Gas Sensor Element
Porous layers in gas sensor elements address stress-induced cracks and electrode peeling, ensuring durability and accuracy under harsh conditions.
Patent Information
- Application Number
- JP2021161469
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Conventional gas sensor elements face issues with structural destruction and detection accuracy deterioration due to stress concentration at corners under harsh environments, leading to cracks and electrode peeling.
Incorporation of porous layers with specific porosity and thickness between solid electrolyte layers to act as stress buffers, preventing crack formation and electrode peeling by reducing modulus and improving adhesion.
The gas sensor element maintains functionality for a longer period without issues under harsh conditions by alleviating stress and preventing cracks and electrode detachment.
Smart Images

Figure 0007588572000003 
Figure 0007588572000004 
Figure 0007588572000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas sensor element. [Background technology]
[0002] Conventionally, there has been known a gas sensor element having a laminated structure in which first and second solid electrolyte layers are laminated via a spacer layer of a predetermined thickness made of a solid electrolyte, and a measurement gas flow section is provided between the first and second solid electrolyte layers, through which a measurement gas is introduced and flows.
[0003] For example, Patent Document 1 listed below discloses a gas sensor in which a buffer space is provided between a gas inlet and a treatment space in a measurement gas flow section. Patent Document 2 discloses a gas sensor in which a measurement electrode for detecting a specific gas concentration in a measurement gas is independently provided in a space included in the measurement gas flow section. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-237362 [Patent Document 2] JP 2015-200643 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have found that the conventional gas sensor element having the above-mentioned laminated structure has the following problems. That is, the gas sensor element may be used in a harsh environment, for example, when used as an exhaust gas sensor. It is desirable for the gas sensor element to continue to operate for a long period of time even in such a harsh environment without incurring problems such as deterioration of detection accuracy or inability to detect.
[0006] However, during repeated use of the gas sensor element, loads may occur inside the gas sensor element due to various factors. For example, stress may occur in the internal space of the gas sensor element (i.e., the measurement gas flow portion) due to changes in temperature, air pressure, etc. If this stress occurs repeatedly, the internal space of the gas sensor element may be destroyed. In particular, under severe operating conditions, this stress is likely to occur, and the internal space may be easily destroyed.
[0007] Furthermore, in the internal space, a corner is formed at the boundary between the solid electrolyte layer and the spacer. The above-mentioned stress is likely to concentrate at this corner, and as a result, cracks are likely to occur at the corner and in its vicinity. The present inventors have found that the above-mentioned causes can cause the internal space to be destroyed, which can lead to detection problems.
[0008] In one aspect, the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a gas sensor element that can be used for a relatively long period of time without any problems even under harsh operating environments. [Means for solving the problem]
[0009] In order to solve the above-mentioned problems, the present invention employs the following configuration.
[0010] A gas sensor element according to one aspect of the present invention includes a laminate having an internal space into which a gas to be measured is introduced, and one or more porous layers arranged to face the internal space. The laminate is composed of a first solid electrolyte layer, a second solid electrolyte layer, and a spacer layer. The first solid electrolyte layer and the second solid electrolyte layer are laminated in the laminate with the spacer layer interposed therebetween, so that the internal space is provided between the first solid electrolyte layer and the second solid electrolyte layer. The one or more porous layers include at least one of a first porous layer and a second porous layer, and the porosity of each of the one or more porous layers is 10% or more and 50% or less. The first porous layer is in contact with both at least one side surface of the spacer layer facing the internal space and the first solid electrolyte layer. That is, the first porous layer is arranged to face the internal space in contact with both at least one side surface of the spacer layer facing the internal space and the first solid electrolyte layer. The second porous layer is in contact with both at least one side surface of the spacer layer facing the internal space and the second solid electrolyte layer, i.e., the second porous layer is disposed in contact with both at least one side surface of the spacer layer facing the internal space and the second solid electrolyte layer and faces the internal space.
[0011] In this configuration, the first porous layer is disposed so as to face the internal space at a position corresponding to a corner of the internal space in the conventional gas sensor element, particularly a corner formed at the boundary between the spacer layer and the first solid electrolyte layer (a contact point between the spacer layer and the first solid electrolyte layer). Similarly, the second porous layer is disposed so as to face the internal space at a position corresponding to a corner of the internal space in the conventional gas sensor element, particularly a corner formed at the boundary between the spacer layer and the second solid electrolyte layer (a contact point between the spacer layer and the second solid electrolyte layer). That is, at least one of the first porous layer and the second porous layer is disposed so as to face the internal space at a position corresponding to the corner of the internal space in the conventional gas sensor element. By at least one of the first porous layer and the second porous layer disposed in this manner, that is, by the one or more porous layers, stress concentrated at a position corresponding to the corner of the internal space in the conventional gas sensor element can be alleviated.
[0012] The inventors of the present invention have confirmed through experiments (heating tests) that the one or more porous layers can suppress the occurrence of cracks by setting the porosity of each of the one or more porous layers to 50% or less. In addition, each of the one or more porous layers is set to have a porosity of 10% or more due to its "porous" nature. Therefore, the porosity of each of the one or more porous layers is set to 10% or more and 50% or less.
[0013] Therefore, the gas sensor element according to one aspect of the present invention can prevent cracks from occurring at or near the corners, which would destroy the internal space, and can be used for a relatively long period of time without any problems, even in harsh operating environments.
[0014] In one example, the first porous layer may be disposed so as to be in contact with the lower end of the side surface of the spacer layer facing the internal space and the upper surface of the first solid electrolyte layer, and to face the internal space. That is, the first porous layer facing the internal space may be disposed between the spacer layer and the first solid electrolyte layer, so as to be in contact with both and sandwiched between them. In this configuration, the first porous layer disposed between the spacer layer and the first solid electrolyte layer can reduce the Young's modulus of the gas sensor element (particularly, the laminate) and can relieve stress concentrated at and near the corners of the internal space. That is, by disposing the first porous layer as a buffer material between the spacer layer and the first solid electrolyte layer, it is possible to prevent a situation in which stress is concentrated and cracks are generated at and near the corners of the internal space.
[0015] In one example, the second porous layer may be disposed in contact with the upper end of the side surface of the spacer layer facing the internal space and the lower surface of the second solid electrolyte layer, so as to face the internal space. That is, the second porous layer facing the internal space may be disposed between the spacer layer and the second solid electrolyte layer so as to be in contact with both and sandwiched between them. In this configuration, the second porous layer disposed between the spacer layer and the second solid electrolyte layer can reduce the Young's modulus of the gas sensor element (particularly, the laminate) and can relieve stress concentrated at and near the corners of the internal space. That is, by disposing the second porous layer as a buffer material between the spacer layer and the second solid electrolyte layer, it is possible to prevent a situation in which stress is concentrated and cracks are generated at and near the corners of the internal space.
[0016] In the gas sensor element according to the above aspect, the thickness of each of the one or more porous layers may be 40 μm or less. Here, if the thickness of each of the one or more porous layers arranged to face the internal space is too large, the amount of oxygen taken in by each of the one or more porous layers increases, and the time required to pump oxygen out or in from the internal space (light-off time) increases. Therefore, in consideration of the light-off time, it is desirable to suppress the thickness of each of the one or more porous layers to a predetermined value, and the present inventors have confirmed that it is desirable to set the thickness to 40 μm or less. By setting the thickness of each of the one or more porous layers to 40 μm or less, the light-off time can be set to a range that can withstand actual use (normal use) of the gas sensor element.
[0017] In the gas sensor element according to the above aspect, the thickness of each of the one or more porous layers may be 10 μm or more. If the thickness of each of the first porous layer and the second porous layer is too thin, the effect of preventing stress concentration and suppressing the destruction (occurrence of cracks) of the internal space by at least one of the first porous layer and the second porous layer cannot be fully expected. Therefore, each of the first porous layer and the second porous layer, that is, each of the one or more porous layers, is desirably to have a predetermined thickness, and the present inventors have confirmed that it is desirable to set the thickness to 10 μm or more. According to this configuration, the effect of preventing stress concentration and suppressing the destruction (occurrence of cracks) of the internal space can be fully exhibited compared to the case where the thickness of each of the one or more porous layers is less than 10 μm.
[0018] In the gas sensor element according to the above aspect, the internal space may include one or more chambers from which oxygen is pumped in or out, and one or more of the one or more porous layers may extend into at least one of the chambers. In this case, the total volume of the portions of the one or more porous layers extending into the chambers is preferably 5% (percent) or more and 30% (percent) or less of the volume of the chambers.
[0019] Here, if the total volume of the one or more porous layers extending into the interior of the void is greater than 30% of the volume of the void, the time required to pump out or pump in oxygen from the void (light-off time) increases. In consideration of the light-off time, it is desirable to set the total volume of the one or more porous layers extending into the interior of the void to 30% or less of the volume of the void. In addition, the present inventors have confirmed through experiments (heating tests) that the occurrence of cracks can be effectively suppressed by setting the total volume of the one or more porous layers extending into the interior of the void to 5% or more of the volume of the void. Therefore, the destruction of the internal space (occurrence of cracks) can be effectively suppressed by setting the total volume of the one or more porous layers extending into the interior of the void to 5% or more and 30% or less of the volume of the void.
[0020] In the gas sensor element according to the above aspect, at least one of the one or more porous layers may be configured to include a non-exposed portion. The non-exposed portion is a portion located between the spacer layer and at least one of the first solid electrolyte layer and the second solid electrolyte layer. The non-exposed portion is in contact with both the spacer layer and at least one of the first solid electrolyte layer and the second solid electrolyte layer, and does not face the internal space. For example, the non-exposed portion is a portion disposed between the spacer layer and the first solid electrolyte layer so as to be in contact with both and sandwiched between them, and does not face the internal space. Also, for example, the non-exposed portion is a portion disposed between the spacer layer and the second solid electrolyte layer so as to be in contact with both and sandwiched between them, and does not face the internal space. When the porous layer includes the non-exposed portion, it is desirable that the volume of the non-exposed portion is 10% or more of the volume of the porous layer including the non-exposed portion.
[0021] According to this configuration, for example, the non-exposed portion is disposed between the spacer layer and the first solid electrolyte layer so as to be in contact with both and sandwiched therebetween, and the non-exposed portion can be used as a buffer between the spacer layer and the first solid electrolyte layer. However, if the volume of the non-exposed portion is made too small, the effect of the non-exposed portion as a buffer between the spacer layer and the first solid electrolyte layer is not fully exerted. Therefore, it is desirable for the non-exposed portion to have a predetermined volume. Therefore, the present inventors have repeatedly examined the volume of the non-exposed portion and confirmed that the volume of the non-exposed portion is desirably 10% or more of the volume of the porous layer including the non-exposed portion. It has also been confirmed that the volume of the non-exposed portion disposed between the spacer layer and the second solid electrolyte layer so as to be in contact with both and sandwiched therebetween is desirably 10% or more of the volume of the porous layer including the non-exposed portion. Therefore, by making the volume of the non-exposed portion 10% or more of the volume of the porous layer including the non-exposed portion, it is possible to prevent stress from concentrating and causing cracks at and near the corners of the internal space.
[0022] In the gas sensor element according to the above aspect, at least one of the one or more porous layers may overlap a portion of at least one electrode disposed in the internal space. Specifically, the porous layer may overlap at least a portion of a surface of the electrode that faces a surface in contact with at least one of the first solid electrolyte layer and the second solid electrolyte layer.
[0023] The present inventors have noticed that the following problems may occur with respect to the electrodes disposed inside the internal space. That is, when platinum (Pt) is used for the electrodes, for example, platinum oxide may be generated when the gas sensor element is used repeatedly for a long time. Since platinum oxide evaporates more easily than platinum at high temperatures, the evaporation of platinum oxide may cause peeling at the interface between the electrodes and the solid electrolyte layer (the first solid electrolyte layer or the second solid electrolyte layer) with which the electrodes are in contact. The present inventors have noticed that there is a problem in that the electrodes disposed inside the internal space may peel off from the solid electrolyte layer due to the above-mentioned causes, which may cause a malfunction in the detection of the gas sensor element. In particular, when the gas sensor element is used as an exhaust gas sensor, the electrodes disposed inside the internal space are often exposed to high temperatures, and therefore peeling from the solid electrolyte layer may easily occur.
[0024] Therefore, the inventors of the present invention have conceived of preventing the peeling of the electrode by arranging the porous layer so as to overlap at least a part of the surface of the electrode disposed inside the internal space opposite the surface that contacts the solid electrolyte layer. That is, the inventors thought that the electrode could be prevented from peeling off from the solid electrolyte layer by pressing the electrode against the solid electrolyte layer with which the electrode is in contact with the porous layer. The inventors of the present invention have confirmed through experiments (electrode peeling tests) that peeling of the electrode can be suppressed by arranging the porous layer so as to overlap at least a part of the surface of the electrode opposite the surface that contacts the solid electrolyte layer.
[0025] Therefore, with this configuration, it is possible to prevent the electrodes from peeling off from the solid electrolyte layer to which the electrodes are in contact, and it is possible to provide a gas sensor element that can be used for a relatively long period of time without any malfunctions, even under harsh operating environments.
[0026] In the gas sensor element according to the above aspect, an area of the electrode where the porous layer overlaps may be 0.5% or more and 20% or less of an area of the opposing surface of the electrode.
[0027] Here, if the ratio of the area of the electrode where the porous layer overlaps with the area of the opposing surface of the electrode is made larger than 20%, the performance of the electrode (e.g., detection accuracy, etc.) may be reduced, so the area of the electrode where the porous layer overlaps with the area of the opposing surface of the electrode is set to 20% or less.
[0028] Furthermore, the inventors of the present invention confirmed through experiments (electrode peeling tests) that peeling of the electrode can be effectively suppressed by making the area of the portion of the electrode where the porous layer overlaps 0.5% or more of the area of the opposing surface of the electrode.
[0029] In other words, by setting the area of the portion of the electrode where the porous layer overlaps to 0.5% to 20% of the area of the opposing surface of the electrode, it is possible to effectively suppress peeling of the electrode while preventing deterioration of the performance of the electrode. Therefore, according to this configuration, it is possible to provide a gas sensor element that can be used for a relatively long period of time without causing any problems, even under harsh operating conditions, by effectively suppressing peeling of the electrode while preventing deterioration of the performance of the electrode.
[0030] In the gas sensor element according to the above aspect, the content of zirconia (ZrO2) in each of the one or more porous layers may be 50 wt% or more. Here, as described above, the first porous layer is in contact with the first solid electrolyte layer, and the second porous layer is in contact with the second solid electrolyte layer. The first solid electrolyte layer and the second solid electrolyte layer are each, for example, made of an oxygen ion conductive solid electrolyte layer such as zirconia. Therefore, when each of the one or more porous layers is made of the same material as the first solid electrolyte layer and the second solid electrolyte layer, the adhesion between the first porous layer and the first solid electrolyte layer can be improved, and the adhesion between the second porous layer and the second solid electrolyte layer can be improved. Therefore, by making the content of zirconia (ZrO2) in each of the one or more porous layers 50 wt% or more, the adhesion between the first porous layer and the first solid electrolyte layer can be improved, and the adhesion between the second porous layer and the second solid electrolyte layer can be improved.
