Ammonia synthesis catalyst, method for producing ammonia synthesis catalyst, and method for synthesizing ammonia

A composite oxide carrier with cerium and praseodymium, supporting ruthenium, addresses the inefficiencies of existing catalysts by enhancing electron donation and promoting the nitrogen-hydrogen reaction for efficient ammonia synthesis.

JP7590730B2Active Publication Date: 2024-11-27KK TOYOTA CHUO KENKYUSHO +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020169151
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-06
Publication Date
2024-11-27
Estimated Expiration
2040-10-06

AI Technical Summary

Technical Problem

Existing ammonia synthesis catalysts, such as those described in JP2016-155123A, JP2017-1037, and JP2017-18907, and the study by LIN Jianxin et al., do not achieve sufficient ammonia production activity, and the effectiveness of alternative carriers beyond Pr6O11, CeO2, and La2O3 has not been demonstrated.

Method used

A composite oxide carrier containing cerium and praseodymium with a molar ratio of 20/80 to 90/10, supporting ruthenium, is used to enhance ammonia production activity by facilitating electron donation from trivalent Ce to Ru, promoting the nitrogen-hydrogen reaction.

Benefits of technology

The catalyst achieves higher ammonia production efficiency by optimizing the cerium-to-praseodymium ratio, leading to improved catalytic activity and efficient ammonia synthesis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590730000002
    Figure 0007590730000002
  • Figure 0007590730000003
    Figure 0007590730000003
  • Figure 0007590730000001
    Figure 0007590730000001
Patent Text Reader

Abstract

To provide an ammonia synthesis catalyst that has excellent ammonia formation activity and can more efficiently synthesize ammonia.SOLUTION: Provided is an ammonia synthesis catalyst that is characterized by comprising a composite oxide carrier containing cerium and praseodymium, and ruthenium supported on the composite oxide carrier, and having a mole ratio of cerium and praseodymium ([cerium] / [praseodymium]) contained in the composite oxide carrier of 20 / 80 to 90 / 10.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ammonia synthesis catalyst, a method for producing an ammonia synthesis catalyst, and a method for synthesizing ammonia. [Background technology]

[0002] In recent years, ammonia has been attracting attention as a component that can be used as an energy carrier for hydrogen energy, etc. As a method for synthesizing such ammonia, the Haber-Bosch process using an iron-based catalyst has been used industrially, but in recent years, research on various types of ammonia synthesis catalysts has been conducted with the aim of synthesizing ammonia under milder conditions than those of the Haber-Bosch process.

[0003] For example, JP 2016-155123 A (Patent Document 1) discloses an ammonia synthesis catalyst in which ruthenium is supported in layers on a praseodymium oxide carrier. In addition, JP 2017-1037 A (Patent Document 2) discloses a catalyst composition for ammonia production, which is a composition in which a carrier made of a compound containing lanthanoid is used as a forming material, a first component containing ruthenium, an alloy containing ruthenium, or a compound containing ruthenium supported on the carrier, and a second component which is a compound containing an alkali metal and / or a porous metal complex are mixed. In addition, JP 2017-18907 A (Patent Document 3) discloses, in Examples 1 to 3, a catalyst composition obtained by subjecting a ruthenium-praseodymium oxide composition in which ruthenium is supported on praseodymium oxide and a milled mixed composition of cesium carbonate to hydrogen reduction. However, the catalysts and catalyst compositions disclosed in Patent Documents 1 to 3 were not sufficient in terms of ammonia production activity. In addition, although Patent Document 2 describes a carrier made of a compound containing lanthanoid as a carrier for the first component, the carrier for the first component actually demonstrated in the examples is Pr 6 O 11 , CEO 2 Or La 2 O 3However, the effects of the first component using other carriers have not been demonstrated.

[0004] Furthermore, LIN Jianxin et al., “Effects of Pr Doping on Structure and Catalytic Performance of Ru / CeO 2 In "CeO Catalyst for Ammonia Synthesis", Chinese Journal of Catalysis, vol. 33, No. 3, pp. 536-542, 2012, it is described that the content (addition amount) of Pr (metal) relative to the metal components in the carrier is 0 mol%, 1 mol%, 2 mol%, 4 mol%, and 6 mol%. 2 A support with Pr added (CeO 2 (Solo) or CeO 2 -PrO 2 ) supported by Ru was investigated for use in the synthesis of ammonia, and CeO 2 A support with Pr added (CeO 2 -PrO 2 The catalyst with Ru supported on CeO 2 (Single) Ru-supported catalyst (Ru / CeO 2 It has been reported that the catalyst exhibits higher activity than that of the catalyst described in Non-Patent Document 1, and that the amount of ammonia produced is maximum when the Pr content (addition amount) is 4 mol %. However, even the catalyst described in Non-Patent Document 1 does not have sufficient ammonia production activity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-155123 A [Patent Document 2] JP 2017-1037 A [Patent Document 3] JP 2017-18907 A [Non-patent literature]

[0006] [Non-Patent Document 1] LIN Jianxin et al., “Effects of Pr Doping on Structure and Catalytic Performance of Ru / CeO2 Catalyst for Ammonia Synthesis”, Chinese Journal of Catalysis, 2012, vol. 33, No. 3, pp. 536-542 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the problems associated with the above-mentioned conventional techniques, and an object of the present invention is to provide an ammonia synthesis catalyst which is excellent in ammonia generating activity and enables ammonia to be synthesized more efficiently, a method for producing an ammonia synthesis catalyst which enables the efficient production of the ammonia synthesis catalyst, and a method for synthesizing ammonia using the ammonia synthesis catalyst. [Means for solving the problem]

[0008] As a result of intensive research into achieving the above-mentioned object, the inventors have found that an ammonia synthesis catalyst comprising a composite oxide support containing cerium and praseodymium; and ruthenium supported on the composite oxide support, in which the molar ratio of cerium to praseodymium contained in the composite oxide support ([cerium] / [praseodymium]) is 20 / 80 to 90 / 10, can provide an excellent ammonia production activity of the catalyst, thereby enabling ammonia to be synthesized more efficiently, and have completed the present invention.

