Anti-fog glass
A bubble region between the adhesive layer and glass plate near the boundary of the shielding layer and opening in anti-fog glass mitigates thermal stress, preventing peeling and maintaining appearance while effectively preventing fogging.
Patent Information
- Application Number
- JP2020179881
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-08
- Filing Date
- 2020-10-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Anti-fog films or electric heating films on vehicle windshields can peel off due to thermal expansion differences with black ceramic shielding layers, affecting appearance and functionality, especially when exposed to sunlight.
Incorporating a bubble region with a specific area and bubble density between the adhesive layer and the glass plate near the boundary of the shielding layer and opening, where the anti-fog or electric heating film extends, to alleviate thermal stress and improve adhesion.
Significantly suppresses peeling of the anti-fog or electric heating film without impairing the aesthetic appearance, ensuring effective fog prevention on vehicle windshields.
Smart Images

Figure 0007593052000003 
Figure 0007593052000004 
Figure 0007593052000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an anti-fogging glass. [Background technology]
[0002] In recent years, in response to the increasing demand for safe driving and automated driving of vehicles, it has become common to attach an information acquisition device to the windshield of an automobile, etc. For example, a camera for acquiring information on the area ahead of the vehicle is attached to the upper center portion of the windshield of the vehicle.
[0003] Typically, a shielding layer made of black ceramic is provided on the periphery of the windshield and on the protruding portion that protrudes from the approximate center of the upper portion toward the lower side.
[0004] However, if such a shielding layer is present in a position facing the camera, the field of view of the camera is blocked, so a region without a shielding layer, i.e., an opening, is provided in the portion of the windshield facing the camera.
[0005] Additionally, if this opening becomes fogged while the vehicle is being driven, this again can obscure the camera's view and affect its operation.
[0006] Therefore, in order to avoid such fogging problems, an anti-fog film or an electric heating film is installed over the opening of the windshield so as to cover the opening (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2018 / 016454 [Patent Document 2] International Publication No. 2010 / 149649 Summary of the Invention [Problem to be solved by the invention]
[0008] The anti-fog film is installed above the opening so that the periphery of the anti-fog film overlaps with the shielding layer. As described above, the shielding layer is made of black ceramics, so the shielding layer is prone to absorbing heat from sunlight and to thermal expansion.
[0009] Therefore, if the windshield of the vehicle is continuously exposed to sunlight, the difference in thermal expansion between the anti-fog film and the shielding layer may cause the anti-fog film to peel off.
[0010] On the other hand, if various measures are taken to prevent such peeling, the aesthetic appeal of the windshield may be impaired. For example, if the anti-fog film is made significantly thinner in order to improve its adhesion, the unevenness around the opening may become noticeable, which may impair the appearance.
[0011] Such problems may also occur in anti-fogging glass having an electric heating film instead of an anti-fogging film.
[0012] The present invention has been made in consideration of the above background, and an object of the present invention is to provide an anti-fogging glass that can significantly suppress peeling of the anti-fogging film or electric heating film without adversely affecting the appearance. [Means for solving the problem]
[0013] In the present invention, A glass plate and a shielding layer disposed on one surface of the glass plate so as to define an opening, the shielding layer defining a boundary between the opening and the shielding layer in a top view; When viewed from above, an anti-fogging film or an electric heating film is installed so as to cover the opening and extend outside the boundary; having The anti-fog film has an adhesive layer and an anti-fog layer from the side closer to the glass plate, The electric heating film has an adhesive layer and an electric heating body from the side closer to the glass plate, A bubble region including a plurality of bubbles is provided between the adhesive layer and the glass plate or in the adhesive layer on the inner side of the boundary near the boundary, 1 mm of the bubble area 2 In the region, the total area occupied by the plurality of bubbles is 0.01 mm 2 ~0.13mm 2 An anti-fogging glass is provided. Effect of the Invention
[0014] The present invention can provide an anti-fogging glass that can significantly suppress peeling of the anti-fogging film or electric heating film without adversely affecting the appearance. [Brief description of the drawings]
[0015] [Figure 1] 1 is a top view showing a schematic configuration example of an anti-fogging glass according to an embodiment of the present invention. FIG. [Figure 2(a)] 3 is an enlarged view showing the vicinity of a second portion of the shielding layer in the anti-fogging glass according to one embodiment of the present invention. FIG. [Figure 2(b)] FIG. 2 is an enlarged view of the vicinity of a second portion of the shielding layer in an anti-fogging glass according to another embodiment of the present invention. [Figure 2(c)] 10 is an enlarged view showing the vicinity of a second portion of the shielding layer in an anti-fogging glass according to still another embodiment of the present invention. FIG. [Diagram 3] FIG. 2(b) is a schematic diagram showing a cross section taken along line II in FIG. 2(a). [Figure 3A] FIG. 2 is a schematic diagram showing a part of a cross section of an anti-fogging glass according to another embodiment of the present invention. [Figure 3B] FIG. 2 is a schematic top view of an electric heating film in an anti-fog glass according to another embodiment of the present invention. [Figure 4] FIG. 1 is a flow diagram illustrating a method for producing anti-fogging glass according to one embodiment of the present invention. [Diagram 5] FIG. 1 is a cross-sectional view showing a schematic diagram of one embodiment of an anti-fog film. [Figure 6] FIG. 2 is a top view showing a schematic configuration of an anti-fogging glass sample produced in the examples. [Figure 7] 1 is a micrograph of the vicinity of the boundary between the glass sheet and the shielding layer in a sample of anti-fog glass according to one embodiment of the present invention. [Figure 8] 8 is an enlarged photograph of a portion of the section in FIG. 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, one embodiment of the present invention will be described.
