Curable resin composition and cured product thereof
A curable resin composition with epoxy resin and biomass-modified acid anhydrides addresses the low biomass and performance issues of existing epoxy resins, offering enhanced heat resistance and low dielectric properties for advanced materials and electronic components.
Patent Information
- Application Number
- JP2024539608
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-15
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Existing epoxy resin compositions using furfural as a raw material have a low biomass content and struggle to maintain performance requirements, particularly in terms of heat resistance and dielectric properties.
A curable resin composition is developed using an epoxy resin represented by formula (1) and biomass-modified acid anhydrides such as myrcene-modified, farnesene-modified, and α-terpinene-modified acid anhydrides, with a biomass content of 20% or more, to enhance heat resistance and low dielectric properties.
The composition achieves high biomass content with improved heat resistance and low dielectric properties, suitable for applications in carbon fiber reinforced plastics, semiconductor element sealing, and printed wiring boards.
Smart Images

Figure 0007594711000007 
Figure 0007594711000001 
Figure 0007594711000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition containing a specific epoxy resin and a specific acid anhydride, and a cured product thereof, which is suitably used in the fields of sealing materials for semiconductor elements, electric and electronic components such as printed wiring boards and build-up laminates, lightweight and high-strength materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, 3D printing applications, and adhesives. [Background technology]
[0002] Epoxy resins are widely used in the fields of electrical and electronic parts, structural materials, adhesives, paints, etc., due to their workability and the excellent electrical properties, heat resistance, adhesiveness, and moisture resistance (water resistance) of the cured products. In recent years, with the development of the electrical and electronic fields in particular, there has been a demand for further improvement in the properties of resins, such as heat resistance, low dielectric constant, and low dielectric tangent. In addition, as structural materials, there is a demand for lightweight materials with excellent mechanical properties for aerospace materials, leisure and sports equipment applications, etc.
[0003] In recent years, biomass resources have been attracting attention as carbon-neutral resources from the viewpoint of environmental issues. Furfural is known as a compound derived from biomass, and Patent Document 1 discloses an epoxy resin using furfural as a raw material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-211254 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, since Patent Document 1 uses fullerenol as a raw material, mixes it with an epoxy resin and a phenol novolac resin which is a curing agent derived from petrochemicals to form an epoxy resin composition, the biomass content of the composition is low.
[0006] Generally, when trying to increase the biomass content, it becomes difficult to maintain the performance required for the curable resin composition. Therefore, a curable resin composition having a high biomass content and satisfying the required characteristics has been demanded.
[0007] The present invention has been made in view of the above situation, and an object thereof is to provide a curable resin composition having a high biomass content and excellent high heat resistance and low dielectric properties, and a cured product thereof.
Means for Solving the Problems
[0008] That is, the present invention relates to the following [1] to [9]. In the present invention, “(numerical value 1) to (numerical value 2)” indicates that the upper and lower limit values are included. [1] A curable resin composition containing an epoxy resin represented by the following formula (1) and a biomass-modified acid anhydride.
[0009]
Chemical formula
[0010] (In formula (1), n is the average value of the number of repetitions, and represents a real number of 1 < n < 15.) [2] The curable resin composition according to the above item [1], wherein the biomass-modified acid anhydride is one or more selected from myrcene-modified acid anhydride, farnesene-modified acid anhydride, and α-terpinene-modified acid anhydride. [3] The curable resin composition according to the above item [1] or [2], wherein the biomass content of the biomass-modified acid anhydride is 20% or more. [4] The curable resin composition according to any one of items [1] to [3] above, wherein the epoxy resin has an ICI viscosity (150° C.) of 0.01 to 0.20 Pa·s. [5] The curable resin composition according to any one of the above [1] to [4], having a biomass ratio of 20% or more. [6] The curable resin composition according to any one of the preceding items [1] to [5], which is for use in carbon fiber reinforced plastics. [7] The curable resin composition according to any one of the above [1] to [5], which is used for semiconductor element encapsulation. [8] The curable resin composition according to any one of the above [1] to [5], which is for a printed wiring board. [9] A cured product obtained by curing the curable resin composition according to any one of the above items [1] to [8]. Effect of the Invention
[0011] The present invention relates to a curable resin composition having a high biomass content and excellent heat resistance and low dielectric properties. Therefore, the present invention is useful for insulating materials for electric and electronic components (such as highly reliable semiconductor encapsulation materials), laminates (such as printed wiring boards and build-up boards), various composite materials including CFRP, adhesives, etc. [Brief description of the drawings]
[0012] [Figure 1] 1 shows a GPC chart of Synthesis Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The curable resin composition of the present embodiment contains an epoxy resin represented by the following formula (1) and a biomass-modified acid anhydride.