[0031] In the gas sensor element according to the above aspect, each of the one or more porous layers may be configured as an insulating layer. Effect of the Invention
[0032] According to the present invention, it is possible to provide a gas sensor element that can be used for a relatively long period of time without any problems even under severe operating conditions. [Brief description of the drawings]
[0033] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating an example of the configuration of a sensor element according to an embodiment. [Diagram 2] FIG. 2 is an enlarged view for explaining a main part of the sensor element of FIG. [Diagram 3] FIG. 3 is a cross-sectional schematic view illustrating a structure of a sensor element according to a modified example, showing an example of a first porous layer that does not extend into the measurement gas flow portion. [Figure 4]FIG. 4 is a cross-sectional schematic diagram illustrating the configuration of a sensor element according to a modified example, showing an example of a first porous layer overlapping a part of the upper surface of the measurement electrode 44. [Diagram 5] FIG. 5 is a schematic cross-sectional view illustrating a configuration of a sensor element according to a modified example, showing an example of a second porous layer in contact with the front side surface of the spacer layer facing the third internal space and the second solid electrolyte layer. [Figure 6] FIG. 6 is a cross-sectional schematic diagram illustrating a configuration of a sensor element according to a modified example, illustrating an example of a porous layer in contact with a front side surface of the spacer layer facing the third internal space, the first solid electrolyte layer, and the second solid electrolyte layer. [Figure 7] FIG. 7 is a cross-sectional schematic view illustrating an outline of the configuration of a sensor element according to a modified example, showing an example of a porous layer in contact with the right side surface of the spacer layer facing the first internal space. [Figure 8] FIG. 8 is a cross-sectional schematic view illustrating an outline of the configuration of a sensor element according to a modified example, showing an example of a porous layer in contact with the right side surface of the spacer layer facing the second internal space. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Hereinafter, an embodiment according to one aspect of the present invention (hereinafter, also referred to as "the present embodiment") will be described with reference to the drawings. However, the present embodiment described below is merely an example of the present invention in every respect. It goes without saying that various improvements and modifications can be made without departing from the scope of the present invention. In other words, in implementing the present invention, a specific configuration according to the embodiment may be appropriately adopted.
[0035] [Configuration example] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of the gas sensor element 100 according to the present embodiment. The gas sensor element 100 has, for example, a long and narrow plate shape extending along the longitudinal direction (axial direction) and is formed into, for example, a rectangular parallelepiped shape. The gas sensor element 100 shown in FIG. 1 has a front end and a rear end as ends in the longitudinal direction, and in the following description, the front end is the end on the left side of FIG. 1 (i.e., the front end), and the rear end is the end on the right side of FIG. 1 (i.e., the rear end). However, the shape of the gas sensor element 100 is not limited to this example and may be appropriately selected depending on the embodiment. In the following description, the back side of the paper in FIG. 1 is the right side of the gas sensor element 100, and the front side of the paper is the left side of the gas sensor element 100.
[0036] The gas sensor element 100 has a structure in which six layers, a first substrate layer 1, a second substrate layer 2, a third substrate layer 3, a first solid electrolyte layer 4, a spacer layer 5, and a second solid electrolyte layer 6, each of which is made of an oxygen ion conductive solid electrolyte layer such as zirconia (ZrO2), are laminated in this order from the bottom in the cross-sectional view of FIG. 1. That is, the gas sensor element 100 includes a laminated body made of the first solid electrolyte layer 4, the second solid electrolyte layer 6, and the spacer layer 5. The solid electrolytes forming the six layers, the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6, may be dense. The term "dense" refers to a porosity of 5% or less.
[0037] The gas sensor element 100 is manufactured, for example, by performing processes such as predetermined processing and printing of wiring patterns on ceramic green sheets corresponding to each layer, stacking them, and further firing them to integrate them. As an example, the gas sensor element 100 is a laminate of a plurality of ceramic layers. In this embodiment, the upper surface of the second solid electrolyte layer 6 constitutes the upper surface of the gas sensor element 100, the lower surface of the first substrate layer 1 constitutes the lower surface of the gas sensor element 100, and each side surface of the layers 1 to 6 constitutes each side surface of the gas sensor element 100.
[0038] At one tip portion of the gas sensor element 100, between the lower surface of the second solid electrolyte layer 6 and the upper surface of the first solid electrolyte layer 4, a gas inlet 10, a first diffusion rate-controlling portion 11, a buffer space 12, a second diffusion rate-controlling portion 13, a first internal void 20, a third diffusion rate-controlling portion 30, a second internal void 40, a fourth diffusion rate-controlling portion 16, and a third internal void 17 are formed adjacent to each other and communicated with each other in this order.
[0039] The gas inlet 10, the buffer space 12, the first internal space 20, the second internal space 40, and the third internal space 17 are spaces provided by hollowing out the spacer layer 5, and are spaces (internal spaces) within the gas sensor element 100 that are bounded at the top by the underside of the second solid electrolyte layer 6 and at the bottom by the upper surface of the first solid electrolyte layer 4.
[0040] The first diffusion rate-controlling section 11 is provided as two horizontally elongated slits (the opening has a long side direction perpendicular to the drawing). The second diffusion rate-controlling section 13, the third diffusion rate-controlling section 30, and the fourth diffusion rate-controlling section 16 are each provided as a hole whose length extending in the direction perpendicular to the drawing is shorter than that of the first internal space 20, the second internal space 40, and the third internal space 61, respectively.
[0041] As illustrated in FIG. 1, the second diffusion rate-controlling section 13 and the third diffusion rate-controlling section 30 may be provided as two horizontally elongated slits (the opening has a long side direction perpendicular to the drawing) similar to the first diffusion rate-controlling section 11. In contrast, the fourth diffusion rate-controlling section 16 may be provided as one horizontally elongated slit (the opening has a longitudinal direction perpendicular to the drawing) formed as a gap with the lower surface of the second solid electrolyte layer 6. That is, the fourth diffusion rate-controlling section 16 may be in contact with the upper surface of the first solid electrolyte layer 4. The second diffusion rate-controlling section 13, the third diffusion rate-controlling section 30, and the fourth diffusion rate-controlling section 16 will be described in detail later. The portion (internal space) from the gas inlet 10 to the third internal space 17 is referred to as the measurement gas flow section 8.
[0042] 1, the rear side of the measurement gas flow section 8 (specifically, the third internal space 17) is blocked by a front side surface 59f of the spacer layer 5 and a side surface of the first porous layer 7a in contact with the lower end of the front side surface 59f, the side surface facing the third internal space 17. As will be described in detail later, at least one side surface (at least one of the front side, rear side, right side, and left side) of the measurement gas flow section 8 is blocked by the spacer layer 5 and the porous layer 7. Specifically, at least one side surface of the measurement gas flow section 8 is blocked by the side surface 59 of the spacer layer 5 and a surface of the porous layer 7 in contact with the end (lower end, upper end) of the side surface 59, the surface facing the measurement gas flow section 8.
[0043] The first porous layer 7a (porous layer 7) is a porous layer, and "porous" refers to a porosity of 10% or more. The porous layer 7 may be made of a material containing a large amount of zirconia (ZrO2), and the zirconia content may be 50 wt% or more. The porous layer 7 may also be configured as an insulating layer. The thickness of the porous layer 7 is, for example, 10 μm or more and 40 μm or less.
[0044] The porous layer 7 is disposed so as to face the measurement gas flow section 8, and in the example shown in FIG. 1, the first porous layer 7a is disposed so as to face the measurement gas flow section 8, particularly so as to face the third internal space 17. The porous layer 7 also contacts at least one side surface 59 of the spacer layer 5, particularly the end (lower end, upper end) of at least one side surface 59 of the spacer layer 5. In the example shown in FIG. 1, the first porous layer 7a contacts the front side surface 59f of the spacer layer 5, particularly the lower end of the front side surface 59f of the spacer layer 5. The porous layer 7 also contacts at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6, particularly facing at least one of the upper surface of the first solid electrolyte layer 4 and the lower surface of the second solid electrolyte layer 6. In the example shown in FIG. 1, the first porous layer 7a contacts the first solid electrolyte layer 4, particularly facing the upper surface of the first solid electrolyte layer 4. In this way, at least one of the sides of the measurement gas flow section 8 is blocked by the side surface 59 of the spacer layer 5 and the surface of the porous layer 7 facing the measurement gas flow section 8. In the example shown in Fig. 1, the rear side of the measurement gas flow section 8 (i.e., the rear side of the third internal space 17) is blocked by the front side surface 59f of the spacer layer 5 and the surface of the first porous layer 7a in contact with the front side surface 59f of the spacer layer 5 facing the measurement gas flow section 8.
[0045] A reference gas introduction space 43 is provided between the upper surface of the third substrate layer 3 and the lower surface of the spacer layer 5 at a position farther from the tip side (front side of the gas sensor element 100) than the measurement gas flow section 8, and at a position defined by the side surface of the first solid electrolyte layer 4. A reference gas such as the atmosphere is introduced into the reference gas introduction space 43. However, the configuration of the gas sensor element 100 is not limited to this example. As another example, the first solid electrolyte layer 4 may be configured to extend to the rear end of the gas sensor element 100, and the reference gas introduction space 43 may be omitted. In this case, the atmosphere introduction layer 48 may be configured to extend to the rear end of the gas sensor element 100.
[0046] The air introducing layer 48 is made of porous alumina, and is configured so that the reference gas is introduced through the reference gas introducing space 43. In addition, the air introducing layer 48 is formed so as to cover the reference electrode 42.
[0047] The reference electrode 42 is formed so as to be sandwiched between the upper surface of the third substrate layer 3 and the first solid electrolyte layer 4, and is surrounded by an air introduction layer 48 connected to the reference gas introduction space 43. The reference electrode 42 is used to measure the oxygen concentrations (oxygen partial pressures) in the first internal space 20, the second internal space 40, and the third internal space 17. Details will be described later.
[0048] The gas inlet 10 is a portion of the measurement gas flow section 8 that opens to the external space. The measurement gas is introduced into the gas sensor element 100 from the external space through the gas inlet 10. In this embodiment, as illustrated in FIG. 1, the gas inlet 10 is disposed on the front surface of the gas sensor element 100. That is, the measurement gas flow section 8 is configured to have an opening on the front surface of the gas sensor element 100. However, it is not essential that the measurement gas flow section 8 has an opening on the front surface of the gas sensor element 100, that is, that the gas inlet 10 is disposed on the front surface of the gas sensor element 100. As long as the gas sensor element 100 can introduce the measurement gas from the external space into the measurement gas flow section 8, the gas inlet 10 may be disposed on the right surface or the left surface of the gas sensor element 100, for example.
[0049] When the gas inlet 10 is disposed on the front surface of the gas sensor element 100, the measurement gas flow section 8 may be blocked by a dense ceramic layer on each side surface (right side surface and left side surface) of the gas sensor element 100. The ceramic layer may be made of a material such as zirconia (ZrO2). When the measurement gas flow section 8 is blocked by a dense ceramic layer on each side surface of the gas sensor element 100, the gas sensor element 100 is configured to take in the measurement gas from the external space into the gas sensor element 100 through the gas inlet 10.
[0050] However, it is not essential for the gas sensor element 100 to block the measurement gas flow portion 8 on each side of the gas sensor element 100 with a dense ceramic layer. Also, it is not essential for the gas sensor element 100 to have the gas inlet 10. That is, it is sufficient for the gas sensor element 100 to be able to take in the measurement gas from the external space into the measurement gas flow portion 8, and it is not essential for the gas sensor element 100 to take in the measurement gas from the external space through the gas inlet 10. For example, the gas sensor element 100 may take in the measurement gas from the external space into the measurement gas flow portion 8 without providing the gas inlet 10 by leaving at least one of the side surfaces 59 of the spacer layer 5 open instead of being blocked by a dense ceramic layer.
[0051] The first diffusion rate-controlling portion 11 is a portion that applies a predetermined diffusion resistance to the measurement gas taken in through the gas inlet 10.
[0052] The buffer space 12 is a space provided for guiding the measurement gas introduced from the first diffusion rate-controlling portion 11 to the second diffusion rate-controlling portion 13 .
[0053] The second diffusion rate-controlling portion 13 is a portion that imparts a predetermined diffusion resistance to the measurement gas introduced from the buffer space 12 into the first internal space 20 .
[0054] When the measurement gas is introduced from the outside of the gas sensor element 100 into the first internal space 20, the measurement gas is suddenly taken into the gas sensor element 100 from the gas inlet 10 due to pressure fluctuations of the measurement gas in the external space (exhaust pressure pulsations if the measurement gas is automobile exhaust gas), but is not introduced directly into the first internal space 20, but is introduced into the first internal space 20 after the concentration fluctuations of the measurement gas are canceled through the first diffusion rate-controlling part 11, the buffer space 12, and the second diffusion rate-controlling part 13. As a result, the concentration fluctuations of the measurement gas introduced into the first internal space can be almost negligible.
[0055] The first internal space 20 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the second diffusion rate-controlling part 13. The oxygen partial pressure is adjusted by the operation of the main pump cell 21.
[0056] The main pump cell 21 is an electrochemical pump cell including an inner pump electrode 22 having a ceiling electrode portion 22a provided over almost the entire lower surface of the second solid electrolyte layer 6 facing the first internal space 20, an outer pump electrode 23 provided in a region corresponding to the ceiling electrode portion 22a on the upper surface of the second solid electrolyte layer 6 (the upper surface of the gas sensor element 100) so as to be exposed to the external space, and the second solid electrolyte layer 6 sandwiched between these electrodes.
[0057] The inner pump electrode 22 is formed across the upper and lower solid electrolyte layers (the second solid electrolyte layer 6 and the first solid electrolyte layer 4) that define the first internal space 20, and the spacer layer 5 that provides the side walls. Specifically, a ceiling electrode portion 22a is formed on the lower surface of the second solid electrolyte layer 6 that provides the ceiling surface of the first internal space 20, and a bottom electrode portion 22b is formed on the upper surface of the first solid electrolyte layer 4 that provides the bottom surface. Then, side electrode portions (not shown) are formed on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side wall portions of the first internal space 20 so as to be connected to the ceiling electrode portion 22a and the bottom electrode portion 22b. That is, the inner pump electrode 22 is arranged in a tunnel-shaped structure at the arrangement portion of the side electrode portion.
[0058] The inner pump electrode 22 and the outer pump electrode 23 are formed as porous cermet electrodes (for example, cermet electrodes made of Pt and ZrO2 containing 1% Au). The inner pump electrode 22, which comes into contact with the measurement gas, is used to measure nitrogen oxides (NO x ) are formed using materials that have weakened reducing ability against the components.
[0059] The gas sensor element 100 is configured to be able to pump oxygen from within the first internal space 20 to the external space or pump oxygen from the external space into the first internal space 20 by applying a desired pump voltage Vp0 between the inner pump electrode 22 and the outer pump electrode 23 in the main pump cell 21 and flowing a pump current Ip0 in a positive or negative direction between the inner pump electrode 22 and the outer pump electrode 23. When oxygen from within the first internal space 20 is pumped to the external space, the pumped oxygen is discharged from the outer pump electrode 23.
[0060] In addition, in order to detect the oxygen concentration (oxygen partial pressure) in the atmosphere in the first internal space 20, the inner pump electrode 22, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42 constitute an oxygen partial pressure detection sensor cell 80 for controlling the main pump (i.e., an electrochemical sensor cell).
[0061] The gas sensor element 100 is configured to be able to identify the oxygen concentration (oxygen partial pressure) in the first internal space 20 by measuring the electromotive force V0 in the main pump control oxygen partial pressure detection sensor cell 80. Furthermore, the pump current Ip0 is controlled by feedback controlling Vp0 so that the electromotive force V0 is constant. This allows the oxygen concentration in the first internal space 20 to be kept at a predetermined constant value.
[0062] The third diffusion rate-controlling section 30 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the main pump cell 21 in the first internal space 20, and guides the measurement gas to the second internal space 40.
[0063] In the second internal space 40, the gas sensor element 100 is configured such that, after the oxygen concentration (oxygen partial pressure) is previously adjusted in the first internal space 20, the oxygen partial pressure of the measurement gas introduced through the third diffusion rate-controlling part is further adjusted by the auxiliary pump cell 50. This makes it possible to keep the oxygen concentration in the second internal space 40 constant with high accuracy, and therefore, in the gas sensor element 100, it is possible to perform highly accurate NO x It becomes possible to measure the concentration.
[0064] The auxiliary pump cell 50 is an auxiliary electrochemical pump cell including an auxiliary pump electrode 51, an outer pump electrode 23 (not limited to the outer pump electrode 23, but a gas sensor element 100 and an appropriate outer electrode will suffice), and a second solid electrolyte layer 6. The auxiliary pump electrode 51 has a ceiling electrode portion 51a provided on substantially the entire lower surface of the second solid electrolyte layer 6 facing the second internal space 40.