[0009] That is, the ammonia synthesis catalyst of the present invention is a composite oxide support containing cerium and praseodymium; Ruthenium supported on the composite oxide support; and The molar ratio of cerium to praseodymium contained in the composite oxide support ([cerium] / [praseodymium]) is 25 / 75 It is characterized in that:

[0013] The method for synthesizing ammonia of the present invention is characterized in that a gas containing hydrogen and nitrogen is brought into contact with the ammonia synthesis catalyst of the present invention to synthesize ammonia.

[0014] Although the reason why the above object is achieved by the present invention is not necessarily clear, the present inventors speculate as follows. That is, first, in the ammonia synthesis catalyst of the present invention, a composite oxide support containing cerium (Ce) and praseodymium (Pr) is used as a support. Here, since praseodymium oxide is more easily reduced than cerium oxide, it is considered that the oxygen shared by cerium and praseodymium in the composite oxide support is in a state in which it is easier to attract electrons from praseodymium than cerium (a state in which it is easier to be reduced by praseodymium). Therefore, it is considered that the cerium in the composite oxide support is in a state in which it is easier to reduce. Therefore, in such a composite oxide support, the valence of Ce is more likely to change from 4 to 3 due to the presence of Pr in the support, and the CeO in the support is more likely to be reduced. 2The reducibility of is further improved. Here, in the present invention, the molar ratio of Ce to Pr (Ce / Pr ratio) contained in the composite oxide support is 20 / 80 to 90 / 10. Thus, in the composite oxide support according to the present invention, Pr is contained in an amount of 10 mol% to 80 mol% with respect to the total molar amount (total molar amount) of Ce and Pr in the composite oxide support. Since Pr is contained in such a ratio, in the present invention, the amount of Ce in the composite oxide is sufficient, and the effect of changing the valence of Ce from tetravalent to trivalent in the composite oxide can be sufficiently and efficiently caused. As a result, in the ammonia synthesis catalyst of the present invention, it is possible to more efficiently cause electron donation from trivalent Ce to Ru, which is an active species, and when nitrogen is brought into contact with Ru, it is possible to more efficiently cause activation of nitrogen. Therefore, the present inventors presume that the reaction between nitrogen and hydrogen is promoted, and the generation of ammonia proceeds more efficiently. As described above, the present inventors presume that in the present invention, based on the configuration of the composite oxide support, it is possible to sufficiently and efficiently bring about the effect of changing the valence of Ce from tetravalent to trivalent, which enables the active species Ru to more efficiently donate electrons, resulting in higher ammonia production activity and enabling ammonia to be synthesized more efficiently. Effect of the Invention

[0015] According to the present invention, it is possible to provide an ammonia synthesis catalyst that has excellent ammonia generating activity and enables ammonia to be synthesized more efficiently, a method for producing an ammonia synthesis catalyst that enables the efficient production of the ammonia synthesis catalyst, and a method for synthesizing ammonia using the ammonia synthesis catalyst. [Brief description of the drawings]

[0016] [Figure 1] 1 is a graph showing the ammonia production rates of the catalysts obtained in Example 1, Reference Examples 1 to 3, and Comparative Examples 1 to 6. [Diagram 2]1 is a graph showing the relationship between the praseodymium content (mol %) in the composite oxide support used in the catalysts obtained in Example 1, Reference Examples 1 to 3, and Comparative Examples 1 to 6, and the ammonia production rate of the catalysts obtained in Example 1, Reference Examples 1 to 3, and Comparative Examples 1 to 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below based on preferred embodiments thereof.

[0018] [Ammonia synthesis catalyst] The ammonia synthesis catalyst of the present invention comprises a composite oxide support containing cerium and praseodymium; and ruthenium supported on the composite oxide support, and is characterized in that the molar ratio of cerium to praseodymium contained in the composite oxide support ([cerium] / [praseodymium]) is 20 / 80 to 90 / 10.

[0019] The composite oxide support according to the present invention is a composite oxide support containing cerium and praseodymium. Such a composite oxide support may contain cerium and praseodymium, and may further contain other components (other metals) known to be used in catalyst supports in the field of ammonia synthesis. In such a composite oxide support, the content of cerium and praseodymium relative to the total metal components contained in the composite oxide support is preferably 70 to 100 mol%, more preferably 80 to 100 mol%, and particularly preferably 90 to 100 mol%, calculated as metal.

[0020] In addition, in the composite oxide carrier according to the present invention, the molar ratio of cerium and praseodymium contained in the composite oxide carrier ([cerium] / [praseodymium]) must be 20 / 80 to 90 / 10. With regard to such a molar ratio, if the content of cerium is less than the lower limit, the amount of cerium that donates electrons to the active species Ru is reduced, and the catalytic activity is reduced. On the other hand, if the content of cerium in the molar ratio exceeds the upper limit, cerium cannot be sufficiently reduced, and therefore cerium cannot sufficiently donate electrons to the active species Ru, and the catalytic activity is reduced. From the same viewpoint, the molar ratio of cerium and praseodymium contained in such a composite oxide carrier ([cerium] / [praseodymium]) is more preferably 25 / 75 to 80 / 20, and even more preferably 25 / 75 to 75 / 25. The "molar ratio of cerium and praseodymium" referred to here refers to the molar ratio of cerium and praseodymium, which are metal components constituting the composite oxide carrier, in terms of metal.

