Porous Asphalt Paving Mixture

A polymer-modified asphalt pavement mixture with waste carbon black and controlled additives addresses aggregate scattering and UV degradation, enhancing durability and cost-effectiveness by recycling waste materials.

JP7595853B2Active Publication Date: 2024-12-09YONEKURA INST OF SOCIAL INFRASTRUCTURE TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019012227
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-01-28
Publication Date
2024-12-09
Estimated Expiration
2039-01-28

AI Technical Summary

Technical Problem

Existing porous asphalt pavements with high porosity suffer from aggregate scattering and reduced lifespan due to UV exposure, and the use of waste carbon black in asphalt mixtures leads to unstable quality and potential steam explosions during mixing.

Method used

A porous asphalt pavement mixture composed of polymer-modified asphalt type H, waste carbon black, and specific additives, with controlled moisture and impurity levels, is formulated to enhance UV resistance and prevent aggregate scattering, while recycling waste carbon black to reduce costs and environmental impact.

Benefits of technology

The mixture maintains high porosity for water permeability, reduces aggregate scattering, and extends lifespan to match or exceed that of dense-grained asphalt, with improved UV resistance and safe mixing processes, lowering costs through waste carbon black recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595853000009
    Figure 0007595853000009
  • Figure 0007595853000010
    Figure 0007595853000010
  • Figure 0007595853000011
    Figure 0007595853000011
Patent Text Reader

Abstract

To provide a porous asphalt pavement mixture in which recycling of waste carbon black and Cantabro loss factor of porous asphalt pavement mixture exposed to UV light satisfy the criterion.SOLUTION: A porous asphalt pavement mixture 10, 20 is made to contain polymer-modified asphalt H-type 40a and any of new carbon black, waste carbon black, waste rubber carbonized material, waste tire carbonized material or water-containing waste tire carbonized material, so that the porous asphalt pavement mixture allows the polymer-modified asphalt H-type still to remain on a surface aggregate surface to cover the aggregate surface even after several years.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous asphalt pavement mixture using polymer-modified asphalt and carbon black, which is used for a pavement having a water-permeable function. [Background technology]

[0002] Patent Document 1 discloses an invention of a porous asphalt pavement mixture using polymer-modified asphalt H type, which uses recycled aggregate produced by a washing process for washing and removing fine particles from granular asphalt waste material obtained by demolishing an existing asphalt pavement consisting of an asphalt mixture composed of aggregate, filler, and asphalt-based binder, and a grinding process for removing the asphalt adhering to the asphalt waste material after washing. It also lists the results of a Candabro test on recycled porous asphalt using polymer-modified asphalt H type. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-208606 A Summary of the Invention [Problem to be solved by the invention]

[0004] Dense-graded asphalt pavement, which is normal asphalt pavement, has a void ratio of 3 to 5%, so as shown in Figure 2, when there is rainfall 4, rainwater flows over the surface of the dense-graded asphalt pavement 2 as rainwater pavement surface flow 5b, causing the problem of water accumulating on the road pavement surface. In order to drain the road pavement surface, porous asphalt pavement 1 is an asphalt pavement with a void ratio of about 20%, which increases the number of voids in the asphalt pavement and enhances the permeability so that rainfall 4 can drip through the voids in the asphalt within the pavement. In the case of porous asphalt pavement 1, as shown in Figure 1, rainfall 4 permeates through the asphalt pavement as shown in the rainwater infiltration flow 5a, flows along the top of the impermeable layer 3, and flows into the drainage ditch.

[0005] The invention of Patent Document 1 states that the results of the Cantabro test, which evaluates the wear and aggregate scattering resistance of recycled porous asphalt (polymer modified H type), are 8.0 to 11.4% against a standard loss rate of 20% in Table 19 of Patent Document 1. However, even if the standard loss rate of 20% is cleared, the porous asphalt pavement is prone to aggregate scattering due to its high void ratio and other factors over many years of use, and its lifespan is only 60 to 70% compared to dense-graded asphalt pavement. For example, if normal asphalt pavement is repaired in about 12 years, as shown in Figure 4, when a sample was taken from an actual road and an asphalt pavement test such as the Cantabro test was conducted, the performance of the pavement decreased in about 9 years, and it no longer met the required performance of asphalt pavement, and the surface layer had to be repaired.

[0006] The current Cantabro test for evaluating abrasion and aggregate scattering resistance involves placing one specimen in the drum of a Los Angeles testing machine, rotating the drum 300 times without using steel balls, and measuring the weight loss of the specimen to determine the amount of loss. It is usually performed at room temperature in a dry state, but it can also be performed at low temperatures or using specimens that have been immersed in water. This test does not specify that specimens be tested after exposure to ultraviolet light.