[0065] The auxiliary pump electrode 51 is disposed in the second internal space 40 in a tunnel-shaped structure similar to the inner pump electrode 22 provided in the first internal space 20. That is, a ceiling electrode portion 51a is formed on the second solid electrolyte layer 6 that provides the ceiling surface of the second internal space 40, and a bottom electrode portion 51b is formed on the first solid electrolyte layer 4 that provides the bottom surface of the second internal space 40. Side electrode portions (not shown) that connect the ceiling electrode portion 51a and the bottom electrode portion 51b are formed on both wall surfaces of the spacer layer 5 that provides the side walls of the second internal space 40. As a result, the auxiliary pump electrode 51 has a tunnel-shaped structure.
[0066] Like the inner pump electrode 22, the auxiliary pump electrode 51 is also made of a material with a weakened ability to reduce nitrogen oxide components in the measurement gas.
[0067] The gas sensor element 100 is configured so that, by applying a desired voltage Vp1 between the auxiliary pump electrode 51 and the outer pump electrode 23 in the auxiliary pump cell 50, oxygen in the atmosphere within the second internal space 40 can be pumped out to the external space or pumped in from the external space into the second internal space 40.
[0068] In addition, in order to control the oxygen partial pressure in the atmosphere within the second internal space 40, the auxiliary pump electrode 51, the reference electrode 42, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, and the third substrate layer 3 constitute an oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump (i.e., an electrochemical sensor cell).
[0069] The auxiliary pump cell 50 pumps with the variable power supply 52, the voltage of which is controlled based on the electromotive force V1 detected by the auxiliary pump control oxygen partial pressure detection sensor cell 81. As a result, the oxygen partial pressure in the atmosphere in the second internal space 40 is adjusted to NO x The partial pressure is controlled to a low level that has virtually no effect on the measurement of
[0070] In addition, the pump current Ip1 is used to control the electromotive force of the main pump control oxygen partial pressure detection sensor cell 80. Specifically, the pump current Ip1 is input as a control signal to the main pump control oxygen partial pressure detection sensor cell 80, and the electromotive force V0 is controlled so that the gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling portion 30 into the second internal space 40 is always constant. x When used as a sensor, the oxygen concentration in the second internal space 40 is maintained at a constant value of about 0.001 ppm by the action of the main pump cell 21 and the auxiliary pump cell 50.
[0071] The fourth diffusion rate-controlling section 16 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the auxiliary pump cell 50 in the second internal space 40, and guides the measurement gas to the third internal space 17. The fourth diffusion rate-controlling section 16 controls the NO x It plays a role in limiting the amount of
[0072] The third internal space 17 is configured to adjust the oxygen concentration (oxygen partial pressure) in advance in the second internal space 40, and then to adjust the nitrogen oxide (NO x The space is provided for carrying out the process related to the measurement of NO concentration. x The concentration is measured primarily by the operation of the measuring pump cell 41 in the third internal space 17 .
[0073] In the third internal space 17 illustrated in Figure 1, the rear side of the third internal space 17 is blocked by the front side 59f of the spacer layer 5 and the surface of the first porous layer 7a in contact with the front side 59f of the spacer layer 5 that faces the measured gas flow section 8 (third internal space 17).
[0074] The measuring pump cell 41 detects NO in the measurement gas in the third internal space 17. x The concentration is measured. The measurement pump cell 41 is an electrochemical pump cell including a measurement electrode 44, an outer pump electrode 23, a second solid electrolyte layer 6, a spacer layer 5, and a first solid electrolyte layer 4. The measurement electrode 44 is provided on the upper surface of the first solid electrolyte layer 4 facing the third internal space 17, at a position spaced apart from the third diffusion rate-controlling part 30.
[0075] The measurement electrode 44 is a porous cermet electrode. x The measurement electrode 44 is made of a material having a higher reduction ability for the NOx component than the inner pump electrode 22. x Reduce NO x It also functions as a reduction catalyst.
[0076] The gas sensor element 100 is configured so that the measurement pump cell 41 can pump out oxygen produced by decomposition of nitrogen oxides in the atmosphere surrounding the measurement electrode 44, and detect the amount of oxygen produced as a pump current Ip2.
[0077] In order to detect the oxygen partial pressure around the measurement electrode 44, a measurement pump control oxygen partial pressure detection sensor cell 82 (i.e., an electrochemical sensor cell) is configured by the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the measurement electrode 44, and the reference electrode 42. The variable power supply 46 is controlled based on the voltage (electromotive force) V2 detected by the measurement pump control oxygen partial pressure detection sensor cell 82.
[0078] The measurement gas introduced into the second internal space 40 reaches the measurement electrode 44 in the third internal space 17 through the fourth diffusion rate-controlling part 16 under the condition that the oxygen partial pressure is controlled. Nitrogen oxides in the measurement gas around the measurement electrode 44 are reduced (2NO→N2+O2) to generate oxygen. The generated oxygen is then pumped by the measurement pump cell 41, and the voltage Vp2 of the variable power supply is controlled so that the control voltage V2 detected by the measurement pump control oxygen partial pressure detection sensor cell 82 is constant. The amount of oxygen generated around the measurement electrode 44 is proportional to the concentration of nitrogen oxides in the measurement gas, so that the pump current Ip2 in the measurement pump cell 41 is used to calculate the nitrogen oxide concentration in the measurement gas.
[0079] In addition, the measurement electrode 44, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42 are combined to form an electrochemical sensor cell to form an oxygen partial pressure detection means, thereby detecting NO in the atmosphere around the measurement electrode 44. x It is possible to detect the electromotive force corresponding to the difference between the amount of oxygen generated by the reduction of the components and the amount of oxygen contained in the reference atmosphere, which makes it possible to determine the concentration of nitrogen oxide components in the measurement gas.
[0080] An electrochemical sensor cell 83 is formed by the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the outer pump electrode 23, and the reference electrode 42. The gas sensor element 100 is configured to be able to detect the oxygen partial pressure in the measurement gas outside the sensor by the electromotive force Vref obtained by the sensor cell 83.
[0081] In the gas sensor element 100 having the above-mentioned configuration, the main pump cell 21 and the auxiliary pump cell 50 are operated to always maintain the oxygen partial pressure at a constant low value (NO x Therefore, the gas sensor element 100 can detect the NO concentration in the measurement gas in a manner substantially proportional to the concentration of nitrogen oxides in the measurement gas. xThe nitrogen oxide concentration in the measurement gas can be determined based on a pump current Ip2 that flows when oxygen generated by reduction of the nitrogen oxide is pumped out of the measurement pump cell 41.
[0082] Furthermore, the gas sensor element 100 includes a heater 70 that adjusts the temperature by heating and keeping the gas sensor element 100 warm in order to increase the oxygen ion conductivity of the solid electrolyte. In the example of Fig. 1, the heater 70 further includes a heater electrode 701, a heat generating portion 702, a lead portion 73, a heater insulating layer 74, and a pressure release hole 75. The lead portion 73 may be formed of a through hole.
[0083] In this embodiment, the heater 70 is disposed on the lower surface side of the gas sensor element 100, facing the upper surface of the gas sensor element 100. That is, the heater 70 is disposed at a position closer to the lower surface of the gas sensor element 100 than to the upper surface of the gas sensor element 100 in the thickness direction (vertical direction / stacking direction) of the gas sensor element 100.
[0084] The heater electrode 701 is an electrode formed in a manner to contact the lower surface (the lower surface of the gas sensor element 100) of the first substrate layer 1. By connecting the heater electrode 701 to an external power supply, it is possible to supply power to the heater 70 from the outside.
[0085] The heating portion 702 is an electric resistor sandwiched between the second substrate layer 2 and the third substrate layer 3. The heating portion 702 is connected to a heater electrode 701 via a lead portion 73, and generates heat when power is supplied from the outside through the heater electrode 701, thereby heating and keeping warm the solid electrolyte that constitutes the gas sensor element 100.
[0086] Moreover, the heat generating portion 702 is embedded throughout the entire area from the first internal space 20 to the second internal space 40, making it possible to adjust the temperature of the entire gas sensor element 100 to a temperature at which the solid electrolyte is activated.
[0087] Heater insulating layer 74 is an insulating layer made of an insulator such as alumina formed on the upper and lower surfaces of heat generating portion 702. Heater insulating layer 74 is formed for the purpose of obtaining electrical insulation between second substrate layer 2 and heat generating portion 702, and between third substrate layer 3 and heat generating portion 702.
[0088] The pressure relief hole 75 is a portion that penetrates the third substrate layer 3 and is provided so as to communicate with the reference gas introduction space 43, and is formed for the purpose of mitigating the increase in internal pressure that accompanies an increase in temperature within the heater insulation layer 74.
[0089] <Porous layer> Fig. 2 is an enlarged view for explaining a main part of the gas sensor element 100 of Fig. 1. Specifically, Fig. 2 is a view showing the details of the first porous layer 7a (porous layer 7) closing the rear side of the third internal space 17 (measurement gas flow portion 8) and the spacer layer 5. As described above, the porous layer 7 is a porous layer having a porosity of 10% or more.
[0090] 2 faces the measured gas flow section 8 (third internal space 17) and is in contact with both a front side surface 59f of the spacer layer 5, which is a surface facing the measured gas flow section 8, and the first solid electrolyte layer 4. That is, the first porous layer 7a faces the measured gas flow section 8 and is in contact with a lower end of the front side surface 59f of the spacer layer 5 and an upper surface of the first solid electrolyte layer 4. In other words, the first porous layer 7a is in contact with a lower end of the front side surface 59f of the spacer layer 5 and faces the measured gas flow section 8 and the upper surface of the first solid electrolyte layer 4.
[0091] The first porous layer 7a facing the measured gas flow section 8 is disposed between the spacer layer 5 and the first solid electrolyte layer 4 so as to be in contact with and sandwiched between them, and the following effects can be expected. That is, the first porous layer 7a disposed between the spacer layer 5 and the first solid electrolyte layer 4 is expected to reduce the Young's modulus of the gas sensor element 100 (particularly, of the laminate) and to relieve stress concentrated at and near the corners of the measured gas flow section 8. That is, by disposing the first porous layer 7a as a buffer material between the spacer layer 5 and the first solid electrolyte layer 4, it is expected to prevent a situation in which stress is concentrated and cracks are generated at and near the corners of the measured gas flow section 8.
[0092] As will be described in detail later, the present inventors have confirmed through experiments (temperature rise tests) that in order to fully exert the crack suppression effect of the first porous layer 7a (porous layer 7), the porosity of the first porous layer 7a is preferably 50% or less. As described above, the porosity of the first porous layer 7a (porous layer 7) is 10% or more, and therefore, by disposing the first porous layer 7a having a porosity of 10% or more and 50% or less at the positions exemplified in Figures 1 and 2, it is possible to suppress the occurrence of cracks (destruction of the measurement gas flow section 8).
[0093] Here, in the gas sensor element 100, the thickness of the first porous layer 7a (porous layer 7) is, for example, 40 μm or less. If the thickness of the first porous layer 7a arranged to face the measurement gas flow section 8 is too large, the amount of oxygen taken in by the first porous layer 7a increases, and the time required for pumping out or pumping in oxygen from the measurement gas flow section 8 (particularly the void space (the third internal void space 17 in the example of FIG. 1) facing the first porous layer 7a) becomes long (light-off time). Therefore, in consideration of the light-off time, it is desirable to suppress the thickness of the first porous layer 7a to a predetermined value, and the present inventors have confirmed that it is desirable to make it 40 μm or less. By making the thickness of the first porous layer 7a 40 μm or less, the light-off time can be made within a range that can withstand actual use (normal use) of the gas sensor element 100.
[0094] In the gas sensor element 100, the thickness of the first porous layer 7a (porous layer 7) is, for example, 10 μm or more. If the thickness of the first porous layer 7a is too thin, the effect of preventing stress concentration and suppressing damage (occurrence of cracks) of the measurement gas flow section 8 by the first porous layer 7a cannot be fully expected. For this reason, the first porous layer 7a desirably has a predetermined thickness, and the present inventors have confirmed that a thickness of 10 μm or more is desirable. With this configuration, the effect of preventing stress concentration and suppressing damage (occurrence of cracks) of the measurement gas flow section 8 can be fully exhibited compared to a case in which the thickness of the first porous layer 7a (porous layer 7) is less than 10 μm.
[0095] In the gas sensor element 100, the first porous layer 7a (porous layer 7) may be configured as a porous layer having a zirconia (ZrO2) content of 50 wt% or more. As described above, the first porous layer 7a is in contact with the first solid electrolyte layer 4. The first solid electrolyte layer 4 is configured of an oxygen ion conductive solid electrolyte layer such as zirconia. Therefore, when the first porous layer 7a is made of the same material as the first solid electrolyte layer 4, the adhesion between the first porous layer 7a and the first solid electrolyte layer 4 can be improved. Therefore, by making the zirconia content in the first porous layer 7a 50 wt% or more, the adhesion between the first porous layer 7a and the first solid electrolyte layer 4 can be improved.
[0096] In the gas sensor element 100, the first porous layer 7a (porous layer 7) may be configured as, for example, an insulating layer.
[0097] The first porous layer 7a, which is disposed between the lower end of the front side surface 59f of the spacer layer 5 and the upper surface of the first solid electrolyte layer 4 so as to be in contact with and sandwiched between them as illustrated in Fig. 2, is formed, for example, as follows. That is, an adhesive layer including the porous layer 7 is used as an adhesive layer that bonds the upper surface of the first solid electrolyte layer 4 and the lower surface of the spacer layer 5. Then, the adhesive layer (porous layer 7) may be left in a portion of the spacer layer 5 located at the lower end of the front side surface 59f facing the measurement gas flow section 8 (third internal space 17) (and its periphery) to form the first porous layer 7a as illustrated in Fig. 2.
[0098] That is, the first porous layer 7a may be formed by leaving an adhesive layer including the porous layer 7 that bonds the upper surface of the first solid electrolyte layer 4 and the lower surface of the spacer layer 5 in a portion (and its surroundings) located at the lower end of one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8.
[0099] 2, the first porous layer 7a faces the measurement gas flow section 8 (third internal space 17) in a state where it is sandwiched between the lower end of the front side surface 59f of the spacer layer 5 and the upper surface of the first solid electrolyte layer 4 and in contact with both. The first porous layer 7a may be considered to face the measurement gas flow section 8 in a state where it is sandwiched between the lower end of the front side surface 59f of the spacer layer 5 and the upper surface of the first solid electrolyte layer 4 so that they do not come into contact with each other.
[0100] 1, in the gas sensor element 100, the measurement gas flow section 8 includes one or more chambers where oxygen is pumped in or out, such as the first internal space 20, the second internal space 40, and the third internal space 17. The first porous layer 7a shown in FIG. 2 includes an exposed portion 71 that faces the third internal space 17, and a non-exposed portion 72 that does not face the third internal space 17.
[0101] The exposed portion 71 is a portion extending into the inside of the measurement gas flow section 8 (third internal space 17), that is, a portion exposed to the inside of the measurement gas flow section 8 (third internal space 17). The exposed portion 71 illustrated in FIG. 2 extends into the inside of the measurement gas flow section 8 (third internal space 17) and contacts both the front side surface 59f of the spacer layer 5 and the first solid electrolyte layer 4. In other words, the exposed portion 71 contacts the lower end of the front side surface 59f of the spacer layer 5 and faces the measurement gas flow section 8 and the upper surface of the first solid electrolyte layer 4. The exposed portion 71 is a portion extending into the inside of the measurement gas flow section 8 from a position where the end (lower end, upper end) of the side surface 59 of the spacer layer 5 facing the measurement gas flow section 8 contacts the surface of the porous layer 7 facing the measurement gas flow section 8. The exposed portion 71 illustrated in FIG. 2 extends from a position where the lower end of the front side surface 59f of the spacer layer 5 contacts the surface of the porous layer 7 facing the measured gas flow portion 8, into the inside of the measured gas flow portion 8, and faces the upper surface of the first solid electrolyte layer 4.
[0102] In the first porous layer 7a illustrated in FIG. 2, the volume of the exposed portion 71 extending into the third inner space 17 is, for example, 5% or more and 30% or less of the volume of the third inner space 17.
