Fluorine-based resin particle-containing fiber and fiber assembly
By integrating water-insoluble resins with fluororesin particles, the fibers achieve enhanced water repellency and processability, addressing the challenges of processing fluororesins into fibers, and resulting in fibers with improved properties.
Patent Information
- Application Number
- JP2020177562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-10-22
AI Technical Summary
Existing fluororesins like PTFE are difficult to process into fibers due to their solvent resistance and lack of fluidity, resulting in fibers that are not water-repellent when polyethylene oxide is used.
Incorporating water-insoluble resins such as polyvinylidene fluoride and polytetrafluoroethylene particles into the fibers to enhance water repellency and processability.
The resulting fibers exhibit excellent water repellency, chemical resistance, and heat resistance, with improved processability and increased specific surface area, forming bulky fiber aggregates with high air permeability.
Smart Images

Figure 0007588493000002 
Figure 0007588493000001
Abstract
Description
[Technical field]
[0001] The present invention relates to fibers containing fluororesin particles such as polytetrafluoroethylene particles, and a fiber assembly constituted from the fibers. [Background technology]
[0002] Fluorine-based resins such as polytetrafluoroethylene (PTFE) are known to have excellent water repellency, chemical resistance, and heat resistance, but many fluorine-based resins such as PTFE are known to be difficult to process, such as by fiberization, because they do not dissolve in solvents and do not exhibit fluidity even when heated. Patent Document 1 discloses a filter made of PTFE fiber, and in the examples it is disclosed that the filter was manufactured by mixing water-soluble polyethylene oxide with an aqueous dispersion of PTFE particles and subjecting the mixture to electrospinning. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2015-511173 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the fibers constituting the filter of Patent Document 1 contain polyethylene oxide, which is a water-soluble resin, and therefore are not water-repellent fibers.
[0005] The present invention has been made in light of these circumstances, and has an object to provide a fiber which contains a fluorine-based resin such as PTFE and has excellent water repellency. [Means for solving the problem]
[0006] The invention according to claim 1 of the present invention is "fibers containing fluororesin particles and a water-insoluble resin."
[0007] The invention according to claim 2 of the present invention is "the fiber according to claim 1, wherein the fluororesin particles are polytetrafluoroethylene particles."
[0008] The invention of claim 3 of the present invention is "the fiber according to claim 1 or 2, wherein the water-insoluble resin is at least one of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polybenzimidazole, polyimide, polyamideimide, polyetherimide, polyethersulfone, and polyacrylonitrile."
[0009] The invention according to claim 4 of the present invention is "a fiber assembly composed of the fibers according to any one of claims 1 to 3." Effect of the Invention
[0010] The fiber according to claim 1 of the present invention contains fluororesin particles and also contains a water-insoluble resin, and therefore is a fiber with excellent water repellency.
[0011] The fiber according to claim 2 of the present invention is a fiber having superior water repellency since the fluororesin particles contained in the fiber are particles made of polytetrafluoroethylene, which is a fluororesin that has particularly excellent water repellency.
[0012] The fiber according to claim 3 of the present invention has a water-insoluble resin contained in the fiber which is at least one type of resin selected from the group consisting of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polybenzimidazole, polyimide, polyamideimide, polyetherimide, polyethersulfone, and polyacrylonitrile, which are particularly poorly soluble in water, and thus has superior water repellency.
[0013] The fiber assembly according to claim 4 of the present invention is a fiber assembly having excellent water repellency, since it is composed of fibers having excellent water repellency. [Brief description of the drawings]
[0014] [Figure 1] 1 is a photograph of a fiber having the configuration of the present invention taken at a magnification of 10,000 times using an SEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The fiber of the present invention contains fluororesin particles and a water-insoluble resin. By containing fluororesin particles in the fiber, the fiber can have excellent water repellency, chemical resistance, heat resistance, electrical insulation, and non-stickiness. In addition, by using fluororesin particles, the specific surface area of the fiber is large, and the fiber aggregate formed by assembling the fibers is bulky and has excellent breathability. Furthermore, by containing a water-insoluble resin in the fiber, while it is difficult to form the fiber using only fluororesin particles, it is possible to form the fiber by combining with the water-insoluble resin, and the fiber can have water repellency. The fluororesin contained in the fluororesin particles refers to a resin containing fluorine in the repeating unit of the resin, and may be, for example, polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), polyvinyl fluoride (PVF), perfluoroalkoxy fluororesin (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, and copolymers of various monomers that constitute the resin. These fluororesins may be modified, for example, by introducing functional groups such as hydroxyl groups and carboxyl groups. Among these fluororesins, polytetrafluoroethylene, which is a resin that is particularly excellent in water repellency, is more preferable. The structure of the fluororesin may be either linear or branched, and the structure of the resin may be a block copolymer or a random copolymer. Furthermore, the three-dimensional structure of the resin and the presence or absence of crystallinity are not particularly limited.