[0021] In addition, when such a composite oxide support contains a metal other than cerium and praseodymium, such a metal is not particularly limited, and any metal that can be used as a catalyst support in the field of ammonia synthesis can be appropriately used. Examples of such a metal include Sc, Y, La, etc.

[0022] The shape of such a composite oxide support is not particularly limited, and may be a conventionally known shape such as a ring shape, a sphere shape, a cylinder shape, a particulate shape, a pellet shape, etc. From the viewpoint of being able to contain more Ru in a highly dispersible state, it is preferable to use a particulate one. When such a composite oxide support is particulate, the average particle diameter of the support is preferably 0.1 to 100 μm.

[0023] The specific surface area of ​​such a composite oxide support is not particularly limited, but is preferably 1 to 300 m 2 / g, and 10 to 200m 2 / g is more preferable. If the specific surface area is less than the lower limit, the dispersibility of the supported Ru decreases, and the catalytic performance (ammonia production activity) tends to decrease, while if the specific surface area exceeds the upper limit, the heat resistance of the support decreases, and the catalytic performance tends to decrease. Note that such a specific surface area can be calculated as a BET specific surface area from the adsorption isotherm using the BET isothermal adsorption formula. Note that such a BET specific surface area can be determined using a commercially available device.

[0024] As a method for producing such a composite oxide support, it is preferable to adopt a method for producing a composite oxide support by the same process as the "process for obtaining a composite oxide support containing cerium and praseodymium" in the method for producing an ammonia synthesis catalyst of the present invention described below. In addition, such a composite oxide support is preferably one produced by producing a precipitate by a coprecipitation method using a cerium salt and a praseodymium salt, and then calcining the precipitate. When a composite oxide support obtained by such a coprecipitation method is used, the uniformity of cerium and praseodymium in the support is improved, making it possible to obtain better catalytic activity.

[0025] In the ammonia synthesis catalyst of the present invention, ruthenium is supported on the composite oxide carrier. The amount of ruthenium supported is not particularly limited, but is preferably 0.5 to 10 parts by mass (more preferably 1 to 5 parts by mass) in terms of metal (metal equivalent) of ruthenium relative to 100 parts by mass of the composite oxide carrier. If the amount of ruthenium supported is less than the lower limit, there is a tendency that a sufficiently high ammonia production activity cannot be obtained, while if the amount of ruthenium supported is more than the upper limit, sintering of ruthenium is likely to occur depending on the usage environment, and the degree of dispersion of ruthenium, which is an active site, is likely to decrease, making it difficult to obtain an effect corresponding to the amount of ruthenium used, which tends to be disadvantageous in terms of cost, etc.

[0026] The particle size (average particle size) of ruthenium supported on the composite oxide carrier is not particularly limited, but is preferably 0.5 to 100 nm (more preferably 1 to 50 nm). If the particle size of ruthenium is less than the lower limit, it tends to be difficult to utilize it in a metallic state, while if it exceeds the upper limit, the amount of active sites as a catalyst tends to decrease significantly.

[0027] In the ammonia synthesis catalyst of the present invention, other known supported components (additives, etc.) that are used in the field of ammonia synthesis catalysts by being supported on a support may be appropriately supported on the composite oxide support within a range that does not impair the effects of the present invention. Examples of such other supported components include Sc, Y, La, etc.

[0028] The form of the ammonia synthesis catalyst of the present invention is not particularly limited, and can be, for example, a honeycomb-shaped monolith catalyst, a pellet-shaped pellet catalyst, or the like, and can also be in the form of a powder catalyst that is directly placed at a desired location. The method for obtaining such various forms of ammonia synthesis catalyst is not particularly limited, and can be manufactured by appropriately adopting a known molding method for the ammonia synthesis catalyst, and for example, a method of molding the ammonia synthesis catalyst into a pellet shape to obtain an ammonia synthesis catalyst in the form of a pellet shape, or a method of coating the ammonia synthesis catalyst on a catalyst substrate to obtain an ammonia synthesis catalyst in the form of a catalyst substrate coated (fixed) thereon, and the like may be appropriately adopted. The catalyst substrate is not particularly limited, and can be appropriately selected depending on the method of use of the ammonia synthesis catalyst, and for example, a monolith-shaped substrate, a pellet-shaped substrate, a plate-shaped substrate, and the like can be suitably adopted. The material of such a catalyst substrate is also not particularly limited, and can be, for example, a substrate made of ceramics such as cordierite, silicon carbide, or mullite, or a substrate made of metal such as stainless steel containing chromium and aluminum, and the like. Furthermore, the ammonia synthesis catalyst of the present invention may be used in combination with other catalysts.

[0029] In addition, the method for producing such an ammonia synthesis catalyst of the present invention is not particularly limited, but it is preferable to employ the method for producing the ammonia synthesis catalyst of the present invention described below, since it enables the ammonia synthesis catalyst of the present invention to be formed more efficiently.

