Method for forming tungsten pillars
The method of depositing and converting amorphous silicon to tungsten pillars addresses the challenge of filling high aspect ratio trenches, achieving efficient device isolation and patterned film formation in semiconductor manufacturing.
Patent Information
- Application Number
- JP2022186147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-05-02
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2038-05-02
AI Technical Summary
The semiconductor industry faces challenges in filling high aspect ratio trenches with high quality dielectric materials, particularly in forming patterned films with smaller critical dimensions and achieving effective isolation between devices.
A method involving the deposition of an amorphous silicon film in trenches, followed by etching and conversion to tungsten pillars, maintaining shape fidelity and filling gaps without seams, using processes like pyrolysis and hydrogen plasma etching.
Enables efficient filling of high aspect ratio trenches with tungsten pillars, ensuring device isolation and maintaining shape fidelity, suitable for conformal and self-aligned patterning applications.
Smart Images

Figure 0007591018000001 
Figure 0007591018000002 
Figure 0007591018000003
Abstract
Description
[Technical field]
[0001]
[0001] The present disclosure relates generally to methods of depositing and processing thin films, and more particularly, to a process for filling trenches in a substrate. [Background technology]
[0002]
[0002] In the semiconductor industry, chips with increasingly smaller transistor dimensions are being rapidly developed to increase functionality per unit area. As device dimensions shrink, the gaps / spaces between devices also shrink, making it increasingly difficult to physically isolate devices from each other. Filling in the high aspect ratio trenches / spaces / gaps between devices, which are often irregularly shaped with high quality dielectric materials, is becoming increasingly challenging to implement using existing methods, including gap filling, hard mask, and spacer applications. Selective deposition methods typically include depositing a mask material on a substrate and patterning the mask material to form a patterned mask. Then, after patterning the mask, areas of the substrate may be exposed through the patterned mask. To expose non-implanted areas of the substrate, the patterned mask can be removed from the substrate, and materials can be selectively deposited on selected areas of the substrate.
[0003]
[0003] There is a need in the art for new methods for the design of chips with smaller critical dimensions. In addition, there is a current need for high quality metal oxide films in hard mask and spacer applications, and in methods for forming patterned films on substrates. Summary of the Invention
[0004]
[0004] One or more embodiments of the present disclosure are directed to a processing method that includes providing a patterned film forming at least one feature on a substrate surface. The at least one feature extends a depth from a top surface to a bottom surface of the patterned film. The at least one feature has a width defined by a first sidewall and a second sidewall. A film is deposited on the patterned film to fill the at least one feature and extend above the top surface of the patterned film. The film is recessed to lower a top of the film to a height equal to or less than the top surface of the patterned film to form a recessed film. The recessed film is converted to a tungsten film. The tungsten film is expanded to form a pillar extending from the at least one feature.
[0005]
[0005] A further embodiment of the present disclosure is directed to a processing method including providing a patterned film forming at least one feature on a substrate surface. The at least one feature extends a depth from a top surface to a bottom surface and has a width defined by a first sidewall and a second sidewall. The substrate surface is exposed to a precursor including one or more of silane, disilane, trisilane, or tetrasilane, and an amorphous silicon film is deposited on the substrate surface by pyrolysis to fill the at least one feature and extend above the substrate surface. The amorphous silicon film is etched with a hydrogen plasma or hydrogen radicals to recess the amorphous silicon film to lower an upper portion of the film to a height equal to or less than an upper surface of the patterned film, thereby forming a recessed amorphous silicon film. The recessed amorphous silicon film is exposed to a tungsten precursor. The tungsten precursor reacts with the recessed amorphous silicon film to convert substantially all of the amorphous silicon film to a tungsten film. The tungsten film is oxidized to expand the tungsten film, forming a tungsten pillar extending substantially straight up from the at least one feature.