[0016] The fluororesin particles may be composed of one type of fluororesin or two or more types of fluororesin. The presence of fluororesin particles contained in the fiber can be confirmed by magnifying and observing the fiber with a microscope to confirm that the fluororesin contained in the fiber is a particle. For example, FIG. 1 shows a fiber having the configuration of the present invention magnified 10,000 times with a SEM, which is a type of electron microscope, and the protruding parts constituting the fiber are fluororesin particles.
[0017] The particle size of the fluororesin particles is not particularly limited, but may be 10 to 2000 nm, 50 to 1000 nm, or 100 to 500 nm. Note that the particle size in the present invention is the average value of the longest major axis of the particle and the minor axis perpendicular to the major axis at the midpoint of the major axis, measured from an electron microscope image.
[0018] The higher the proportion of fluororesin particles contained in the fiber, the more excellent the water repellency, chemical resistance, heat resistance, electrical insulation, and non-stickiness of the fiber, so the proportion is preferably 20 mass% or more, more preferably 30 mass% or more, and even more preferably 40 mass% or more. The upper limit of the proportion of fluororesin particles contained in the fiber is realistically 99 mass% or less, because if the proportion of fluororesin particles contained in the fiber is too high, the fiber shape may not be maintained.
[0019] The water-insoluble resin contained in the fiber of the present invention may be, for example, a fluororesin such as polyvinylidene fluoride (PVDF), vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, and copolymers of various monomers constituting the above resin; a polyolefin resin such as polyethylene (PE) or polypropylene (PP); a polyester resin such as polystyrene resin, polyethylene terephthalate (PET) or polyethylene naphthalate (PEN), polybenzimidazole (PBI), polyimide (PI), polyamideimide (PAI), polyetherimide (PEI), polyamide (PA), polyphenylene sulfide (PPS), polyethersulfone (PES), polysulfone (PSU), polyurethane (PU), polyacrylonitrile (PAN), polyacrylonitrile copolymer, an epoxy resin, or a cellulose resin. Among these water-insoluble resins, since the strength of the fiber tends to be high when the resin is spun into a fiber, any of polyvinylidene fluoride, polyvinylidene fluoride copolymer, polybenzimidazole, polyimide, polyamideimide, polyetherimide, polyethersulfone, and polyacrylonitrile is more preferable, and polyvinylidene fluoride is even more preferable. The structure of the water-insoluble resin may be either linear or branched, and may be a block copolymer or a random copolymer, and the three-dimensional structure of the resin and the presence or absence of crystallinity are not particularly limited. The fiber may contain only one type of water-insoluble resin, or may contain two or more types of water-insoluble resin.
[0020] The higher the ratio of the water-insoluble resin contained in the fiber, the better the strength of the fiber, so the ratio is preferably 1 mass% or more, more preferably 5 mass% or more, and even more preferably 10 mass% or more. The upper limit of the ratio of the water-insoluble resin contained in the fiber is realistically 80 mass% or less, because if the ratio of the water-insoluble resin is too high, the content of the fluororesin particles is low and water repellency may be poor.
[0021] The fiber of the present invention contains fluororesin particles and a water-insoluble resin, but may contain additives such as dispersants, crosslinking agents, and spinning aids, provided that the additives do not affect the water repellency of the fiber.
[0022] The fiber diameter of the fiber of the present invention is preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less so as to have excellent performances such as separation performance, liquid retention performance, wiping performance, insulation performance, or flexibility. The lower limit of the average fiber diameter can be appropriately selected, but 50 nm or more is realistic so as to obtain a fiber with excellent strength. The "fiber diameter" in the present invention refers to the diameter of a circle in a direction perpendicular to the longitudinal axis of the fiber, measured based on an electron microscope photograph of the fiber at 1000 to 10000 times magnification. When the cross section of the fiber is a non-circular irregular cross section, the cross-sectional area of the irregular cross section is measured, and the diameter of a circle having that cross-sectional area is regarded as the fiber diameter.