[0014] [ka]
[0015] (In formula (1), n is the average value of the number of repetitions and represents a real number where 1 < n < 15.)
[0016] In the above formula (1), the value of n can be determined from the number average molecular weight obtained by measuring the epoxy resin by gel permeation chromatography (GPC, detector: RI), or from the area ratio of each of the separated peaks. It is preferable that n is a real number where 1 < n < 15, more preferably 1 < n < 10, and particularly preferably 1 < n < 5.)
[0017] The epoxy resin represented by the above formula (1) can be obtained by reacting a phenol resin represented by the following formula (2) with epihalohydrin.)
[0018] [Chemical formula]
[0019] (In formula (2), n is the average value of the number of repetitions and represents a real number where 1 < n < 15.)
[0020] The preferable range of n in the above formula (2) is the same as that of the above formula (1).
[0021] The epihalohydrin can be easily obtained from the market. The amount of epihalohydrin used is preferably 2.0 to 10 moles, more preferably 3.0 to 8.0 moles, and even more preferably 3.5 to 6.0 moles per 1 mole of the hydroxyl group of the raw material phenol mixture.)
[0022] In the above reaction, an alkali metal hydroxide can be used as a catalyst for promoting the epoxidation step. Examples of the alkali metal hydroxide that can be used include sodium hydroxide and potassium hydroxide. A solid may be used, or an aqueous solution thereof may be used. In this embodiment, in particular, it is preferable to use a solid formed into flakes in terms of solubility and handling.) The amount of the alkali metal hydroxide used is preferably 0.90 to 1.5 mol, more preferably 0.95 to 1.25 mol, and further preferably 0.99 to 1.15 mol, per mol of hydroxyl groups in the raw material phenol mixture.
[0023] In order to promote the reaction, a quaternary ammonium salt such as tetramethylammonium chloride, tetramethylammonium bromide, trimethylbenzylammonium chloride, etc. may be added as a catalyst. The amount of the quaternary ammonium salt used is preferably 0.1 to 15 g, more preferably 0.2 to 10 g, per mole of hydroxyl groups in the raw material phenol mixture.
[0024] The reaction temperature is preferably 30 to 90° C., more preferably 35 to 80° C. In particular, in this embodiment, for higher purity epoxidation, the reaction temperature is preferably 50° C. or higher, and particularly preferably 60° C. or higher. The reaction time is preferably 0.5 to 10 hours, more preferably 1 to 8 hours, and particularly preferably 1 to 3 hours. If the reaction time is too short, the reaction will not proceed to completion, and if the reaction time is too long, by-products will be produced, which is not preferred. The reaction product of these epoxidation reactions is washed with water or heated under reduced pressure to remove epihalohydrin and solvent. Furthermore, in order to obtain an epoxy resin with a smaller amount of hydrolyzable halogen, the recovered epoxy resin can be dissolved in a ketone compound having 4 to 7 carbon atoms (e.g., methyl isobutyl ketone, methyl ethyl ketone, cyclopentanone, cyclohexanone, etc.) as a solvent, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is added to carry out the reaction to ensure ring closure. In this case, the amount of the alkali metal hydroxide used is preferably 0.01 to 0.3 mol, more preferably 0.05 to 0.2 mol, relative to 1 mol of hydroxyl groups in the raw material phenol mixture used in the epoxidation. The reaction temperature is preferably 50 to 120°C, and the reaction time is preferably 0.5 to 2 hours.
[0025] After the reaction is completed, the salt formed is removed by filtration, washing with water, etc., and the solvent is then distilled off under heating and reduced pressure to obtain the epoxy resin represented by the above formula (1).
[0026] In the synthesis method of the phenolic resin represented by the formula (2) above, when furfural is reacted (condensed) with a phenol, the amount of the phenol is preferably in the range of 1.5 to 20 moles, particularly preferably 3 to 10 moles, per mole of furfural.
[0027] Examples of phenols include disubstituted phenols such as catechol, resorcinol, and hydroquinone, and monosubstituted phenols such as phenol. These may be used alone or in combination of two or more kinds.