[0006]
[0006] A further embodiment of the present disclosure is directed to a processing method including providing a patterned film forming at least one feature on a substrate surface. The at least one feature extends a depth from a top surface to a bottom surface and has a width defined by a first sidewall and a second sidewall. The substrate surface is exposed to a silicon precursor including one or more of silane, disilane, trisilane, or tetrasilane, and an amorphous silicon film is deposited on the substrate surface by pyrolysis to fill the at least one feature and extend above the top surface of the patterned film. The pyrolysis is performed in the absence of a silicon co-reactant and in the absence of a plasma at a temperature in the range of about 300°C to about 550°C, or in the absence of a plasma at a temperature in the range of about -100°C to about 50°C. The amorphous silicon film is etched with a hydrogen plasma or hydrogen radicals to recess the amorphous silicon film to lower the top of the film to a height equal to or less than the top surface of the patterned film, thereby forming a recessed amorphous silicon film. The recessed amorphous silicon film is exposed to a tungsten precursor comprising WF6 at a temperature in the range of about 300°C to about 550°C. The tungsten precursor reacts with the recessed amorphous silicon film to convert substantially all of the amorphous silicon film to a tungsten film. The tungsten film is oxidized to expand the tungsten film, forming a tungsten pillar extending substantially straight up from at least one feature. [Brief description of the drawings]
[0007]
[0007] So that the features of the present disclosure described above can be understood in detail, a more particular description of the present disclosure briefly summarized above can be had by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the present disclosure may admit of other equally effective embodiments, and therefore, that the accompanying drawings illustrate only typical embodiments of the present disclosure and should not be considered as limiting the scope of the present disclosure. [Figure 1] 1 illustrates a cross-sectional view of a feature of a substrate in accordance with one or more embodiments of the present disclosure. [Figure 2A] 1A-1D depict schematic cross-sectional views of a gap filling process according to one or more embodiments of the present disclosure. [Figure 2B] 1A-1D depict schematic cross-sectional views of a gap filling process according to one or more embodiments of the present disclosure. [Figure 2C] 1A-1D depict schematic cross-sectional views of a gap filling process according to one or more embodiments of the present disclosure. [Figure 2D] 1A-1D depict schematic cross-sectional views of a gap filling process according to one or more embodiments of the present disclosure. [Figure 2E] 1A-1D depict schematic cross-sectional views of a gap filling process according to one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008]
[0010] Before describing certain example embodiments of the present disclosure, it is to be understood that the present disclosure is not limited to the details of construction or process steps set forth in the following description as the present disclosure is capable of other embodiments and of being practiced or carried out in various ways.
[0009]
[0011] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment may be performed include materials such as silicon, silicon oxide, strained silicon, silicon-on-insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials, depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes to polish, etch, reduce, oxidize, hydroxylate, anneal, UV cure, electron beam (e-beam) cure, and / or bake the substrate surface. In addition to film treatment directly on the surface of the substrate itself, in this disclosure, any of the disclosed film treatment steps may also be performed on an underlying layer formed on the substrate, which is disclosed in more detail below. The term "substrate surface" is intended to include such underlying layers as the context indicates. Thus, for example, when a film / layer or partial film / layer is being deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.
[0010]
[0012] One or more embodiments of the present disclosure are directed to methods of depositing metal oxide films for any conformal, non-conformal, and / or low to high aspect ratio self-aligned patterning or gap / trench / void filling applications. Embodiments of the present disclosure advantageously provide methods of depositing films (e.g., metal oxide films) in high aspect ratio (AR) structures with small dimensions. Some embodiments of the present disclosure advantageously provide methods of filling gaps without forming seams in the gaps. One or more embodiments of the present disclosure advantageously provide methods of forming self-aligned patterns.
[0011]
[0013] FIG. 1 shows a partial cross-sectional view of a substrate 100 having a feature 110. This drawing shows a substrate with a single feature for illustrative purposes, but one of ordinary skill in the art will understand that there may be one or more features. The shape of the feature 110 may be any suitable shape, including, but not limited to, a trench and a cylindrical via. In a particular embodiment, the feature 110 is a trench. The term "feature" as used in this manner means any intentional surface irregularity. Suitable examples of features include a trench having a top, two sidewalls, and a bottom, a beak having a top and two sidewalls extending upward from a surface, and a via having a sidewall extending downward from a surface and an open bottom. The feature or trench may have any suitable aspect ratio (ratio of the depth of the feature to the width of the feature). In some embodiments, the aspect ratio is about 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, or 40:1 or more.