[0030] [Method for producing ammonia synthesis catalyst] The method for producing an ammonia synthesis catalyst of the present invention is a method characterized by comprising the steps of: using a composite oxide support forming solution containing a cerium salt and a praseodymium salt in a molar ratio of cerium to praseodymium ([cerium] / [praseodymium]) of 20 / 80 to 90 / 10, generating a precipitate containing cerium and praseodymium in the solution by a coprecipitation method, and then calcining the precipitate to obtain a composite oxide support containing cerium and praseodymium (hereinafter sometimes simply referred to as a "support preparation step"); and supporting ruthenium on the composite oxide support using a solution of a ruthenium salt, and then calcining the support under a reducing gas atmosphere or an inert gas atmosphere to obtain the ammonia synthesis catalyst of the present invention (hereinafter sometimes simply referred to as a "catalyst preparation step").

[0031] <Carrier preparation process> In the method for producing an ammonia synthesis catalyst of the present invention, first, a composite oxide support forming solution containing a cerium salt and a praseodymium salt in a molar ratio of cerium to praseodymium ([cerium] / [praseodymium]) of 20 / 80 to 90 / 10 is used, and a precipitate containing cerium and praseodymium is generated in the solution by a coprecipitation method, and then the precipitate is calcined to obtain a composite oxide support containing cerium and praseodymium (support preparation step).

[0032] The cerium salt used in such a carrier preparation step is not particularly limited, and sulfates, nitrates, chlorides, acetates, various complexes, etc. can be appropriately used, for example, cerium nitrate, ceric ammonium nitrate, cerium acetate, etc. In addition, the praseodymium salt is also not particularly limited, and sulfates, nitrates, chlorides, acetates, various complexes, etc. can be appropriately used, for example, praseodymium nitrate, praseodymium acetate, etc.

[0033] The solvent of the composite oxide support forming solution containing the cerium salt and the praseodymium salt is not particularly limited, but a solvent capable of dissolving the cerium salt and the praseodymium salt to form their ions (cerium ions, praseodymium ions) can be preferably used. Examples of such a solvent include water and alcohol, and water can be preferably used from the viewpoints of cost and safety.

[0034] Moreover, such a composite oxide support forming solution contains the cerium salt and the praseodymium salt in a molar ratio of cerium to praseodymium ([cerium] / [praseodymium]) of 20 / 80 to 90 / 10 (more preferably 25 / 75 to 80 / 20, and even more preferably 25 / 75 to 75 / 25). By using the cerium salt and the praseodymium salt in such a molar ratio, it becomes possible to obtain a composite oxide support that contains cerium and praseodymium and has a molar ratio of cerium to praseodymium ([cerium] / [praseodymium]) of 20 / 80 to 90 / 10 (more preferably 25 / 75 to 80 / 20, and even more preferably 25 / 75 to 75 / 25). In this way, the molar ratio of cerium to praseodymium in the solution for forming a composite oxide support can basically be directly reflected in the molar ratio of cerium to praseodymium in the obtained composite oxide support, and therefore it is preferable to set the molar ratio of Ce to Pr in the solution within the above-mentioned ratio range depending on the design of the composite oxide support.

[0035] In the carrier preparation step using such a composite oxide carrier forming solution, a precipitate containing cerium and praseodymium is formed in the solution by a coprecipitation method. The coprecipitation method is not particularly limited as long as it is a method capable of coprecipitating cerium ions and praseodymium ions in the composite oxide carrier forming solution, and any known method can be appropriately adopted.

[0036] In addition, in the present invention, from the viewpoint of facilitating the production of particles having a more uniform size, shape and composition, it is preferable to adopt a method of using the above-mentioned composite oxide support forming solution further containing urea and heating the solution to produce a precipitate (co-precipitate) containing cerium and praseodymium as the co-precipitation method. In this way, by heating the above-mentioned composite oxide support forming solution further containing urea, the urea is hydrolyzed to produce ammonia and carbon dioxide (CO 2 ) to generate a more uniform precipitate, and it is possible to obtain a precipitate in which cerium and praseodymium are more finely dispersed and mixed. From the viewpoint of generating a more uniform precipitate, it is preferable that the composite oxide support forming solution further contains urea. Moreover, it is preferable that such a composite oxide support forming solution further contains urea in a molar amount that is 8 to 20 times (more preferably 10 to 15 times) the total molar amount of cerium and praseodymium contained in the solution. If the content of urea is less than the lower limit, it becomes difficult to precipitate all of the cerium ions and praseodymium ions in the composite oxide support forming solution, and it tends to be difficult to form a composite oxide support of the intended design. On the other hand, if the content exceeds the upper limit, no further effect of addition of urea is obtained, and the economic efficiency tends to decrease.

[0037] In addition, when the method of heating the solution for forming a composite oxide support containing urea is adopted for generating the precipitate (co-precipitate), the heating temperature is preferably 90°C or higher, more preferably 90 to 98°C. If the heating temperature is less than the lower limit, urea is not hydrolyzed, and a precipitate tends not to be generated. In addition, when the solution for forming a composite oxide support containing urea is heated in this way, from the viewpoint of obtaining a precipitate in which cerium and praseodymium are more uniformly dispersed, it is preferable to heat the solution for forming a composite oxide support while stirring it to generate a precipitate (co-precipitate) containing cerium and praseodymium. In addition, when the solution for forming a composite oxide support containing urea is heated, the heating time (the time for performing the reaction for generating a precipitate, and the stirring and heating time when stirring is performed) is not particularly limited, but is preferably 5 to 12 hours (more preferably 5 to 8 hours). If the heating time is less than the lower limit, the precipitate cannot be sufficiently formed, and it tends to be difficult to form a composite oxide support of the intended design.

