How zinc is produced

By employing an alkali hydroxide solution and a chlorine concentration adjustment step, the method addresses the issue of increased chlorine concentration in zinc production from electric furnace dust and secondary dust, achieving high-quality zinc production with reduced impurities and stable yield.

JP7591834B2Active Publication Date: 2024-11-29KINOTECH CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022566983
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-04
Filing Date
2021-12-02
Publication Date
2024-11-29
Estimated Expiration
2041-12-02

AI Technical Summary

Technical Problem

Existing methods for producing zinc from electric furnace dust and secondary dust suffer from increased chlorine concentration in the alkali hydroxide aqueous solution and electrolytic tailings, affecting the quality of the electrolytic product.

Method used

A method involving the use of an alkali hydroxide aqueous solution as an extraction solvent, followed by a chlorine concentration adjustment step to separate chlorine components, and subsequent electrolysis to produce zinc with reduced chlorine concentration, utilizing a dechlorination agent and pH control to maintain optimal conditions.

Benefits of technology

The method effectively reduces chlorine concentration in the zinc-containing aqueous solution and electrolytic tailings, ensuring the production of high-quality zinc with reduced impurity contamination and stable yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591834000002
    Figure 0007591834000002
  • Figure 0007591834000003
    Figure 0007591834000003
  • Figure 0007591834000004
    Figure 0007591834000004
Patent Text Reader

Abstract

A zinc production method, according to the present invention, further comprises chlorine concentration adjustment steps 101, 101', and 105 for using a hydroxylated alkaline aqueous solution as an extraction solvent for selectively extracting a zinc component during a zinc-containing aqueous solution generation step 102, and separating the chlorine component contained in electrical-furnace dust or secondary dust at a stage prior to an electrolysis step 103 so as to reduce the chlorine concentration in a zinc-containing aqueous solution.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing zinc, and in particular to a method for producing zinc using so-called secondary dust as a raw material, such as electric furnace dust generated during the melting and smelting of scrap in the electric furnace process, which is one of the steelmaking processes, secondary dust (crude zinc oxide) generated in a reduction furnace when part of the electric furnace dust is recycled as a zinc raw material, and secondary dust (crude zinc oxide) generated in the blast furnace process, which is one of the steelmaking processes, and recovered as a zinc-containing oxide in a rotary hearth furnace. [Background technology]

[0002] In the electric furnace process, which is one of the steelmaking processes, electric furnace dust is generated as industrial waste containing zinc oxide and accounts for approximately 1.5% to 2.0% of the steel produced during the melting and smelting of scrap. It is said that 8 million tons of electric furnace dust is generated worldwide, and 400,000 tons is generated in Japan.

[0003] Most of the iron scrap is from abandoned buildings, discarded home appliances, or scrapped automobiles. The paint base of abandoned buildings, discarded home appliances, or scrapped automobiles is zinc-plated. The scrap also contains paint, plastic, oil, and the like. Therefore, electric furnace dust contains heavy metals such as zinc and lead, as well as harmful organic matter such as chlorides and dioxins. On the other hand, electric furnace dust contains about 20-30% iron and 20-30% zinc. Furthermore, crude zinc oxide contains about 10% iron and about 60% zinc. Therefore, electric furnace dust and secondary dust (crude zinc oxide) are very useful resources.

[0004] Under such circumstances, Patent Document 1 discloses a method for producing zinc ingot, which includes the steps of: producing a zinc-containing aqueous solution containing a zinc component using electric furnace dust or secondary dust generated when electric furnace dust is reduced in a reduction furnace as a raw material; converting the zinc component in the zinc-containing aqueous solution into a zinc-containing compound in at least one form of carbonate, hydroxide, and oxide, and chlorinating the zinc component of the zinc-containing compound to produce purified zinc chloride containing purified zinc chloride; dehydrating the purified zinc chloride to produce anhydrous molten purified zinc chloride containing dehydrated molten purified zinc chloride; and electrolyzing the anhydrous molten purified zinc chloride to produce zinc ingot as an electrolysis product. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-119895 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, according to the inventor's investigation, the configuration disclosed in Patent Document 1 repeatedly uses the filtrate obtained in the step of producing purified zinc chloride as an alkaline agent for selectively extracting zinc components from electric furnace dust or secondary dust, and repeatedly uses chlorine gas, which is by-produced in the step of producing zinc bullion as an electrolytic product by electrolyzing anhydrous molten purified zinc chloride, as a chlorinating agent for producing purified zinc chloride, but does not disclose or suggest anything about aqueous solution electrolysis using a zinc-containing aqueous solution as an electrolytic bath.Furthermore, it does not disclose or suggest anything about repeatedly using the electrolytic effluent obtained by electrolysis in the step of producing a zinc-containing aqueous solution.

[0007] In particular, according to the inventors' investigations, when the zinc component in the electric furnace dust or secondary dust is selectively extracted using an aqueous alkali hydroxide solution as an extraction solvent to prepare a zinc-containing aqueous solution, and this zinc-containing aqueous solution is electrolyzed to obtain zinc as the electrolysis product, and the final electrolysis solution is returned as it is to the aqueous alkali hydroxide solution as the extraction solvent, the amount of chlorine components in the zinc-containing aqueous solution and the final electrolysis solution increases, raising the chlorine concentration, which undesirably affects the properties of the aqueous alkali hydroxide solution as the extraction solvent and thus has room for improvement in that it undesirably affects the properties of the zinc as the electrolysis product.

[0008] The present invention has been made based on the above-mentioned considerations, and has an object to provide a method for producing zinc, which can reduce the chlorine concentration during the process of selectively extracting zinc components in electric furnace dust or secondary dust using an aqueous alkali hydroxide solution as an extraction solvent to obtain a zinc-containing aqueous solution, and then electrolyzing the zinc-containing aqueous solution to produce zinc as an electrolytic product. [Means for solving the problem]

[0009] In order to achieve the above object, a method for producing zinc in a first aspect of the present invention includes a zinc-containing aqueous solution production step of using electric furnace dust or secondary dust generated when the electric furnace dust is reduced in a reduction furnace as a raw material, selectively extracting a zinc component in the raw material to produce a zinc-containing aqueous solution containing the zinc component, and an electrolysis step of performing electrolysis using the zinc-containing aqueous solution as an electrolyte to produce zinc, and returning the electrolysis tail solution, which is the electrolyte after the electrolysis, to the zinc-containing aqueous solution production step, wherein the method further includes a chlorine concentration adjustment step of separating a chlorine component contained in the electric furnace dust or the secondary dust at a stage prior to the electrolysis step to reduce the chlorine concentration of the zinc-containing aqueous solution, and the chlorine concentration adjustment step is performed by: The zinc-containing aqueous solution is obtained by diluting the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution production step. Alkaline hydroxide solution as cleaning solution 、 The chlorine component is separated by washing, and the chlorine concentration adjustment step is By diluting the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution production step,When the electric furnace dust or the secondary dust is washed with the aqueous alkali hydroxide solution as the washing solution, the pH value of the slurry dust obtained by immersing the electric furnace dust or the secondary dust in the aqueous alkali hydroxide solution of the washing solution and stirring the same is set to a value lower than the pH value of the aqueous alkali hydroxide solution used as the extraction solvent in the zinc-containing aqueous solution generating step. , in the range of 3 to 5 The pH is adjusted to a range of 8.5 to 10.5, and the aqueous alkali hydroxide solution, which is the cleaning solution after cleaning containing the separated chlorine components, is The cleaning solution is repeatedly used to clean the electric furnace dust or the secondary dust within the range in which the chlorine components can be dissolved, and then The electric furnace dust or the secondary dust from which the chlorine component has been separated is sent to the zinc-containing aqueous solution producing step, while the electric furnace dust or the secondary dust is discharged outside the system without being sent to the zinc-containing aqueous solution producing step and the electrolysis step.

[0012] The present invention also relates to the first 1 In addition to the above-mentioned aspect, the electrolytic tail solution is returned to the chlorine concentration adjustment step, the aqueous alkali hydroxide solution in the chlorine concentration adjustment step contains the electrolytic tail solution, and the chlorine concentration adjustment step includes adjusting the pH value of the slurry dust obtained by stirring the slurry dust while immersed in the aqueous alkali hydroxide solution containing the electrolytic tail solution. 2 The situation is as follows.

[0013] The present invention also relates to the first 1 Or 2 In addition to the above, the chlorine concentration adjusting step is characterized in that a target value is set to a predetermined value within a range of 8.5 to 10.5, which is smaller than the pH value of the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution generating step, and the amount of the alkaline agent and the amount of water for obtaining the aqueous alkali hydroxide solution in the chlorine concentration adjusting step are controlled according to a deviation between the target value and a measured pH value of the slurry dust. 3 The situation is as follows.

[0014] The present invention also relates to the first to third embodiments. 3 In addition to any one of the above aspects, the chlorine concentration adjusting step comprises contacting the zinc-containing aqueous solution with a dechlorinating agent to separate the chlorine component. 4 The situation is as follows.