[0103] In the first porous layer 7a illustrated in FIG. 2, if the volume of the exposed portion 71 is made larger than 30% of the volume of the third internal space 17, the time required to pump out or pump in oxygen from the third internal space 17 (light-off time) increases. In consideration of the light-off time, it is preferable that the volume of the exposed portion 71 of the first porous layer 7a is 30% or less of the volume of the third internal space 17. Furthermore, the present inventors confirmed through an experiment (heating test) described later that the occurrence of cracks can be effectively suppressed by making the volume of the exposed portion 71 of the first porous layer 7a 5% or more of the volume of the third internal space 17. Therefore, by making the volume of the exposed portion 71 of the first porous layer 7a 5% or more and 30% or less of the volume of the third internal space 17, the destruction (occurrence of cracks) of the measurement gas flow section 8 can be effectively suppressed.
[0104] The non-exposed portion 72 is a portion of the porous layer 7 located between the spacer layer 5 and the first solid electrolyte layer 4, which is in contact with (facing) both the spacer layer 5 and the first solid electrolyte layer 4 and does not face the measured gas flow section 8 (third internal space 17). The non-exposed portion 72 illustrated in FIG. 2 is sandwiched between the spacer layer 5 and the first solid electrolyte layer 4. The non-exposed portion 72 is a portion extending from a position where the end (lower end, upper end) of the side surface 59 of the spacer layer 5 facing the measured gas flow section 8 contacts the surface of the porous layer 7 facing the measured gas flow section 8 into the spacer layer 5. The non-exposed portion 72 illustrated in FIG. 2 extends from a position where the lower end of the front side surface 59f of the spacer layer 5 contacts the surface of the porous layer 7 facing the measured gas flow section 8 into the spacer layer 5 and faces the upper surface of the first solid electrolyte layer 4.
[0105] According to this configuration, for example, by disposing non-exposed portion 72 between spacer layer 5 and first solid electrolyte layer 4 so as to be in contact with both and sandwiched between them, non-exposed portion 72 can be used as a buffer material between spacer layer 5 and first solid electrolyte layer 4.
[0106] However, if the volume of the non-exposed portion 72 is made too small, the effect of the non-exposed portion 72 as a buffer between the spacer layer 5 and the first solid electrolyte layer 4 is not fully exhibited. Therefore, it is preferable that the non-exposed portion 72 has a predetermined volume. Therefore, the inventors of the present invention have repeatedly examined the volume of the non-exposed portion 72 and confirmed that the volume of the non-exposed portion 72 is preferably 10% or more of the volume of the porous layer 7 including the non-exposed portion 72.
[0107] Therefore, in the first porous layer 7a illustrated in Fig. 2, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the first porous layer 7a illustrated in Fig. 2. Therefore, by making the volume of the non-exposed portion 72 10% or more of the volume of the porous layer 7 including the non-exposed portion 72, it is possible to prevent a situation in which cracks are generated at or near the corners of the measurement gas flow portion 8 due to stress concentration.
[0108] In addition, the second porous layer 7b (porous layer 7) described below using FIG. 5 and the like has a porosity of 10% or more and 50% or less, and a thickness of 10 μm or more and 40 μm or less, similar to the first porous layer 7a. Similarly to the first porous layer 7a, the second porous layer 7b (porous layer 7) may be configured as a porous layer having a zirconia content of 50 wt% or more, or may be configured as an insulating layer. Furthermore, similar to the first porous layer 7a, when the second porous layer 7b (porous layer 7) includes a non-exposed portion 72, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the porous layer 7 (second porous layer 7b) including the non-exposed portion 72.
[0109] 1 and 2 show an example of the first porous layer 7a (porous layer 7) facing the third internal space 17 (measurement gas flow section 8) and in contact with the front side surface 59f of the spacer layer 5. However, the porous layer 7 facing the third internal space 17 may be in contact with at least one of the right side surface 59r and the left side surface 59l of the spacer layer 5 that defines the third internal space 17 (measurement gas flow section 8). In addition, when the gas inlet 10 is not disposed on the front surface of the gas sensor element 100, the porous layer 7 facing the measurement gas flow section 8 may be in contact with the rear side surface 59b of the spacer layer 5 that defines the front side of the measurement gas flow section 8.
[0110] <Features> 1, the gas sensor element 100 includes a laminate in which a measurement gas flow section 8, which is an internal space into which a measurement gas is introduced, is provided, and one or more porous layers 7 arranged to face the measurement gas flow section 8. The laminate is composed of a first solid electrolyte layer 4, a second solid electrolyte layer 6, and a spacer layer 5. In the laminate, the first solid electrolyte layer 4 and the second solid electrolyte layer 6 are laminated with the spacer layer 5 interposed therebetween, so that the measurement gas flow section 8 is provided between the first solid electrolyte layer 4 and the second solid electrolyte layer 6.
[0111] The one or more porous layers 7 of the gas sensor element 100 arranged to face the measured gas flow section 8 include at least one of a first porous layer 7a as illustrated in Figs. 1 and 2 and a second porous layer 7b as described with reference to Figs. 5, 7 and 8. The first porous layer 7a contacts both at least one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8 (e.g., any one of the front side surface 59f, the rear side surface 59b, the right side surface 59r and the left side surface 59l) and the first solid electrolyte layer 4. That is, the first porous layer 7a is arranged to face the measured gas flow section 8 while contacting both at least one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8 and the first solid electrolyte layer 4. The second porous layer 7b is in contact with both at least one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8 (for example, any one of the front side surface 59f, the rear side surface 59b, the right side surface 59r, and the left side surface 59l) and the second solid electrolyte layer 6. That is, the second porous layer 7b is in contact with both at least one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8 and the second solid electrolyte layer 6, and is disposed so as to face the measured gas flow section 8. The porosity of each of the one or more porous layers 7 included in the gas sensor element 100 is 10% or more and 50% or less.
[0112] In this configuration, the first porous layer 7a is disposed so as to face the internal space at a position corresponding to a corner of the internal space in the conventional gas sensor element, particularly a corner formed at the boundary between the spacer layer and the first solid electrolyte layer (a contact point between the spacer layer and the first solid electrolyte layer). Similarly, the second porous layer 7b is disposed so as to face the internal space at a position corresponding to a corner of the internal space in the conventional gas sensor element, particularly a corner formed at the boundary between the spacer layer and the second solid electrolyte layer (a contact point between the spacer layer and the second solid electrolyte layer). That is, at least one of the first porous layer 7a and the second porous layer 7b is disposed so as to face the internal space at a position corresponding to the corner of the internal space in the conventional gas sensor element. At least one of the first porous layer 7a and the second porous layer 7b disposed in this manner, that is, the porous layer 7, can relieve stress concentrated at a position corresponding to the corner of the internal space in the conventional gas sensor element.
[0113] The present inventors have confirmed through experiments (heating tests described later) that the porous layer 7 can suppress the occurrence of cracks by setting the porosity of the porous layer 7 to 50% or less. In addition, the porous layer 7 has a porosity of 10% or more due to its "porous" nature. Therefore, the porosity of the porous layer 7 (first porous layer 7a and second porous layer 7b) is set to 10% or more and 50% or less.
[0114] Therefore, the gas sensor element 100 can prevent cracks from occurring at or near the corners, which would destroy the internal space (measurement gas flow section 8), and can be used for a relatively long period of time without any problems, even in harsh operating environments.
[0115] In the gas sensor element 100, the porous layer 7 may be disposed so as to face the measurement gas flow section 8, for example, so as to face at least one of the first internal space 20, the second internal space 40, and the third internal space 17 included in the measurement gas flow section 8. In other words, the porous layer 7 may face at least one of the chambers (the first internal space 20, the second internal space 40, and the third internal space 17) included in the measurement gas flow section 8 (internal space) from which oxygen is pumped in or out.
[0116] In the gas sensor element 100, the first porous layer 7a may be disposed in contact with at least one of the side surfaces 59 of the spacer layer 5 facing the measurement gas flow section 8 and with the first solid electrolyte layer 4, and may be disposed so as to face the measurement gas flow section 8. The first porous layer 7a may be disposed in contact with a lower end of any one of the front side surface 59f, the rear side surface 59b, the right side surface 59r, and the left side surface 59l, and with an upper surface of the first solid electrolyte layer 4, and may be disposed so as to face the measurement gas flow section 8.
[0117] In the gas sensor element 100, the second porous layer 7b may be disposed in contact with at least one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8 and with the second solid electrolyte layer 6, and may be disposed so as to face the measured gas flow section 8. The second porous layer 7b may be disposed in contact with an upper end of any one of the front side surface 59f, the rear side surface 59b, the right side surface 59r, and the left side surface 59l, and with the lower surface of the second solid electrolyte layer 6, and may be disposed so as to face the measured gas flow section 8.
[0118] [Variations] Although the embodiments of the present invention have been described above, the above description of the embodiments is merely an example of the present invention in every respect. Various improvements and modifications may be made to the above embodiments. Regarding each component of the above embodiments, components may be omitted, replaced, or added as appropriate. Furthermore, the shape and dimensions of each component of the above embodiments may be modified as appropriate depending on the embodiment. For example, the following modifications are possible. In the following, the same reference numerals are used for components similar to those of the above embodiments, and the description of the same points as those of the above embodiments is omitted as appropriate. The following modifications may be combined as appropriate.
[0119] (Whether or not the measurement gas flow section needs to be extended inward) 3 is a cross-sectional schematic diagram illustrating the configuration of a gas sensor element 100 according to a modified example, showing an example of a first porous layer 7a that does not extend into the measurement gas flow section 8. The porous layer 7 (first porous layer 7a) illustrated in FIGS. 1 and 2 includes an exposed portion 71 that extends into the measurement gas flow section 8 (third internal space 17). However, it is not essential for the porous layer 7 to include the exposed portion 71. For example, as illustrated in FIG. 3, the porous layer 7 may include a non-exposed portion 72 and not include the exposed portion 71.
[0120] 1 and 2, the first porous layer 7a (porous layer 7) illustrated in FIG. 3 is in contact with both the front side surface 59f of the spacer layer 5 and the first solid electrolyte layer 4. That is, the first porous layer 7a illustrated in FIG. 3 is in contact with the lower end of the front side surface 59f of the spacer layer 5 and is in contact with (facing) the upper surface of the first solid electrolyte layer 4. The first porous layer 7a illustrated in FIG. 3 faces the measured gas flow section 8 (third internal space 17), but does not extend into the measured gas flow section 8, i.e., does not include the exposed portion 71.
[0121] 3, the first porous layer 7a (porous layer 7) needs only to be in contact with at least one side surface (e.g., the front side surface 59f) of the spacer layer 5 facing the measured gas flow section 8 and with the first solid electrolyte layer 4, and to face the measured gas flow section 8. The first porous layer 7a does not need to extend into the measured gas flow section 8, that is, it does not need to include an exposed portion 71 extending into the measured gas flow section 8.
[0122] 5 and the like, it is sufficient that the second porous layer 7b (porous layer 7) is in contact with at least one side surface (e.g., the front side surface 59f) of the spacer layer 5 facing the measured gas flow section 8 and with the second solid electrolyte layer 6, and faces the measured gas flow section 8. The second porous layer 7b does not have to extend into the measured gas flow section 8, that is, it does not have to include an exposed portion 71 extending into the measured gas flow section 8.
[0123] (Whether or not the electrode surface facing the gas flow area to be measured must be partially overlapped) Fig. 4 is a cross-sectional schematic diagram illustrating the configuration of a gas sensor element 100 according to a modified example, showing an example of a first porous layer 7a overlapping a part of the upper surface of the measurement electrode 44. The porous layer 7 (first porous layer 7a) illustrated in Figs. 1 and 2 does not overlap the surface of the measurement electrode 44 facing the measurement gas flow section 8 (third internal space 17). However, as illustrated in Fig. 4, the first porous layer 7a (porous layer 7) may overlap a part of the surface of the measurement electrode 44 facing the measurement gas flow section 8 (third internal space 17).
[0124] That is, the first porous layer 7a (porous layer 7) may overlap at least a part of the surface of an electrode (e.g., the measurement electrode 44) disposed inside the measurement gas flow section 8, the surface facing the first solid electrolyte layer 4. In the example shown in FIG. 4, the first porous layer 7a overlaps a part of the upper surface of the measurement electrode 44.
[0125] Similarly, the second porous layer 7b (porous layer 7) may overlap at least a part of the surface of an electrode (e.g., ceiling electrode portion 22a, ceiling electrode portion 51a) disposed inside the measured gas flow portion 8, the surface facing the second solid electrolyte layer 6. The configuration in which the second porous layer 7b overlaps at least a part of the surface facing the second solid electrolyte layer 6 of an electrode disposed inside the measured gas flow portion 8 will be described in detail later with reference to Figs. 7 and 8.
[0126] Here, the present inventors have noticed that the following problems may occur with respect to the electrodes disposed inside the measurement gas flow section 8. That is, when platinum (Pt) is used for the electrodes, platinum oxide may be generated when the gas sensor element is used repeatedly for a long time. Since platinum oxide evaporates more easily than platinum at high temperatures, the evaporation of platinum oxide may cause peeling at the interface between the electrodes and the solid electrolyte layer (the first solid electrolyte layer 4 or the second solid electrolyte layer 6) with which the electrodes are in contact. The present inventors have noticed that there is a problem in that the electrodes disposed inside the measurement gas flow section 8 may peel off from the solid electrolyte layer due to the above-mentioned causes, which may cause a malfunction in the detection of the gas sensor element. In particular, when the gas sensor element is used as an exhaust gas sensor, the electrodes disposed inside the measurement gas flow section 8 are often exposed to high temperatures, and therefore peeling from the solid electrolyte layer may easily occur.
[0127] Therefore, the present inventors have conceived of preventing peeling of the electrode by arranging the porous layer 7 so as to overlap at least a part of the surface of the electrode disposed inside the measurement gas flow section 8, which faces the surface that contacts the solid electrolyte layer. That is, they thought that peeling of the electrode from the solid electrolyte layer could be prevented by pressing the electrode against the solid electrolyte layer with which the electrode is in contact with the porous layer 7. Then, the present inventors confirmed through an experiment (electrode peeling test described later) that peeling of the electrode can be suppressed by arranging the porous layer 7 so as to overlap at least a part of the surface of the electrode which faces the surface that contacts the solid electrolyte layer.
[0128] Therefore, with this configuration, it is possible to prevent the electrodes from peeling off from the solid electrolyte layer to which the electrodes are in contact, and it is possible to provide a gas sensor element that can be used for a relatively long period of time without any malfunctions, even under harsh operating environments.
[0129] 4, the first porous layer 7a (porous layer 7) overlaps a part of the surface of the measurement electrode 44 disposed inside the measurement gas flow section 8 (third internal space 17) that faces the first solid electrolyte layer 4. Therefore, the gas sensor element 100 can prevent the measurement electrode 44 from peeling off from the first solid electrolyte layer 4 with which the measurement electrode 44 is in contact, and can be used for a relatively long period of time without any problems even under harsh operating conditions.
[0130] In the gas sensor element 100 illustrated in FIG. 4, the area of the portion of the measurement electrode 44 that is overlapped by the first porous layer 7a is, for example, 0.5% or more and 20% or less of the area of the opposing surface of the measurement electrode 44 that contacts the first solid electrolyte layer 4.
[0131] Here, if the ratio of the area of the portion overlapping with the first porous layer 7a to the entire area of the opposing surface of the measurement electrode 44 in contact with the first solid electrolyte layer 4 is made larger than 20%, the performance (e.g., detection accuracy, etc.) of the measurement electrode 44 may be degraded. Therefore, the area of the portion of the measurement electrode 44 overlapping with the first porous layer 7a is set to 20% or less of the area of the opposing surface of the measurement electrode 44 in contact with the first solid electrolyte layer 4.
[0132] Furthermore, the present inventors confirmed through experiments (electrode peeling tests) that peeling of the measurement electrode 44 can be effectively suppressed by making the area of the portion of the measurement electrode 44 where the first porous layer 7a overlaps 0.5% or more of the area of the surface of the measurement electrode 44 facing the surface in contact with the first solid electrolyte layer 4.