[0028] Examples of the solvent include, but are not limited to, methanol, ethanol, propanol, isopropanol, toluene, xylene, etc., and these may be used alone or in combination of two or more. When a solvent is used, the amount of the solvent used is preferably 5 to 500 parts by weight, more preferably 10 to 300 parts by weight, based on 100 parts by weight of phenol.
[0029] In the above condensation reaction, it is preferable to use a base catalyst. Although polycondensation is possible with an acid catalyst, the reaction between furfurals also occurs, resulting in a large amount of by-products. In addition, there is a method using an organometallic compound, but it is disadvantageous in terms of cost. Specific examples of the base catalyst include alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, and potassium hydroxide, alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide, alkali metal alkoxides such as sodium methoxide, sodium ethoxide, potassium methoxide, potassium ethoxide, and potassium-tert-butoxide, and alkaline earth metal alkoxides such as magnesium methoxide and magnesium ethoxide, but are not limited thereto, and may be used alone or in combination of two or more kinds. The amount of the catalyst used is preferably 0.005 to 2.0 times the moles, more preferably 0.01 to 1.1 times the moles, relative to 1 mole of phenol.
[0030] The condensation reaction in the presence of these base catalysts is preferably carried out in the range of 40 to 180° C., particularly preferably in the range of 80 to 165° C., and the reaction time is preferably selected in the range of 0.5 to 10 hours. The reaction product thus obtained is neutralized so that the system becomes neutral, or repeatedly washed with water in the presence of a solvent, and then the water is separated and drained, and the solvent and unreacted materials are removed under heating and reduced pressure to obtain the phenolic resin represented by the formula (2).
[0031] The curable resin composition of the present embodiment contains a biomass-modified acid anhydride together with the epoxy resin represented by formula (1). The biomass-modified acid anhydride is an acid anhydride modified using a biomass raw material, and examples thereof include myrcene-modified acid anhydride, farnesene-modified acid anhydride, and α-terpinene-modified acid anhydride. These can be obtained by reacting a terpene compound such as myrcene, farnesene, or α-terpinene with an acid anhydride such as maleic anhydride, itaconic anhydride, or citraconic anhydride. The curable resin composition of the present embodiment may also be used in combination with an acid anhydride other than the biomass-modified acid anhydride, and examples thereof include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride. These can be used in any ratio, but it is preferable that the ratio of the biomass-modified acid anhydride in the total amount of acid anhydrides used is 30 to 100% by weight, since this increases the biomass degree. The acid anhydride is preferably 0.7 to 1.2 equivalents per equivalent of the epoxy group of the epoxy resin represented by the formula (1). If the amount is less than 0.7 equivalents per equivalent of the epoxy group, or if it exceeds 1.2 equivalents, curing may be incomplete and good cured physical properties may not be obtained.
[0032] From the viewpoint of environmental issues, the biomass degree of the epoxy resin represented by the formula (1) is preferably 20% or more. The biomass degree of the biomass-modified acid anhydride is preferably 20% or more, more preferably 40% or more, and particularly preferably 60% or more. The biomass degree of the curable resin composition of the present embodiment is preferably 20% or more, more preferably 30% or more, and particularly preferably 40% or more. The upper limit of the biomass degree is not particularly limited and may be 100%, but is preferably 60% in consideration of the balance with the cured physical properties. A high biomass degree can also reduce the amount of fossil resource-based materials, such as petroleum, used, and is therefore meaningful in terms of sustainable use of resources.
[0033] The biomass content of each material and the curable resin composition can be determined by accelerator gravimetric analysis in accordance with ASTM D6866-21.
[0034] In the curable resin composition of the present embodiment, the epoxy resin represented by the formula (1) can be used alone or in combination with other epoxy resins. When used in combination, the proportion of the epoxy resin represented by the formula (1) in the total epoxy resin is preferably 5 to 95% by weight, more preferably 10 to 95% by weight, and even more preferably 15 to 95% by weight. If the amount added is small, sufficient heat resistance may not be achieved.