[0023] The smaller the CV value of the fiber diameter of the fiber of the present invention, the more uniform the fiber diameter is. Since uniform fiber diameters prevent the physical properties of the fiber of the present invention, such as water repellency, chemical resistance, and heat resistance, from differing from fiber to fiber, the CV value is preferably 0.80 or less, more preferably 0.60 or less, even more preferably 0.40 or less, and ideally 0. The CV value of the fiber diameter is the value obtained by dividing the standard deviation of the fiber diameters by the average fiber diameter, that is, (standard deviation of fiber diameters / average fiber diameter). The "average fiber diameter" refers to the average fiber diameters of 50 fibers, and the "standard deviation of fiber diameters" is a value calculated from the fiber diameters of 50 fibers selected when measuring the average fiber diameter described below.
[0024] The fiber length of the fiber of the present invention is not particularly limited. In the present invention, the "fiber length" refers to the length in the longitudinal direction of the fiber measured based on an electron microscope photograph of the fiber at 50 to 5000 times magnification.
[0025] The fibers of the present invention may be short fibers having an aspect ratio of 200 or less, which can be expressed as (fiber length / fiber diameter), or long fibers having an aspect ratio of more than 200. Furthermore, among long fibers, the fibers may be continuous fibers having a particularly long fiber length. Note that continuous fibers mean that both ends of the majority of the fibers cannot be confirmed in an electron microscope photograph of the fibers at 500 times magnification. Furthermore, the fibers may be a fiber aggregate formed by accumulating fibers, regardless of whether the fibers are short fibers or long fibers.
[0026] When the fiber of the present invention is a fiber assembly, the basis weight and thickness of the fiber assembly are not particularly limited because the optimal basis weight and thickness vary depending on the application. 2 The thickness refers to the thickness when a load of 3.5N is applied.
[0027] The fiber of the present invention can be produced, for example, by the following method.
[0028] First, fluororesin particles in powder form or dispersed in an organic solvent, a water-insoluble resin, and a solvent capable of dissolving the water-insoluble resin are mixed to produce a spinning solution in which the water-insoluble resin is dissolved and the fluororesin particles are dispersed. The solvent is not particularly limited and can be selected appropriately since it varies depending on the fluororesin particles and water-insoluble resin used. In addition, the solvent in which the fluororesin particles are dispersed and the solvent capable of dissolving the water-insoluble resin may be the same solvent or different solvents, but if different solvents are contained during spinning, there is a risk of the spinning solution gelling or separation due to the spinning solution causing a decrease in storage stability, so it is preferable that the solvent in which the fluororesin particles are dispersed and the solvent capable of dissolving the water-insoluble resin are the same solvent. The solid content concentration of the fluororesin particles and the water-insoluble resin in the spinning solution can be adjusted appropriately because the optimal value varies depending on the fluororesin particles and water-insoluble resin used.
[0029] Next, the spinning solution is spun to form fibers. As the spinning method, a conventionally known spinning method can be adopted. For example, the fibers can be formed by spinning using a wet spinning method, a dry spinning method, a flash spinning method, a centrifugal spinning method, an electrostatic spinning method, a spinning method using a gas shearing force as disclosed in JP-A-2009-287138, or a spinning method using a gas shearing force in addition to the action of an electric field as disclosed in JP-A-2011-32593. Among these, the electrostatic spinning method is preferable because it is easy to spin fibers with a small fiber diameter. In addition, a fiber aggregate in which the spun fibers are accumulated may be produced.
[0030] In addition, when spinning by electrostatic spinning, if the conductivity of the spinning solution is insufficient, the spinnability may be poor and it may be difficult to form fibers, so in such cases, the conductivity can be adjusted by adding an appropriate amount of salt (spinning aid) to the spinning solution. In addition, the fibers may be heat-treated for the purpose of removing the solvent contained in the fibers and improving the strength by improving the crystallinity of the constituent resin of the fibers.
[0031] By pulverizing long fibers or fiber aggregates having an aspect ratio of 200 or more, short fibers having an aspect ratio of 200 or less can be obtained. The pulverization method is not particularly limited, but examples thereof include methods using a stone mill, a pin mill, an ultrasonic pulverizer, and a cutter. EXAMPLES
[0032] The present invention will be described below with reference to specific examples, but the present invention is not limited to these specific examples.