[0133] That is, by setting the area of the portion of the measurement electrode 44 where the first porous layer 7a overlaps to 0.5% or more and 20% or less of the area of the surface of the measurement electrode 44 in contact with the first solid electrolyte layer 4, it is possible to effectively suppress peeling of the measurement electrode 44 while preventing a decrease in performance of the measurement electrode 44. Therefore, the gas sensor element 100 can effectively suppress peeling of the measurement electrode 44 while preventing a decrease in performance of the measurement electrode 44, and can be used for a relatively long period of time without causing any problems even under harsh usage environments. The electrode peeling test will be described in detail later.
[0134] (Example with second porous layer) FIG. 5 is a cross-sectional schematic diagram showing the configuration of a gas sensor element 100 according to a modified example, and shows an example of the second porous layer 7b in contact with the front side surface 59f of the spacer layer 5 facing the third internal space 17 and the second solid electrolyte layer 6. The gas sensor element 100 described above with reference to FIGS. 1 to 4 includes the first porous layer 7a in contact with the front side surface 59f of the spacer layer 5 and the first solid electrolyte layer 4 facing the measurement gas flow section 8 (the third internal space 17). However, the porous layer 7 included in the gas sensor element 100 is not limited to the first porous layer 7a, and may be the second porous layer 7b. The gas sensor element 100 shown in FIG. 5 includes the second porous layer 7b in contact with the front side surface 59f of the spacer layer 5 and the second solid electrolyte layer 6 facing the measurement gas flow section 8 (the third internal space 17).
[0135] 5, the second porous layer 7b faces the measurement gas flow section 8 (third internal space 17) and is in contact with both the front side surface 59f of the spacer layer 5 and the second solid electrolyte layer 6. That is, the second porous layer 7b faces the measurement gas flow section 8 and is in contact with an upper end of the front side surface 59f of the spacer layer 5 and a lower surface of the second solid electrolyte layer 6. In other words, the second porous layer 7b is in contact with an upper end of the front side surface 59f of the spacer layer 5 and faces the measurement gas flow section 8 and the lower surface of the second solid electrolyte layer 6.
[0136] The second porous layer 7b, which is disposed between the upper end of the front side surface 59f of the spacer layer 5 and the lower surface of the second solid electrolyte layer 6 so as to be in contact with and sandwiched between them as illustrated in Fig. 5, is formed, for example, as follows. That is, an adhesive layer including the porous layer 7 is used as an adhesive layer that bonds the lower surface of the second solid electrolyte layer 6 and the upper surface of the spacer layer 5. Then, the adhesive layer (porous layer 7) may be left in a portion (and its periphery) of the spacer layer 5 located at the upper end of the front side surface 59f facing the measurement target gas flow section 8 (third internal space 17), thereby forming the second porous layer 7b as illustrated in Fig. 5.
[0137] That is, the second porous layer 7b may be formed by leaving an adhesive layer including the porous layer 7 that bonds the lower surface of the second solid electrolyte layer 6 and the upper surface of the spacer layer 5 in a portion (and its surroundings) located at the upper end of one of the side surfaces 59 of the spacer layer 5 facing the measured gas flow section 8.
[0138] In one example, as illustrated in FIG. 5, FIG. 7 and FIG. 8, the second porous layer 7b may be disposed in contact with the upper end of the side surface 59 of the spacer layer 5 facing the measured gas flow section 8 and the lower surface of the second solid electrolyte layer 6, so as to face the measured gas flow section 8. That is, the second porous layer 7b facing the measured gas flow section 8 may be disposed between the spacer layer 5 and the second solid electrolyte layer 6 so as to be in contact with both and sandwiched between them. In this configuration, the second porous layer 7b disposed between the spacer layer 5 and the second solid electrolyte layer 6 can reduce the Young's modulus of the gas sensor element (particularly, the laminate) and can relieve stress concentrated at and near the corners of the internal space. That is, by disposing the second porous layer 7b as a buffer material between the spacer layer 5 and the second solid electrolyte layer 6, it is possible to prevent a situation in which stress is concentrated and cracks are generated at and near the corners of the measured gas flow section 8.
[0139] In the second porous layer 7b (porous layer 7) illustrated in FIG. 5, as in the first porous layer 7a, the porosity is preferably 10% or more and 50% or less, and the thickness is preferably 10 μm or more and 40 μm or less. If the thickness of the second porous layer 7b arranged to face the measurement gas flow section 8 is too large, the amount of oxygen taken into the second porous layer 7b increases, and the time required to pump out or pump in oxygen from the measurement gas flow section 8 (particularly the void space (the third internal void space 17 in the example of FIG. 5) facing the second porous layer 7b) increases (light-off time). Therefore, in consideration of the light-off time, it is preferable to suppress the thickness of the second porous layer 7b to a predetermined value, and the present inventors have confirmed that it is preferable to set the thickness to 40 μm or less. By setting the thickness of the second porous layer 7b to 40 μm or less, the light-off time can be set to a range that can withstand actual use (normal use) of the gas sensor element 100. Similarly to the first porous layer 7a, the second porous layer 7b (porous layer 7) may be configured as a porous layer having a zirconia content of 50 wt% or more. As described above, the second porous layer 7b is in contact with the second solid electrolyte layer 6. The second solid electrolyte layer 6 is configured of an oxygen ion conductive solid electrolyte layer such as zirconia. Therefore, when the second porous layer 7b is made of the same material as the second solid electrolyte layer 6, the adhesion between the second porous layer 7b and the second solid electrolyte layer 6 can be improved. Therefore, by making the zirconia content in the second porous layer 7b 50 wt% or more, the adhesion between the second porous layer 7b and the second solid electrolyte layer 6 can be improved. Furthermore, the second porous layer 7b (porous layer 7) may be configured as an insulating layer, for example.
[0140] The second porous layer 7b (porous layer 7) illustrated in FIG. 5 includes an exposed portion 71 that faces the third internal space 17 and a non-exposed portion 72 that does not face the third internal space 17, similar to the first porous layer 7a described with reference to FIGS. 1 and 2. In the second porous layer 7b illustrated in FIG. 5, the exposed portion 71 extends from a position where the upper end of the front side surface 59f of the spacer layer 5 contacts the surface of the second porous layer 7b that faces the measurement gas flow section 8 into the third internal space 17 and faces the lower surface of the second solid electrolyte layer 6. In the second porous layer 7b illustrated in FIG. 5, the volume of the exposed portion 71 that extends into the third internal space 17 is, for example, 5% or more and 30% or less of the volume of the third internal space 17.
[0141] In the second porous layer 7b (porous layer 7) illustrated in FIG. 5, the non-exposed portion 72 is a portion of the second porous layer 7b located between the spacer layer 5 and the second solid electrolyte layer 6. The non-exposed portion 72 is in contact with (faces) both the spacer layer 5 and the second solid electrolyte layer 6, and does not face the measurement target gas flow section 8 (third internal space 17). In the second porous layer 7b illustrated in FIG. 5, the non-exposed portion 72 extends from a position where the upper end of the front side surface 59f of the spacer layer 5 contacts the surface of the porous layer 7 facing the measurement target gas flow section 8 into the spacer layer 5, and faces the lower surface of the second solid electrolyte layer 6. In the second porous layer 7b illustrated in FIG. 5, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the second porous layer 7b illustrated in FIG. 5.
[0142] The gas sensor element 100 may include at least one of the first porous layer 7a described with reference to Figures 1 to 4 and the second porous layer 7b described with reference to Figure 5, and may include, for example, both the first porous layer 7a and the second porous layer 7b.
[0143] (Example in which a porous layer is provided in contact with the first solid electrolyte layer and the second solid electrolyte layer) FIG. 6 is a cross-sectional schematic diagram illustrating the configuration of a gas sensor element 100 according to a modified example, and illustrates an example of the porous layer 7 in contact with the front side surface 59f of the spacer layer 5 facing the third internal space 17, the first solid electrolyte layer 4, and the second solid electrolyte layer 6. The gas sensor element 100 described above with reference to FIGS. 1 to 5 includes the porous layer 7 in contact with the front side surface 59f of the spacer layer 5 and the first solid electrolyte layer 4 or the second solid electrolyte layer 6 facing the measurement gas flow section 8 (third internal space 17). However, the porous layer 7 of the gas sensor element 100 is not limited to the porous layer 7 in contact with the first solid electrolyte layer 4 or the second solid electrolyte layer 6, and may be the porous layer 7 in contact with both the first solid electrolyte layer 4 and the second solid electrolyte layer 6.
[0144] The porous layer 7 illustrated in FIG. 6 faces the measured gas flow section 8 (third internal space 17) and is in contact with the front side surface 59f of the spacer layer 5 facing the measured gas flow section 8, the first solid electrolyte layer 4, and the second solid electrolyte layer 6. The porous layer 7 illustrated in FIG. 6 can be regarded as an example in which the first porous layer 7a, which faces the measured gas flow section 8 (third internal space 17) and is in contact with both the front side surface 59f of the spacer layer 5 and the first solid electrolyte layer 4, is further in contact with (facing) the second solid electrolyte layer 6. The porous layer 7 illustrated in FIG. 6 can also be regarded as an example in which the second porous layer 7b, which faces the measured gas flow section 8 (third internal space 17) and is in contact with both the front side surface 59f of the spacer layer 5 and the second solid electrolyte layer 6, is further in contact with (facing) the first solid electrolyte layer 4.
[0145] As illustrated in FIG. 6, the gas sensor element 100 may include a porous layer 7 that faces the measurement gas flow section 8 (third internal space 17) and is in contact with the front side surface 59f of the spacer layer 5, the first solid electrolyte layer 4, and the second solid electrolyte layer 6.
[0146] The porous layer 7 illustrated in Fig. 6 has a porosity of 10% or more and 50% or less and a thickness of 10 μm or more and 40 μm or less, similar to the first porous layer 7a and the second porous layer 7b described above. The porous layer 7 illustrated in Fig. 6 may be configured as a porous layer having a zirconia content of 50 wt% or more, similar to the first porous layer 7a and the second porous layer 7b, or may be configured as an insulating layer.
[0147] (An example having a porous layer facing the first internal space) FIG. 7 is a cross-sectional schematic diagram showing an outline of the configuration of the gas sensor element 100 according to the modified example, and shows an example of the porous layer 7 (the first porous layer 7a and the second porous layer 7b) in contact with the right side surface 59r of the spacer layer 5 facing the first internal space 20. The gas sensor element 100 described above with reference to FIGS. 1 to 6 includes the porous layer 7 facing the measurement gas flow section 8 (the third internal space 17) and in contact with the front side surface 59f of the spacer layer 5 and at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6. However, the porous layer 7 of the gas sensor element 100 does not necessarily face the third internal space 17. Moreover, the porous layer 7 of the gas sensor element 100 does not necessarily face the front side surface 59f of the spacer layer 5.
[0148] 7 faces the measured gas flow section 8 (first internal space 20) and is in contact with both a right side surface 59r of the spacer layer 5, which is a surface facing the measured gas flow section 8, and the first solid electrolyte layer 4. That is, the first porous layer 7a faces the measured gas flow section 8 and is in contact with a lower end of the right side surface 59r of the spacer layer 5 and an upper surface of the first solid electrolyte layer 4. In other words, the first porous layer 7a is in contact with a lower end of the right side surface 59r of the spacer layer 5 and faces the measured gas flow section 8 and the upper surface of the first solid electrolyte layer 4.
[0149] 7 faces the measured gas flow section 8 (first internal space 20) and is in contact with both a right side surface 59r of the spacer layer 5, which is the surface facing the measured gas flow section 8, and the second solid electrolyte layer 6. That is, the second porous layer 7b faces the measured gas flow section 8 and is in contact with an upper end of the right side surface 59r of the spacer layer 5 and a lower surface of the second solid electrolyte layer 6. In other words, the second porous layer 7b is in contact with an upper end of the right side surface 59r of the spacer layer 5 and faces the measured gas flow section 8 and the lower surface of the second solid electrolyte layer 6.
[0150] The first porous layer 7a (porous layer 7) illustrated in FIG. 7 overlaps at least a portion of the opposing surface (the upper surface in the figure) of the bottom electrode portion 22b disposed inside the measurement gas flow portion 8 (first internal space 20) that contacts (faces) the first solid electrolyte layer 4.
[0151] Similarly, the second porous layer 7b (porous layer 7) illustrated in Figure 7 overlaps at least a portion of the opposite surface (the lower surface in the figure) of the ceiling electrode portion 22a arranged inside the measured gas flow portion 8 (first internal space 20) to the surface that contacts (faces) the second solid electrolyte layer 6.
[0152] 7 shows an example in which the gas sensor element 100 includes a first porous layer 7a and a second porous layer 7b. However, the porous layer 7 included in the gas sensor element 100 may be at least one of the first porous layer 7a and the second porous layer 7b, and it is not essential that the gas sensor element 100 includes both the first porous layer 7a and the second porous layer 7b.
[0153] 7, the first porous layer 7a overlaps a part of the upper surface of the bottom electrode portion 22b, and the second porous layer 7b overlaps a part of the lower surface of the ceiling electrode portion 22a. However, for the gas sensor element 100, it is not essential that the first porous layer 7a overlaps a part of the upper surface of the bottom electrode portion 22b, and the first porous layer 7a does not have to overlap a part of the upper surface of the bottom electrode portion 22b. Similarly, for the gas sensor element 100, it is not essential that the second porous layer 7b overlaps a part of the lower surface of the ceiling electrode portion 22a, and the second porous layer 7b does not have to overlap a part of the lower surface of the ceiling electrode portion 22a.
[0154] Each of the first porous layer 7a and the second porous layer 7b illustrated in FIG. 7 has a porosity of 10% or more and 50% or less, and a thickness of 10 μm or more and 40 μm or less, similar to the first porous layer 7a and the second porous layer 7b described above. Each of the first porous layer 7a and the second porous layer 7b illustrated in FIG. 7 may be configured as a porous layer having a zirconia content of 50 wt% or more, similar to the first porous layer 7a and the second porous layer 7b described above. Each of the first porous layer 7a and the second porous layer 7b illustrated in FIG. 7 may be configured as an insulating layer, similar to the first porous layer 7a and the second porous layer 7b described above.
[0155] Each of the first porous layer 7a and the second porous layer 7b illustrated in Figure 7 includes an exposed portion 71 and a non-exposed portion 72, similar to the first porous layer 7a and the second porous layer 7b previously described using Figures 1 to 2 and Figures 4 to 5.
[0156] 7, the exposed portion 71 extends from a position where the lower end of the right side surface 59r of the spacer layer 5 contacts the surface of the first porous layer 7a facing the first internal space 20 into the first internal space 20 and faces the upper surface of the first solid electrolyte layer 4. In the second porous layer 7b shown in FIG. 7, the exposed portion 71 extends from a position where the upper end of the right side surface 59r of the spacer layer 5 contacts the surface of the second porous layer 7b facing the first internal space 20 into the first internal space 20 and faces the lower surface of the second solid electrolyte layer 6.
[0157] In FIG. 7, the sum of the volume of the exposed portion 71 of the first porous layer 7a and the volume of the exposed portion 71 of the second porous layer 7b is, for example, 5% or more and 30% or less of the volume of the first inner space 20.
[0158] In the first porous layer 7a illustrated in FIG. 7, the non-exposed portion 72 is a portion of the first porous layer 7a that is located between the spacer layer 5 and the first solid electrolyte layer 4 and does not face the first internal space 20 (measurement gas flow section 8). The non-exposed portion 72 of the first porous layer 7a illustrated in FIG. 7 extends from a position where the lower end of the right side surface 59r of the spacer layer 5 contacts the surface of the first porous layer 7a that faces the first internal space 20 into the spacer layer 5 and faces the upper surface of the first solid electrolyte layer 4. In the first porous layer 7a illustrated in FIG. 7, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the first porous layer 7a illustrated in FIG. 7.
[0159] In the second porous layer 7b illustrated in FIG. 7, the non-exposed portion 72 is a portion of the second porous layer 7b that is located between the spacer layer 5 and the second solid electrolyte layer 6 and does not face the first internal space 20 (measurement gas flow portion 8). The non-exposed portion 72 of the second porous layer 7b illustrated in FIG. 7 extends from a position where the upper end of the right side surface 59r of the spacer layer 5 contacts the surface of the second porous layer 7b that faces the first internal space 20 into the spacer layer 5 and faces the lower surface of the second solid electrolyte layer 6. In the second porous layer 7b illustrated in FIG. 7, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the second porous layer 7b illustrated in FIG. 7.