[0038] In the composite oxide carrier preparation step, the precipitate is generated by the coprecipitation method as described above, and then the precipitate is calcined. By such a calcination step, it is possible to prepare a composite oxide carrier containing cerium and praseodymium. The calcination temperature in such a calcination step is preferably 650 to 800°C, more preferably 700 to 800°C. The calcination time is preferably 3 to 20 hours, more preferably 5 to 10 hours. If the calcination temperature or the calcination time is below the lower limit, the carbonates of cerium and praseodymium that may be contained in the precipitate cannot be sufficiently decomposed, and the composite oxide carrier containing the desired cerium and praseodymium tends not to be efficiently obtained. On the other hand, if the calcination temperature or the calcination time exceeds the upper limit, the particles of the composite oxide containing cerium and praseodymium grow and the specific surface area becomes small, so that when Ru is supported, Ru cannot be sufficiently dispersed and supported, and sufficient catalytic performance (catalytic activity) tends not to be obtained. The atmosphere in such a firing step is not particularly limited, but may be an oxidizing atmosphere (e.g., air) or an inert gas (e.g., N 2 ) atmosphere is favorable.

[0039] In the carrier preparation step, from the viewpoint of uniform heating (decomposition), it is preferable to perform a treatment for drying the precipitate before carrying out the calcination step. The method of such a drying treatment is not particularly limited, but it is preferable to adopt a method of leaving it to stand in the air at 70°C to 200°C for 5 to 20 hours.

[0040] <Catalyst preparation process> In the method for producing the ammonia synthesis catalyst of the present invention, after obtaining the composite oxide support as described above, ruthenium is supported on the composite oxide support using a solution of a ruthenium salt, and then the support is calcined under a reducing gas atmosphere or an inert gas atmosphere to obtain the ammonia synthesis catalyst of the present invention (catalyst preparation step).

[0041] The ruthenium salt used in such a catalyst preparation step is not particularly limited, and examples of the ruthenium salt that can be used include ruthenium acetate, ruthenium carbonate, ruthenium nitrate, ruthenium ammonium salt, ruthenium citrate, ruthenium dinitrodiammine salt, and ruthenium complexes (e.g., tetraammine complexes and carbonyl complexes). In addition, the ruthenium salt is not particularly limited, and examples thereof include dodecacarbonyltriruthenium (Ru 3 (CO) 12 ), ruthenium chloride, ruthenium acetylacetonate, ruthenium nitrosyl nitrate, ruthenium nitrate, and the like can be given as suitable examples.

[0042] In addition, the solvent used for such a ruthenium salt solution (a solution containing a ruthenium salt) is not particularly limited, but a solvent capable of forming ruthenium ions by dissolving the ruthenium salt can be appropriately used. For example, tetrahydrofuran (THF), water, alcohol, etc. can be suitably used as such a solvent. The content of the ruthenium salt in such a solution is not particularly limited, and the amount (concentration, etc.) can be appropriately changed depending on the target amount of ruthenium supported.

[0043] The method of supporting ruthenium on the composite oxide support using the ruthenium salt solution is not particularly limited, but for example, a method of supporting ruthenium on the composite oxide support by contacting the solution with the composite oxide support and then drying the composite oxide support can be preferably adopted. The method of contacting the solution with the support is not particularly limited, but for example, a method of impregnating the composite oxide support with the ruthenium salt solution, a method of adsorbing the ruthenium salt solution on the composite oxide support, etc. can be mentioned as a suitable method. The method of drying is not particularly limited, and for example, a method of leaving the composite oxide support after contacting the solution at rest under a temperature condition of 50 to 150 ° C. may be adopted.

[0044] Furthermore, when ruthenium is supported on the composite oxide support, it is preferable to support ruthenium on the composite oxide support using a solution of a ruthenium salt such that the amount of ruthenium (metal) supported on the composite oxide support is 0.5 to 10 parts by mass (more preferably 1 to 5 parts by mass) in terms of ruthenium metal per 100 parts by mass of the composite oxide support.

[0045] In the present invention, after ruthenium is supported on the composite oxide support as described above, the support is calcined in a reducing gas atmosphere or an inert gas atmosphere. By using a reducing gas atmosphere or an inert gas atmosphere during calcination, it becomes possible to reduce ruthenium to a metallic state and support it on the support.

[0046] In addition, the "reducing gas atmosphere" refers to an atmosphere containing a reducing gas (e.g., hydrogen gas, carbon monoxide gas, hydrocarbon gas, etc.), for example, H 2 Ar gas atmosphere containing H 2 N containing gas 2 Examples of the reducing gas atmosphere include a gas atmosphere. The reducing gas atmosphere is preferably an atmosphere consisting of a mixed gas of a reducing gas and an inert gas (e.g., nitrogen, argon, etc.). The reducing gas atmosphere is preferably a gas atmosphere containing a reducing gas at a ratio of 1 to 30% by volume (more preferably 5 to 20% by volume). Furthermore, the reducing gas contained in the reducing gas atmosphere is more preferably hydrogen gas. In addition, the "inert gas atmosphere" as used herein refers to an atmosphere consisting of an inert gas. Examples of such inert gas include nitrogen, helium, neon, krypton, argon, and other gases.