[0012]
[0014] The substrate 100 has a top surface 120. At least one feature 110 forms an opening in the top surface 120. The feature 110 extends from the top surface 120 to a depth D to a bottom surface 112. The feature 110 has a first sidewall 114 and a second sidewall 116 that define a width W of the feature 110. The open area formed by the sidewalls and the bottom surface is also referred to as a gap. Although the feature 110 is shown as a trench formed in the single component substrate 100, one skilled in the art will understand that the feature 110 may be formed by a patterned film on the substrate 100. FIG. 2A illustrates an embodiment in which the feature 110 is formed as a trench or via formed by or within a patterned film 130.
[0013]
[0015] 2A-2C, an exemplary embodiment of the present disclosure is described. The substrate 100 is provided for processing with or without the patterned film 130 thereon. As used in this manner, the term "provided" means that the substrate is placed in a location or environment for further processing. In some embodiments, the patterned film 130 is formed on the substrate 100 and at least one feature 110 is provided. In some embodiments, the substrate 100 is provided with the patterned film 130 already present.
[0014]
[0016] As shown in FIG. 2A, the patterned film can be a different material than the substrate 100 such that there is a first surface 132 and a second surface 134 that is different from the first surface 132. Features 110 are formed in the patterned film 130 such that the bottom surface 112 of the feature 110 provides the first surface 132 and the sidewalls 114, 116 and top surface 120 of the feature 110 provide the second surface 134. The patterned film 130 can be any suitable material. The patterned film 130 of some embodiments includes a low-k dielectric (e.g., SiOC). The patterned film 130 can be selected to be compatible with subsequent processing conditions.
[0015]
[0017] 2B, a film 140 is deposited or formed on the substrate 100 surface, filling the features 110 and extending over the top surface 120 of the patterned film 130. The film 140 can be any suitable film formed by any suitable process, including, but not limited to, chemical vapor deposition, plasma-enhanced chemical vapor deposition, atomic layer deposition, plasma-enhanced atomic layer deposition, and / or physical vapor deposition. In some embodiments, the film 140 is formed by atomic layer deposition or plasma-enhanced atomic layer deposition.
[0016]
[0018] In some embodiments, the precursors, along with an inert gas, a carrier gas, and / or a diluent gas, are flowed into a process chamber containing the substrate 100. The precursors may be chemisorbed onto the substrate 100 or the patterned film 130, thereby leaving a chemisorbed precursor on the substrate or the patterned film. A co-reactant may then be flowed into the process chamber to react with the chemisorbed precursor and deposit the film 140. In some embodiments, the precursors may be co-flowed into the process chamber with the co-reactant. The precursors and the co-reactant may react in the gas phase to form species that are deposited on the substrate or the patterned film, thereby growing the film 140.
[0017]
[0019] In some embodiments, the film 140 is deposited by thermal decomposition of a precursor. In some embodiments, the thermal decomposition does not include a co-reactant with the precursor to deposit the film 140. For example, a silicon precursor may be exposed to the substrate to deposit or form the film 140 on the substrate 100 and within the feature 110.
[0018]
[0020] In some embodiments, film 140 includes amorphous silicon. In one or more embodiments, film 140 consists essentially of amorphous silicon. As used in this manner, the phrase "consists essentially of" means that the film is greater than or equal to about 95%, 98%, or 99% amorphous silicon on a molar basis.
[0019]
[0021] The formation of the amorphous silicon film can be achieved by any suitable technique. In some embodiments, the formation of the amorphous silicon film is achieved by pyrolysis of a silicon precursor in the absence of co-reactants or in the substantial absence of co-reactants. As used in this manner, the phrase "substantially free of co-reactants" means that any species that reacts with the silicon precursor or adsorbed precursor molecules is present in an amount of about 50%, 40%, 30%, 20%, 10%, or 5% or less of the stoichiometric amount of the reaction.
[0020]
[0022] In some embodiments, the amorphous silicon film is deposited using one or more of silane, disilane, trisilane, or tetrasilane. In some embodiments, higher order silanes (e.g., 5, 6, 7, 8, 9, or 10 or more silicon atoms) can be used to deposit the amorphous silicon film.