[0035] Specific examples of epoxy resins that can be used in combination with the epoxy resin represented by the formula (1) include polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.) or phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) with various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.); polycondensates of the phenols and various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, etc.); polycondensates of the phenols and aromatic dimethanols (benzene dimethanol, biphenyl dimethanol, etc.); polycondensates of the phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.); polycondensates of the phenols and aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.); polycondensates of the bisphenols and various aldehydes or alcohols, etc., glycidyl ether epoxy resins, alicyclic epoxy resins, glycidylamine epoxy resins, glycidyl ester epoxy resins, etc. Specific examples of epoxy resins containing plant-derived components include compounds obtained by epoxidizing polycondensates obtained by polycondensing various aldehydes with cardanol derived from cashew oil as the phenols, and compounds obtained by epoxidizing linseed oil or soybean oil. As long as they are commonly used epoxy resins, they are not limited to these. These may be used alone or in combination of two or more.In particular, when used in combination with an epoxy resin containing a plant-derived component, the biomass content can be increased, which is preferable.
[0036] The curable resin composition of the present embodiment may be used in combination with a curing agent other than an acid anhydride. Examples of the curing agent include amine compounds, amide compounds, phenol compounds, and active ester compounds. Specific examples of the curing agent that can be used in combination include amide compounds such as dicyandiamide and polyamide resins synthesized from a dimer of linoleic acid and ethylenediamine; o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, 3,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 2,2'-diaminodiphenylsulfone, diethyltoluenediamine, dimethylthiotoluenediamine, and diaminodiphenylmethane. , 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetramethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetraethyldiphenylmethane, 4,4'-diamino-3,3',5,5'-tetraisopropyldiphenylmethane, 4,4'-methylenebis(N-methylaniline) phosphorus), bis(aminophenyl)fluorene, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, 1,3'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)benzene, 1,4'-bis(4-aminophenoxy)biphenyl, 4,4'-(1,3-phenylenediisopropylidene)bisaniline aromatic amine compounds such as 4,4'-(1,4-phenylenediisopropylidene)bisaniline, naphthalenediamine, benzidine, and dimethylbenzidine; aliphatic amine compounds such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), norbornanediamine, ethylenediamine, propanediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, dimer diamine, and triethylenetetramine;Polycondensates of bisphenols (bisphenol A, bisphenol F, bisphenol S, biphenol, bisphenol AD, etc.) or phenols (phenol, alkyl-substituted phenol, aromatic-substituted phenol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.) with various aldehydes (formaldehyde, acetaldehyde, alkyl aldehyde, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, etc.), or the above phenols with various diene compounds (dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.) phenolic compounds such as polymers of the phenols and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, etc.), polycondensates of the phenols and aromatic dimethanols (benzene dimethanol, biphenyl dimethanol, etc.), polycondensates of the phenols and aromatic dichloromethyls (α,α'-dichloroxylene, bischloromethylbiphenyl, etc.), polycondensates of the phenols and aromatic bisalkoxymethyls (bismethoxymethylbenzene, bismethoxymethylbiphenyl, bisphenoxymethylbiphenyl, etc.), polycondensates of the bisphenols and various aldehydes, and modified products thereof; active ester compounds such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds; and the like, but are not limited thereto;
[0037] The curable resin composition of the present embodiment may be used in combination with a curing accelerator. Examples of the curing accelerator that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol, triethylenediamine, triethanolamine, and 1,8-diazabicyclo[5,4,0]undecene-7, organic phosphines such as triphenylphosphine, diphenylphosphine, and tributylphosphine, metal compounds such as tin octylate, tetra-substituted phosphonium tetra-substituted borates such as tetraphenylphosphonium tetraphenylborate and tetraphenylphosphonium ethyltriphenylborate, tetraphenylboron salts such as 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate, and carboxylic acid compounds such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthoic acid, and salicylic acid. The curing accelerator is used in an amount of 0.01 to 15 parts by weight based on 100 parts by weight of the epoxy resin, if necessary.
[0038] The curable resin composition of the present embodiment may contain an inorganic filler as necessary. Examples of inorganic fillers include, but are not limited to, powders such as crystalline silica, fused silica, alumina, zircon, calcium silicate, calcium carbonate, silicon carbide, silicon nitride, boron nitride, zirconia, fosterite, steatite, spinel, titania, and talc, or beads obtained by sphering these. These may be used alone or in combination. The amount of these inorganic fillers used varies depending on the application, but when used as an encapsulant for semiconductor elements, it is preferable to use the inorganic fillers in an amount of 20% by weight or more in the curable resin composition from the standpoint of heat resistance, moisture resistance, mechanical properties, and flame retardancy of the cured product of the curable resin composition, more preferably 30% by weight or more, and more preferably 70 to 95% by weight in order to improve the linear expansion coefficient with the lead frame.