[0047] The atmosphere for calcining the support after supporting ruthenium is preferably a reducing gas atmosphere from the viewpoint of more efficiently reducing ruthenium to a metal state, and is preferably an inert gas atmosphere from the viewpoint of safety. When the reducing gas atmosphere is used for calcining the support after supporting ruthenium, it is more preferable that the reducing gas atmosphere is a gas atmosphere capable of hydrogen reduction (an atmosphere containing hydrogen gas as a reducing gas) from the viewpoint of more efficiently reducing ruthenium to a metal state.

[0048] In addition, in such calcination under a reducing gas atmosphere or an inert gas atmosphere, the heating temperature is preferably 200 to 500°C (more preferably 300 to 500°C). In addition, in such calcination under a reducing gas atmosphere, the heating time varies depending on the heating temperature and cannot be generally stated, but is preferably 0.5 to 10 hours, more preferably 1 to 3 hours. If the heating temperature and heating time during such calcination are less than the lower limit, all ruthenium cannot be sufficiently reduced to a metal state (metallic state), and ruthenium in a precursor state tends to remain. On the other hand, if the upper limit is exceeded, the supported particles are sintered, making it difficult to support metallic ruthenium in a sufficiently dispersed state, and the catalytic activity tends to decrease.

[0049] In this manner, ruthenium is supported on the composite oxide support, and then the support is calcined under a reducing gas atmosphere or an inert gas atmosphere to obtain the ammonia synthesis catalyst of the present invention (an ammonia synthesis catalyst comprising a composite oxide support containing cerium and praseodymium, and ruthenium supported on the composite oxide support, wherein the molar ratio of cerium to praseodymium contained in the composite oxide support ([cerium] / [praseodymium]) is 20 / 80 to 90 / 10).

[0050] [Method of synthesizing ammonia] The method for synthesizing ammonia of the present invention is a method characterized by synthesizing ammonia by contacting a gas containing hydrogen and nitrogen with the above-mentioned ammonia synthesis catalyst of the present invention.

[0051] Such an ammonia synthesis method of the present invention is not particularly limited except that the above-mentioned ammonia synthesis catalyst of the present invention is used as a catalyst. For example, except that the above-mentioned ammonia synthesis catalyst of the present invention is used as a catalyst, a method similar to a known method of synthesizing ammonia by contacting a gas containing hydrogen and nitrogen with a catalyst may be adopted.

[0052] In the reaction of synthesizing ammonia from hydrogen and nitrogen, theoretically, 2 moles of ammonia can be obtained by reacting 1 mole of nitrogen with 3 moles of hydrogen (N 2 +3H 2 →2NH 3 Therefore, the "gas containing hydrogen and nitrogen" used in the ammonia synthesis method of the present invention has a molar ratio of hydrogen to nitrogen (H 2 / N 2 It is preferable to use a gas having a ratio of 0.5 / 1 to 3 / 1 (more preferably 1.5 / 1 to 3 / 1). The "gas containing hydrogen and nitrogen" used in the synthesis of ammonia may further contain an inert gas (argon, etc.) as a carrier gas in addition to hydrogen gas and nitrogen gas, but from the viewpoint of increasing the amount of product (ammonia), it is preferable to use a gas consisting of only hydrogen gas and nitrogen gas.

[0053] In addition, the method of contacting the ammonia synthesis catalyst with a gas containing hydrogen and nitrogen is not particularly limited, and any known method capable of contacting a catalyst with a gas can be appropriately adopted. As a method of contacting the ammonia synthesis catalyst with a gas containing hydrogen and nitrogen, for example, a method of contacting the ammonia synthesis catalyst with a gas containing hydrogen and nitrogen by filling a sealable reaction vessel with the ammonia synthesis catalyst and then replacing the atmospheric gas in the reaction vessel with the gas containing hydrogen and nitrogen, a method of placing the ammonia synthesis catalyst inside a gas flow pipe and flowing the gas containing hydrogen and nitrogen through the gas flow pipe to contact the ammonia synthesis catalyst with the gas containing hydrogen and nitrogen, etc. can be appropriately adopted.

[0054] Furthermore, when a reaction for synthesizing ammonia is carried out by contacting a gas containing hydrogen and nitrogen with the ammonia synthesis catalyst of the present invention, the reaction temperature is preferably 300 to 500° C., more preferably 350 to 450° C., from the viewpoint that the equilibrium concentration decreases as the temperature increases. The pressure condition when carrying out such a reaction is not particularly limited, and is preferably 0.1 to 10 MPa, more preferably 1 to 8 MPa, since it is possible to further reduce the energy required for ammonia production.

[0055] According to the method for synthesizing ammonia of the present invention, since the ammonia synthesis catalyst of the present invention used as a catalyst has excellent ammonia generating activity, it becomes possible to synthesize ammonia more efficiently. EXAMPLES

[0056] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0057] ( Reference example 1 ) First, cerium (III) nitrate hexahydrate, praseodymium (III) nitrate hexahydrate, and urea were dissolved in ion-exchanged water to obtain a solution for forming a composite oxide support. In preparing such a solution for forming a composite oxide support, cerium (III) nitrate hexahydrate and praseodymium (III) nitrate hexahydrate were used in amounts such that the total amount of metal components cerium (Ce) and praseodymium (Pr) (molar amount of Ce + molar amount of Pr) was 0.15 mol / L per 1 L of solution, and the molar ratio of Ce to Pr (Ce / Pr) was 75 / 25. In addition, in preparing such a solution for forming a composite oxide support, urea was used so that the content of urea in the solution was 2 mol / L (a molar amount that is 13.3 times the total molar amount of Ce and Pr in the solution).