[0017] (Anti-fogging glass according to one embodiment of the present invention) An embodiment of the present invention will be described with reference to FIGS.
[0018] FIG. 1 shows a schematic top view of an anti-fog glass according to one embodiment of the present invention.
[0019] As shown in FIG. 1, an anti-fog glass according to one embodiment of the present invention (hereinafter referred to as "first anti-fog glass") 100 has a glass plate 110 and a shielding layer 120 provided on one surface of the glass plate.
[0020] The glass plate 110 has an upper edge 112, a lower edge 114, and two side edges 116. The shielding layer 120 has a first portion 122 provided along the periphery of the glass plate 110, and a second portion 124 protruding from approximately the center of the upper edge 112 of the glass plate 110 toward the lower edge 114. Note that a portion of the second portion 124 of the shielding layer 120 where the shielding layer 120 is not present, i.e., an opening 130, is provided.
[0021] The first anti-fog glass 100 further includes an anti-fog film 140 disposed so as to cover the opening 130 .
[0022] Fig. 2(a) shows an enlarged view of the vicinity of the second portion 124 of the shielding layer 120 in the first anti-fogging glass 100. Fig. 3 also shows a schematic cross section taken along line II in Fig. 2(a).
[0023] 2(a) and 3, the opening 130 does not have the shielding layer 120 installed therein, and therefore, in a top view, a boundary 132 is defined between the shielding layer 120 and the opening 130. In one embodiment shown in FIG. 2(a), the boundary 132 forms a closed section along the opening 130.
[0024] The shielding layer 120 may be provided so as to define the opening 130, and may have a form as shown in Fig. 2(b) and Fig. 2(c). That is, the boundary 132 may form an open section along the opening 130. Specifically, there may be an area below the opening 130 where the shielding layer 120 is not provided. When there is an area where the shielding layer 120 is not provided, the opening 130 is defined by connecting the start point and the end point of the boundary 132 with a straight line or a curved line.
[0025] Moreover, the anti-fog film 140 is disposed on the opening 130 so as to extend beyond the boundary 132 in a top view. In other words, the anti-fog film 140 is disposed so that its periphery overlaps with the shielding layer 120.
[0026] 2(a), the opening 130 and the anti-fog film 140 have a substantially trapezoidal shape. The anti-fog film 140 has a shape substantially similar to that of the opening 130.
[0027] However, there are no particular limitations on the shapes of the opening 130 and the anti-fog film 140 in the first anti-fog glass 100. The details regarding the shapes of both will be described later.
[0028] As shown in FIG. 3, the anti-fog film 140 has, in order from closest to the glass plate 110, an adhesive layer 150, a base layer 170, and an anti-fog layer 180.
[0029] The adhesive layer 150 allows the anti-fog film 140 to be adhered to the glass plate 110 and the shielding layer 120. The anti-fog layer 180 also serves to suppress fogging of the opening 130.
[0030] In the example shown in Fig. 3, a gap 190 having a substantially triangular cross section is present between the side end of the shielding layer 120 and the adhesive layer 150 of the anti-fog film 140. However, this is merely an example, and the gap 190 may be present in any shape and size. Alternatively, the gap 190 may not be substantially present.
[0031] Here, the first anti-fogging glass 100 has an air bubble region 152 in a predetermined position near the boundary 132 between the shielding layer 120 and the opening 130 when viewed from above, and on the inside of the boundary 132. In this embodiment, the vicinity of the boundary 132 means a region up to 3 mm from the boundary 132 when viewed from above.
[0032] 3, the bubble region 152 is formed at a distance D from the boundary 132. Hereinafter, the portion between the boundary 132 of interest and the bubble region 152 of interest will be referred to as a "transition portion" 158.
[0033] The distance D, ie the width of the transition portion 158, is in the range of 0 to 1 mm.
[0034] In the bubble region 152, a large number of bubbles 154 exist. 2 The area occupied by the air bubbles 154 contained in the hit (hereinafter referred to as the "air bubble occupancy area") is 0.01 mm 2 ~0.13mm 2 The range is.
[0035] The bubble-occupied area in the bubble region 152 can be evaluated by photographing the bubble region 152 with an optical microscope from the side of the first anti-fogging glass 100 on which the anti-fogging film 140 is not installed (the lower side in FIG. 3), and then analyzing the obtained image. Specifically, the area occupied by each bubble in the bubble region 152 in the obtained image is image-analyzed in plan view, and the sum of the areas occupied by each bubble is divided by the area of the bubble region 152 in the photographed section to determine the bubble-occupied area in the bubble region 152. The photographing magnification is 200 to 1000 times.
[0036] The number of bubbles 154 contained in the bubble region 152 is 200 / mm 2 ~700 pieces / mm 2 It is preferable that the average maximum length of the bubbles 154 is in the range of 0.01 mm to 0.06 mm.
[0037] In the present application, the average maximum length of the bubbles 154 represents the average value of the maximum length d of each bubble 154. Such a maximum length d can be evaluated by performing image analysis on the obtained image. That is, the maximum lengths d of all bubbles 154 included in the image are calculated, and the average of the maximum lengths d is calculated to obtain the average maximum length of the bubbles 154.
[0038] Similarly, the density of the air bubbles 154 can be calculated by determining the number of air bubbles from the obtained image and dividing the number by the area of the air bubble region 152 in the imaging section.
[0039] 3, the air bubbles 154 contained in the air bubble region 152 are dispersed almost uniformly throughout the air bubble region 152. However, this is merely an example, and the air bubbles 154 may have a distribution in the thickness direction or planar direction of the adhesive layer 150.