[0039] The curable resin composition of the present embodiment may be blended with a release agent to improve release from the mold during molding. Any of the conventionally known release agents may be used, including, for example, ester waxes such as carnauba wax and montan wax, fatty acids such as stearic acid and palmitic acid and their metal salts, and polyolefin waxes such as oxidized polyethylene and non-oxidized polyethylene. These may be used alone or in combination of two or more. The blending amount of these release agents is preferably 0.5 to 3% by weight based on the total organic components. If the amount is less than this, release from the mold is poor, and if the amount is too much, adhesion to the lead frame or the like is poor.
[0040] The curable resin composition of the present embodiment can be blended with a coupling agent to enhance the adhesion between the inorganic filler and the resin component. Any of the conventionally known coupling agents can be used, including, for example, various alkoxysilane compounds such as vinylalkoxysilane, epoxyalkoxysilane, styrylalkoxysilane, methacryloxyalkoxysilane, acryloxyalkoxysilane, aminoalkoxysilane, mercaptoalkoxysilane, and isocyanatoalkoxysilane, alkoxytitanium compounds, and aluminum chelates. These may be used alone or in combination of two or more. The method of adding the coupling agent may involve treating the surface of the inorganic filler with the coupling agent in advance and then kneading it with the resin, or mixing the coupling agent with the resin and then kneading the inorganic filler.
[0041] The curable resin composition of the present embodiment may contain known additives as necessary. Specific examples of the additives that can be used include polybutadiene and its modified products, modified products of acrylonitrile copolymers, polyphenylene ether, polystyrene, polyethylene, polyimide, fluororesin, maleimide-based compounds, cyanate ester-based compounds, silicone gel, silicone oil, and colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.
[0042] The curable resin composition of the present embodiment can be obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but for example, the composition can be obtained by thoroughly mixing the epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, an additive, etc., using an extruder, a kneader, a roll, a planetary mixer, etc., until the mixture is uniform.
[0043] The obtained curable resin composition can be formed into various forms such as a resin sheet, a prepreg, etc. The prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or the resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.
[0044] The curable resin composition of the present embodiment may be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone as necessary to form a varnish-like composition (hereinafter, simply referred to as varnish), which may be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. The solvent used in this case is in an amount that occupies 10 to 70% by weight, preferably 15 to 70% by weight, of the mixture of the curable resin composition of the present embodiment and the solvent.
[0045] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heated and cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated when laminating the prepreg.
[0046] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods. For example, a resin transfer molding technique (RTM method) can be used in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to prepare a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is hardened, and then the mold is opened to remove the molded product. In addition, a type of RTM method, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process) method, and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-T 2005-527410, can be used, which more appropriately controls the resin injection process, especially the VaRTM method, by evacuating a resin supply tank to a pressure lower than atmospheric pressure, using cyclic compression, and controlling the net molding pressure. In addition, other methods that can be used include the film stacking method, in which the fiber substrate is sandwiched between resin sheets (films), the method of attaching powdered resin to the reinforcing fiber substrate to improve impregnation, the molding method (Powder Impregnated Yarn) that uses a fluidized bed or fluid slurry method in the process of mixing the resin into the fiber substrate, and the method of blending resin fibers into the fiber substrate.
[0047] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among them, acrylic carbon fibers having high tensile strength are preferably used. As the form of carbon fibers, twisted yarn, untwisted yarn, non-twisted yarn, etc. can be used, but untwisted yarn or non-twisted yarn is preferably used because it has a good balance between the formability and strength properties of the fiber-reinforced composite material.
[0048] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP. Examples of the applications include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, printed wiring boards (BGA substrates, build-up substrates, etc.), and electric / electronic parts, 3D printing, as well as additives for other resins, etc.
[0049] The adhesives include adhesives for civil engineering, construction, automobiles, general office use, medical use, and also adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer boards such as build-up boards, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to various uses.
[0050] When the curable resin composition of this embodiment is applied to a semiconductor element encapsulant, the curable resin composition of this embodiment is placed on a lead frame equipped with a semiconductor element, a semiconductor package substrate, and molded by a melt casting method, a transfer molding method, an injection molding method, a compression molding method, or the like, and further heated at 80 to 200° C. for 2 to 10 hours to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like of ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.