[0058] Next, the composite oxide support forming solution was heated to 95°C in the air, and then stirred for 5 hours while maintaining the temperature at 95°C, thereby forming a precipitate in the solvent. The precipitate in the solution was then washed and collected by performing a process of suction filtration while washing with ion-exchanged water. The precipitate was then dried overnight (12 hours) at 100°C, and then calcined at 700°C for 5 hours to obtain a composite oxide support containing Ce and Pr. It is clear that the molar ratio of Ce to Pr (Ce / Pr) in the composite oxide support thus obtained was 75 / 25 due to the composition of the composite oxide support forming solution.

[0059] Next, Ru 3 (CO) 12 In tetrahydrofuran (THF), 3 (CO) 12A THF solution (concentration: 3 mmol / L) was prepared, and the composite oxide support obtained as described above was impregnated with the THF solution. The solvent was then removed to support ruthenium (Ru) on the composite oxide support, thereby obtaining a catalyst precursor. In the step of obtaining such a catalyst precursor, the amount of the THF solution used was adjusted so that the amount of Ru supported in the finally obtained ammonia synthesis catalyst was 3 parts by mass, calculated as Ru metal, per 100 parts by mass of the composite oxide support. The catalyst precursor was then dried by maintaining it at 70° C. for 12 hours. Next, the dried catalyst precursor was subjected to H 2 (10% by volume) and N 2 (90% by volume) at 300°C for 1 hour (reduction treatment), to obtain an ammonia synthesis catalyst comprising the composite oxide support containing Ce and Pr and Ru supported on the composite oxide support.

[0060] Example 1 and Reference Examples 2 to 3 ) When preparing the composite oxide support solution, the molar ratio of Ce and Pr (Ce / Pr) was 50 / 50 ( Reference example 2 ), 25 / 75 (Example 1 ), 90 / 10( Reference example 3 ) except for changing the amounts of cerium(III) nitrate hexahydrate and praseodymium(III) nitrate hexahydrate used. Reference example 1 In the same manner as above, an ammonia synthesis catalyst was obtained.

[0061] (Comparative Examples 1 to 5) In preparing the composite oxide support forming solution, the amounts of cerium (III) nitrate hexahydrate and praseodymium (III) nitrate hexahydrate used were changed so that the molar ratio of Ce to Pr (Ce / Pr) was 100 / 0 (Comparative Example 1), 95 / 5 (Comparative Example 2), 10 / 90 (Comparative Example 3), 5 / 95 (Comparative Example 4), and 0 / 100 (Comparative Example 5), respectively. Reference example 1 In the same manner as above, ammonia synthesis catalysts for comparison were obtained.

[0062] Comparative Example 6 Cerium (III) nitrate hexahydrate and praseodymium (III) nitrate hexahydrate were dissolved in ion-exchanged water to obtain solution (A). In preparing such solution (A), cerium (III) nitrate hexahydrate and praseodymium (III) nitrate hexahydrate were used so that the total amount of Ce and Pr (molar amount of Ce + molar amount of Pr) was 0.2 mol / L per 1 L of solution and the molar ratio of Ce to Pr (Ce / Pr) was 95 / 5.

[0063] Next, K 2 RuO 4 Aqueous solution (K 2 RuO 4 A solution (B) was obtained by dissolving the Ru-containing ruthenium oxide (concentration: 0.4 mol / L) in a KOH aqueous solution (KOH concentration: 2.0 mol / L). When obtaining such a solution (B), the KOH concentration was adjusted so that the amount of Ru supported in the finally obtained ammonia synthesis catalyst was 3 parts by mass in terms of Ru metal per 100 parts by mass of the composite oxide support. 2 RuO 4 The amount of the aqueous solution used was adjusted, and the amount of the aqueous KOH solution used was also adjusted so that the amount of KOH was 4.5 times the total molar amount of Ce and Pr in solution (A).

[0064] Next, while stirring the solution (A), the solution (B) was dropped into the solution (A) to obtain a mixed solution. In addition, a black precipitate was generated in such a mixed solution by dropping the solution (B). Next, the mixed solution was heated to 60°C, and then stirred for 1 hour while maintaining the temperature at 60°C. Thereafter, the precipitate precipitated in the mixed solution was washed and collected by performing a process of suction filtration while washing with ion-exchanged water. Next, the precipitate thus obtained was dried overnight (12 hours) at 85°C, and then calcined at 500°C for 1 hour to obtain an ammonia synthesis catalyst for comparison (a catalyst in which the amount of Ru supported per 100 parts by mass of the composite oxide support is 3 parts by mass in terms of Ru metal). In addition, the method adopted for producing such an ammonia synthesis catalyst for comparison was a method of coprecipitating Ru together with the metal components (Ce and Pr) of the support, with reference to the method described in the above Non-Patent Document 1.