[0040] For example, the air bubbles 154 may be distributed in greater numbers on the side of the adhesive layer 150 close to the interface with the base layer 170, and in particular may be present only on the side of the adhesive layer 150 close to the interface with the base layer 170. Alternatively, the air bubbles 154 may be distributed in greater numbers on the side of the adhesive layer 150 close to the interface with the glass plate 110, and in particular may be present only on the side of the adhesive layer 150 close to the interface with the glass plate 110.
[0041] Moreover, the bubble region 152 does not necessarily have to be formed inside the adhesive layer 150 , but may be formed between the adhesive layer 150 and the glass plate 110 .
[0042] Such a first anti-fogging glass 100 can be applied to, for example, the windshield of a vehicle.
[0043] When the first anti-fog glass 100 is applied to the windshield of a vehicle, the anti-fog film 140 can effectively suppress fogging that may occur at the opening 130 on rainy or snowy days.
[0044] Furthermore, even if the shielding layer 120 is heated by heat radiation from the sun on a sunny day, the presence of the bubble region 152 can significantly reduce thermal stress that may be caused by the difference in thermal expansion between the shielding layer 120 and the anti-fog film 140. As a result, peeling of the anti-fog film 140 can be significantly suppressed.
[0045] Furthermore, in the first anti-fogging glass 100, the bubble-occupied area in the bubble region 152 is 1 mm 2 Per 0.01mm 2 ~0.13mm 2 Therefore, the problem of the appearance of the first anti-fogging glass 100 being impaired due to the presence of the bubble regions 152 is unlikely to occur.
[0046] Due to the effects described above, the first anti-fogging glass 100 can significantly prevent the anti-fogging film 140 from peeling off without impairing the appearance.
[0047] (Components of the anti-fogging glass according to one embodiment of the present invention) Next, each component included in the anti-fogging glass according to one embodiment of the present invention will be described in more detail. In the following description, the components will be described using the above-mentioned first anti-fogging glass 100 as an example. Therefore, the reference symbols used in Figures 1 to 3 will be used to represent each component.
[0048] (Glass Plate 110) The specifications of the glass plate 110 used in the first anti-fogging glass 100, such as the glass composition, structure, and thickness, are not particularly limited.
[0049] For example, laminated glass, such as that used in conventional vehicle windshields, may be used as the glass plate 110. Laminated glass is composed of two glass substrates and an interlayer film between them.
[0050] Alternatively, the glass pane 110 may be constructed from a single piece of glass.
[0051] (shielding layer 120) There is no particular limitation on the specifications of the shielding layer 120, such as the composition, structure, and thickness. The shielding layer 120 may be made of black ceramics, as is used in conventional windshields for vehicles.
[0052] Specifically, the shielding layer 120 may include a low melting point glass powder (glass frit), a heat-resistant black pigment, a filler, and a resin.
[0053] The shielding layer 120 may be formed, for example, by printing a ceramic paste onto the glass plate 110 and then heating the paste to bake it onto the glass plate 110 .
[0054] In this case, the ceramic paste may be prepared by adding a pigment powder together with glass frit to a resin and a solvent, and kneading them together. As a method for printing the ceramic paste, for example, a screen printing method or an inkjet printing method may be used.
[0055] The thickness of the shielding layer 120 is not particularly limited, but is usually in the range of 10 μm to 20 μm.
[0056] The shape of the opening 130 in the second portion 124 of the shielding layer 120 is not particularly limited. The opening 130 may be, for example, substantially triangular or substantially rectangular in shape.
[0057] In this application, the term "substantially rectangular" refers to a concept including a shape that includes a curve or straight lines in addition to the four sides in the mathematical sense. For example, the term "substantially rectangular" may include a shape in which at least one of the four corners of a rectangle is rounded, a shape in which at least one of the four sides is curved, and a shape in which at least one of the four corners is cut off by a straight line. In particular, if at least one of the four sides is curved, it is easier to ensure the angle of view of the camera.
[0058] The terms "substantially triangular" and "substantially ___ shaped" should be interpreted similarly.
[0059] The opening 130 may be, for example, a substantially square, a substantially rectangular, a substantially diamond, or a substantially parallelogram. Alternatively, the opening 130 may be substantially trapezoidal in shape as shown in FIG. 2(a). Also, when the opening 130 is substantially trapezoidal in shape, the interior angles on either side of the bottom side may be different from each other.
[0060] In addition to the above, various shapes of the opening 130 are conceivable.
[0061] (Anti-fog film 140) As described above, the anti-fog film 140 is disposed so that the end portion of the anti-fog film 140 is disposed outside the boundary 132 between the shielding layer 120 and the opening 130. In other words, the anti-fog film 140 is disposed so as to overlap the shielding layer 120 along the periphery of the opening 130.
[0062] As shown in FIG. 3, when the dimension of the overlapping portion is Lo, the minimum value of the dimension Lo is in the range of, for example, 2 mm to 8 mm.
[0063] In particular, it is preferable that the dimension Lo of the overlap portion be in the range of 2 mm to 20 mm over the entire periphery of the opening 130.
[0064] The anti-fog film 140 may be substantially conformal to the shape of the opening 130 .
[0065] The shape of the anti-fog film 140, as viewed from above, desirably has a handle region 142 and a main body region 144. The main body region 144 is a region that covers the opening 130. It is preferable that the main body region 144 and the handle region 142 are substantially rectangular. In terms of workability, it is particularly preferable that the handle region 142 be trapezoidal.
[0066] The corners of the anti-fog film 140 may be cut in a curved or straight line, which can further prevent the anti-fog film 140 from peeling off.
[0067] The anti-fog film 140 is transparent, and therefore each layer constituting the anti-fog film 140 described below is made of a transparent material.