[0021]
[0023] In some embodiments, the amorphous silicon film is deposited by a conformal deposition process. In the conformal deposition process, a silicon precursor is exposed to the substrate 100 and the optional patterned film 130 at a temperature and pressure sufficient to promote thermal decomposition of the precursor. In some embodiments, the temperature during deposition is in the range of about 300° C. to about 550° C., or in the range of about 350° C. to about 500° C. In some embodiments, the pressure during deposition is in the range of about 10 T to about 600 T, or in the range of about 50 T to about 500 T, or in the range of about 100 T to about 400 T. The deposition of the amorphous silicon film by the conformal deposition process can occur with or without plasma exposure. In some embodiments, the conformal deposition process is performed in the absence of plasma exposure.
[0022]
[0024] In some embodiments, the amorphous silicon film is deposited by a flowable film deposition process. The temperature during the flowable film deposition process can be in the range of about -100°C to about 50°C, or in the range of about -50°C to about 25°C. In some embodiments, the flowable film deposition process is performed at a pressure in the range of about 1 T to about 10 T. In one or more embodiments, the flowable film deposition process includes plasma exposure using an RF plasma with a power in the range of about 10 W to about 200 W. The plasma can be a conductively coupled plasma (CCP) or an inductively coupled plasma (ICP).
[0023]
[0025] As shown in FIG. 2C, after deposition, the film 140 is recessed to form a recessed film 145 having an upper portion 141. The upper portion 141 is lowered to a height equal to or lower than the upper surface 120 of the patterned film 130. In some embodiments, the recessed film 145 has an upper portion 141 that is substantially flush with the upper surface 120 of the patterned film 130. The expression "substantially flush" used in this manner means that the upper portion 141 is within 1 Å of the upper surface 120 of the patterned film 130. In some embodiments, the upper portion 141 of the recessed film 145 is within a range of about 20% to about 98% of the height of the patterned film 130. In some embodiments, the upper portion 141 of the recessed film 145 is within a range of about 30% to about 95%, or within a range of about 40% to about 90%, or within a range of about 50% to about 85% of the height of the patterned film 130.
[0024]
[0025] Recessing the film 140 to form the recessed film 145 can be accomplished by any suitable technique. In some embodiments, recessing the film 140 includes etching the film 140. In some embodiments, the etching includes a reactive ion etching (RIE) process. In some embodiments, the RIE uses a bromine-based etchant. In one or more embodiments, etching the film 140 includes exposing the film 140 to a hydrogen plasma or hydrogen radicals. The hydrogen plasma can be a remote plasma or a direct current plasma, and can be a CCP or an ICP. The hydrogen radicals can be generated by any suitable means including plasma generation or by flowing an etchant over a hot wire to generate the radicals.
[0025]
[0027] As shown in FIG. 2D, the recessed film 145 is converted to a tungsten film 150. Conversion of the recessed film can be accomplished by any suitable reaction. In some embodiments, the recessed film is converted to a tungsten film by exposure to a tungsten precursor. The tungsten precursor can be, for example, a tungsten halide that can react with the recessed film to exchange tungsten atoms for silicon atoms.
[0026]
[0028] In some embodiments, the tungsten precursor comprises WF6. In some embodiments, exposure to the tungsten precursor occurs at a temperature in the range of about 300° C. to about 550° C. or at a pressure in the range of about 10 T to about 100 T. The tungsten precursor may be flowed with other gases, which may be a diluent, carrier, or inert gas (e.g., argon), or a reactive gas (e.g., H2). In some embodiments, the tungsten precursor is flowed with a reactive gas that promotes reaction of the tungsten precursor with the recessed film.
[0027]
[0029] In an exemplary embodiment, the recessed film 145 includes or consists essentially of amorphous silicon and the tungsten precursor includes WF. The tungsten precursor is exposed to the amorphous silicon film at a temperature of about 550° C. and a pressure of about 20 Torr.
[0028]
[0030] In some embodiments, substantially all of the recessed film is converted to tungsten. As used in this manner, the phrase "substantially all" means that about 95%, 98%, or 99% or more of the recessed film is converted to tungsten. The amount of time used to convert substantially all of the recessed film depends, for example, on the temperature, pressure, film composition, film thickness, and tungsten precursor. In some embodiments, 200-300 Å of amorphous silicon can be converted to tungsten in about 4 minutes at 550° C. and 20 Torr.