[0015] The present invention also relates to the first to third embodiments. 4 In addition to any one of the above aspects, the zinc Containing aqueous solution generation The zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step is contacted with metallic zinc to reduce and precipitate metal impurity components nobler than zinc in the zinc-containing aqueous solution, and the electrolysis step is performed by using the zinc-containing aqueous solution that has been subjected to the substitution step as the electrolytic solution. 5 The situation is as follows.

[0016] The present invention also relates to the first to third embodiments. 5 In addition to any one of the above aspects, the present invention further includes a deironization / demanganese step of contacting an oxidizing agent with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step to separate iron and manganese components in the zinc-containing aqueous solution, and a substitution step of contacting metallic zinc with the zinc-containing aqueous solution that has been subjected to the iron and manganese removal / demanganese step to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution, and the electrolysis step is characterized in that electrolysis is performed using the zinc-containing aqueous solution that has been subjected to the substitution step as the electrolytic solution. 6 The situation is as follows.

[0017] The present invention also relates to the first 5 Or 6 In addition to the above, the zinc-containing aqueous solution generated in the zinc-containing aqueous solution generation step includes a first zinc-containing aqueous solution and a second zinc-containing aqueous solution having a chlorine concentration lower than that of the first zinc-containing aqueous solution, and the zinc generated by electrolysis using the first zinc-containing aqueous solution as an electrolyte in the electrolysis step is used as the metallic zinc in the substitution step. 7 The situation is as follows. Effect of the Invention

[0018] According to the first aspect of the present invention, the method for producing zinc further includes a chlorine concentration adjustment step of separating the chlorine component contained in the electric furnace dust or the secondary dust to reduce the chlorine concentration of the zinc-containing aqueous solution in a stage prior to the electrolysis step, using an aqueous alkali hydroxide solution as an extraction solvent for selectively extracting the zinc component in the aqueous zinc-containing solution production step, and The zinc-containing aqueous solution is obtained by diluting the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution production process. Alkaline hydroxide solution as cleaning solution 、 The chlorine components are separated by washing, and the chlorine concentration is adjusted. By diluting the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution production step, When electric furnace dust or secondary dust is washed with an aqueous alkali hydroxide solution as a washing solution, the pH value of the slurry dust obtained by immersing the electric furnace dust or secondary dust in the aqueous alkali hydroxide solution as a washing solution and stirring the resulting slurry dust is set to a value lower than the pH value of the aqueous alkali hydroxide solution used as an extraction solvent in the zinc-containing aqueous solution production process. , in the range of 3 to 5 The pH is adjusted to within a range of 8.5 to 10.5, and the alkaline hydroxide aqueous solution, which is the cleaning solution after cleaning containing the separated chlorine components, is It can be reused as a cleaning solution for electric furnace dust or secondary dust within the range where chlorine components can be dissolved, The electric furnace dust or secondary dust from which the chlorine components have been separated is discharged outside the system without being sent to the zinc-containing aqueous solution production process or the electrolysis process, while the electric furnace dust or secondary dust from which the chlorine components have been separated is sent to the zinc-containing aqueous solution production process. This allows the chlorine components to be dissolved from the electric furnace dust or secondary dust without extracting the zinc components, thereby preventing the chlorine concentration in the alkali hydroxide aqueous solution, zinc-containing aqueous solution, and electrolysis solution from increasing, and makes it possible to produce zinc with the required quality characteristics.

[0021] In addition, the present invention 2 According to the zinc manufacturing method of the above aspect, the electrolytic tail solution is returned to the chlorine concentration adjustment step, the aqueous alkali hydroxide solution in the chlorine concentration adjustment step contains the electrolytic tail solution, and the chlorine concentration adjustment step adjusts the pH value of the slurry dust obtained by stirring while immersed in the aqueous alkali hydroxide solution containing the electrolytic tail solution. Therefore, even if the electrolytic tail solution is used as part of the cleaning solution, the chlorine components can be eluted from the electric furnace dust or secondary dust without further extraction of the zinc components, and zinc with the required quality characteristics can be produced.

[0022] In addition, the present invention3 According to the zinc production method of the aspect, the chlorine concentration adjustment step sets a target value within a range of 8.5 to 10.5, which is lower than the pH value of the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution production step, and controls the amount of alkaline agent and the amount of water for obtaining the aqueous alkali hydroxide solution in the chlorine concentration adjustment step according to the deviation between the target value and the measured pH value of the slurry dust. Therefore, the pH value of the slurry dust can be reliably maintained at an appropriate value, and zinc with the required quality characteristics can be produced.

[0023] In addition, the present invention 4 According to the zinc production method of the above aspect, the chlorine concentration adjustment step involves contacting the zinc-containing aqueous solution with a dechlorinating agent to separate the chlorine components. Therefore, between the zinc-containing aqueous solution production step and the electrolysis step, the chlorine components contained in the electric furnace dust or the secondary dust are additionally separated, thereby reliably preventing the chlorine concentrations in the alkali hydroxide aqueous solution, the zinc-containing aqueous solution, and the electrolytic tail solution from increasing, and zinc with the required quality characteristics can be produced.

[0024] In addition, the present invention 5 According to the method for producing zinc in the above aspect, zinc Containing aqueous solution generation The method further includes a substitution step in which metallic zinc is brought into contact with the zinc-containing aqueous solution produced in the step to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution, and the electrolysis step performs electrolysis using the zinc-containing aqueous solution that has been subjected to the substitution step as an electrolyte, so that zinc with reduced impurity contamination can be mass-produced stably with good yield.

[0025] In addition, the present invention 6 According to the method for producing zinc in the above aspect, zinc Containing aqueous solution generationThe method further includes a deironization / demanganese step in which an oxidizing agent is brought into contact with the zinc-containing aqueous solution produced in the step to separate the iron and manganese components in the zinc-containing aqueous solution, and a substitution step in which metallic zinc is brought into contact with the zinc-containing aqueous solution that has been through the deironization / demanganese step to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution. Since the electrolysis step involves electrolysis using the zinc-containing aqueous solution that has been through the substitution step as an electrolyte, zinc with reduced impurity contamination can be stably mass-produced with good yield.

[0026] In addition, the present invention 7 According to the method for producing zinc in the above aspect, zinc Containing aqueous solution generation The zinc-containing aqueous solutions produced in the process include a first zinc-containing aqueous solution and a second zinc-containing aqueous solution having a chlorine concentration lower than that of the first zinc-containing aqueous solution, and the zinc produced by electrolysis using the first zinc-containing aqueous solution as the electrolyte in the electrolysis process is used as metallic zinc in the substitution process. Therefore, the substitution process can be efficiently carried out by effectively utilizing the zinc produced by the electrolysis, and zinc with reduced impurity contamination can be stably mass-produced with good yield. [Brief description of the drawings]

[0027] [Figure 1A] FIG. 1A is a process diagram of a method for producing zinc in a first embodiment of the present invention. [Figure 1B] FIG. 1B is a process diagram for producing secondary dust that can be used as a raw material in the method for producing zinc in this embodiment. [Diagram 2] FIG. 2 is a process diagram of a method for producing zinc in a second embodiment of the present invention. [Figure 3A] FIG. 3A is a process diagram of a method for producing zinc in a third embodiment of the present invention. [Figure 3B] FIG. 3B is a diagram showing a microscope photograph of zinc produced when an electrolytic bath with a high chlorine concentration is used in the zinc production method of the present embodiment. [Figure 4] FIG. 4 is a process diagram of a method for producing zinc in a fourth embodiment of the present invention. [Diagram 5]FIG. 5 is Table 1 showing the results of an experimental example of the first embodiment of the present invention. [Figure 6] FIG. 6 is Table 2 showing the results of an experimental example of the second embodiment of the present invention. [Figure 7] FIG. 7 is Table 3 showing the results of an experimental example of the third embodiment of the present invention. [Figure 8] FIG. 8 is Table 4 showing the results of an experimental example of the fourth embodiment of the present invention. [Figure 9A] FIG. 9A is a process diagram of a method for producing zinc in a fifth embodiment of the present invention. [Figure 9B] FIG. 9B is a schematic diagram showing the configuration of a cleaning machine used in the chlorine concentration adjustment step including pH adjustment in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, the zinc manufacturing method according to each embodiment of the present invention will be described in detail with reference to the drawings as appropriate.

[0029] (First embodiment) First, a method for producing zinc in a first embodiment of the present invention will be described in detail with reference to FIGS. 1A and 1B.

[0030] FIG. 1A is a diagram showing steps of a method for producing zinc in this embodiment, and FIG. 1B is a diagram showing a process for producing secondary dust that can be used as a raw material in the method for producing zinc in this embodiment.

[0031] As shown in Fig. 1A, in this embodiment, a chlorine concentration adjustment step 101, a zinc extraction step 102, and an electrolysis step 103 are carried out in this order. The zinc extraction step 102 corresponds to a zinc-containing aqueous solution production step. This is based on a manufacturing concept in which a priority is given to producing an aqueous solution in which zinc components are extracted from electric furnace dust or secondary dust as a raw material, and the aqueous solution is electrolyzed as an electrolyte to produce zinc as an electrolysis product.