[0065] [Example 1, Reference examples 1~3 and Evaluation of the Performance of Ammonia Synthesis Catalysts Obtained in Comparative Examples 1 to 6] Working Example 1, Reference examples 1~3 The ammonia synthesis catalysts obtained in Comparative Examples 1 to 6 were used to determine the ammonia production rate of each catalyst as follows. A fixed-bed flow-type reactor was used to measure the ammonia production rate. When measuring the ammonia production rate, 0.2 g of the ammonia synthesis catalyst was placed in the gas flow path of the reactor so that the gas (inlet gas) introduced into the gas flow path of the reactor would head toward the outlet of the gas flow path after contacting the ammonia synthesis catalyst (after passing through the catalyst). H 2 and N 2 Contains and H 2 and N 2 Molar ratio (H 2 / N 2 ) was used. First, the ammonia synthesis catalyst placed in the gas flow path was subjected to a pretreatment of holding the ammonia synthesis catalyst at 600°C for 2.5 hours while supplying the inlet gas at a flow rate of 80mL / min under atmospheric pressure (under the condition of 0.1MPa). Next, while supplying the inlet gas under the same condition (flow rate: 80mL / min) under atmospheric pressure, the heating temperature of the ammonia synthesis catalyst was lowered from 600°C to 375°C, and the ammonia synthesis catalyst was held at 375°C for 1 hour. The ammonia concentration in the gas (outlet gas) discharged from the outlet of the gas flow path was measured, and the ammonia production rate per 1g of catalyst was calculated. The ammonia concentration in the outlet gas was measured by IR spectroscopy. The obtained results are shown in Table 1 and FIG. 1. FIG. 2 is a graph showing the relationship between the Pr content (mol%) in the composite oxide carrier of each catalyst and the ammonia production rate.

[0066] [Table 1]

[0067] As is clear from the results shown in Table 1 and Figures 1 and 2, the Pr content (molar ratio) relative to the total molar amount of Ce and Pr was10~75 Ammonia synthesis catalyst using a composite oxide support in the range of mol% (Example 1 and Reference Examples 1 to 3 ) had an ammonia production rate of 2.74 mmol / g h or more per 1 g of catalyst. In contrast, in the ammonia synthesis catalysts for comparison (Comparative Examples 1 to 2 and Comparative Example 6) that used composite oxide supports in which the Pr content (molar ratio) relative to the total molar amount of Ce and Pr was 5 mol % or less, the ammonia production rate per 1 g of catalyst was 2.69 mmol / g h or less. 1 and Reference Examples 1 to 3 In the ammonia synthesis catalysts (Comparative Examples 3 to 5) using a composite oxide support in which the Pr content (molar ratio) relative to the total molar amount of Ce and Pr is 90 mol % or more, the ammonia production rate per 1 g of catalyst is 2.27 mmol / g h or less. Cage , also an example 1 and Reference Examples 1 to 3 The ammonia synthesis catalyst obtained in Example 1 had insufficient ammonia production activity compared to the ammonia synthesis catalyst obtained in Example 2. 1 and Reference Examples 1 to 3 The ammonia synthesis catalyst obtained in Example 1 and Reference Examples 1 to 3 ) was found to be capable of increasing ammonia production activity even under conditions such as 375°C and 0.1 MPa.

[0068] From these results, the Pr content (molar ratio) relative to the total amount of Ce and Pr in the composite oxide support was 10~75 It was confirmed that when the molar ratio of Ce to Pr (Ce / Pr) was within the range of 25 / 75 to 90 / 10, the ammonia production activity of the obtained catalyst could be improved. In consideration of the measurement results of the ammonia production rate, it is clear that the ammonia production efficiency can be further improved by using an ammonia synthesis catalyst in which Ru is supported on a composite oxide support with a molar ratio of Ce to Pr (Ce / Pr) of 20 / 80 to 90 / 10.

[0069] In addition, when comparing Comparative Example 2 and Comparative Example 6, although the manufacturing methods of the catalyst are different, it was confirmed that the ammonia production rate was improved more when the comparative ammonia catalyst was prepared by supporting Ru on the composite oxide support obtained after producing the composite oxide support using the coprecipitation method (Comparative Example 2) than when the comparative ammonia catalyst was prepared by coprecipitating Ru with Ce and Pr (Comparative Example 6). It was also found that a higher level of ammonia production activity can be achieved by supporting Ru after producing the composite oxide support by adopting the coprecipitation method. In addition, when the comparative ammonia catalyst was prepared by coprecipitating Ru with Ce and Pr (Comparative Example 6), the inventors infer that a part of Ru was incorporated into the support when the coprecipitate was calcined, so that the number of active sites was reduced when used as a catalyst, and as a result, the activity was lower than that of the ammonia catalyst obtained in Comparative Example 2. [Industrial Applicability]

[0070] As described above, according to the present invention, it is possible to provide an ammonia synthesis catalyst that has excellent ammonia generation activity and enables ammonia to be synthesized more efficiently, a method for producing the ammonia synthesis catalyst that can efficiently produce the ammonia synthesis catalyst, and a method for synthesizing ammonia using the ammonia synthesis catalyst. Thus, the ammonia synthesis catalyst of the present invention has excellent ammonia generation activity and is therefore particularly useful as a catalyst or the like used in industrially producing ammonia.

Claims

1. a composite oxide support containing cerium and praseodymium; Ruthenium supported on the composite oxide support; and 2. An ammonia synthesis catalyst comprising: a composite oxide support having a molar ratio of cerium to praseodymium ([cerium] / [praseodymium]) of 25 / 75.

2. 2. A method for synthesizing ammonia, comprising contacting a gas containing hydrogen and nitrogen with the ammonia synthesis catalyst according to claim 1 to synthesize ammonia.

Citation Information

Patent Citations

  • Ammonia preparing system and method

    CN105692653A

  • Hydrogen production catalyst, and method and apparatus for producing hydrogen by using the same

    JP2014014813A

  • Ammonia synthesis catalyst and production method thereof

    JP2016155123A

  • Catalyst composition for manufacturing ammonia, manufacturing method of catalyst composition for manufacturing ammonia and ammonia manufacturing method

    JP2017001037A

  • Composition for ammonia synthesis catalyst and method for producing the same, and method for synthesizing ammonia

    JP2017018907A