[0051] When the curable resin composition of the present embodiment is applied to a printed wiring board application, a prepreg can be obtained by heating and melting the composition to reduce the viscosity and impregnating the composition into reinforcing fibers such as glass fibers and polyamide fibers. Specific examples of the composition include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, and / or organic fibers, but are not particularly limited thereto. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. In addition, as the weaving method of the woven fabric, plain weave, sash weave, twill weave, and the like are known, and these known weaves can be appropriately selected and used according to the intended application and performance. In addition, woven fabrics that have been subjected to fiber opening treatment or glass woven fabrics that have been surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. Moreover, the varnish can be impregnated into reinforcing fibers and dried by heating to obtain a prepreg, which can be used to prepare a copper clad laminate (CCL). The obtained prepreg and CCL can be hot-press molded to prepare a laminate using the curable resin composition of the present embodiment. The laminate is not particularly limited as long as it has one or more prepregs, and may have any other layers. Moreover, a sheet-shaped adhesive can be obtained by applying the varnish onto a release film, removing the solvent under heating, and performing B-stage formation. This sheet-shaped adhesive can be used as an interlayer insulating layer in a multilayer board or an adhesive sheet when mounting a semiconductor. The curable resin composition of the present embodiment can also be suitably used for special board materials such as package boards (substrates) and HDI (high density interconnect). EXAMPLES
[0052] The present invention will be described in more detail below with reference to synthesis examples and examples. The materials, processing contents, processing procedures, etc. shown below can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. Hereinafter, parts are parts by weight unless otherwise specified.
[0053] Various analytical methods were carried out under the following conditions. Epoxy equivalent It is measured according to the method described in JIS K-7236, and the unit is g / eq. ·Softening point The measurement was performed according to JIS K-7234 and the unit is °C. Melt Viscosity ICI melt viscosity (150°C) measured by the cone-plate method, the unit is Pa·s. Biomass analysis (accelerator gravimetric analysis) The measurement was performed in accordance with ASTM D6866-21 and the calculation was performed in units of %.
[0054] [Synthesis Example 1] In a flask equipped with a stirrer, a reflux condenser, and a stirrer, 254 parts by weight of phenol, 63 parts by weight of water, and 27 parts by weight of sodium hydroxide were charged, stirred, dissolved, and heated to 110°C, where 44 parts by weight of furfural was dropped over 2 hours. After that, the mixture was reacted at 110°C for 3 hours, and then heated to 145°C. When the temperature was raised, the water distilled out was removed from the system. After reaching 145°C, the mixture was reacted for 4 hours. Then, the mixture was cooled to 80°C, 63 parts by weight of water was charged, and 4 parts by weight of phosphoric acid and 63 parts by weight of 35% hydrochloric acid were added to neutralize. After repeated washing with water, unreacted phenol was distilled off under reduced pressure with heating to obtain 109 parts by weight of phenolic resin. 78 parts by weight of the obtained phenolic resin were charged into a reaction vessel with 254 parts by weight of epichlorohydrin (ECH, hereinafter the same), 64 parts by weight of dimethyl sulfoxide (DMSO, hereinafter the same), and 13 parts by weight of water. After heating, stirring, and dissolving, 23 parts by weight of flake-shaped sodium hydroxide were charged in portions over 2 hours while maintaining the temperature at 45°C. Then, the reaction was further carried out at 45°C for 2 hours and at 70°C for 60 minutes. Next, washing with water was repeated to remove by-product salts and dimethyl sulfoxide, and then excess epichlorohydrin was distilled off from the oil layer under heating and reduced pressure, and 218 parts by weight of methyl isobutyl ketone was added to the residue and dissolved. This methyl isobutyl ketone solution was heated to 70°C, 7 parts by weight of 30% aqueous sodium hydroxide solution was added, and the reaction was carried out for 1 hour. The reaction solution was then repeatedly washed with water until the washing liquid became neutral. Next, methyl isobutyl ketone was distilled off from the oil layer under heating and reduced pressure to obtain 97 parts by weight of epoxy resin A represented by the above formula (1). The epoxy equivalent was 214 g / eq., the softening point was 49°C, the ICI melt viscosity was 0.04 Pa s, the average repeat number n was 2.1 from GPC, and the biomass ratio was 25%. The GPC chart of epoxy resin A is shown in Figure 1.