[0032] Specifically, first, in the chlorine concentration adjustment step 101, electric furnace dust 1 as a raw material containing zinc-containing compounds such as zinc oxide and iron compounds such as iron oxide is washed with a cleaning agent 3, and the chlorine components adsorbed to the electric furnace dust 1 are eluted and separated from the electric furnace dust 1, to obtain washed electric furnace dust 5. The electric furnace dust 1 is washed with the cleaning agent 3, and the used cleaning agent 4 containing the eluted chlorine components adsorbed to the electric furnace dust 1 may be repeatedly used as the cleaning agent 3 for washing the electric furnace dust 1 again within a range in which further chlorine components can be eluted. As the cleaning agent 3, a strong alkaline agent that is highly effective in eluting chlorine components from the electric furnace dust 1 can be suitably used, and specifically, an aqueous solution of such a strong alkaline agent can be suitably used as the cleaning liquid. Furthermore, from the viewpoint of improving efficiency by sharing the same alkaline agent, it is more preferable to use, as the cleaning agent 3, an alkaline agent 6 which is a hydroxide such as sodium hydroxide used in the zinc extraction step 102. Specifically, it is preferable to use, as the cleaning liquid, an aqueous alkali hydroxide solution which is an aqueous solution of the alkaline agent 6 which is a hydroxide such as sodium hydroxide.

[0033] As the raw material to be washed in the chlorine concentration adjustment step 101, instead of the electric furnace dust 1, the secondary dust 2 obtained by reducing the electric furnace dust 1 in a reduction furnace may be used. In addition, as the raw material to be washed in the chlorine concentration adjustment step 101, when the calcination step 104 shown in FIG. 1B is adopted, the secondary dust 2 obtained by mixing and calcining the electric furnace dust 1 with calcium carbonate 11 in that step may be used. By such calcination, the zinc component contained in the zinc ferrite component of the electric furnace dust 1 can be converted in advance into a zinc oxide component that is easily extracted with an alkaline agent in the zinc extraction step 102. In this way, when the secondary dust 2 obtained by calcining the mixture of calcium carbonate 11 is used as the raw material, the calcium component in the residue 7 obtained in the zinc extraction step 102 can be increased. In addition, the carbon dioxide 12 obtained by such calcination can be stored or used as necessary. In addition, in the calcination step 104, the low boiling point component ZnCl 2As the secondary dust 2 volatilizes, it is possible to reduce the chlorine component in the secondary dust 2 compared to that in the electric furnace dust from which the secondary dust 2 originates. In addition, the raw material used in the chlorine concentration adjustment step 101 may be secondary dust such as crude zinc hydroxide obtained from the electric furnace dust 1. In the chlorine concentration adjustment step 101, chlorine is the component to be separated from the electric furnace dust 1 by washing the electric furnace dust 1 with the washing agent 3, but fluorine can also be the component to be separated in addition to or instead of chlorine using a similar method.

[0034] Next, in the zinc extraction step 102, the electric furnace dust 5 from which the chlorine components have been eluted and the chlorine concentration reduced by washing in the chlorine concentration adjustment step 101 is directly contacted with an aqueous solution of an alkaline agent 6 as an extraction solvent for zinc, to selectively extract the zinc components from the zinc-containing compound and produce a zinc-containing aqueous alkaline agent solution 8 containing the zinc components as a zinc extract, while the solid components that do not dissolve in the aqueous solution of the alkaline agent 6 are left as a residue 7.

[0035] Typically, the chemical formula for obtaining a zinc-containing aqueous alkaline agent solution 8, which is a zinc-containing aqueous solution obtained by selectively extracting zinc components from zinc oxide in washed electric furnace dust 5 using sodium hydroxide as an alkaline agent 6, is shown below in Chemical Formula 1. [ka]

[0036] In the zinc extraction step 102, the residue 7, which is a zinc-containing compound, may be directly contacted with an aqueous solution of an alkaline agent 6 to selectively extract the zinc component from the residue 7, thereby producing a zinc-containing aqueous alkaline agent solution 8' containing the zinc component as a zinc extract, and the zinc-containing aqueous alkaline agent solution 8'' may be produced from the residue 7' obtained in this manner in a similar manner. Each time the zinc-containing aqueous alkaline agent solutions 8', 8'' are produced using the residues 7, 7' in this manner, the chlorine concentration in the zinc-containing aqueous alkaline agent solutions 8', 8'' changes, and the properties of the zinc 10', 10'' obtained as the electrolysis product in the electrolysis step 103 change. For example, if the electric furnace dust 1 is not washed enough in the chlorine concentration adjustment step 101, the zinc-containing aqueous alkaline agent solution 8 obtained in the first zinc extraction step 102 will have the highest chlorine concentration, but if the electric furnace dust 1 is washed enough in the chlorine concentration adjustment step 101, the chlorine concentrations of the zinc-containing aqueous alkaline agent solutions 8, 8', 8'', ... obtained in the first and subsequent zinc extraction steps 102 will be approximately equal. Furthermore, regardless of whether the electric furnace dust 1 is washed enough in the chlorine concentration adjustment step 101, the amount of increase in chlorine in the zinc-containing aqueous alkaline agent solutions 8, 8', 8'', ... obtained by selectively extracting the zinc component with the aqueous alkaline agent 6 solution tends to increase each time the electrolytic tail solution obtained in the electrolysis step 103 is repeatedly used as the aqueous solution of the alkaline agent 6 as the zinc extraction solvent.

[0037] Next, in the electrolysis step 103, the zinc-containing alkaline agent aqueous solution 8 containing the zinc component extracted in the zinc extraction step 102 is placed in an electrolytic cell having a pair of electrodes (not shown) and electrolyzed as an electrolyte to deposit zinc 10 on the cathode side, which is then separated into solid and liquid and recovered as a solid, which is used as a product as is. In addition, since the electrolytic tail solution, which is the electrolyte after the zinc 10 is separated into solid and liquid and recovered, contains the alkaline agent 6, the electrolytic tail solution is returned as it is to the zinc extraction step 102 and used as a part of the aqueous solution of the alkaline agent 6 as an extraction solvent for the zinc. In addition, when the alkaline agent 6 used in the zinc extraction step 102 is used as the cleaning agent 3 in the chlorine concentration adjustment step 101, since the electrolytic tail solution contains the alkaline agent 6, it may be returned as it is to the chlorine concentration adjustment step 101 and used as a part of the cleaning agent 3.

[0038] In the zinc production method of the present embodiment described above, an alkali hydroxide aqueous solution is used as an extraction solvent for selectively extracting the zinc component in the zinc-containing aqueous solution production step 102, and a chlorine concentration adjustment step 101 is further provided prior to the electrolysis step 103, in which the chlorine component contained in the electric furnace dust or secondary dust is separated to reduce the chlorine concentration in the zinc-containing aqueous solution. This makes it possible to suppress an increase in the chlorine concentration in the alkali hydroxide aqueous solution, the zinc-containing aqueous solution, and the electrolysis solution, and to produce zinc with the required quality characteristics.

[0039] Furthermore, in the zinc production method of this embodiment, the chlorine concentration adjustment step 101 involves washing the electric furnace dust or secondary dust with an alkaline hydroxide aqueous solution to separate the chlorine components. This ensures that the chlorine components contained in the electric furnace dust or secondary dust are separated at an earlier stage than the zinc-containing aqueous solution production step 102, thereby reliably preventing the chlorine concentrations in the alkaline hydroxide aqueous solution, zinc-containing aqueous solution, and electrolytic solution from increasing, and makes it possible to produce zinc with the required quality characteristics.

[0040] Second Embodiment Next, with reference to FIG. 2, a method for producing zinc according to a second embodiment of the present invention will be described in detail.

[0041] FIG. 2 is a diagram showing steps of a method for producing zinc in this embodiment.

[0042] 2, the zinc production method according to this embodiment is mainly different from the zinc production method according to the first embodiment in that it has a chlorine concentration adjustment step 105 between a zinc extraction step 102 and an electrolysis step 103. In this embodiment, the description will be given focusing on such a difference, and the same components are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0043] Specifically, in the chlorine concentration adjustment step 105 following the zinc extraction step 102, the zinc-containing alkaline agent aqueous solution 8 as the zinc extract containing the zinc component extracted in the zinc extraction step 102 is directly contacted with a dechlorinating agent 13 serving as a silver ion source such as silver oxide or silver nitrate, and a chlorine compound 14 of the dechlorinating agent 13 is generated in the zinc-containing alkaline agent aqueous solution 8, which is separated and removed to obtain a zinc-containing alkaline agent aqueous solution 15 after the chlorine concentration adjustment, that is, a zinc-containing alkaline agent aqueous solution 15 after the chlorine concentration adjustment with a reduced chlorine concentration. In addition, in the chlorine concentration adjustment step 105, a volatilizing agent such as alcohol is added to the zinc-containing alkaline agent aqueous solution 8 as the zinc extract containing the zinc component extracted in the zinc extraction step 102, and heated to volatilize the chloride ions contained in the zinc-containing alkaline agent aqueous solution 8 to the outside as volatile chlorine compounds, thereby obtaining a zinc-containing alkaline agent aqueous solution 15 after the chlorine concentration adjustment with a reduced chlorine concentration. At this time, it is presumed that heavy metals such as manganese components and aluminum components in the raw material function as catalysts in order for the chlorine components to react with such volatilizing agents.