[0160] 7, the first porous layer 7a (porous layer 7) overlaps a part of the surface of the bottom electrode portion 22b disposed inside the measurement gas flow portion 8 (first internal space 20) that faces (contacts) the first solid electrolyte layer 4. In particular, in the gas sensor element 100 illustrated in FIG 7, the area of the portion of the bottom electrode portion 22b that is overlapped by the first porous layer 7a is, for example, 0.5% to 20% of the area of the surface of the bottom electrode portion 22b that faces (contacts) the first solid electrolyte layer 4.
[0161] 7, the second porous layer 7b (porous layer 7) overlaps a part of the opposite surface of the ceiling electrode portion 22a disposed inside the measurement gas flow portion 8 (first internal space 20) that contacts (faces) the second solid electrolyte layer 6. In particular, in the gas sensor element 100 illustrated in FIG 7, the area of the portion of the ceiling electrode portion 22a overlapped by the second porous layer 7b is, for example, 0.5% to 20% of the area of the opposite surface of the ceiling electrode portion 22a that contacts the second solid electrolyte layer 6.
[0162] 7 shows an example of the porous layer 7 (first porous layer 7a, second porous layer 7b) facing the first internal space 20 (measurement gas flow section 8) and in contact with the right side surface 59r of the spacer layer 5. However, the porous layer 7 facing the first internal space 20 may be in contact with the left side surface 59l of the spacer layer 5 that defines the first internal space 20 (measurement gas flow section 8). In addition, when the gas inlet 10 is not disposed on the front surface of the gas sensor element 100, the porous layer 7 facing the measurement gas flow section 8 may be in contact with the rear side surface 59b of the spacer layer 5 that defines the front side of the measurement gas flow section 8.
[0163] (An example having a porous layer facing the second internal space) FIG. 8 is a schematic cross-sectional diagram illustrating the configuration of a modified gas sensor element 100, showing an example of a porous layer 7 (first porous layer 7a and second porous layer 7b) in contact with the right side surface 59r of the spacer layer 5 facing the second internal space 40.
[0164] 8 faces the measured gas flow section 8 (second internal space 40) and is in contact with both a right side surface 59r of the spacer layer 5, which is a surface facing the measured gas flow section 8, and the first solid electrolyte layer 4. That is, the first porous layer 7a faces the measured gas flow section 8 and is in contact with a lower end of the right side surface 59r of the spacer layer 5 and an upper surface of the first solid electrolyte layer 4. In other words, the first porous layer 7a is in contact with a lower end of the right side surface 59r of the spacer layer 5 and faces the measured gas flow section 8 and the upper surface of the first solid electrolyte layer 4.
[0165] 8 faces the measured gas flow section 8 (second internal space 40) and is in contact with both a right side surface 59r of the spacer layer 5, which is the surface facing the measured gas flow section 8, and the second solid electrolyte layer 6. That is, the second porous layer 7b faces the measured gas flow section 8 and is in contact with an upper end of the right side surface 59r of the spacer layer 5 and a lower surface of the second solid electrolyte layer 6. In other words, the second porous layer 7b is in contact with an upper end of the right side surface 59r of the spacer layer 5 and faces the measured gas flow section 8 and the lower surface of the second solid electrolyte layer 6.
[0166] The first porous layer 7a (porous layer 7) illustrated in FIG. 8 overlaps at least a portion of the opposing surface (the upper surface in the figure) of the bottom electrode portion 51b disposed inside the measurement gas flow portion 8 (second internal space 40) that is in contact with (facing) the first solid electrolyte layer 4.
[0167] Similarly, the second porous layer 7b (porous layer 7) illustrated in Figure 8 overlaps at least a portion of the opposite surface (the underside in the figure) of the ceiling electrode portion 51a arranged inside the measured gas flow portion 8 (second internal space 40) to the surface that contacts (faces) the second solid electrolyte layer 6.
[0168] 8 shows an example in which the gas sensor element 100 includes a first porous layer 7a and a second porous layer 7b. However, the porous layer 7 included in the gas sensor element 100 may be at least one of the first porous layer 7a and the second porous layer 7b, and it is not essential that the gas sensor element 100 includes both the first porous layer 7a and the second porous layer 7b.
[0169] 8, the first porous layer 7a overlaps a part of the upper surface of the bottom electrode portion 51b, and the second porous layer 7b overlaps a part of the lower surface of the ceiling electrode portion 51a. However, for the gas sensor element 100, it is not essential that the first porous layer 7a overlaps a part of the upper surface of the bottom electrode portion 51b, and the first porous layer 7a does not have to overlap a part of the upper surface of the bottom electrode portion 51b. Similarly, for the gas sensor element 100, it is not essential that the second porous layer 7b overlaps a part of the lower surface of the ceiling electrode portion 51a, and the second porous layer 7b does not have to overlap a part of the lower surface of the ceiling electrode portion 51a.
[0170] Each of the first porous layer 7a and the second porous layer 7b illustrated in FIG. 8 has a porosity of 10% or more and 50% or less, and a thickness of 10 μm or more and 40 μm or less, similar to the first porous layer 7a and the second porous layer 7b described above. Each of the first porous layer 7a and the second porous layer 7b illustrated in FIG. 8 may be configured as a porous layer having a zirconia content of 50 wt% or more, similar to the first porous layer 7a and the second porous layer 7b described above. Each of the first porous layer 7a and the second porous layer 7b illustrated in FIG. 8 may be configured as an insulating layer, similar to the first porous layer 7a and the second porous layer 7b described above.
[0171] Each of the first porous layer 7a and the second porous layer 7b illustrated in Figure 8 includes an exposed portion 71 and a non-exposed portion 72, similar to the first porous layer 7a and the second porous layer 7b previously described using Figures 1 to 2 and Figures 4 to 5.
[0172] 8, the exposed portion 71 extends from a position where the lower end of the right side surface 59r of the spacer layer 5 and the surface of the first porous layer 7a facing the second internal space 40 contact each other into the second internal space 40 and faces the upper surface of the first solid electrolyte layer 4. In the second porous layer 7b shown in FIG. 8, the exposed portion 71 extends from a position where the upper end of the right side surface 59r of the spacer layer 5 and the surface of the second porous layer 7b facing the second internal space 40 contact each other into the second internal space 40 and faces the lower surface of the second solid electrolyte layer 6.
[0173] In FIG. 8, the sum of the volume of the exposed portion 71 of the first porous layer 7a and the volume of the exposed portion 71 of the second porous layer 7b is, for example, 5% or more and 30% or less of the volume of the second inner space 40.
[0174] In the first porous layer 7a illustrated in FIG. 8, the non-exposed portion 72 is a portion of the first porous layer 7a that is located between the spacer layer 5 and the first solid electrolyte layer 4 and does not face the second internal space 40 (measurement gas flow section 8). The non-exposed portion 72 of the first porous layer 7a illustrated in FIG. 8 extends from a position where the lower end of the right side surface 59r of the spacer layer 5 contacts the surface of the first porous layer 7a that faces the second internal space 40 into the spacer layer 5 and faces the upper surface of the first solid electrolyte layer 4. In the first porous layer 7a illustrated in FIG. 8, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the first porous layer 7a illustrated in FIG. 8.
[0175] In the second porous layer 7b illustrated in FIG. 8, the non-exposed portion 72 is a portion of the second porous layer 7b that is located between the spacer layer 5 and the second solid electrolyte layer 6 and does not face the second internal space 40 (measurement gas flow portion 8). The non-exposed portion 72 of the second porous layer 7b illustrated in FIG. 8 extends from a position where the upper end of the right side surface 59r of the spacer layer 5 contacts the surface of the second porous layer 7b that faces the second internal space 40, toward the inside of the spacer layer 5, and faces the lower surface of the second solid electrolyte layer 6. In the second porous layer 7b illustrated in FIG. 8, the volume of the non-exposed portion 72 is, for example, 10% or more of the volume of the second porous layer 7b illustrated in FIG. 8.
[0176] 8, the first porous layer 7a (porous layer 7) overlaps a part of the surface of the bottom electrode portion 51b disposed inside the measurement gas flow portion 8 (second internal space 40) that faces (contacts) the first solid electrolyte layer 4. In particular, in the gas sensor element 100 illustrated in FIG 7, the area of the portion of the bottom electrode portion 51b that is overlapped by the first porous layer 7a is, for example, 0.5% to 20% of the area of the surface of the bottom electrode portion 51b that faces (contacts) the first solid electrolyte layer 4.
[0177] 8, the second porous layer 7b (porous layer 7) overlaps a part of the opposite surface of the ceiling electrode portion 51a disposed inside the measurement gas flow portion 8 (second internal space 40) to the surface that contacts (faces) the second solid electrolyte layer 6. In particular, in the gas sensor element 100 illustrated in FIG 8, the area of the portion of the ceiling electrode portion 51a overlapped by the second porous layer 7b is, for example, 0.5% to 20% of the area of the opposite surface of the ceiling electrode portion 51a to the surface that contacts the second solid electrolyte layer 6.
[0178] 8 shows an example of the porous layer 7 (first porous layer 7a, second porous layer 7b) facing the second internal space 40 (measurement gas flow section 8) and in contact with the right side surface 59r of the spacer layer 5. However, the porous layer 7 facing the second internal space 40 may be in contact with the left side surface 59l of the spacer layer 5 that defines the second internal space 40 (measurement gas flow section 8). In addition, when the gas inlet 10 is not disposed on the front surface of the gas sensor element 100, the porous layer 7 facing the measurement gas flow section 8 may be in contact with the rear side surface 59b of the spacer layer 5 that defines the front side of the measurement gas flow section 8.
[0179] As illustrated in FIG. 4, FIG. 6 to FIG. 8, in the gas sensor element 100, at least one of the porous layers 7 (first porous layer 7a, second porous layer 7b) overlaps a part of at least one electrode disposed inside the measurement gas flow section 8. Specifically, the porous layer 7 overlaps at least a part of the surface of the electrode that faces at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6. FIG. 4 and FIG. 6 show an example in which the first porous layer 7a (porous layer 7) overlaps a part of the upper surface of the measurement electrode 44. FIG. 7 shows an example in which the first porous layer 7a overlaps a part of the upper surface of the bottom electrode section 22b, and the second porous layer 7b overlaps a part of the lower surface of the ceiling electrode section 22a. FIG. 8 shows an example in which the first porous layer 7a overlaps a part of the upper surface of the bottom electrode section 51b, and the second porous layer 7b overlaps a part of the lower surface of the ceiling electrode section 51a. The measuring electrode 44, the ceiling electrode portion 22a, the bottom electrode portion 22b, the ceiling electrode portion 51a, and the bottom electrode portion 51b are examples of electrodes disposed inside the measurement target gas flow portion 8 (internal space).
[0180] In the gas sensor element 100, the area of the portion of the electrode where the porous layer 7 overlaps is, for example, 0.5% to 20% of the area of the opposing surface of the electrode.
[0181] Points to be noted regarding the gas sensor element 100 described above are given below as examples.
[0182] (I) Vacant spaces facing the porous layer In the gas sensor element 100, the porous layer 7 faces the measurement gas flow section 8. The measurement gas flow section 8 includes one or more chambers from which oxygen is pumped in or out, and the porous layer 7 of the gas sensor element 100 faces at least one of the chambers. For example, the porous layer 7 may face the third internal space 17 of the chambers included in the measurement gas flow section 8 as illustrated in Figs. 1 to 6, or may face the first internal space 20 as illustrated in Fig. 7, or may face the second internal space 40 as illustrated in Fig. 8.
[0183] The gas sensor element 100 may include one or more porous layers 7, and the porous layer 7 may face one or more voids. For example, each of the one or more porous layers 7 included in the gas sensor element 100 may face only the first internal void 20, may face only the second internal void 40, or may face only the third internal void 17.
[0184] Similarly, the gas sensor element 100 may include one or more porous layers 7 facing the first internal space 20 and one or more porous layers 7 facing the second internal space 40. The gas sensor element 100 may also include one or more porous layers 7 facing the first internal space 20 and one or more porous layers 7 facing the third internal space 17. The gas sensor element 100 may also include one or more porous layers 7 facing the second internal space 40 and one or more porous layers 7 facing the third internal space 17. The gas sensor element 100 may also include one or more porous layers 7 facing the first internal space 20, one or more porous layers 7 facing the second internal space 40, and one or more porous layers 7 facing the third internal space 17.
[0185] For example, the gas sensor element 100 may have at least one of a first porous layer 7a facing the first internal void 20, a first porous layer 7a facing the second internal void 40, a first porous layer 7a facing the third internal void 17, a second porous layer 7b facing the first internal void 20, a second porous layer 7b facing the second internal void 40, and a second porous layer 7b facing the third internal void 17.
[0186] Of the porous layers 7, the first porous layer 7a is a porous layer 7 that is in contact with both one of the side surfaces 59 of the spacer layer 5 and the first solid electrolyte layer 4, and the second porous layer 7b is a porous layer 7 that is in contact with both one of the side surfaces 59 of the spacer layer 5 and the second solid electrolyte layer 6.
[0187] It is not essential that the measurement gas flow section 8 includes the first internal space 20, the second internal space 40, and the third internal space 17 as the spaces into which oxygen is pumped out or into. It is not essential that the measurement gas flow section 8 is divided into two or more spaces by one or more diffusion rate-controlling sections (at least one of the first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, the third diffusion rate-controlling section 30, and the fourth diffusion rate-controlling section 16) that impart a predetermined diffusion resistance to the measurement gas. The measurement gas flow section 8 may include one or more spaces, and the example in which the measurement gas flow section 8 is divided into the first internal space 20, the second internal space 40, and the third internal space 17 is merely one example of the gas sensor element 100. The gas sensor element 100 may include a porous layer 7 facing at least one of the one or more void spaces included in the measurement gas flow section 8, and in contact with a side 59 of the spacer layer 5 facing the void space and at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6.
[0188] (II) The side of the spacer layer that is in contact with the porous layer In the gas sensor element 100, the porous layer 7 facing the measurement gas flow section 8 is in contact with at least one of the side surfaces 59 of the spacer layer 5 facing the measurement gas flow section 8. For example, the porous layer 7 may be in contact with the front side surface 59f of the side surfaces 59 of the spacer layer 5 facing the measurement gas flow section 8 as illustrated in Figs. 1 to 6, or may be in contact with the right side surface 59r of the side surfaces 59 of the spacer layer 5 facing the measurement gas flow section 8 as illustrated in Figs. 7 and 8. Although not illustrated, the porous layer 7 may be in contact with the left side surface 59l or the rear side surface 59b of the side surfaces 59 of the spacer layer 5 facing the measurement gas flow section 8.
[0189] In the gas sensor element 100 illustrated in FIG. 1, the gas inlet 10 is disposed on the front side of the gas sensor element 100. However, whether or not the gas inlet 10 is provided in the gas sensor element 100, and if so, which side of the gas sensor element 100 it is provided on, are optional. For example, the gas inlet 10 may be disposed on the right side of the gas sensor element 100. And, for example, when the gas inlet 10 is not provided or when the gas inlet 10 is disposed on the right side of the gas sensor element 100, the porous layer 7 facing the measured gas flow portion 8 may contact the rear side 59b of the spacer layer 5 facing the measured gas flow portion 8. Details of whether or not the gas inlet 10 is provided, and if so, which side of the gas sensor element 100 it is provided on, will be described later.
[0190] The gas sensor element 100 may include one or more porous layers 7, and the porous layer 7 may be in contact with one or more side surfaces 59 of the spacer layer 5. For example, each of the one or more porous layers 7 included in the gas sensor element 100 may be in contact with only the front side surface 59f, only the rear side surface 59b, only the right side surface 59r, or only the left side surface 59l of the spacer layer 5.