[0029]
[0031] After converting the recessed film 145 to tungsten 150, the height of the top 151 of the tungsten film 150 may be the same as or different from the height of the recessed film. The height of the tungsten film 150 relative to the recessed film depends, for example, on the species present in the film and the atomic radius of the species. In some embodiments, the height of the tungsten film 150 is such that the top 151 of the film 150 is equal to or less than the top surface 120 of the patterned film 130.
[0030]
[0032] As shown in FIG. 2E, the tungsten film 150 can be expanded to cause a volume expansion of the tungsten film 150 to form a tungsten pillar 155 extending from the top surface 120. In some embodiments, the tungsten pillar 155 extends straight up from the surface 120. The expansion of the film 150 can be in the range of about 10% to about 1000%, or in the range of about 50% to about 800%, or in the range of about 100% to about 700%. In some embodiments, the film 130 expands by an amount of about 150%, 200%, 250%, 300%, or 350% or more. In some embodiments, the film 150 expands by an amount in the range of about 300% to about 400%. In some embodiments, the tungsten pillars 155 have a height greater than the tungsten film 150 by an amount greater than or equal to about 50%, 60%, 70%, 80%, 90%, 100%, 125%, 150%, 175%, or 200% or more of the height of the tungsten film 150.
[0031]
[0033] In some embodiments, film 150 expands upon exposure to a silicide agent or silicide conditions, converting the metal or metal-containing film to a metal silicide film. The silicide agent can be any suitable silicide agent, including, but not limited to, silane, disilane, trisilane, tetrasilane, pentasilane, hexasilane, trimethylsilane, compounds with trimethylsilyl substituents, and combinations thereof. In some embodiments, the silicide conditions include thermal silicidation, plasma enhanced siliciding, remote plasma siliciding, microwave and radio frequency (e.g., ICP, CCP).
[0032]
[0034] In some embodiments, the film 150 expands upon exposure to a germanium agent or germanicide conditions, converting the metal or metal-containing film into a metal germanicide film. The germanicide agent can be any suitable germanicide agent, including, but not limited to, germane, digermane, trigermane, tetragermane, pentagermane, hexagermane, trimethylgermanium, compounds with trimethylgermanyl substituents, and combinations thereof. In some embodiments, the germanicide conditions include thermal germanicide, plasma enhanced germanicide, remote plasma germanicide, microwave, and radio frequency (e.g., ICP, CCP).
[0033]
[0035] As shown in Figure 2E, during expansion, the fidelity of the feature's shape is maintained at the top of the feature and the membrane 150 grows straight up from the feature 110. As used in this manner, the phrase "straight up" means that the sides of the expanded membrane or post 155 are substantially flush with the sidewalls 114, 116 of the feature 110. The surface is flush with the sidewall 114 and the angle formed at the junction of the sidewall 114 with the surface is ±10°.
[0034]
[0036] In some embodiments, tungsten film 150 is doped with a dopant prior to expansion. The dopant may be incorporated into tungsten film 150 simultaneously with the formation of tungsten film 150 or in a separate process consecutive to the film deposition. For example, deposition of tungsten film 150 may occur in either the same processing chamber or a different processing chamber after doping tungsten film 150 with a dopant in a separate process.
[0035]
[0037] According to one or more embodiments, the substrate is subjected to a process before and / or after the formation of the layer. This process can be performed in the same chamber or in one or more separate process chambers. In some embodiments, the substrate is transferred from the first chamber to another second chamber for further processing. The substrate may be transferred directly from the first chamber to another process chamber or from the first chamber to one or more transfer chambers and then to another process chamber. Thus, the processing apparatus may comprise multiple chambers in communication with a transfer station. This type of apparatus may be referred to as a "cluster tool" or a "cluster system" or the like.