[0044] In the zinc extraction step 102, the residue 7, which is a zinc-containing compound, is directly contacted with an aqueous solution of an alkaline agent 6 to selectively extract the zinc component from the residue 7 to produce a zinc extract solution containing the zinc component, an aqueous zinc-containing alkaline agent solution 8', and if the process of similarly producing an aqueous zinc-containing alkaline agent solution 8'' from the residue 7' obtained in this step is repeated, then in the chlorine concentration adjustment step 105, zinc-containing aqueous alkaline agent solutions 15', 15'' after the chlorine concentration adjustment are correspondingly obtained.

[0045] Next, in the electrolysis step 103, the zinc-containing alkaline agent aqueous solutions 15, 15', 15'' after the chlorine concentration adjustment in the chlorine concentration adjustment step 105 are electrolyzed as electrolytes, and zinc 10, 10', 10'' is precipitated on the cathode side, which is recovered as a solid by solid-liquid separation, and this is used as a product as is. In addition, the electrolysis tail liquid, which is the electrolyte after zinc 10, 10', 10'' is recovered by solid-liquid separation, contains the alkaline agent 6, so the electrolysis tail liquid is returned as it is to the zinc extraction step 102.

[0046] In this embodiment, when the chlorine concentration of the electric furnace dust 1 or the secondary dust 2 used as the raw material is low, it is possible to provide only the chlorine concentration adjustment step 105 instead of providing both the chlorine concentration adjustment steps 101 and 105.

[0047] According to the method for producing zinc of the present embodiment, in addition to the configuration of the first embodiment, an alkali hydroxide aqueous solution is used as an extraction solvent for selectively extracting the zinc component in the zinc-containing aqueous solution production step 102, and chlorine concentration adjustment steps 101, 105 are further provided prior to the electrolysis step 103 to separate the chlorine component contained in the electric furnace dust or secondary dust and reduce the chlorine concentration in the zinc-containing aqueous solution. This makes it possible to suppress an increase in the chlorine concentration in the alkali hydroxide aqueous solution, the zinc-containing aqueous solution, and the electrolysis tail solution, and to produce zinc with the required quality characteristics.

[0048] Furthermore, in the zinc production method of this embodiment, the chlorine concentration adjustment step 105 involves contacting the zinc-containing aqueous solution with a dechlorinating agent to separate the chlorine components. Therefore, between the zinc-containing aqueous solution production step 102 and the electrolysis step 103, the chlorine components contained in the electric furnace dust or secondary dust are additionally separated, thereby reliably preventing the chlorine concentrations in the alkali hydroxide aqueous solution, the zinc-containing aqueous solution, and the electrolytic tail solution from increasing, and zinc with the required quality characteristics can be produced.

[0049] (Third embodiment) Next, referring to FIG. 3A and FIG. 3B, 3The method for producing zinc in this embodiment will now be described in detail.

[0050] FIG. 3A is a process diagram of the zinc production method of this embodiment, and FIG. 3B is a micrograph of zinc produced when an electrolytic bath with a high chlorine concentration is used in the zinc production method of this embodiment.

[0051] 3A, the zinc production method according to this embodiment is mainly different from the zinc production method according to the first embodiment in that it has a substitution step (cementation step) 106 between a zinc extraction step 102 and an electrolysis step 103. In this embodiment, the description will be given focusing on such a difference, and the same components are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0052] Specifically, in the substitution step 106 following the zinc extraction step 102, a zinc-containing alkaline agent aqueous solution 8 serving as a zinc extract containing the zinc component extracted in the zinc extraction step 102 is directly contacted with metallic zinc 16 such as zinc fine particles to reduce and precipitate metal impurity components 17 such as copper, lead, cadmium, etc., which are more noble than zinc in the zinc-containing alkaline agent aqueous solution 8, thereby obtaining a zinc-containing alkaline agent aqueous solution 18 in which the concentrations of the impurity components in the zinc-containing alkaline agent aqueous solution 8 have been reduced.

[0053] In the zinc extraction step 102, the residue 7, which is a zinc-containing compound, is directly contacted with an aqueous solution of an alkaline agent 6 to selectively extract the zinc component from the residue 7 to produce a zinc extract solution containing the zinc component, a zinc-containing aqueous alkaline agent solution 8', and if the process of similarly producing a zinc-containing aqueous alkaline agent solution 8'' from the residue 7' obtained in this process is repeated, then in the replacement step 106, zinc-containing aqueous alkaline agent solutions 18', 18'' after the concentration of the impurity components has been reduced and metal impurity components 17', 17'' are correspondingly obtained.

[0054] Next, in the electrolysis step 103, the zinc-containing alkaline agent aqueous solutions 18, 18', 18'' in which the concentrations of impurity components have been reduced in the substitution step 106 are used as electrolytes for electrolysis, and zinc 10, 10', 10'' is precipitated on the cathode side, which is then recovered as a solid by solid-liquid separation, and this is used as the product as is. In addition, the electrolysis tail liquid, which is the electrolyte after zinc 10, 10', 10'' is recovered by solid-liquid separation, contains the alkaline agent 6, and so the electrolysis tail liquid is returned as it is to the zinc extraction step 102. Furthermore, in the zinc extraction step 102, when the electric furnace dust 5 and the residue 7, 7', which are zinc-containing compounds, are directly contacted with an aqueous solution of an alkaline agent 6 to selectively extract the zinc component from the electric furnace dust 5 and the residue 7, 7', and zinc-containing aqueous alkaline agent solutions 8, 8', 8'' containing the zinc component are repeatedly produced as a zinc extract obtained by selectively extracting the zinc component from the electric furnace dust 5 and the residue 7, 7', if the chlorine concentration of the zinc-containing aqueous alkaline agent solution 18, 18', 18'' after the substitution step 106 is high, for example, the zinc 10 produced in the electrolysis step 103 tends to become metallic zinc fine particles as shown in FIG. 3B, and therefore the zinc 10 produced as the electrolysis product may be returned to the substitution step 106 as metallic zinc fine particles 16 for use.

[0055] In addition, the chlorine concentration adjustment step 105 in the zinc production method of the second embodiment may be provided between the zinc extraction step 102 and the replacement step 106 in the zinc production method of the present embodiment.

[0056] According to the method for producing zinc of the present embodiment, in addition to the configuration of the first or second embodiment, it further includes a substitution step 106 in which metallic zinc is brought into contact with the zinc-containing aqueous solution produced in the zinc extraction step 102 to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution, and the electrolysis step 103 performs electrolysis using the zinc-containing aqueous solution that has been subjected to the substitution step 106 as the electrolyte, so that zinc with reduced impurity contamination can be stably mass-produced with good yield.

[0057] In addition, in the zinc manufacturing method of this embodiment, the zinc-containing aqueous solution generated in the zinc-containing aqueous solution generation step 102 is a first zinc-containing aqueous solution and a second zinc-containing aqueous solution having a chlorine concentration lower than that of the first zinc-containing aqueous solution, and the zinc generated by electrolysis using the first zinc-containing aqueous solution as an electrolyte in the electrolysis step 103 is used as metallic zinc in the substitution step 106. Therefore, the zinc produced by the electrolysis can be effectively used to efficiently perform the substitution step 106, and zinc with reduced impurity contamination can be stably mass-produced with good yield.

[0058] (Fourth embodiment) Next, with reference to FIG. 4, a zinc production method according to a fourth embodiment of the present invention will be described in detail.

[0059] FIG. 4 is a process diagram of the zinc production method in this embodiment.

[0060] 4, the zinc production method according to this embodiment is mainly different from the zinc production method according to the third embodiment in that it has a deironization / demanganization step 107 between the zinc extraction step 102 and the substitution step 106. In this embodiment, the description will be given focusing on such a difference, and the same components are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0061] In this embodiment, the provision of the deironization / demanganese step 107 is particularly effective when the iron or manganese components contained in the electric furnace dust are alkali-soluble Fe(II) and Mn(II), and is also effective even when the iron or manganese components are alkali-insoluble, because when a zinc-containing aqueous solution in which alkali-insoluble Fe(III) and Mn(IV) are suspended is treated in the substitution step, they are reduced to alkali-soluble Fe(II) and dissolved in the zinc-containing aqueous solution. In addition, since alkali-soluble iron or manganese components may be generated in the substitution step 106, the substitution step may be provided not only after the deironization / demanganese step, but also before the deironization / demanganese step. Specific methods for the deironization / demanganese step 107 include aeration and oxidation by adding permanganate, and when the soluble manganese component is Mn(VII), a method of contacting with activated carbon may be used.

[0062] Specifically, in the deferrication / demanganese step 107 following the zinc extraction step 102, in order to remove the iron and soluble manganese contained in the zinc-containing alkaline agent aqueous solution 8 as the zinc extract containing the zinc component extracted in the zinc extraction step 102, the iron or soluble manganese contained in the zinc-containing alkaline agent aqueous solution 8 is oxidized, and the iron and manganese components in the zinc-containing alkaline agent aqueous solution 8 are separated and removed as insoluble precipitate sludge 21 to obtain a zinc-containing alkaline agent aqueous solution 20 with a reduced concentration of impurity components. Specifically, an oxidizing agent 19 such as air, oxygen, permanganate, hydrogen peroxide, persulfate, chlorate, or chlorine dioxide is added to the zinc-containing alkaline agent aqueous solution 8 to oxidize the ferrous component in the zinc-containing alkaline agent aqueous solution 8 to the ferric component, and the soluble manganese is oxidized to convert it to insoluble manganese dioxide, which is separated and removed as sludge 21. In addition, the iron component in the zinc-containing alkaline agent aqueous solution 8 can be converted into magnetic iron oxide such as maghemite, which contains both ferrous and ferric components, by controlling the temperature, alkali concentration, and oxidation-reduction potential (ORP) value.