[0191] Similarly, two or more of the side surfaces 59 of the front side surface 59f, the rear side surface 59b, the right side surface 59r, and the left side surface 59l of the spacer layer 5 may be in contact with the porous layer 7. For example, the gas sensor element 100 may include one or more porous layers 7 in contact with the front side surface 59f of the spacer layer 5 and one or more porous layers 7 in contact with the rear side surface 59b of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with the front side surface 59f of the spacer layer 5 and one or more porous layers 7 in contact with the right side surface 59r of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with the front side surface 59f of the spacer layer 5 and one or more porous layers 7 in contact with the left side surface 59l of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with the rear side surface 59b of the spacer layer 5 and one or more porous layers 7 in contact with the right side surface 59r of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with the rear side surface 59b of the spacer layer 5 and one or more porous layers 7 in contact with the left side surface 59l of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with the right side surface 59r of the spacer layer 5 and one or more porous layers 7 in contact with the left side surface 59l of the spacer layer 5.
[0192] The gas sensor element 100 may include one or more porous layers 7 in contact with each of the front side 59f, the rear side 59b, and the right side 59r of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with each of the front side 59f, the rear side 59b, and the left side 59l of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with each of the front side 59f, the right side 59r, and the left side 59l of the spacer layer 5. The gas sensor element 100 may include one or more porous layers 7 in contact with each of the rear side 59b, the right side 59r, and the left side 59l of the spacer layer 5.
[0193] The gas sensor element 100 may include one or more porous layers 7 in contact with the front side 59f, the rear side 59b, the right side 59r, and the left side 59l of the spacer layer 5, respectively.
[0194] (III) About the solid electrolyte layer in contact with the porous layer The gas sensor element 100 may include, as the porous layer 7 arranged to face the measurement gas flow section 8, at least one of a first porous layer 7a in contact with the first solid electrolyte layer 4 and a second porous layer 7b in contact with the second solid electrolyte layer 6. That is, the gas sensor element 100 may include the porous layer 7 arranged to face the measurement gas flow section 8 and in contact with at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6.
[0195] The gas sensor element 100 may include, for example, a first porous layer 7a as illustrated in Figures 1 to 4, a second porous layer 7b as illustrated in Figure 5, or the first porous layer 7a and the second porous layer 7b as illustrated in Figures 7 and 8. The porous layer 7 of the gas sensor element 100 is not limited to being in contact with only one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6, and may be in contact with both the first solid electrolyte layer 4 and the second solid electrolyte layer 6 as illustrated in Figure 6.
[0196] (IV) Number of porous layers The gas sensor element 100 needs to include at least one of the first porous layer 7a and the second porous layer 7b, and may include only the first porous layer 7a, only the second porous layer 7b, or both the first porous layer 7a and the second porous layer 7b.
[0197] 1 to 6 show an example of the gas sensor element 100 including one porous layer 7 facing one chamber and in contact with one of the side surfaces 59 of the spacer layer 5. Also, FIGS. 7 and 8 show an example of the gas sensor element 100 including two porous layers 7 facing one chamber and in contact with one of the side surfaces 59 of the spacer layer 5. However, the gas sensor element 100 may include a plurality of porous layers 7 facing one chamber, and one of the porous layers 7 may be in contact with the right side surface 59r of the spacer layer 5 and another of the porous layers 7 may be in contact with the left side surface 59l of the spacer layer 5. Also, when the measurement gas flow section 8 is divided into two or more chambers, the gas sensor element 100 may include a plurality of porous layers 7 each facing one of the plurality of chambers. For example, the gas sensor element 100 may include a porous layer 7 facing the first internal space 20, a porous layer 7 facing the second internal space 40, and a porous layer 7 facing the third internal space 17. The gas sensor element 100 may include the porous layer 7 facing the measurement target gas flow section 8 (one of the spaces included in the measurement target gas flow section 8) and in contact with the side surface 59 of the spacer layer 5 and at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6.
[0198] (V) Whether the measurement gas flow section needs to be extended inward The gas sensor element 100 may include a porous layer 7 disposed to face the measured gas flow section 8 and in contact with a side surface 59 of the spacer layer 5 facing the measured gas flow section 8 and at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6. It is not essential that the porous layer 7 of the gas sensor element 100 extends into the measured gas flow section 8, and the porous layer 7 may or may not extend into the measured gas flow section 8. That is, as illustrated in FIG. 1, FIG. 2, and FIG. 4 to FIG. 8, the porous layer 7 may extend into the measured gas flow section 8, that is, it may include an exposed portion 71. Also, as illustrated in FIG. 3, the porous layer 7 may not extend into the measured gas flow section 8, that is, it may not include an exposed portion 71.
[0199] As described above, the exposed portion 71 is a portion that extends from the position where the ends (lower end, upper end) of the side 59 of the spacer layer 5 facing the measured gas flow section 8 contact the surface of the porous layer 7 facing the measured gas flow section 8, into the inside of the measured gas flow section 8.
[0200] In the gas sensor element 100, when one or more porous layers 7 extend inside one vacant space included in the measurement gas flow section 8, the total volume of the exposed portions 71 of the one or more porous layers 7 is preferably 5% to 30% of the volume of the vacant space. For example, as illustrated in Figs. 1 to 2 and Figs. 4 to 5, when only one porous layer 7 extends inside one vacant space, the volume of the exposed portion 71 of the one porous layer 7 is preferably 5% to 30% of the volume of the one vacant space. Furthermore, for example, as illustrated in Figs. 7 to 8, when multiple porous layers 7 extend inside one vacant space, the total volume of the exposed portions 71 of the multiple porous layers 7 is preferably 5% to 30% of the volume of the one vacant space.
[0201] In addition, when a plurality of porous layers 7 extend inside one cavity, each of the plurality of porous layers 7 may be in contact with the same side surface 59 of the spacer layer 5, or may be in contact with each of a plurality of different side surfaces 59 of the spacer layer 5. For example, two porous layers 7 facing the third internal void 17 may both be in contact with the right side surface 59r of the spacer layer 5, and in this case, the total volume of the exposed portions 71 of these two porous layers 7 may be 5% or more and 30% or less of the volume of the third internal void 17. Also, for example, a certain porous layer 7 facing the third internal void 17 may be in contact with the right side surface 59r of the spacer layer 5, and another porous layer 7 facing the third internal void 17 may be in contact with the left side surface 59l of the spacer layer 5. In this case, the sum of the volume of the exposed portion 71 of the one porous layer 7 and the volume of the exposed portion 71 of the other porous layer 7 may be 5% or more and 30% or less of the volume of the third inner space 17.
[0202] (VI) Whether the spacer layer needs to be extended inward In the gas sensor element 100 described so far, the porous layer 7 includes the non-exposed portion 72. That is, the porous layer 7 described so far includes the non-exposed portion 72, which is a portion sandwiched between the first solid electrolyte layer 4 or the second solid electrolyte layer 6 and the spacer layer 5 and does not face the measurement target gas flow portion 8. The gas sensor element 100 of FIG. 1 to FIG. 8 includes at least one of the first porous layer 7a disposed between the first solid electrolyte layer 4 and the spacer layer 5 in contact with both, and the second porous layer 7b disposed between the second solid electrolyte layer 6 and the spacer layer 5 in contact with both. For example, in the gas sensor element 100 illustrated in FIG. 2, the first porous layer 7a is disposed between the side surface 59 (particularly, the lower end) of the spacer layer 5 facing the measurement target gas flow portion 8 and the first solid electrolyte layer 4 (particularly, the upper surface) so as not to be in contact with each other. For example, in the gas sensor element 100 illustrated in FIG. 5, a second porous layer 7b is disposed between the spacer layer 5 and the second solid electrolyte layer 6 (particularly, its lower surface) so that the side 59 (particularly, its upper end) of the spacer layer 5 facing the measured gas flow section 8 and the second solid electrolyte layer 6 (particularly, its lower surface) are not in contact with each other.
[0203] However, in the gas sensor element 100, the porous layer 7 is disposed to face the measurement gas flow portion 8 and is in contact with a side surface 59 of the spacer layer 5 facing the measurement gas flow portion 8 and at least one of the first solid electrolyte layer 4 and the second solid electrolyte layer 6. That is, it is not essential for the gas sensor element 100 that the porous layer 7 includes the non-exposed portion 72; the porous layer 7 may or may not include the non-exposed portion 72.
[0204] For example, the porous layer 7 may be disposed at a position corresponding to a corner of a conventional measured gas flow section so as to face the measured gas flow section 8. Specifically, the first porous layer 7a may be disposed inside the measured gas flow section 8 in contact with a contact position between the side surface 59 (particularly, its lower end) of the spacer layer 5 facing the measured gas flow section 8 and the first solid electrolyte layer 4 (particularly, its upper surface). Similarly, the second porous layer 7b may be disposed inside the measured gas flow section 8 in contact with a contact position between the side surface 59 (particularly, its upper end) of the spacer layer 5 facing the measured gas flow section 8 and the second solid electrolyte layer 6 (particularly, its lower surface).
[0205] That is, in the gas sensor element 100, the side surface 59 of the spacer layer 5 facing the measurement gas flow section 8 may be in contact with the upper surface of the first solid electrolyte layer 4 (or the lower surface of the second solid electrolyte layer 6). When the side surface 59 of the spacer layer 5 facing the measurement gas flow section 8 is in contact with the upper surface of the first solid electrolyte layer 4 (or the lower surface of the second solid electrolyte layer 6), the gas sensor element 100 only needs to be provided with the porous layer 7 that is in contact with the contact position between the two and faces the measurement gas flow section 8.
[0206] By disposing the porous layer 7 at a position corresponding to the corner of a conventional measurement gas flow section so as to face the measurement gas flow section 8, it is possible to relieve the stress concentrated at the corner and to prevent cracks from occurring at the corner and its vicinity. Therefore, the gas sensor element 100 can avoid a situation in which "stress is concentrated at the corner of the measurement gas flow section 8, causing cracks at the corner and its vicinity," and can be used for a relatively long period of time without any malfunction, even under harsh operating conditions.
[0207] As described above, the non-exposed portion 72 may be rephrased as a portion extending from the position where the ends (lower end, upper end) of the side 59 of the spacer layer 5 facing the measured gas flow section 8 contact the surface of the porous layer 7 facing the measured gas flow section 8, into the inside of the spacer layer 5.
[0208] (VII) Whether or not there is overlap with the electrode In the gas sensor element 100, the porous layer 7 may or may not overlap a part of the surface of the electrode disposed inside the measured gas flow portion 8 that faces the measured gas flow portion 8.
[0209] For example, as illustrated in Figs. 1 to 3 and 5, the first porous layer 7a may not overlap a part of the surface of the electrode (measurement electrode 44 in the figures) disposed inside the measured gas flow section 8, facing the measured gas flow section 8. As illustrated in Figs. 4, 6 to 8, the first porous layer 7a (porous layer 7) may overlap a part of the surface of the electrode (measurement electrode 44, bottom electrode portion 22b, bottom electrode portion 51b in the figures) disposed inside the measured gas flow section 8, facing the measured gas flow section 8. As illustrated in Figs. 6 to 8, the second porous layer 7b (porous layer 7) may overlap a part of the surface of the electrode (measurement electrode 44, ceiling electrode portion 22a, ceiling electrode portion 51a in the figures) disposed inside the measured gas flow section 8, facing the measured gas flow section 8.
[0210] In the gas sensor element 100 illustrated in Figures 4, 6 to 8, the area of the portion of the electrode disposed inside the measured gas flow section 8 that is overlapped by the porous layer 7 is, for example, 0.5% to 20% of the area of the surface of the electrode facing the measured gas flow section 8.
[0211] (VIII) Configuration of gas sensor element Regarding each component of the gas sensor element 100 in the above embodiment, components may be omitted, replaced, or added as appropriate. In the case where the gas sensor element 100 is configured by stacking solid electrolyte layers, the number of stacked solid electrolyte layers may be changed as appropriate as long as the gas sensor element 100 includes a plurality of solid electrolyte layers.
[0212] In addition, it is not essential for the gas sensor element 100 that the measurement gas flow section 8 is divided into two or more chambers by one or more diffusion rate-controlling sections that provide a predetermined diffusion resistance to the measurement gas. In the examples described so far, the measurement gas flow section 8 is divided into the first internal space 20, the second internal space 40, and the third internal space 17 by the first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, the third diffusion rate-controlling section 30, and the fourth diffusion rate-controlling section 16. However, it is sufficient for the measurement gas flow section 8 to include one or more chambers from which oxygen is pumped out or pumped in, and it is not essential that the measurement gas flow section 8 includes a plurality of chambers. For example, the measurement gas flow section 8 may include two chambers from which oxygen is pumped out or pumped in, or may include only one chamber. In addition, it is not essential for the gas sensor element 100 to include one or more diffusion rate-controlling sections.
[0213] (IX) Arrangement of gas inlet and gas exhaust In the above embodiment, an example has been described in which the gas inlet 10 is provided on the front surface of the gas sensor element 100, but it is not essential for the gas sensor element 100 that the gas inlet 10 is provided on the front surface of the gas sensor element 100. The gas sensor element 100 only needs to be able to take in the measurement gas from the external space into the measurement gas flow portion 8, and the gas inlet 10 may be provided on the right surface or the left surface of the gas sensor element 100, for example.
[0214] Furthermore, the gas sensor element 100 does not necessarily have to include the gas inlet 10. In other words, the gas sensor element 100 is only required to be able to take in the measurement gas from the external space into the measurement gas flow portion 8, and it is not essential that the measurement gas is taken in from the external space through the gas inlet 10. For example, the gas sensor element 100 may take in the measurement gas from the external space into the measurement gas flow portion 8 without including the gas inlet 10 by leaving at least one of the side surfaces 59 of the spacer layer 5 open and not blocked by a dense ceramic layer.
[0215] [Example A (heating test)] In order to verify the effects of the present invention (particularly the effect of inhibiting crack generation), gas sensors according to the following examples and comparative examples were fabricated, although the present invention is not limited to the following examples.
[0216] 1 and 2 were employed for the gas sensor element, and gas sensor elements according to Examples 1 to 11, Comparative Example 2, and Comparative Example 3 were fabricated. Comparative Example 1 is a conventional gas sensor element not provided with a porous layer 7, that is, a gas sensor element in which the rear side of the measurement target gas flow section 8 (e.g., the third internal space 17) is blocked by the front side surface 59f of the spacer layer 5, and the gas sensor element is not provided with a porous layer 7 facing the measurement target gas flow section 8. Except for not providing the porous layer 7, Comparative Example 1 has the same structure as the gas sensor element 100 described so far (e.g., the gas sensor element 100 in FIG. 1). That is, the difference between Comparative Example 1 and Examples 1 to 11, Comparative Example 2, and Comparative Example 3 is whether or not the porous layer 7 is provided.
[0217] As described above, the porous layer 7 is a porous layer, and "porous" means that the porosity is 10% or more. Therefore, the porosity of the porous layer 7 included in the gas sensor elements according to Examples 1 to 11, Comparative Example 2, and Comparative Example 3 is set to 10% or more. The porosity of the porous layer 7 included in the gas sensor elements according to Examples 1 to 11, Comparative Example 2, and Comparative Example 3 is a value measured by analyzing SEM images obtained by observing the porous layer 7 with a scanning electron microscope (SEM).
[0218] 1 and 2, the gas sensor elements according to Examples 1 to 11, Comparative Example 2, and Comparative Example 3 had a porosity of 50% or less in the porous layer 7 (first porous layer 7a) of the gas sensor elements in Examples 1 to 11. In contrast, the porosity of the porous layer 7 of the gas sensor elements in Comparative Examples 2 and 3 was set to a value greater than 50%.
[0219] Specifically, the porosity of the porous layer 7 is 10% in Examples 1 and 2, 15% in Example 3, 20% in Example 4, 25% in Example 5, and 30% in Example 6. It is also 40% in Example 7, 45% in Example 8, 50% in Examples 9 and 10, and 25% in Example 11. In contrast, the porosity of the porous layer 7 in Comparative Example 2 is 55%, and the porosity of the porous layer 7 in Comparative Example 3 is 60%.
[0220] 1 and 2, among the gas sensor elements according to Examples 1 to 11, Comparative Example 2, and Comparative Example 3, Examples 1 to 10 and Comparative Examples 2 to 3 are different from Example 11 in the following respect. That is, Examples 1 to 10 and Comparative Examples 2 to 3 are different from Example 11 in the "ratio of the volume of the exposed portion 71 of the porous layer 7 to the volume of the void (third internal void 17) into which the porous layer 7 (first porous layer 7a) extends." Hereinafter, the "ratio of the volume of the exposed portion 71 of the porous layer 7 to the volume of the void (third internal void 17) into which the porous layer 7 (first porous layer 7a) extends" may be simply referred to as the "volume ratio of the exposed portion 71."