[0068] (adhesive layer 150) The adhesive layer 150 of the anti-fog film 140 has a function of adhering the anti-fog film 140 to the opening 130. In addition, the adhesive layer 150 is made of a material that forms an air bubble region 152 having the above-mentioned characteristics inside the opening 130 when the anti-fog film 140 is adhered to the opening 130.
[0069] The adhesive layer 150 may be made of an acrylic material or a rubber material.
[0070] Alternatively, the adhesive layer 150 may be made of a resin, for example, obtained by copolymerizing an acrylic monomer and a methacrylic monomer and setting the resin to a desired glass transition temperature.
[0071] As the acrylic monomer, methyl acrylate, ethyl acrylate, butyl acrylate, stearyl acrylate, 2-ethylhexyl acrylate, and the like can be used.
[0072] As the methacrylic monomer, ethyl methacrylate, butyl methacrylate, isobutyl methacrylate, stearyl methacrylate, and the like can be used.
[0073] When the insulating layer is formed by heat lamination or the like, an organic material that softens at the lamination temperature may be used.
[0074] For example, in the case of a resin obtained by copolymerizing a methacrylic monomer and an acrylic monomer, the glass transition temperature can be adjusted by changing the compounding ratio of each monomer. The glass transition temperature of the adhesive layer 150 is preferably 10° C. or lower. By setting the glass transition temperature at 10° C. or lower, it becomes easier to ensure an area occupied by air bubbles.
[0075] Furthermore, the shear storage modulus of the adhesive layer 150 at 25° C. and a frequency of 1 Hz is preferably 0.01 MPa to 5 MPa. By setting it to 0.01 MPa or more, it becomes easier to ensure the air bubble-occupied area. The shear storage modulus is more preferably 0.2 MPa or more, and particularly preferably 0.4 MPa or more.
[0076] In particular, a preferred material for the adhesive layer 150 is, for example, a (meth)acrylic polymer containing alkyl (meth)acrylate. Such an adhesive layer 150 has a relatively suitable hardness. Therefore, when such an adhesive layer 150 is placed around the opening 130, the size and density of the bubbles 154 contained in the bubble region 152, as well as the area occupied by the bubbles, can be relatively easily adjusted.
[0077] The thickness of the adhesive layer 150 is t a The thickness of the shielding layer 120 is t s Then, the ratio t a / t s is preferably in the range of 1.5 to 3.3.
[0078] comparison a / t s By setting the ratio t to 1.5 or more, the step at the boundary 132 can be made inconspicuous. a / t s is preferably 1.7 or more.
[0079] comparison a / t s By setting the value to 3.3 or less, the influence of deterioration due to moisture absorption of the material constituting the adhesive layer 150 can be reduced.
[0080] The thickness of the adhesive layer 150 is t a The thickness of the base layer 170 is t b Then, the ratio t a / t b is preferably in the range of 0.25 to 1.0.
[0081] comparison a / t b By setting the ratio t to 0.25 or more, the step at the boundary 132 can be made inconspicuous. a / t b By making the ratio of the anti-fog film 140 to be 1.0 or less, the workability when adhering the anti-fog film 140 along the periphery of the opening 130 can be improved.
[0082] (Base material layer 160) As the substrate layer 160 of the anti-fog film 140, a conventional substrate layer 160 can be used.
[0083] The base layer 160 may be made of a resin such as polyethylene or polyethylene terephthalate (PET).
[0084] There is no particular limitation on the thickness of the base layer 160. The base layer 160 may have a thickness of 20 μm to 100 μm.
[0085] (Anti-fog layer 180) The anti-fog layer 180 of the anti-fog film 140 is not particularly limited as long as it has an anti-fog function. The anti-fog layer 180 may be, for example, a conventionally used material.
[0086] For convenience, the anti-fogging layer 180 is roughly divided into two types: a passive type and an active type. Here, the passive type refers to an anti-fogging layer 180 that constantly exerts an anti-fogging function. On the other hand, the active type refers to an anti-fogging layer 180 that can switch the anti-fogging function by turning it on and off.
[0087] Both types will be explained below.
[0088] (passive type) The passive type anti-fogging layer 180 has a water-absorbent resin or a hydrophilic resin.
[0089] Examples of water-absorbent resins include epoxy, urethane, acrylic, and polyvinyl acetal.
[0090] Moreover, an example of the hydrophilic resin is polyvinylpyrrolidone.
[0091] (active type) The active type anti-fogging layer 180 is formed by coating the base layer 170 with a transparent film made of a predetermined material.
[0092] The transparent film may be composed of, for example, ITO (indium tin oxide), silver, silver nanowires, conductive polymers (PEDOT / PSS), carbon nanotubes, graphene, etc. Alternatively, the transparent film may be composed of copper mesh.
[0093] Alternatively, the active anti-fogging layer 180 may be formed by forming a thin linear pattern on the substrate layer 170. Such a linear pattern may be made of, for example, silver.
[0094] In both the passive type and the active type, the thickness of the antifogging layer 180 is, for example, in the range of 5 μm to 50 μm, although it is not limited thereto.
[0095] (Bubble region 152) As described above, the bubble region 152 is formed at a position spaced a distance D from the boundary 132 in a top view.
[0096] The distance D is in the range of 0 to 1 mm. The distance D is preferably in the range of 0.2 mm to 0.7 mm.
[0097] 3, that is, the width V of the bubble region 152 may be in the range of 0.1 mm to 1.0 mm. The width V of the bubble region 152 is preferably in the range of 0.2 mm to 0.5 mm.
[0098] It should be noted that the bubble region 152 does not necessarily have to be formed around the entire periphery of the boundary 132 , and the bubble region 152 may be formed along only a portion of the boundary 132 .
[0099] For example, if, in a top view, the opening 130 and boundary 132 are substantially rectangular in shape, bubble region 152 may be formed along only one side, two sides, or three sides.