[0063] When permanganate is used as the oxidizing agent 19, the end point of demanganization can be determined by supplying permanganate until an excess of permanganic acid remains in the zinc-containing aqueous alkaline agent solution 8, and the remaining permanganate is directly brought into contact with activated carbon and converted into insoluble manganese dioxide, which is then removed.

[0064] Furthermore, in the zinc extraction step 102, the residue 7, which is a zinc-containing compound, is directly contacted with an aqueous solution of an alkaline agent 6 to selectively extract the zinc component from the residue 7, thereby producing a zinc-containing aqueous alkaline agent solution 8' containing the zinc component as a zinc extract, and if the process of similarly producing a zinc-containing aqueous alkaline agent solution 8'' from the residue 7' obtained in this process is repeated, then in the iron removal and manganese removal step 107, zinc-containing aqueous alkaline agent solutions 20', 20'' and sludge 21', 21'' after the concentrations of impurity components have been reduced are correspondingly obtained.

[0065] Next, in the substitution step 106, the zinc-containing aqueous alkaline agent solution 20, 20', 20'' in which the concentration of impurity components has been reduced in the iron removal / manganese removal step 107 is contacted with metallic zinc 16 such as zinc fine particles to reduce and precipitate metal impurity components 17 such as copper, lead, cadmium, etc. which are more noble than zinc in the zinc-containing aqueous alkaline agent solution 20, 20', 20'', thereby obtaining zinc-containing aqueous alkaline agent solutions 18, 18', 18'' in which the concentrations of impurity components in the zinc-containing aqueous alkaline agent solution 20, 20', 20'' have been further reduced.

[0066] Regarding the order of carrying out the deironization / demanganese step 107 and the replacement step 106, the deironization / demanganese step 107 may be carried out after the replacement step 106. For example, when the raw material is a material that has been subjected to an iron reduction step, such as secondary dust, the raw material may contain a large amount of divalent iron (Fe(II): ferrous component), and it is therefore more reasonable to carry out the replacement step 106 first when treating such raw material. This also applies to an embodiment in which the deironization / demanganese step 107 is separated into a deironization step and a demanganese step, each of which is carried out individually.

[0067] Next, in the electrolysis step 103, the zinc-containing alkaline agent aqueous solutions 18, 18', 18'' in which the concentrations of impurity components have been reduced in the substitution step 106 are used as electrolytes for electrolysis, and zinc 10, 10', 10'' is precipitated on the cathode side, which is then recovered as a solid by solid-liquid separation, and this is used as the product as is. In addition, the electrolysis tail liquid, which is the electrolyte after zinc 10, 10', 10'' is recovered by solid-liquid separation, contains the alkaline agent 6, and so the electrolysis tail liquid is returned as it is to the zinc extraction step 102.

[0068] In the zinc production method of this embodiment, as in the third embodiment, when the chlorine concentration in the zinc-containing aqueous alkaline agent solution 18, 18', 18'' after the substitution step 106 is high, the zinc 10 produced by electrolysis may be returned to the substitution step 106 as fine particle-like metallic zinc 16. The chlorine concentration adjustment step 105 in the zinc production method of the second embodiment may be provided between the zinc extraction step 102 and the deironization and demanganization step 107 in the zinc production method of this embodiment.

[0069] According to the method for producing zinc of the present embodiment, in addition to the configuration of the first or second embodiment, the method further includes a deferrication / demanganese step 107 in which an oxidizing agent is brought into contact with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step 102 to separate the iron and manganese components in the zinc-containing aqueous solution, and a substitution step 106 in which metallic zinc is brought into contact with the zinc-containing aqueous solution that has been through the deferrication / demanganese step 107 to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution. Since the electrolysis step 103 performs electrolysis using the zinc-containing aqueous solution that has been through the substitution step 106 as the electrolyte, zinc with reduced impurity contamination can be stably mass-produced with good yield.

[0070] Finally, in contrast to the present embodiment described above, experimental examples representatively corresponding to the first to fourth embodiments will be described in detail with reference to FIGS. 5 to 8. FIG.

[0071] FIG. 5 is Table 1 showing the results of Experimental Example 1 of the first embodiment of the present invention, FIG. 6 is Table 2 showing the results of Experimental Example 2 of the second embodiment of the present invention, and FIG. 7 is Table 3 showing the results of Experimental Example 3 of the third embodiment of the present invention. 3 8 is an experimental example of the fourth embodiment of the present invention. 4 The results are shown in Table 4. In the table, ND means not detected. Also, blank spaces in the table mean that electric furnace dust, secondary dust, and residue were below the detection limit or not detected, and for items other than electric furnace dust, secondary dust, and residue, they are outside the scope of the analysis.

[0072] (Experimental Example 1) This experimental example corresponds to the first embodiment of the present invention, and the results are shown in Table 1 of FIG.

[0073] First, in the chlorine concentration adjustment step 101, 60.5g of secondary dust 2 was taken from 870g of secondary dust obtained by previously mixing and calcining 441g of calcium carbonate 11 and 762.8g of electric furnace dust 1 in the calcination step 104, and the secondary dust 2 thus taken was washed with a 0.8% NaOH aqueous solution as the cleaning agent 3 to elute the chlorine components and obtain secondary dust 5 with a reduced chlorine concentration. The NaOH aqueous solution as the cleaning agent 3 was reused in the chlorine concentration adjustment step 101.

[0074] Next, in the zinc extraction step 102, the secondary dust 5, which has been washed in the chlorine concentration adjustment step 101 to reduce the chlorine concentration, is contacted with an aqueous NaOH solution having a concentration of 16.5% per 1000 g as an aqueous solution of the alkaline agent 6, and the solid matter that does not dissolve in the aqueous solution of the alkaline agent 6 is separated by filtration to obtain a zinc extract (zinc-containing aqueous alkaline agent solution) 8 having a chlorine concentration of 480 mg / l and a volume of 770 ml as the remaining liquid. In addition, the solid matter that does not dissolve in the aqueous solution of the alkaline agent 6 is filtered, washed with pure water, and then dried to obtain a residue 7 having a weight of 46.2 g. The extraction conditions in the zinc extraction step 102 are a temperature of 95°C and normal pressure, and the contact time between the aqueous solution of the alkaline agent 6 and the secondary dust 2 is 8 hours. The filtrate from which the residue 7 is filtered (the filtrate from which extractable components are extracted from the insoluble solid matter) is repeatedly used as the alkaline agent 6 for dissolving the secondary dust 2.

[0075] Next, in the electrolysis step 103, electrolysis was performed using the zinc-containing alkaline agent aqueous solution 8 containing the zinc component extracted in the zinc extraction step 102 as an electrolyte to obtain smooth metallic zinc (foil) 10 weighing 8.7 g. The electrolytic tail solution, which is the electrolyte after the zinc 10 is recovered by solid-liquid separation, was returned directly to the zinc extraction step 102 and repeatedly used as part of the aqueous solution of the alkaline agent 6 as the extraction solvent for the zinc. The electrolysis conditions in the electrolysis step 103 were as follows: stainless steel (SUS304) flat plates with a plate thickness of 1 mm were used as the electrodes (cathode and anode), the distance between the cathode and anode was set to 20 mm, and the geometric area-based current density was 62.5 mA / cm 2 The electrolysis was carried out for a period of 8.5 hours while controlling the constant current at 1 A so that the zinc deposition current efficiency was 84%.

[0076] (Experimental Example 2) This experimental example corresponds to the second embodiment of the present invention, and the results are shown in Table 2 of FIG.

[0077] The electrolytic tail solution obtained in the electrolysis step 103 in Experimental Example 1 was returned to the zinc extraction step 102 and repeatedly used as part of the aqueous solution of the alkaline agent 6 as the extraction solvent for zinc. In the zinc extraction step 102, the chlorine concentration of the zinc extract solution (zinc-containing aqueous alkaline agent solution) 8 was concentrated to 1,500 mg / l.

[0078] Next, in the chlorine concentration adjustment step 105, silver nitrate is added as a dechlorinating agent 13 to the zinc-containing alkaline agent aqueous solution 8 extracted in the zinc extraction step 102, and AgCl precipitated in the zinc-containing alkaline agent aqueous solution 8 is removed as chlorine compound 14 by filtration to obtain a zinc-containing alkaline agent aqueous solution with a chlorine concentration reduced to 240 mg / l. In addition, zinc particles are brought into contact with this zinc-containing alkaline agent aqueous solution to precipitate the remaining Ag therein and filter it out to obtain a zinc-containing alkaline agent aqueous solution 15 with a chlorine concentration reduced to 240 mg / l and from which Ag has been removed.

