensor element; Equipped with The pattern forming step includes: an internal electrode film forming step of forming an internal electrode paste film at a predetermined forming position of an internal electrode forming green sheet which is one of the plurality of green sheets; Equipped with The internal electrode film forming step includes: A first application step of applying a two-component mixed paste obtained by mixing two components, a precious metal and the solid electrolyte, with an organic component to at least one of the formation positions; a second application step of applying a three-component mixed paste obtained by mixing three components, the noble metal, the solid electrolyte, and a pore-forming material, with an organic component, in a superimposed manner on the formation position where the two-component mixed paste has been applied; a pressing step of pressing the coating film formed at the formation position by the second coating step, and causing the particles of the precious metal and a part of the particles of the pore-forming material to penetrate into the coating film of the two-component mixed paste formed by the first coating step; A method for manufacturing a sensor element of a NOx sensor, comprising:
Citation Information
Patent Citations
Pump electrode and reference electrode of gas sensor
CN107949785A
Nox decomposition electrode, and nox concentration measuring apparatus
JP2003322634A
Pump electrode and reference electrode for gas sensor
JP2017020838A
Gas sensor element and gas sensor
JP2019052973A
Method and device for measuring NOx concentration in gas to be measured
JP2885336B2