[0036]
[0038] Generally, a cluster tool is a modular system with multiple chambers to perform various functions including center detection and orientation, degassing, annealing, deposition, and / or etching of the substrate. In one or more embodiments, the cluster tool includes at least a first chamber and a central transfer chamber. The central transfer chamber may house a robot capable of transferring the substrate to and from multiple processing chambers and multiple load lock chambers. The transfer chamber is typically maintained at vacuum conditions. The transfer chamber also provides an intermediate stage for transferring the substrate to and from one chamber to the other chamber and / or to a load lock chamber located at the front end of the cluster tool. Two well-known cluster tools that may be adapted for the present invention are the Centura® and Endura®, both available from Applied Materials, Inc., Santa Clara, Calif. However, the exact arrangement and combination of chambers may be altered for the purpose of performing the specific steps of the processes described herein. Other processing chambers that can be used include, but are not limited to, cyclic layer deposition (CLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), physical vapor deposition (PVD), etching, pre-cleaning, chemical cleaning, thermal treatments such as RTP, plasma nitridation, degassing, alignment, hydroxylation, and other substrate processing. By performing the process in a chamber on a cluster tool, surface contamination of the substrate from impurities in the air can be avoided without oxidation before depositing the next film.
[0037]
[0039] According to one or more embodiments, the substrate is continuously under vacuum or "load-lock" conditions and is not exposed to ambient air when it is transferred from one chamber to the next. The transfer chamber is therefore under vacuum and is "pumped down" under vacuum pressure. An inert gas may be present in the processing or transfer chamber. In some embodiments, the inert gas is used as a purge gas to remove some or all of the reactants. According to one or more embodiments, a purge gas is injected at the outlet of the deposition chamber to prevent the transfer of reactants from the deposition chamber to the transfer chamber and / or additional processing chambers. Thus, a flow of inert gas forms a curtain at the outlet of the chamber.
[0038]
[0040] Substrates can be processed in single-substrate deposition chambers, where a single substrate is loaded, processed, and unloaded before other substrates are processed. Substrates can also be processed in a continuous manner similar to a conveyor system, where multiple substrates are individually loaded into a first portion of the chamber, moved through the chamber, and unloaded from a second portion of the chamber. The geometry of the chamber and associated conveyor system can form a linear or curved path. Additionally, the processing chamber can be a carousel, where multiple substrates move around a central axis and are exposed to processes such as deposition, etching, annealing, cleaning, etc. throughout the path of the carousel.
[0039]
[0041] During processing, the substrate may be heated or cooled. Such heating or cooling may be accomplished by any suitable means, including, but not limited to, changing the temperature of the substrate support and flowing a heated or cooled gas over the substrate surface. In some embodiments, the substrate support includes a heater / cooler that can be controlled to conductively change the substrate temperature. In one or more embodiments, the gas utilized (reactive or inert) is heated or cooled to locally change the substrate temperature. In some embodiments, a heater / cooler is positioned within the chamber adjacent to the substrate surface to change the substrate temperature by convection.
[0040]
[0042] During processing, the substrate may further be stationary or rotated. The rotating substrate may rotate continuously or in discrete steps. For example, the substrate may be rotated throughout the entire process, or the substrate may be rotated in small increments between exposures to various reactive or purge gases. Rotating the substrate (continuously or in steps) during processing may help, for example, to minimize the effects of local variability in gas flow profiles, resulting in a more uniform deposition or etch.
[0041]
[0043] References throughout this specification to "one embodiment," "a particular embodiment," "one or more embodiments," or "an embodiment" mean that the particular features, structures, materials, or characteristics described in connection with those embodiments are included in at least one embodiment of the disclosure. Thus, the appearances of "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification are not necessarily all referring to the same embodiment of the disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.
[0042]
[0044] Although the disclosure of this specification has been described with reference to specific embodiments, it should be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed method and apparatus without departing from the spirit and scope of the disclosure. Thus, the disclosure is intended to cover such modifications and variations as come within the scope of the appended claims and their equivalents.
Claims
1. A processing method comprising the steps of: providing a patterned film forming at least one feature on a substrate surface, the at least one feature extending a depth from a top surface to a bottom surface of the patterned film, the at least one feature having a width defined by a first sidewall and a second sidewall; depositing an amorphous silicon film onto the patterned film at a temperature range of about −100° C. to about 50° C. so as to fill the at least one feature and extend over the top surface of the patterned film, wherein depositing the amorphous silicon film comprises exposing the substrate surface to a precursor comprising one or more of silane, disilane, trisilane, or tetrasilane; recessing the amorphous silicon film to lower a top portion of the amorphous silicon film to a height equal to or less than the top surface of the patterned film to form a recessed amorphous silicon film; converting the recessed amorphous silicon film into a tungsten film; expanding the tungsten film to form a pillar extending from the at least one feature; The method includes:
2. 10. The method of claim 1, wherein depositing the film is performed at a pressure within a range of about 1 T to about 10 T.