[0079] Next, in the electrolysis step 103, the zinc-containing alkaline agent aqueous solution 15, in which the chlorine concentration had been reduced in the chlorine concentration adjustment step 105, was used as the electrolyte to obtain smooth metallic zinc (foil) 10 weighing 3.7 g. The electrolytic tail solution, which is the electrolyte solution obtained after the zinc 10 is recovered by solid-liquid separation, was returned directly to the zinc extraction step 102 and repeatedly used as part of the aqueous solution of the alkaline agent 6 as the extraction solvent for the zinc. The electrolysis conditions in the electrolysis step 103 were as follows: stainless steel (SUS304) flat plates with a thickness of 1 mm were used as the electrodes (cathode and anode), the distance between the cathode and anode was set to 20 mm, and the size in the liquid was set to 20 mm wide and 30 mm high, and the geometric area-based current density was set to 62.5 mA / cm 2 The electrolysis was carried out for a period of 10 hours while controlling the constant current at 375 mA so that the zinc deposition current efficiency was 81%, and the average value of the voltage between the cathode and anode was 2.4 V.

[0080] (Experimental Example 3) This experimental example corresponds to the third embodiment of the present invention, and the results are shown in Table 3 of FIG.

[0081] In the zinc extraction step 102 following the chlorine concentration adjustment step 101, 100g of secondary dust (crude zinc hydroxide sample) 5 derived from electric furnace dust, which was washed in the chlorine concentration adjustment step 101 to reduce the chlorine concentration, was contacted with a 16.5% NaOH aqueous solution as an aqueous solution of an alkaline agent 6, and the entire amount of solids that do not dissolve in the aqueous solution of the alkaline agent 6 were filtered and separated to obtain a residue 7, and the remaining liquid was a zinc extract (zinc-containing aqueous alkaline agent) 8. Next, this residue 7 was contacted with a 16.5% NaOH aqueous solution as a new aqueous solution of an alkaline agent 6, and the entire amount of solids that do not dissolve in the aqueous solution of the alkaline agent 6 were filtered and separated to obtain a residue 7', and the remaining liquid was a zinc extract (zinc-containing aqueous alkaline agent) 8'. The conditions in the zinc extraction step 102 in this experimental example were the same as those in experimental example 1.

[0082] Next, in the substitution step 106, a zinc-containing alkaline agent aqueous solution 8 serving as a zinc extract containing the zinc component extracted in the zinc extraction step 102 is brought into contact with zinc particles serving as metallic zinc 16, whereby metal impurity components 17 such as copper, lead, cadmium and the like which are more noble than zinc in the zinc-containing alkaline agent aqueous solution 8 are reduced and precipitated, and a zinc-containing alkaline agent aqueous solution 18 having a reduced concentration of the impurity components is obtained.

[0083] Next, in the electrolysis step 103, the zinc-containing alkaline agent aqueous solution 18 in which the concentration of impurity components was reduced in the substitution step 106 was electrolyzed as an electrolyte with a chlorine concentration of 2000 mg / l to obtain 2.6 g of metallic zinc (powder with a particle size of approximately 500 μm) 10 with a purity of 92%. The electrolytic tail solution, which is the electrolyte after the zinc 10 is recovered by solid-liquid separation, is returned directly to the zinc extraction step 102 and repeatedly used as part of the aqueous solution of the alkaline agent 6 as the extraction solvent for the zinc. The electrolysis conditions in the electrolysis step 103 were as follows: stainless steel (SUS304) flat plates with a plate thickness of 1 mm were used as the electrodes (cathode and anode), the distance between the cathode and anode was set to 20 mm, and the size in the liquid was set to 20 mm wide and 20 mm high, and the geometric area-based current density was 62.5 mA / cm 2The electrolysis was carried out for a period of 8 hours while controlling the constant current at 250 mA so that the zinc deposition current efficiency was 97.7%, and the average value of the voltage between the cathode and the anode was 2.35 V.

[0084] Next, in the second substitution step 106, the metallic zinc 10 thus obtained (powder having a particle size of approximately 500 μm) is brought into contact with the zinc-containing aqueous alkaline agent solution 8' obtained in the zinc extraction step 102, whereby metal impurity components 17' such as copper, lead, cadmium and the like which are more noble than zinc in the zinc-containing aqueous alkaline agent solution 8' are reduced and precipitated, and a zinc-containing aqueous alkaline agent solution 18' in which the concentrations of the impurity components are reduced is obtained.

[0085] Next, in the second electrolysis step 103, the zinc-containing alkaline agent aqueous solution 18' in which the concentration of impurity components had been reduced in the second substitution step 106 was electrolyzed as an electrolyte with a chlorine concentration of 250 mg / l to obtain metallic zinc (foil) 10'. The electrolytic tail solution, which is the electrolyte solution obtained after the zinc 10' was recovered by solid-liquid separation, was returned directly to the zinc extraction step 102 and repeatedly used as part of the aqueous solution of the alkaline agent 6 as an extraction solvent for the zinc. The electrolysis conditions in the second electrolysis step 103 were set to be the same as those in the second electrolysis step 103.

[0086] (Experimental Example 4) This experimental example corresponds to the fourth embodiment of the present invention, and the results are shown in Table 4 of FIG.

[0087] In the zinc extraction step 102 following the chlorine concentration adjustment step 101, the secondary dust (crude zinc hydroxide sample) 5 derived from the electric furnace dust having a weight of 300 g, which has been washed in the chlorine concentration adjustment step 101 to reduce the chlorine concentration, is contacted with a 16.5% NaOH aqueous solution as an aqueous solution of an alkaline agent 6, and the entire amount is filtered after stirring. The entire amount of solids that do not dissolve in the aqueous solution of the alkaline agent 6 are filtered and separated to obtain a residue 7, and 1800 ml of zinc extract (zinc-containing aqueous alkaline agent) 8 is obtained as the remaining liquid. Next, this residue 7 is contacted with a 16.5% NaOH aqueous solution as a new aqueous solution of the alkaline agent 6, and the entire amount of solids that do not dissolve in the aqueous solution of the alkaline agent 6 are filtered and separated to obtain a residue 7', and 1800 ml of zinc extract (zinc-containing aqueous alkaline agent) 8' is obtained as the remaining liquid. The conditions in the zinc extraction step 102 in this experimental example were the same as those in experimental example 1.

[0088] Next, in the deironization and demanganization process 107 following the zinc extraction process 102, 0.1 g of KMnO4 crystals were added as an oxidizing agent 11 to the zinc-containing alkaline agent aqueous solution 8, 8'. red 10 g of activated carbon was added to the liquid under heating, and after confirming that the liquid became transparent, the liquid was filtered through a membrane filter with a filtration accuracy of 0.1 μm to obtain a filtrate (deironized and demanganized zinc-containing alkaline agent aqueous solution 20, 20'). As the solid content on the filter paper, deironized and demanganized sludge 21, 21' with a weight of 263 mg was obtained.

[0089] Next, the substitution step 106 following the iron removal / manganese removal step 107 was carried out in the same manner as in Experimental Example 3 using the zinc-containing alkaline agent aqueous solutions 20 and 20' to obtain zinc-containing alkaline agent aqueous solutions 18 and 18', respectively, and the electrolysis step 103 was carried out using the zinc-containing alkaline agent aqueous solutions 18 and 18' as electrolytic baths to obtain metallic zinc 10 and 10' similar to those in Experimental Example 3. The electrolytic tail solution, which is the electrolyte after the recovery of zinc 10, was returned as it was to the zinc extraction step 102 and was repeatedly used as a part of the aqueous solution of alkaline agent 6 as the extraction solvent for zinc. The electrolysis conditions in the electrolysis step 103 were set to be the same as those in the electrolysis step 103 in Experimental Example 3.

[0090] Fifth embodiment Finally, a method for producing zinc according to the fifth embodiment of the present invention will be described in detail with reference to FIGS. 9A and 9B.

[0091] FIG. 9A is a diagram showing the steps of a zinc production method in this embodiment, and FIG. 9B is a schematic diagram showing the configuration of a cleaning machine used in the chlorine concentration adjustment step, which includes adjusting the pH (hydrogen ion exponent) in this embodiment.

[0092] As shown in Fig. 9A, the zinc manufacturing method according to this embodiment is mainly different from the zinc manufacturing method according to the first embodiment in that the chlorine concentration adjusting step 101' adjusts the pH value in addition to adjusting the chlorine concentration. In this embodiment, the description will be focused on such a difference, and the same components are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0093] First, according to the investigations of the present inventors, assuming a configuration in which a strong alkaline agent, typically an alkaline agent which is a hydroxide, is used as the cleaning agent 3 in the chlorine concentration adjustment step 101 as in the first embodiment, and the electric furnace dust 1 or the secondary dust 2 (hereinafter referred to as electric furnace dust 1) is brought into contact with an alkaline aqueous solution which is a cleaning liquid prepared by dissolving and separating the chlorine components adsorbed to the electric furnace dust 1, specifically, the electric furnace dust 1 which has been crushed into a predetermined size or smaller is immersed in the alkaline aqueous solution, and the electric furnace dust 1 in this immersed state is stirred in the alkaline aqueous solution for about a predetermined time to form a slurry, and the chlorine components which have adhered to the electric furnace dust 1 are eluted from the electric furnace dust 1 in the slurry state.