[0033] Example 1 (Production of spinning solution A) Polyvinylidene fluoride (PVDF) (A) with a molecular weight of 1 million was dissolved in N,N-dimethylacetamide (DMAc) to produce a PVDF (A) solution (solid concentration: 7.5 mass%). Next, a polytetrafluoroethylene (PTFE) dispersion (solvent: DMAc, solid concentration: 40 mass%) was mixed into the PVDF (A) solution so as to produce a fiber assembly showing the mass ratio described below, to produce spinning solution A. (Manufacturing of fiber assemblies) Spinning solution A was electrostatically spun under the following conditions, and the electrostatically spun fiber was heat-treated at 160°C for 30 minutes to obtain a fiber aggregate composed of PTFE particles and PVDF (A) (mass ratio of PTFE particles to PVDF (A) = 90:10, PTFE particle diameter: 200-300 nm, fiber diameter: 760 nm, fiber length: continuous fiber, basis weight: 7.9 g / m 2 , thickness: 17 μm) was produced. <Spinning conditions> Electrode: Metal nozzle (inner diameter: 0.33 mm) Collector: Grounded stainless steel drum Nozzle discharge rate: 1g / hour Distance between nozzle tip and collector: 8cm ·Temperature and humidity inside the spinning chamber: 25℃ / 35%RH Voltage applied to the nozzle: 10kV
[0034] Example 2 (Production of spinning solution B) The same PVDF (A) solution and PTFE dispersion as in Example 1 were mixed so as to produce a fiber aggregate having the mass ratio described below, to produce spinning solution B. (Manufacturing of fiber assemblies) The spinning solution B was electrostatically spun under the same conditions as in Example 1, and the electrostatically spun product was heat-treated at 160°C for 30 minutes to obtain a fiber aggregate composed of PTFE particles and PVDF (A) (mass ratio of PTFE particles to PVDF (A) = 80:20, PTFE particle diameter: 200 to 300 nm, fiber diameter: 910 nm, fiber length: continuous fiber, basis weight: 4.8 g / m 2 , thickness: 10 μm) was produced.
[0035] Example 3 (Production of spinning solution C) PVDF (B) having a molecular weight of 750,000 was dissolved in DMAc to produce a PVDF (B) solution (solid concentration: 14 mass%). Next, the same PTFE dispersion as in Example 1 was mixed with the PVDF (B) solution so as to produce a fiber aggregate having the mass ratio described below, to produce spinning solution C. (Manufacturing of fiber assemblies) Spinning solution C was electrostatically spun under the following conditions, and the electrostatically spun fiber was heat-treated at 160°C for 30 minutes to obtain a fiber aggregate composed of PTFE particles and PVDF (B) (mass ratio of PTFE particles to PVDF (B) = 90:10, PTFE particle diameter: 200-300 nm, fiber diameter: 310 nm, fiber length: continuous fiber, basis weight: 5.2 g / m 2 , thickness: 13 μm) was produced. <Spinning conditions> Electrode: Metal nozzle (inner diameter: 0.33 mm) Collector: Grounded stainless steel drum Nozzle discharge rate: 1g / hour Distance between nozzle tip and collector: 10cm ·Temperature and humidity inside the spinning chamber: 25℃ / 35%RH Voltage applied to the nozzle: 15kV
[0036] Example 4 (Production of spinning solution D) The same PVDF (B) solution and PTFE dispersion as in Example 3 were mixed so as to produce a fiber aggregate having the mass ratio described below, to produce spinning solution D. (Manufacturing of fiber assemblies) The spinning solution D was electrostatically spun under the same conditions as in Example 3, and the electrostatically spun product was heat-treated at 160°C for 30 minutes to obtain a fiber aggregate composed of PTFE particles and PVDF (B) (mass ratio of PTFE particles to PVDF (B) = 80:20, PTFE particle diameter: 200 to 300 nm, fiber diameter: 300 nm, fiber length: continuous fiber, basis weight: 5.0 g / m 2 , thickness: 12 μm) was produced.