[0100] Furthermore, when the opening 130 and the boundary 132 are substantially circular in top view, the bubble region 152 may be formed along at least ¼ of the circumference.
[0101] However, from the viewpoint of effectively preventing the anti-fog film 140 from peeling off, it is preferable that the bubble region 152 be formed along the entire periphery of the boundary 132 .
[0102] In the bubble region 152, the maximum length of each bubble 154 is preferably 0.2 mm or less.
[0103] (Anti-fogging glass according to another embodiment of the present invention) As described above, the anti-fogging layer 180 is roughly divided into two types, a passive type and an active type, for convenience.
[0104] Of these, the active type anti-fogging layer 180 can be applied to an electric heating film in addition to an anti-fogging film.
[0105] Therefore, hereinafter, a specific embodiment of an anti-fogging glass having an electric heating film instead of an anti-fogging film (hereinafter, such an anti-fogging glass is referred to as a "second anti-fogging glass") will be described with reference to FIG. 3A.
[0106] The configuration of the second anti-fogging glass is substantially the same as that of the first anti-fogging glass 100 described above, except for the electric heating film. Therefore, a top view of the second anti-fogging glass is omitted here. In addition, when describing members and the like corresponding to those of the first anti-fogging glass 100 described above, reference numerals obtained by adding 200 to the reference numerals shown in Figures 1 to 3 are used.
[0107] FIG. 3A shows a schematic cross-sectional view of a second anti-fog glass 300.
[0108] 3A, the second anti-fog glass 300 has a glass plate 310 and a shielding layer 320 disposed on one surface of the glass plate. As described above, a portion of the shielding layer 320 is provided with a portion where the shielding layer 320 is not present, i.e., an opening 330.
[0109] The second anti-fog glass 300 further includes an electric heating film 341 disposed to cover the opening 330 .
[0110] The shielding layer 320 is not provided in the opening 330, and therefore, in a top view, a boundary 332 is defined between the shielding layer 320 and the opening 330. The boundary 332 forms a closed section along the opening 330.
[0111] Moreover, the electric heating film 341 is disposed on the opening 330 so as to extend beyond the boundary 332 in a top view. In other words, the electric heating film 341 is disposed so that its periphery overlaps with the shielding layer 320.
[0112] As shown in FIG. 3A, the electric heating film 341 includes, in order from closest to the glass plate 310, an adhesive layer 350, a base layer 370, and an electric heating element 381.
[0113] The adhesive layer 350 and the substrate layer 370 are similar to the adhesive layer 150 and the substrate layer 170 included in the anti-fog film 140 in the first anti-fog glass 100 described above.
[0114] On the other hand, the electric heating element 381 functions as an electric resistor, and is composed of at least one of a heatable coating, a printed conductor, a mesh, and a heating wire, for example.
[0115] If the heating element 381 is comprised of a heatable coating or printed conductor, the heating element 381 preferably has a sheet resistance of 0.5 ohms per square to 100 ohms per square at a voltage of 12 V to 15 V. Also, if the heating element 381 is comprised of a mesh or heating wire, the diameter of the mesh or heating wire may be in the range of 10 μm to 100 μm, for example.
[0116] The heatable coatings, meshes and heating wires may also include fluorine-doped tin dioxide (F:SnO2), tin-doped indium oxide (ITO), silver, copper, tin, gold, aluminum, iron, tungsten, chromium, or alloys thereof. Additionally or alternatively, the heatable coatings and heating wires may include at least one conductive organic polymer.
[0117] The heatable coatings and printed conductors have, for example, a layer thickness of 0.01 μm to 50 μm, preferably 0.05 μm to 10 μm.
[0118] The heatable coating may optionally have antistatic functionality, water absorbency, hydrophilic, hydrophobic, oleophobic, and hydrophobic properties.
[0119] The heatable coating may be composed of a hydrophilic polyester. Alternatively, the heatable coating may include hydrophilic polymers such as polysaccharides, cellulose derivatives, and polyethylene oxide. The heatable coating may also include halogenated hydrocarbons having -CHF-, -CF2-, and / or -CF3- groups to impart hydrophobicity.
[0120] Heater 381 may be deposited by conventional techniques such as, for example, chemical vapor deposition (CVD), physical vapor deposition (PVD), or sputtering.
[0121] In the second anti-fogging glass 300, the electric heating film 341 can be attached to the glass plate 310 and the shielding layer 320 by the adhesive layer 350. In addition, the electric heating element 381 has the role of suppressing fogging of the opening 330.
[0122] Here, the second anti-fogging glass 300 has an air bubble region 352 in a predetermined position near a boundary 332 between the shielding layer 320 and the opening 330 in a top view and inside the boundary 332. In this embodiment, the vicinity of the boundary 332 means a region up to 3 mm from the boundary 332 in a top view.
[0123] 3A, bubble region 352 is formed at a distance D from boundary 332. As previously mentioned, the portion between intended boundary 332 and intended bubble region 352 is referred to as a "transition portion" 358.
[0124] The distance D, ie, the width of the transition portion 358, is in the range of 0 to 1 mm.
[0125] The configuration of the bubble region 352 is similar to that of the bubble region 152 in the first anti-fogging glass 100 described above.
[0126] Such a second anti-fogging glass 300 can also be applied to, for example, the windshield of a vehicle.
[0127] When the second anti-fogging glass 300 is applied to the windshield of a vehicle, the effect of the electric heating film 341 can significantly suppress fogging that may occur at the opening 330 on rainy or snowy days.
[0128] Furthermore, even if the shielding layer 320 is heated by heat radiation from the sun on a sunny day, the presence of the bubble region 352 can significantly reduce the thermal stress that may be caused by the difference in thermal expansion between the shielding layer 320 and the electric heating film 341. As a result, peeling of the electric heating film 341 can be significantly suppressed.