3. The method of claim 2 , wherein the depositing of the film is performed using an RF plasma having a power in the range of about 10 W to about 200 W.
4. The method of claim 3 , wherein the depositing of the film is performed in the absence of a co-reactant for the precursor.
5. The method of claim 1 , wherein recessing the amorphous silicon film comprises etching the amorphous silicon film.
6. 6. The method of claim 5, wherein etching the amorphous silicon film comprises a reactive ion etching process using a bromine-based etchant.
7. The method of claim 5 , wherein recessing the amorphous silicon film comprises exposing the amorphous silicon film to a hydrogen plasma or hydrogen radicals.
8. The step of converting the recessed amorphous silicon film into a tungsten film comprises converting the recessed amorphous silicon film into a tungsten film by a method comprising the steps of: 6 The method of claim 1 , comprising exposing the
9. W.F. 6 9. The method of claim 8, wherein the exposing to is carried out at a temperature in the range of about 300° C. to about 550° C. and at a pressure in the range of about 10 T to about 100 T.
10. 10. The method of claim 9, wherein substantially all of the recessed amorphous silicon film is converted to tungsten.
11. The method of claim 1 , wherein expanding the tungsten film comprises oxidizing the tungsten film.
12. The method of claim 11 , wherein the post extends substantially straight up from the at least one feature.
13. A processing method comprising the steps of: providing a patterned film forming at least one feature on a substrate surface, the at least one feature extending a depth from a top surface to a bottom surface, the at least one feature having a width defined by a first sidewall and a second sidewall; exposing the substrate surface to a silicon precursor comprising one or more of silane, disilane, trisilane, or tetrasilane to deposit an amorphous silicon film by pyrolysis on the substrate surface, filling the at least one feature and extending over the substrate surface; recessing the amorphous silicon film with a hydrogen plasma or hydrogen radicals to lower the amorphous silicon film to a height equal to or less than the top surface of the patterned film to form a recessed amorphous silicon film; exposing the recessed amorphous silicon film to a tungsten precursor to react with the recessed amorphous silicon film and convert substantially all of the amorphous silicon film to a tungsten film; and oxidizing the tungsten film to expand the tungsten film to form a tungsten pillar extending substantially straight up from the at least one feature.
14. A processing method comprising the steps of: providing a patterned film forming at least one feature on a substrate surface, the at least one feature extending a depth from a top surface to a bottom surface, the at least one feature having a width defined by a first sidewall and a second sidewall; exposing the substrate surface to a silicon precursor comprising one or more of silane, disilane, trisilane, or tetrasilane to deposit an amorphous silicon film by thermal decomposition on the substrate surface, filling the at least one feature and extending over the top surface of the patterned film, the thermal decomposition occurring in the absence of a silicon co-reactant and at a temperature range of about 300° C. to about 550° C. in the absence of a plasma or about −100° C. to about 50° C. in the presence of a plasma; etching the amorphous silicon film with a hydrogen plasma or hydrogen radicals to recess the top of the amorphous silicon film to a height equal to or less than the top surface of the patterned film to form a recessed amorphous silicon film; The recessed amorphous silicon film is treated with WF 6 at a temperature in the range of about 300° C. to about 550° C. to react with the recessed amorphous silicon film and convert substantially all of the amorphous silicon film to a tungsten film; and oxidizing the tungsten film to expand the tungsten film to form a tungsten pillar extending substantially straight up from the at least one feature.
Citation Information
Patent Citations
Manufacture of semiconductor integrated circuit
JP1987298110A
Semiconductor device and manufacture thereof
JP1990090518A
Formation of contact plug
JP1994112155A
Dry etching method and dry etching treatment apparatus
JP1995094491A
Manufacture of semiconductor device
JP1995147321A