[0037] Example 5 (Production of spinning solution E) A polyamic acid solution (solvent: DMAc, solids concentration: 22 mass%), which is a precursor of a polyimide (PI) resin, and the same PTFE dispersion as in Example 1 were mixed so as to produce a fiber aggregate having the mass ratio described below, to produce spinning solution E. (Manufacturing of fiber assemblies) Spinning solution E was electrostatically spun under the following conditions, and the electrostatically spun yarn was heat-treated at 300°C for 30 minutes to dehydrate and cyclize the polyamic acid to convert it to PI, resulting in a fiber aggregate composed of PTFE particles and PI (PTFE particle to PI mass ratio = 40:60, PTFE particle diameter: 200-300 nm, fiber diameter: 260 nm, fiber length: continuous fiber, basis weight: 2.2 g / m 2 , thickness: 5.0 μm) was produced. <Spinning conditions> Electrode: Metal nozzle (inner diameter: 0.33 mm) Collector: Grounded stainless steel drum Nozzle discharge rate: 1g / hour Distance between nozzle tip and collector: 10cm ·Temperature and humidity inside the spinning chamber: 25℃ / 35%RH Voltage applied to the nozzle: 15kV
[0038] Comparative Example 1 (Manufacturing of fiber assemblies) The PVDF (A) solution described in Example 1 was electrospun and heat-treated under the same conditions as in Example 1 to obtain a fiber aggregate containing only PVDF (fiber diameter: 190 nm, fiber length: continuous fiber, basis weight: 2.9 g / m 2 , thickness: 7.0 μm) was produced.
[0039] Comparative Example 2 (Manufacturing of fiber assemblies) The PVDF (B) solution described in Example 3 was electrospun and heat-treated under the same conditions as in Example 3 to obtain a fiber aggregate containing only PVDF (fiber diameter: 390 nm, fiber length: continuous fiber, basis weight: 3.1 g / m 2 , thickness: 11 μm) was produced.
[0040] Comparative Example 3 (Manufacturing of fiber assemblies) The polyamic acid described in Example 5 was electrospun and heat-treated under the same conditions as in Example 5 to obtain a fiber assembly composed only of PI (fiber diameter: 480 nm, fiber length: continuous fiber, basis weight: 1.6 g / m 2 , thickness: 7.0 μm) was produced.
[0041] Next, the fiber assemblies of the examples and comparative examples were evaluated by the following methods.
[0042] (Contact angle measurement) 3 μL of water was dropped onto the fiber assemblies of the examples and comparative examples, and the contact angle (°) after 10 seconds was measured at θ / 2 using a contact angle measuring device (DM-500, manufactured by Kyowa Interface Science Co., Ltd.) The larger the contact angle, the more difficult it was to wet the fiber assembly, and the higher the water repellency was evaluated to be.
[0043] The constituent resins and physical properties of the fiber assemblies of the examples and comparative examples, and the contact angles of the fiber assemblies are shown in Table 1 below.
[0044] [Table 1]
[0045] Although the fiber assemblies of Examples 1 to 5 contained PTFE resin, which is difficult to form into fibers, the fiber assemblies could be produced. In addition, the contact angle measurement results showed that the fiber assemblies of Examples 1 to 5, which contained PTFE particles, which are fluororesin particles, had higher water repellency than the fiber assemblies of Comparative Examples 1 to 3, which did not contain PTFE particles. [Industrial Applicability]
[0046] The fibers and fiber assemblies of the present invention have water repellency, chemical resistance, and heat resistance, and therefore can be used in a variety of industrial applications requiring these physical properties, such as moisture-permeable and waterproof fabrics, gas filters, liquid filters, separators for electrochemical devices, fuel cell materials, and medical materials.
Claims
1. A fiber containing fluororesin particles and water-insoluble polyvinylidene fluoride or polyimide, the fluororesin particles having a particle size of 10 to 1000 nm and contained in the fiber in a protruding state at a rate of 40 mass% or more.
2. 2. The fiber according to claim 1, wherein the fluororesin particles are polytetrafluoroethylene particles.
3. A fiber assembly comprising fibers containing fluororesin particles and a resin insoluble in water, wherein the fluororesin particles have a particle size of 10 to 1000 nm and are contained in the fibers in a protruding state at a ratio of 40 mass% or more, and wherein the contact angle of the fiber assembly with water is greater than 139°.
4. A fiber assembly as described in claim 3, wherein the water-insoluble resin is polyvinylidene fluoride or polyimide.
Citation Information
Patent Citations
Fiber excellent in low frictional characteristics and stainproofness
JP1990026919A
Electrospun porous material
JP2015511173A
Thermoplastic fiber having excellent abrasion resistance and method for producing the same
JP2020070536A