[0094] Here, according to the study by the present inventors, it has been found that in order to practically dissolve the chlorine components from the electric furnace dust 1 that has become a slurry in the alkaline aqueous solution, it is necessary to maintain the pH value of the slurried electric furnace dust 1 at 8.5 or more and 10.5 or less, which is lower than the pH value of the alkaline aqueous solution that is the aqueous solution of the alkaline agent 6 used in the zinc extraction process 102. This is because, first, with regard to the lower limit, if the pH value is less than 8.5, it is not possible to ensure a practical amount of chlorine components to be dissolved from the electric furnace dust 1, and it has been found that unnecessary dissolution of zinc components and lead components from the electric furnace dust 1 occurs. On the other hand, with regard to the upper limit, if the pH value is 10.5This is because, if the pH exceeds 10, the zinc component will be extracted from the electric furnace dust 1, and the amount of the zinc component in the cleaned electric furnace dust 5 to be sent to the zinc extraction step 102 in the next stage will decrease, which will defeat the purpose of providing the zinc extraction step 102. Furthermore, according to the study by the present inventors, the pH value of the alkaline aqueous solution, which is the aqueous solution of the alkaline agent 6 used in the zinc extraction step 102, needs to be at least 13 or more in order to increase the amount of the zinc component extracted from the cleaned electric furnace dust 5 and obtain a practical amount of the zinc component, and this also indicates that it is a prerequisite that the pH value of the slurry-like electric furnace dust 1 in the chlorine concentration adjustment step 101 be set lower than the pH value of the alkaline aqueous solution used in the zinc extraction step 102. In other words, if the pH value of the aqueous alkaline solution, which is the aqueous solution of the alkaline agent 6 used in the zinc extraction step 102, is taken as a reference, the pH value of the electric furnace dust 1 made into a slurry state in the chlorine concentration adjustment step 101 may be set to a value that is smaller than the pH value of the aqueous alkaline solution, which is the aqueous solution of the alkaline agent 6 used in the zinc extraction step 102, within the range of 3 to 5. This contributes to easily and quickly calculating the initial amount of water to be added to the alkaline agent 6 in order to realize a pH value that is smaller than the known pH value within the range of 3 to 5, when, for example, the alkaline agent 6 in the zinc extraction step 102 is stored as the alkaline agent 6 that is practically available and capable of extracting the maximum amount of zinc components, and when the alkaline agent 6 with a known pH value is diluted and used as the cleaning agent 3 in the chlorine concentration adjustment step 101. Note that a typical example that is practically suitable as the cleaning agent 3 and the alkaline agent 6 is sodium hydroxide.

[0095] That is, specifically, in this embodiment, as shown in FIG. 9A , in the chlorine concentration adjustment step 101′, a strong alkaline agent, specifically an alkaline agent which is a hydroxide, is used as the cleaning agent 3, and an alkaline aqueous solution is prepared as a cleaning liquid by dissolving the strong alkaline agent in an aqueous solution. Electric furnace dust 1 which has been crushed to a predetermined size or less is immersed in the alkaline aqueous solution, and the electric furnace dust 1 thus immersed is stirred in the alkaline aqueous solution for about a predetermined time to form a slurry. The chlorine components are separated from the electric furnace dust 1 by dissolving them out of the electric furnace dust 1, and washed electric furnace dust 5 is obtained.

[0096] Here, the alkaline aqueous solution, which is a cleaning solution in which the cleaning agent 3 is homogeneously dissolved in water 30, and the electric furnace dust 1 to be immersed therein are supplied from a supply system 202 capable of freely supplying each of the electric furnace dust 1, the cleaning agent 3, and the water 30, and are contained in a cleaning tank 201 of a cleaning machine 200, as shown in Fig. 9B. The initial pH value of the alkaline aqueous solution, which is the cleaning solution, is set to a value within a range of 8.5 to 10.5, which is smaller than the pH value of the alkaline aqueous solution, which is the aqueous solution of the alkaline agent 6 used in the zinc extraction step 102 (a value that is smaller than this value within a range of 3 to 5, taking the pH value of the alkaline aqueous solution, which is the aqueous solution of the alkaline agent 6 used in the zinc extraction step 102, as a reference), so that the initial pH value of the slurry-like electric furnace dust 1 is roughly given. The alkaline aqueous solution and the electric furnace dust 1 immersed in it are continuously stirred by a stirring member 204b that can rotate around a rotating shaft 204a in a stirrer 204, and as a result, the solution takes on the properties of a slurry, and becomes slurry-like dust 203 in the cleaning tank 201.

[0097] The cleaning tank 201 is also provided with a pH meter 205 for measuring the pH value therein, and the pH meter 205 measures the pH value in the cleaning tank 201, specifically, the pH value of the slurry-like dust 203 in the cleaning tank 201. A detection signal indicating a voltage representing the pH value measured by the pH meter 205 is sent to a controller 300 including a processor, memory, and the like (not shown). The controller 300, to which the detection signal from the pH meter 205 is input, calculates the deviation between the measured pH value represented by the detection signal and a target pH value (for example, a value of 9.5, which is the median value within a range of 8.5 to 10.5, which is smaller than the pH value of the aqueous alkaline solution that is the aqueous solution of the alkaline agent 6 used in the zinc extraction process 102), and adjusts the amount of cleaning agent 3 supplied to the cleaning tank 201 and the amount of water 30 supplied to the cleaning tank 201 according to the deviation so that the actual pH value coincides with the target pH value. In detail, the controller 300 reads a control program and control data stored in advance in the memory, and refers to the control data to control the supply amount of the water 30 to be increased according to the difference (e.g., positive value) between the measured pH value and the target pH value when the measured pH value is greater than the target pH value, while performing feedback control to increase the supply amount of the cleaning agent 3 according to the difference (e.g., negative value) between the measured pH value and the target pH value when the measured pH value is smaller than the target pH value, thereby making the actual pH value closer to the target pH value and equal to it. Note that, when the measured pH value and the target pH value are equal, the controller 300 does not change the supply amount of the cleaning agent 3 and the supply amount of the water 30, but maintains them as they are. Also, the control data for adjusting the supply amount of the cleaning agent 3 and the supply amount of the water 30 according to the difference (deviation) between the measured pH value and the target pH value is map data that predefines the relationship between the deviation between the measured pH value and the target pH value and the supply amount of the cleaning agent 3 and the supply amount of the water 30 so that the actual pH value matches the target pH value. The supply amount of the cleaning agent 3 and the supply amount of the water 30 are adjusted by adjusting the opening degree of a valve (not shown) provided in the supply system 202 and the driving force of a supply pump. From the viewpoint of ensuring the stability of the feedback control, when the absolute value of the difference between the measured pH value and the target pH value is equal to or less than a predetermined small value, the controller 300 may maintain the supply amount of the cleaning agent 3 and the supply amount of the water 30 as they are without changing them.

[0098] Then, when the stirring by the stirrer 204, typically the rotation of the rotating shaft 204a at a constant rotation speed, is continued for a predetermined time that is set in advance as the time required for dissolving the chlorine components, the adjustment of the chlorine concentration by dissolving the chlorine components while adjusting the pH value of the slurry dust 203 in the chlorine concentration adjustment step 101′ is completed, and the slurry dust 203 is subjected to solid-liquid separation to obtain a used cleaning agent 4 containing the eluted chlorine components and having an increased chlorine concentration, and a cleaned electric furnace dust 5 with a reduced chlorine content.

[0099] The zinc extraction step 102 and the electrolysis step 103 in the subsequent steps are the same as those in the first embodiment. However, when the electrolysis tail solution containing the alkaline agent 6 containing the zinc component and having a high pH value in the electrolysis step 103 is returned to the chlorine concentration adjustment step 101' to be reused as a part of the cleaning agent 3, the pH value of the electrolysis tail solution of the cleaning agent 3 is adjusted to be within the range of 8.5 to 10.5, so that further extraction of the zinc component from the electric furnace dust 1 does not occur. Therefore, it is possible to return the electrolysis tail solution in the electrolysis step 103 to the zinc extraction step 102 to use it as a part of the aqueous solution of the alkaline agent 6 as an extraction solvent for the zinc component, and also to return the electrolysis tail solution to the chlorine concentration adjustment step 101' to use it as a practical cleaning solution for the chlorine component. In addition, as an experimental example of this embodiment, an experiment was performed under the same conditions as in Experimental Example 1 corresponding to the first embodiment, and the same results as in Experimental Example 1 were stably obtained.

[0100] The chlorine concentration adjustment step 101' in the present embodiment may be provided in place of the chlorine concentration adjustment step 101 in the second to fourth embodiments. Also in the chlorine concentration adjustment step 101' in the present embodiment, the target to be separated from the electric furnace dust 1 by cleaning the electric furnace dust 1 with the cleaning agent 3 may be fluorine in addition to or instead of chlorine.

[0101] In the zinc production method of the present embodiment described above, the chlorine concentration adjustment step 101' adjusts the pH value of the slurry dust obtained by stirring the electric furnace dust or secondary dust while immersed in an aqueous alkali hydroxide solution during cleaning to within the range of 8.5 to 10.5, which is lower than the pH value of the aqueous alkali hydroxide solution used in the zinc-containing aqueous solution production step 102. Therefore, the chlorine component can be eluted from the electric furnace dust or secondary dust without extracting the zinc component, and zinc with the required quality characteristics can be produced.