[0221] That is, while the "volume ratio of exposed portion 71" was 5% or more in Examples 1 to 10 and Comparative Examples 2 and 3, in Example 11 it was less than 5%.
[0222] Specifically, the volume percentage of exposed portion 71 is 5.3% in Example 1, 20% in Example 2, 5% in Examples 3 and 5, 16% in Example 4, and 7% in Example 6. The volume percentage of exposed portion 71 is 25% in Example 7, 30% in Example 8, 12% in Example 9, and 24% in Example 10. The volume percentage of exposed portion 71 is 18% in Comparative Example 2 and 20% in Comparative Example 3. In contrast, the volume percentage of exposed portion 71 is 3% in Example 11.
[0223] In order to adjust the "volume ratio of exposed portion 71" in each of Examples 1 to 11, Comparative Example 2, and Comparative Example 3, the thickness of the porous layer 7 (first porous layer 7a) in each of Examples 1 to 11, Comparative Example 2, and Comparative Example 3, in particular the thickness of the exposed portion 71, was set to 10 to 40 μm. That is, by setting the thickness of the exposed portion 71 in each of Examples 1 to 11, Comparative Example 2, and Comparative Example 3 to 10 to 40 μm, the "volume ratio of exposed portion 71" was adjusted for each of Examples 1 to 11, Comparative Example 2, and Comparative Example 3.
[0224] In the gas sensor elements according to Examples 1 to 11, Comparative Example 2, and Comparative Example 3, the volume ratio of the exposed portion 71 was set to 30% or less for the following reasons. That is, if the volume ratio of the exposed portion 71 is set to be greater than 30%, the time required for pumping (discharging) oxygen from the void (third internal void 17) into which the porous layer 7 (first porous layer 7a) extends and for pumping oxygen into the void increases. That is, if the volume ratio of the exposed portion 71 is set to be greater than 30%, the light-off time (the time from when the current starts to flow to the heat generating portion 702 until the NOx concentration can be detected correctly) increases. Therefore, in order to set the light-off time within a range that can withstand the actual use (normal use) of the gas sensor element, the volume ratio of the exposed portion 71 is set to be 30% or less.
[0225] The gas sensor elements according to the above-mentioned respective examples and comparative examples were subjected to the following temperature rise test to evaluate the occurrence of cracks (crack suppression). That is, in the temperature rise test, a current larger than that during actual use (normal use) of the gas sensor element was temporarily passed through the heat generating portion 702 to apply a thermal overload to the gas sensor element. After that, the state of the gas sensor element was inspected to evaluate the occurrence of cracks (crack suppression).
[0226] In the evaluation, the "crack suppression" was rated as "◯" for those in which no cracks occurred even after applying thermal overload (no cracks). The "crack suppression" was rated as "△" for those in which minute cracks occurred after applying thermal overload (there were minute cracks). The "crack suppression" was rated as "×" for those in which cracks that were not minute occurred after applying thermal overload (there were cracks). Table 1 below shows the results of the evaluation of crack occurrence. In Table 1, "Porous layer presence" indicates whether or not the porous layer 7 is provided, and "Porosity" indicates the porosity of the porous layer 7 when the porous layer 7 is provided. In addition, "crack suppression" indicates the presence or absence of cracks after applying thermal overload, and the scale (size) of the cracks if cracks occur.
[0227] [Table 1]
[0228] As shown in the evaluation results in Table 1, each of the Examples had better crack suppression than each of the Comparative Examples. This result shows that the present invention can provide a gas sensor element that can be used for a relatively long period of time without any problems even under severe operating conditions by suppressing the destruction of the internal space (specifically, the occurrence of cracks).
[0229] In particular, in Table 1, the "crack suppression" of Comparative Example 1 is marked with "x", and also Comparative Example 2 in which the porosity of the porous layer 7 is set to 55% and Comparative Example 3 in which the porosity of the porous layer 7 is set to 60% are marked with "x". In contrast, the "crack suppression" of Examples 1 to 10 is marked with "o", and the "crack suppression" of Example 11 is marked with "△". In other words, compared with Comparative Example 1 not provided with the porous layer 7 and Comparative Examples 2 to 3 provided with the porous layer 7 having a porosity greater than 50%, Examples 1 to 11 provided with the porous layer 7 having a porosity of 50% or less were able to improve crack suppression.
[0230] As described above, the porosity of the porous layer 7 is 10% or more. Therefore, it was found that the gas sensor element can suppress the occurrence of cracks (destruction of the internal space) by including the porous layer 7 having a porosity of 10% or more and 50% or less.
[0231] Furthermore, among the gas sensor elements including the porous layer 7 with a porosity of 50% or less, the "crack suppression" of Examples 1 to 10 is "good", whereas the "crack suppression" of Example 11 is "defective". In other words, compared with Example 11 in which the volume ratio of the exposed portion 71 is less than 5%, Examples 1 to 10 in which the volume ratio of the exposed portion 71 is 5% or more were able to improve crack suppression.
[0232] As described above, in consideration of the light-off time, it is preferable that the volume ratio of the exposed portion 71 is 30% or less. Therefore, it has been found that the gas sensor element including the porous layer 7 having a porosity of 10% or more and 50% or less can more effectively suppress the occurrence of cracks (destruction of the internal space) by setting the volume ratio of the exposed portion 71 to 5% or more and 30% or less.
[0233] From these results, it was verified that the above embodiment and modified examples can provide a gas sensor element that can be used for a relatively long period of time without any problems even under harsh operating environments.
[0234] In addition, when the gas sensor element 100 has one or more porous layers 7 facing a certain chamber, it is preferable that the ratio of the total volume of the exposed portions 71 of the one or more porous layers 7 to the volume of the certain chamber is 5% or more and 30% or less.
[0235] For example, when the gas sensor element 100 includes a first porous layer 7a(r) in contact with a right side surface 59r of the spacer layer 5 facing the third internal void 17, and a first porous layer 7a(l) in contact with a left side surface 59l of the spacer layer 5 facing the third internal void 17, the following applies: That is, the sum of the volume of the exposed portion 71a(r) of the first porous layer 7a(r) and the volume of the exposed portion 71a(l) of the first porous layer 7a(l) is 5% or more and 30% or less of the volume of the third internal void 17.
[0236] [Example B (electrode peeling test)] In order to verify the effects of the present invention (particularly, the effect of suppressing electrode peeling), gas sensors according to the following examples were fabricated, although the present invention is not limited to the following examples.
[0237] The gas sensor elements according to Examples 1 to 5 were produced using the gas sensor elements in which no cracks were generated in the above-mentioned temperature rise test. Specifically, the gas sensor elements according to Examples 1 to 5 were produced using the gas sensor elements having the configuration shown in Figs. 1 and 2, in which the porosity of the porous layer 7 was 25%, and the volume ratio of the exposed portion 71 was 15%. Specifically, in the gas sensor elements according to Examples 1 to 5, the thickness of the porous layer 7 (first porous layer 7a), particularly the thickness of the exposed portion 71, was made constant, specifically 20 µm, so that the "volume ratio of the exposed portion 71" of the gas sensor elements according to Examples 1 to 5 was made 15%. As described above, the "volume ratio of the exposed portion 71" refers to the "ratio of the volume of the exposed portion 71 of the porous layer 7 to the volume of the void (third internal void 17) into which the porous layer 7 (first porous layer 7a) extends inwardly."
[0238] In particular, in the gas sensor elements according to Examples 1 to 5, as illustrated in FIG. 4, the porous layer 7 (first porous layer 7a) overlaps a part of the surface of the electrode (measurement electrode 44) disposed inside the cavity (third internal cavity 17) that faces the cavity. The gas sensor elements according to Examples 1 to 5 differ from one another in "the ratio of the area of the part of the surface of the electrode (measurement electrode 44) facing the cavity that is overlapped by the porous layer 7 to the entire area of the surface of the electrode facing the cavity (third internal cavity 17)." Hereinafter, "the ratio of the area of the part of the surface of the electrode facing the cavity that is overlapped by the porous layer 7 to the entire area of the surface of the electrode facing the cavity" may be simply referred to as "area ratio."
[0239] Specifically, the area ratio is 0.25% in Example 1, 5% in Example 2, 10% in Example 3, 15% in Example 4, and 20% in Example 5.
[0240] In the gas sensor elements according to Examples 1 to 5, the area ratio was set to 20% or less for the following reason. That is, if the area ratio was made larger than 20%, the performance of the electrodes (e.g., detection accuracy, etc.) may be degraded. Therefore, in the gas sensor elements according to Examples 1 to 5, the area ratio was set to 20% or less.
[0241] The gas sensor elements according to the above-mentioned respective examples were subjected to an electrode peeling test using the following evaluation system ES to evaluate the electrode peeling suppression effect. That is, the evaluation system ES includes an air blower BL, a gas flow path FP connected to the air blower BL, and the gas sensor elements according to the respective examples fixed to the gas flow path FP.
[0242] In the electrode peeling test, first, the evaluation system ES is placed under an atmospheric atmosphere at room temperature. Then, the flow rate of the gas flow (air flow) by the air blower BL is set to 0 m / sec. Under this condition, the inter-electrode voltage of the measurement pump cell 41 is measured (called the first voltage). Next, one cycle of one minute of normal control (normal use) and one minute of control stop following the normal control is repeated 80,000 times. By the normal control, power is supplied to the heater 70 and signals are transmitted to and received from the electrodes of the gas sensor element according to each embodiment. By the control stop, both the power supply to the heater 70 and the transmission and reception of signals to and from the electrodes of the gas sensor element according to each embodiment are stopped. During the 80,000 cycles, the flow rate by the air blower BL is maintained at 0 m / sec. Next, under the same condition as the first voltage, the inter-electrode voltage of the measurement pump cell 41 is measured (called the second voltage). After the second voltage is measured, the gas sensor element according to each embodiment is disconnected. Then, the boundary between the electrode (measurement electrode 44) and the solid electrolyte layer (first solid electrolyte layer 4) in the cross section was observed using an SEM.
[0243] After 80,000 cycles, the boundary between the measurement electrode 44 and the first solid electrolyte layer 4 was observed, and the "electrode peeling suppression" was evaluated as "A" for those in which no peeling occurred, and the "electrode peeling suppression" was evaluated as "B" for those in which minute peeling occurred. Table 2 below shows the results of evaluating the electrode peeling suppression (electrode peeling suppression effect). "Area ratio (%) of the part where the porous layer overlaps in the electrode" in Table 2 indicates the above-mentioned "area ratio". That is, "area ratio (%) of the part where the porous layer overlaps in the electrode" is another way of saying "the ratio of the area of the part where the porous layer 7 overlaps on the surface of the electrode facing the vacant space to the entire area of the surface of the electrode facing the vacant space". In addition, "electrode peeling suppression" indicates the presence or absence and the scale (size) of peeling of the electrode (measurement electrode 44) from the solid electrolyte layer (first solid electrolyte layer 4) after 80,000 cycles are performed.
[0244] [Table 2]
[0245] As shown in the evaluation results in Table 2, each Example had a good effect of suppressing electrode peeling. That is, it was confirmed that the electrode disposed inside the measured gas flow section 8 (internal space) can be prevented from peeling off from the solid electrolyte layer by arranging the porous layer 7 so as to overlap a part of the surface of the electrode disposed inside the measured gas flow section 8 (internal space) facing the measured gas flow section 8. From this result, it was found that the present invention can provide a gas sensor element that can be used for a relatively long period of time without causing any problems even under severe operating conditions by suppressing the destruction of the internal space (specifically, peeling of the electrode disposed inside the measured gas flow section 8 (internal space) from the solid electrolyte layer).
[0246] In particular, in Table 2, the "electrode peeling prevention" of Example 1 is rated as "B," while the "electrode peeling prevention" of Examples 2 to 5 is rated as "A." In other words, compared to Example 1, in which the area ratio is less than 5%, Examples 2 to 5, in which the area ratio is 5% or more, were able to improve the electrode peeling prevention effect.
[0247] As described above, in consideration of the performance of the electrodes, it is preferable that the area ratio is 20% or less. Therefore, it has been confirmed that in a gas sensor element in which the porous layer 7 is arranged so as to overlap the electrodes disposed inside the measurement gas flow portion 8, peeling of the electrodes (destruction of the internal space) can be more effectively suppressed by setting the area ratio to 0.5% or more and 20% or less. [Explanation of symbols]
[0248] 100...sensor element, 4...first solid electrolyte layer, 4...second solid electrolyte layer, 5...spacer layer, 59f...front side surface (side surface of the spacer layer facing the internal space), 59b... rear surface (a surface of the spacer layer facing the internal space), 59l...left side surface (side surface of the spacer layer facing the internal space), 59r...right side surface (side surface of the spacer layer facing the internal space), 7 ... porous layer, 8 ... measurement gas flow section (internal space), 20…First internal void (vacant), 40…Second internal void (vacant), 17...third internal space (vacant space), 44...measuring electrode (electrode), 22a...Ceiling electrode part (electrode), 22b...Bottom electrode part (electrode), 51a...Ceiling electrode part (electrode), 51b...Bottom electrode part (electrode), 71: exposed portion (portion of the porous layer extending into the cavity), 72: non-exposed portion
Claims
1. a laminate including a first solid electrolyte layer, a second solid electrolyte layer, and a spacer layer, the first solid electrolyte layer and the second solid electrolyte layer being laminated with the spacer layer interposed therebetween, thereby providing an internal space between the first solid electrolyte layer and the second solid electrolyte layer into which a gas to be measured is introduced; One or more porous layers arranged to face the internal space; Equipped with The one or more porous layers include a first porous layer, at least a portion of which is in contact with both at least one side surface of the spacer layer facing the internal space and the first solid electrolyte layer, and is sandwiched between the spacer layer and the first solid electrolyte layer; and a second porous layer, at least a portion of which is in contact with both at least one side surface of the spacer layer facing the internal space and the second solid electrolyte layer, and is sandwiched between the spacer layer and the second solid electrolyte layer; At least one of The porosity of each of the one or more porous layers is 10% or more and 50% or less. Gas sensor element.
2. The thickness of each of the one or more porous layers is 40 μm or less. The gas sensor element according to claim 1 .
3. The thickness of each of the one or more porous layers is 10 μm or more.
3. The gas sensor element according to claim 1.
4. The interior space includes one or more chambers through which oxygen is pumped in or out; one or more of the porous layers extends into at least one of the one or more cavities; the total volume of the portions of the one or more porous layers extending into the voids is 5% or more and 30% or less of the volume of the voids; The gas sensor element according to claim 1 .
5. At least one of the one or more porous layers comprises: a non-exposed portion that is a portion located between the spacer layer and at least one of the first solid electrolyte layer and the second solid electrolyte layer, the non-exposed portion being in contact with both the spacer layer and at least one of the first solid electrolyte layer and the second solid electrolyte layer and not facing the internal space, the volume of the non-exposed portion is 10% or more of the volume of the porous layer including the non-exposed portion; The gas sensor element according to claim 1 .
6. At least one of the one or more porous layers overlaps at least a part of a surface of at least one electrode disposed inside the internal space, the surface being in contact with at least one of the first solid electrolyte layer and the second solid electrolyte layer. The gas sensor element according to claim 1 .
7. an area of the electrode where the porous layer overlaps is 0.5% or more and 20% or less of an area of the opposing surface of the electrode; The gas sensor element according to claim 6.
8. In each of the one or more porous layers, the zirconia content is 50 wt % or more. The gas sensor element according to claim 1 .
9. each of the one or more porous layers is an insulating layer; The gas sensor element according to claim 1 .
Citation Information
Patent Citations
Gas sensor
JP1999237362A
Gas sensor and nitrogen oxide sensor
JP2000028576A
Gas sensor element and method for manufacturing the same
JP2011214848A
Method for manufacturing gas sensor element
JP2011214852A
Gas sensor
JP2015200643A