[0129] Furthermore, in the second anti-fogging glass 300, the bubble-occupied area in the bubble region 352 is 1 mm 2 Per 0.01mm 2 ~0.13mm 2 Therefore, the problem of the appearance of the second anti-fogging glass 300 being impaired due to the presence of the bubble region 352 is unlikely to occur.
[0130] Due to the above-mentioned effects, in the second anti-fogging glass 300, it is possible to significantly prevent the peeling of the electric heating film 341 without impairing the appearance.
[0131] In the above description, it is assumed that the electric heating film 341 has, in order from closest to the glass plate 310, the adhesive layer 350, the base layer 370, and the electric heating body 381. However, the electric heating film 341 may have, in order from closest to the glass plate 310, the adhesive layer 350, the electric heating body 381, and the base layer 370.
[0132] Moreover, the electric heating film 341 does not necessarily have to be disposed so as to surround the entire opening 330 when viewed from above.
[0133] FIG. 3B shows a schematic top view of an electrothermal film 341A placed over the opening 330A.
[0134] In the example shown in Fig. 3B, the electric heating film 341A does not cover the top and bottom of the opening 330. In this embodiment, the generation of air bubbles can be significantly suppressed when the electric heating film 341A is placed in the opening 330. In addition, in this embodiment, the electric heating film 341A can be easily positioned, and the electric heating film 341A can be placed in an appropriate position. The electric heating film 341A may have bus bars 349A on both ends.
[0135] (Method of manufacturing anti-fogging glass according to one embodiment of the present invention) Next, an example of a method for producing the anti-fogging glass according to one embodiment of the present invention will be described with reference to FIG.
[0136] FIG. 4 shows a schematic flow of a method for producing an anti-fogging glass according to one embodiment of the present invention (hereinafter referred to as a "first production method").
[0137] As shown in FIG. 4, the first manufacturing method includes the following steps: A step (S110) of providing a shielding layer on one surface of a glass plate so that an opening is formed; A step (S120) of placing an anti-fog film to cover the opening, thereby forming an air bubble region inside the opening when viewed from above; has.
[0138] Each step will be described below. In the following description, the case of producing the above-mentioned first anti-fogging glass 100 will be described as an example of an anti-fogging glass according to one embodiment of the present invention. Therefore, the reference symbols used in Figs. 1 to 3 will be used to represent each component.
[0139] (Step S110) First, a glass plate 110 is prepared. As described above, the glass plate 110 has an upper edge 112, a lower edge 114, and two side edges 116.
[0140] Next, a shielding layer 120 is applied to one surface of the glass plate 110 in a predetermined pattern.
[0141] There is no particular limitation on the method for providing the shielding layer 120. The shielding layer 120 may be provided by, for example, a printing method.
[0142] The shielding layer 120 is provided having a first portion 122 and a second portion 124 as previously described.
[0143] 1, the first portion 122 is provided in a frame shape along the periphery of the glass plate 110. In contrast, the second portion 124 is provided so as to protrude from approximately the center of the upper side 112 of the glass plate 110 toward the lower side 114. The second portion 124 is provided so as to form a portion where the shielding layer 120 is not present, i.e., an opening 130, at a predetermined position.
[0144] The shape of the opening 130 may be, for example, substantially trapezoidal.
[0145] (Step S120) An anti-fog film 140 is then placed over the opening 130 in the second portion 124 .
[0146] The anti-fog film 140 is disposed around the periphery of the opening 130 so as to overlap the shielding layer 120 .
[0147] The anti-fog film 140 has, in order from the glass plate 110 , an adhesive layer 150 , a base layer 170 , and an anti-fog layer 180 .
[0148] 5, the anti-fog film 140 may have a protective layer 195 on the surface of the anti-fog layer 180. The protective layer 195 preferably has the same shape as the anti-fog layer 180. Furthermore, the anti-fog film 140 may have a separator film 197 on the side of the adhesive layer 150 opposite the base material layer 170. The separator film 197 may have a slit when viewed from above. The separator film 197 is preferably provided so as to cover the surface of the adhesive layer 150 when viewed from above.
[0149] The anti-fog film 140 is placed on the glass plate 110 with the adhesive layer 150 facing inward. If the anti-fog film 140 has a separator film 197, the separator film 197 is first peeled off. After a part of the exposed adhesive layer 150 is temporarily fixed on the shielding layer 120, the anti-fog film 140 is adhered to the opening 130 using a squeegee so as to cover the opening 130.
[0150] By providing the anti-fog film 140, an air bubble region 152 containing a large number of air bubbles 154 is formed at a position a distance D away from the boundary 132 between the shielding layer 120 and the opening 130 toward the inside of the boundary 132 when viewed from above.
[0151] In particular, the material, hardness (storage modulus), thickness t a , as well as the aforementioned ratio t a / t s and ratio t a / t b By appropriately selecting, the bubble-occupied area in the bubble region 152 can be adjusted to a predetermined range.
[0152] Through the above steps, the first anti-fogging glass 100 can be manufactured.
[0153] It should be noted that the second anti-fogging glass 200 can also be manufactured by a method similar to the above-mentioned first manufacturing method. EXAMPLES
[0154] Next, examples of the present invention will be described. However, it should be noted that the present invention is not limited to the following examples.
[0155] In the following description, Examples 1 to 5 are working examples, and Examples 11 and 12 are comparative examples.
[0156] (Example 1) Anti-fog glass samples were prepared by the following method.