[0102] Furthermore, in the zinc production method of this embodiment, the electrolytic tail solution from the electrolysis step 103 is returned to the chlorine concentration adjustment step 101', the aqueous alkali hydroxide solution in the chlorine concentration adjustment step 101' contains the electrolytic tail solution, and the chlorine concentration adjustment step 101' adjusts the pH value of the slurry dust obtained by stirring while immersed in the aqueous alkali hydroxide solution containing the electrolytic tail solution. Therefore, even if the electrolytic tail solution is used as part of the cleaning solution, the chlorine components can be eluted from the electric furnace dust or secondary dust without further extraction of the zinc components, and zinc with the required quality characteristics can be produced.

[0103] Furthermore, in the zinc production method of this embodiment, the chlorine concentration adjustment step 101' sets a target value at a predetermined value within the range of 8.5 to 10.5, which is lower than the pH value of the alkali hydroxide aqueous solution used in the zinc-containing aqueous solution production step 102, and controls the amount of alkaline agent and the amount of water for obtaining the alkali hydroxide aqueous solution in the chlorine concentration adjustment step 101' according to the deviation between the target value and the measured pH value of the slurry dust. Therefore, the pH value of the slurry dust can be reliably maintained at an appropriate value, and zinc with the required quality characteristics can be produced.

[0104] In addition, the shape, arrangement, number, etc. of the components of the present invention are not limited to the above-mentioned embodiment, and such components can be appropriately modified within the scope of the gist of the invention, such as by appropriately replacing such components with those that achieve equivalent effects. [Industrial Applicability]

[0105] As described above, the present invention provides a method for producing zinc in which the chlorine concentration can be reduced during the process of selectively extracting the zinc component in electric furnace dust or secondary dust using an aqueous alkali hydroxide solution as an extraction solvent to produce a zinc-containing aqueous solution, and then electrolyzing the zinc-containing aqueous solution to produce zinc as an electrolytic product. Therefore, due to its versatile and universal nature, it is expected to be widely applicable to zinc production methods that use electric furnace dust generated during the melting and smelting of scrap in the electric furnace process, which is one of the steelmaking processes, or secondary dust generated in a reduction furnace when part of the electric furnace dust is recycled as a steelmaking raw material. [Explanation of symbols]

[0106] 1. Electric furnace dust 2...Secondary dust 3. Cleaning agent 4. Used cleaning agent 5...Cleaned electric furnace dust 6. Alkaline agent 7...Residue 8. Zinc-containing alkaline solution 10. Zinc 11...Calcium carbonate 12...Carbon dioxide 13... Dechlorination agent 14...Chlorine compounds 15...Zinc-containing alkaline solution with adjusted chlorine concentration 16...Zinc metal 17...Metal impurities 18...Zinc-containing alkaline aqueous solution with reduced impurities 19...Oxidizing agent 20…Zinc-containing alkaline aqueous solution with reduced impurities 21. Sludge 30…Water 101...Chlorine concentration adjustment process 101'...Chlorine concentration adjustment process including pH adjustment 102...Zinc extraction process (zinc-containing aqueous solution production process) 103...Electrolysis process 104...Caking process 105...Chlorine concentration adjustment process 106...Replacement process 107…Iron removal and manganese removal process 200…Cleaning machine 201...Cleaning tank 202…Supply system 203...Slurry electric furnace dust 204...Mixer 204a...rotation shaft 204b...Agitating member 205...pH meter

Claims

1. a zinc-containing aqueous solution producing step of selectively extracting zinc components from electric furnace dust or secondary dust generated when the electric furnace dust is reduced in a reducing furnace as a raw material to produce a zinc-containing aqueous solution containing the zinc components; an electrolysis step of producing zinc by electrolysis using the zinc-containing aqueous solution as an electrolyte, and returning the electrolyte solution after the electrolysis to the zinc-containing aqueous solution production step; A method for producing zinc comprising the steps of: An aqueous solution of an alkali hydroxide is used as an extraction solvent for selectively extracting the zinc component in the zinc-containing aqueous solution producing step, The method further includes a chlorine concentration adjustment step of separating a chlorine component contained in the electric furnace dust or the secondary dust prior to the electrolysis step to reduce the chlorine concentration of the zinc-containing aqueous solution, The chlorine concentration adjustment step includes washing the electric furnace dust or the secondary dust with an aqueous alkali hydroxide solution as a washing liquid obtained by diluting the aqueous alkali hydroxide solution used in the aqueous zinc-containing solution production step to separate the chlorine component; The chlorine concentration adjustment step is a step of adjusting a pH value of a slurry dust obtained by stirring the electric furnace dust or the secondary dust while immersed in the alkaline hydroxide aqueous solution of the cleaning solution when the electric furnace dust or the secondary dust is washed with the alkaline hydroxide aqueous solution as the cleaning solution, to a range of 8.5 to 10.5 which is smaller than a pH value of the alkaline hydroxide aqueous solution used as the extraction solvent in the zinc-containing aqueous solution production step by diluting the alkaline hydroxide aqueous solution used in the zinc-containing aqueous solution production step by using the alkaline hydroxide aqueous solution as the cleaning solution, and adjusting the pH value of the slurry dust obtained by stirring the electric furnace dust or the secondary dust while immersed in the alkaline hydroxide aqueous solution of the cleaning solution, to a range of 3 to 5, within a range of 8.5 to 10.5, and adjusting the pH value of the alkaline hydroxide aqueous solution used as the extraction solvent in the zinc-containing aqueous solution production step by using the alkaline hydroxide aqueous solution as the cleaning solution after washing containing the separated chlorine component as the cleaning solution again within a range in which the chlorine component can be eluted, and then discharging the alkaline hydroxide aqueous solution, which is the cleaning solution after washing, to a range in which the chlorine component can be eluted, outside the system without sending it to the zinc-containing aqueous solution production step and the electrolysis step, while sending the electric furnace dust or the secondary dust from which the chlorine component has been separated to the zinc-containing aqueous solution production step.

2. The electrolytic tail solution is returned to the chlorine concentration adjustment step, and the alkaline hydroxide aqueous solution in the chlorine concentration adjustment step contains the electrolytic tail solution, 2. The method for producing zinc according to claim 1, wherein the chlorine concentration adjusting step adjusts the pH value of the slurry dust obtained by immersing the slurry dust in the aqueous alkali hydroxide solution containing the electrolytic solution and stirring the resulting slurry dust.

3. 3. The method for producing zinc according to claim 1, wherein the chlorine concentration adjusting step has a target value within a range of 8.5 to 10.5, which is smaller than the pH value of the alkali hydroxide aqueous solution used in the zinc-containing aqueous solution generating step, and controls the amount of the alkaline agent and the amount of water for obtaining the alkali hydroxide aqueous solution in the chlorine concentration adjusting step according to the deviation between the target value and the measured pH value of the slurry dust.

4. 4. The method for producing zinc according to claim 1, wherein the chlorine concentration adjusting step comprises contacting the zinc-containing aqueous solution with a dechlorinating agent to separate the chlorine component.

5. The method further includes a substitution step of contacting the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step with metallic zinc to reduce and precipitate metal impurity components more noble than zinc in the zinc-containing aqueous solution, The method for producing zinc according to any one of claims 1 to 4, wherein the electrolysis step is performed by using the zinc-containing aqueous solution that has been subjected to the substitution step as the electrolyte.

6. a deironization / demanganese process in which the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production process is contacted with an oxidizing agent to separate iron components and manganese components in the zinc-containing aqueous solution; a substitution step of contacting the zinc-containing aqueous solution that has been subjected to the iron and manganese removal step with metallic zinc to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution; and The method for producing zinc according to any one of claims 1 to 5, wherein the electrolysis step is performed by using the zinc-containing aqueous solution that has been subjected to the substitution step as the electrolyte.

7. The zinc-containing aqueous solution produced in the zinc-containing aqueous solution production process is a first zinc-containing aqueous solution and a second zinc-containing aqueous solution having a chlorine concentration lower than that of the first zinc-containing aqueous solution, and the zinc produced by electrolysis using the first zinc-containing aqueous solution as an electrolyte in the electrolysis process is used as the metallic zinc in the substitution process.

8. A method for producing zinc as described in claim 4, wherein the dechlorinating agent is silver oxide or silver nitrate.

9. A method for producing zinc described in any one of claims 1 to 8, in which calcined dust obtained in a calcination process in which calcium carbonate is mixed with the electric furnace dust and calcined is used as the raw material in the chlorine concentration adjustment process.

Citation Information

Patent Citations

  • Method for producing zinc powder adopting electrolytic leaching of zinc alloy ash pulp

    CN107419111A

  • Yosetsunokoshino genshohoho

    JP1976017143A

  • Ryusanaenyoekikaraensoojokyosuruhoho

    JP1976033798A

  • Heavy metal recovery in ferrous metal production processes

    JP1982501384A

  • Method for recovering heavy metal from molten fry ash

    JP1998109077A