[0055] [Synthesis Example 2] 49.1 g of toluene and 25.8 parts of α-terpinene (manufactured by Guangxi Jie Xin Fragrance Co., Ltd.) were placed in a four-neck flask and heated to 85°C and stirred. 16.7 parts of maleic anhydride were added to this solution in four portions over one hour. After the addition was completed, the mixture was stirred at 85°C for one hour. After the reaction was completed, the mixture was concentrated under reduced pressure at 185°C to obtain 37 parts of acid anhydride A.
[0056] [Example 1] The epoxy resin A obtained in Synthesis Example 1 was used as the base resin, the acid anhydride A obtained in Synthesis Example 2 was used as the curing agent, and 2E4MZ (2-ethyl-4-methylimidazole, manufactured by Shikoku Kasei Co., Ltd.) was used as the anionic polymerization initiator. These were mixed and kneaded in the weight ratio shown in the composition in Table 1, and cured at 160°C for 6 hours to produce a cured product. The biomass content of the cured product was 48.6%.
[0057] [Comparative Example 1] The epoxy resin A obtained in Synthesis Example 1 was used as the base resin, and Kayahard MCD (methylnadic anhydride, manufactured by Nippon Kayaku Co., Ltd.) as the curing agent and 2E4MZ (2-ethyl-4-methylimidazole, manufactured by Shikoku Kasei Co., Ltd.) as the anionic polymerization initiator were mixed and kneaded in the weight ratio shown in the composition in Table 1, and cured at 160°C for 6 hours to produce a cured product. The biomass content of the cured product was 15.2%.
[0058] [Comparative Example 2] The epoxy resin A obtained in Synthesis Example 1 was used as the base resin, PN (phenol novolac resin, manufactured by Meiwa Chemical Industry Co., Ltd., hydroxyl equivalent 103 g / eq.) as the curing agent, and TPP (triphenylphosphine) as the curing accelerator were mixed and kneaded in the weight ratio shown in the composition in Table 1, and cured at 180°C for 6 hours to produce a cured product. The biomass content of the cured product was 16.6%.
[0059] The physical properties were measured under the following conditions. <Heat resistance (Tg) measurement conditions> Dynamic viscoelasticity measuring instrument: TA-instruments, DMA-Q800 Measurement temperature range: 25~300℃ Heating rate: 2℃ / min Tg: The peak point of Tan δ was taken as Tg. <Dielectric constant and dielectric loss tangent test> The test was performed at 25° C. using a 10 GHz cavity resonator manufactured by AET Co., Ltd., using a cavity resonator perturbation method. The sample size was 2.5 mm wide x 50 mm long, and the thickness was 0.3 mm.
[0060] [Table 1]
[0061] From the results in Table 1, it was confirmed that Example 1 had a high biomass content, high heat resistance, and excellent low dielectric properties.
Claims
1. The epoxy resin contains an epoxy resin represented by the following formula (1) and a biomass-modified acid anhydride, The curable resin composition, wherein the biomass-modified acid anhydride is at least one selected from the group consisting of a myrcene-modified acid anhydride, a farnesene-modified acid anhydride, and an α-terpinene-modified acid anhydride. 【Chemistry 1】 (In formula (1), n is the average number of repetitions and is a real number in the range of 1<n<15.)
2. The curable resin composition according to claim 1 , wherein the biomass-modified acid anhydride has a biomass degree of 20% or more.
3. The curable resin composition according to claim 1, wherein the epoxy resin has an ICI viscosity (150°C) of 0.01 to 0.20 Pa·s.
4. The curable resin composition according to claim 1 , having a biomass ratio of 20% or more.
5. The curable resin composition according to claim 1 , which is for use in carbon fiber reinforced plastics.
6. The curable resin composition according to claim 1 , which is used as an encapsulating material for semiconductor elements.
7. The curable resin composition according to claim 1 , which is for use in a printed wiring board.
8. A cured product obtained by curing the curable resin composition according to claim 1 .
Citation Information
Patent Citations
Method for preparing 1-methyl-4-isopropyl-bicyclo [2,2,2] octane-2,3 diacid anhydride
CN1562990A
Curing agent for epoxy resin
JP1978120800A
Epoxy resin composition
JP1989163211A
Liquid epoxy resin composition for sealing semiconductor
JP1999021421A
Thermosetting resin composition and its cured product
JP2000319345A
Cited By
Coating layer comprising bio-based resin and home appliance comprising same
WO2026146706A1