[0157] First, a glass plate having a length of 100 mm, a width of 100 mm, and a thickness of 3.5 mm was prepared. Next, a shielding layer was formed on the first surface of the glass plate (one surface of the length of 100 mm × width of 100 mm). The shielding layer was formed by screen printing a paste for the shielding layer in a predetermined pattern, followed by heat treatment at 560 ° C for 7 minutes. For the paste for the shielding layer, a composition containing glass frit, a filler, a pigment, and an acrylic resin-based vehicle was used.
[0158] As shown in FIG. 6, the shielding layer 220 was provided on only half of the first surface 218 of the glass plate 210. The thickness t s was approximately 15 μm.
[0159] Next, an anti-fog film 240 was prepared in the following manner.
[0160] First, the base layer is made of a material with a thickness of t b A PET film (A4300; manufactured by Toyobo Co., Ltd.) having a thickness of 100 μm was prepared. Next, an anti-fogging layer was formed on one surface of the base layer. The anti-fogging layer was formed by spin-coating the anti-fogging layer composition on the base layer.
[0161] The anti-fogging layer composition was prepared in the following manner.
[0162] 31.4g of water-soluble epoxy denacol EX1610 (manufactured by Nagase Chemtex Corporation), 33.4g of chelating compound solution A1, 18.4g of neoalcohol IPM (manufactured by Taishin Chemical Co., Ltd.), 8.5g of ion-exchanged water, 0.09g of nitric acid (60wt%, manufactured by Junsei Chemical Co., Ltd.), and 8.1g of alkoxysilane compound KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.) were added to a glass container. The glass container was stirred at room temperature for 60 minutes to obtain a composition for anti-fogging layer.
[0163] The chelate compound solution A1 was prepared by mixing 3.0 g of aluminum trisacetylacetonate (Sigma-Aldrich) and 97.0 g of methanol (special grade; Junsei Chemical Co., Ltd.) and stirring the mixture at 25° C. for 10 minutes.
[0164] After spin coating, the base layer was held at 100° C. for 30 minutes to form an anti-fogging layer on the base layer.
[0165] Next, an adhesive layer was placed on the opposite side of the base layer to the anti-fogging layer. The adhesive layer was made of an adhesive (CS9861UAS; manufactured by Nitto Denko Corporation). The thickness of the adhesive layer was t a is 25 μm.
[0166] This resulted in an anti-fog film having a thickness of 145 μm.
[0167] 6, an anti-fog film 240 measuring 50 mm×50 mm was placed approximately in the center of the first surface 218 of the glass plate 210. The anti-fog film 240 was attached to the center of the first surface 218 with the adhesive layer side facing the glass plate 210.
[0168] Then, while the squeegee was pressed against one end of the anti-fog film 240 (the left end in FIG. 6), the squeegee was moved toward the shielding layer 220 (to the right in FIG. 6) to bring the anti-fog film 240 into close contact with the glass plate 210 and the shielding layer 220.
[0169] In this way, an anti-fogging glass sample (hereinafter referred to as "Sample 1") was produced.
[0170] (Example 2) In the same manner as in Example 1, an anti-fogging glass sample (hereinafter referred to as "Sample 2") was produced.
[0171] However, in Example 2, the thickness of the adhesive layer t a The other manufacturing conditions were the same as in Example 1.
[0172] (Example 3) In the same manner as in Example 1, an anti-fogging glass sample (hereinafter referred to as "Sample 3") was produced.
[0173] However, in Example 3, the thickness of the adhesive layer t a The other manufacturing conditions were the same as in Example 1.
[0174] (Example 4) In the same manner as in Example 1, an anti-fogging glass sample (hereinafter referred to as "Sample 4") was produced.
[0175] However, in Example 4, the thickness of the base layer t b The other manufacturing conditions were the same as in Example 1.
[0176] (Example 5) In the same manner as in Example 1, an anti-fogging glass sample (hereinafter referred to as "Sample 5") was produced.
[0177] However, in Example 5, the thickness of the base layer t b is 50 μm, and the thickness of the adhesive layer t a The other manufacturing conditions were the same as in Example 1.
[0178] (Examples 11 and 12) Anti-fogging glass samples (hereinafter referred to as "Sample 11" and "Sample 12", respectively) were produced in the same manner as in Example 1.
[0179] However, in Examples 11 and 12, the thickness t b was changed from that in Example 1. The other production conditions were the same as in Example 1.
[0180] Table 1 below shows the thickness of the substrate layer for each sample. b , the thickness of the shielding layer t s , thickness of adhesive layer t a , ratio t a / t s , and the ratio t a / t b are shown together.
[0181] [Table 1]
[0182] (evaluation) The following evaluation tests were carried out using each sample.
[0183] (Appearance evaluation) For each sample, the vicinity of the boundary (see 260 in FIG. 6) between the glass plate 210 and the shielding layer 220 was visually observed from the side where the anti-fog film 240 was not installed. When the bubble region was not noticeable near the boundary, it was judged as ◯, and when it was noticeable, it was judged as ×.
[0184] (Observation of bubble regions) In each sample, the vicinity of the boundary 260 between the glass plate 210 and the shielding layer 220 was observed with an optical microscope.
[0185] The location of the bubble region, the size of the bubble region, the average maximum length of the bubbles contained in the bubble region, the bubble density, and the bubble-occupied area were measured.
[0186] For the measurements, a microscope (VHX-5000; Keyence) and its associated image analysis software or the image analysis software ImageJ were used. As described above, the average maximum length and density of bubbles were evaluated by photographing the bubble region at a magnification of 1000 times and then analyzing the resulting images. The bubble-occupied area was evaluated by photographing the bubble region at a magnification of 200 times and then analyzing the resulting images.
[0187] Fig. 7 shows an example of a micrograph taken near the boundary 260 in sample 1. Fig. 8 shows an enlarged view of the vicinity of the boundary 260 in Fig. 7.
[0188] 7 and 8, in sample 1, bubble regions 152 were observed near the boundary 260 between the shielding layer 220 and the glass plate 210. Note that in sample 2, bubble regions 152 of a similar shape were also observed.
[0189] (Thermal shock test) The peel resistance of the anti-fog film of each sample was evaluated by a thermal shock test. The appearance of the anti-fog film was visually observed before and after the thermal shock test. The case where there was no change in appearance before and after the test was judged as ◯, and the case where at least one of lifting or peeling occurred in the anti-fog film after the test was judged as ×.
[0190] The thermal shock test was carried out in accordance with JIS C 60068. Specifically, the sample was subjected to 10 cycles of holding at 100° C. for 30 minutes and then holding at −40° C. for 30 minutes.
[0191] The sample heating and cooling rates were both 15° C. / min.
[0192] Table 2 below shows the evaluation results obtained for each sample.
[0193] [Table 2]
[0194] From the results in Table 2, the bubble area in the bubble region is 0.003 mm 2 It was found that in Sample 11, the adhesion of the anti-fog film was deteriorated and the anti-fog film was easily peeled off.
[0195] In addition, the bubble area in the bubble region is 0.153 mm 2 In sample 12, the bubble regions became noticeable even when visually inspected, and it was found that the appearance was undesirable.
[0196] In contrast, the area occupied by the air bubble is 0.01 mm 2 ~0.13mm 2 It was found that in Samples 1 to 5 within this range, the bubble regions were not noticeable and the peel resistance of the anti-fog film was also good.
[0197] In this way, the area occupied by the air bubble is 0.01 mm 2 ~0.13mm 2 It has been confirmed that by forming the bubble region so as to be in the range, peeling of the anti-fog film can be significantly suppressed without adversely affecting the appearance of the anti-fog glass. [Explanation of symbols]
[0198] 100 No. 1 Anti-Fog Glass 110 Glass Plate 112 Top 114 Bottom 116 side 120 Shielding layer 122 First Part 124 Second Part 130 Aperture 132 Boundary 140 Anti-fog film 142 Handle area 144 Body area 150 Adhesive layer 152 Bubble Region 154 Bubbles 158 Transition part 170 Base material layer 180 Anti-fog layer 190 Gap 195 Protective layer 197 Separator Film 198 Break 210 Glass Plate 218 First Surface 220 Shielding layer 240 Anti-fog film 260 Boundary 300 Second anti-fog glass 310 Glass Plate 320 Shielding layer 330 aperture 332 Boundary 341, 341A Electric heating film 349A Busbar 350 adhesive layer 352 Bubble Region 354 Bubbles 358 Transition part 370 Base material layer 381 Electric Heater 390 Gap
Claims
1. A glass plate and a shielding layer disposed on one surface of the glass plate so as to define an opening, the shielding layer defining a boundary between the opening and the shielding layer in a top view; When viewed from above, an anti-fogging film or an electric heating film is installed so as to cover the opening and extend outside the boundary; having The anti-fog film has an adhesive layer and an anti-fog layer from the side closer to the glass plate, The electric heating film has an adhesive layer and an electric heating body from the side closer to the glass plate, A bubble region including a plurality of bubbles is provided between the adhesive layer and the glass plate or in the adhesive layer on the inner side of the boundary near the boundary, 1 mm of the bubble region 2 In the region, the total area occupied by the plurality of bubbles is 0.01 mm 2 ~0.13mm 2 That is, anti-fog glass.
2. 2. The anti-fogging glass according to claim 1, wherein the bubble region is present at a position 0.2 mm to 0.7 mm away from the boundary.
3. The anti-fogging glass according to claim 1 , wherein the bubble region is formed along the entire periphery of the boundary.
4. 4. An anti-fogging glass according to claim 1, wherein the maximum length of each bubble is 0.1 mm or less.
5. The thickness of the adhesive layer is t a and the thickness of the shielding layer is t s Then, the ratio t a / t s The anti-fogging glass according to any one of claims 1 to 4, wherein the σ is in the range of 1.5 to 3.
3.
6. The anti-fogging glass according to claim 1 , wherein the anti-fogging film has a shape similar to that of the opening.
7. 7. The anti-fog glass according to claim 1, wherein the opening is substantially rectangular in shape.
8. 8. The anti-fog glass of claim 7, wherein the opening has a substantially trapezoidal shape.
9. The anti-fogging glass according to claim 7, wherein the rectangular shape has at least one curved side.
10. 10. The anti-fog glass according to claim 7, wherein the anti-fog film or the electric heating film covers one pair of opposite sides of the opening and does not cover another pair of opposite sides of the opening.
11. The anti-fogging glass according to any one of claims 1 to 10, wherein the minimum overlapping area between the anti-fogging film or the electric heating film and the shielding layer over the entire circumference of the opening when viewed from above is in the range of 2 mm to 8 mm.
12. The anti-fogging glass according to any one of claims 1 to 11, wherein an overlap between the anti-fogging film or the electric heating film and the shielding layer over the entire circumference of the opening is in the range of 2 mm to 20 mm.
13. The anti-fogging glass according to claim 1 , wherein the anti-fogging film or the electric heating film has a substrate layer between the adhesive layer and the anti-fogging layer or the electric heating body.
14. The anti-fogging glass according to claim 13, wherein a value obtained by dividing the thickness of the adhesive layer by the thickness of the substrate layer is 0.25 to 1.0.
Citation Information
Patent Citations
Windshield
JP2017214059A
Disc with a heatable, optically transparent sensor array
WO2010149649A1
Windshield and windshield manufacturing method
WO2018016453A1
Antifog film
WO2018016454A1