[0007] In addition, waste carbon black that falls onto the floor during the carbon black manufacturing process is collected by a dust collector, including the surrounding area, and is collected together with moisture and dust that has fallen onto the floor. This waste carbon black does not meet the shipping quality standards for carbon black, so it cannot be shipped and is incinerated, and there was a problem that it was discarded and not recycled.

[0008] In addition, because waste carbon black contains a certain amount of moisture, there are problems in that in the process of producing asphalt mixtures, where aggregate and stone powder heated to about 180°C are mixed with the waste carbon black containing moisture, which is predicted to cause a steam explosion; the ultrafine waste carbon black particles form agglomerates and the mixture is not mixed uniformly, making the quality of the mixture unstable; and the adhesive strength between asphalt and aggregate that has been mixed with the waste carbon black containing moisture decreases. As a result, there are problems with waste carbon black containing moisture, which means that it cannot be shipped as a product.

[0009] In addition, there was a problem in that the dry-distilled carbonized material containing moisture was predicted to pose a risk of steam explosion during the process of mixing aggregate and stone powder heated to approximately 180°C with waste carbon black containing moisture in the production of asphalt paving mixture.

[0010] The present invention was devised in consideration of these problems, and its objective is to provide a porous asphalt pavement mixture for road pavement that has a large void ratio, allowing rainwater to easily permeate, and is less likely to cause aggregate scattering. [Means for solving the problem]

[0011] The inventors noticed that the difference between a dense-graded asphalt pavement mixture using straight asphalt and a porous asphalt pavement mixture using polymer-modified asphalt H-type is that the void ratio is about 4 to 6 times larger, and that polymer-modified asphalt H-type adds polymers such as resin to straight asphalt. In addition, in the case of a porous asphalt pavement mixture 20 that does not contain carbon black (CB) as shown in Figure 3(a), the polymer-modified asphalt H-type 40a covers aggregates 30 such as gravel at the time of construction, but over the years, the polymer-modified asphalt H-type 40a deteriorates and the aggregates 30 are exposed as shown in Figure 3(b).

[0012] Carbon black also includes new carbon black, which is fine carbon particles having a diameter of about 3 to 500 nm that are manufactured under industrial quality control; waste carbon black, which is collected as carbon black that has fallen to the floor during the carbon black manufacturing process or bagging operation or carbon black that has remained in the process; carbonized waste rubber; carbonized waste tire; and water-containing carbonized waste tire carbonized waste that has been passed through water when carbonized waste tire carbonized waste is separated into radial tire steel and carbonized waste tire.

[0013] Incidentally, the waste carbon black includes waste carbon black that does not contain moisture and waste carbon black that contains moisture, and carbonized waste rubber does not contain moisture.

[0014] The porous asphalt pavement mixture according to claim 1 is a mixture of polymer modified asphalt H type and waste carbon black having a composition of 88.9 to 96.1% by weight of carbon black, 0.3 to 6% by weight of moisture, and 0.1 to 2.1% by weight of impurities such as dust and fine particles. And, crushed It is characterized by being made by blending stones, crushed sand, and stone powder.

[0015] The porous asphalt pavement mixture according to claim 2 is the waste carbon black according to claim 1, which has a composition of 88.9 to 96.1% by weight of carbon black, 0.3 to 6% by weight of moisture, and 0.1 to 2.1% by weight of impurities such as dust and fine particles. before The amount of the additive added to the porous asphalt pavement mixture is 0.01 to 10% by weight. Effect of the Invention

[0016] The inventors considered that although the current Candabro test for evaluating wear and aggregate scattering resistance is performed without exposure to ultraviolet light, as asphalt pavement is exposed to ultraviolet light from sunlight, it is also necessary to perform a Candabro test on the specimen after exposure to ultraviolet light. They decided to perform a Candabro test on the specimen after exposure to ultraviolet light, and performed the ultraviolet light exposure using a weather resistance test device (Model Metal Weather KU-R5, manufactured by Daipla Wintes Co., Ltd.) under conditions of illuminance 75mV / cm2, temperature 60℃, time 40 days, and filter KF-1 (for visible light and ultraviolet light), which is equivalent to 20 years of sunlight in Japan.

[0017] The Cantabro test is performed without UV exposure, and the standard is a loss rate of 20% or less. When the Cantabro test was performed on specimens that were not exposed to UV and those that were exposed to UV, as shown in Table 8, in the case of polymer modified asphalt type II, the specimen with a loss rate of 19.6% without UV exposure had a loss rate of 42.5% after UV exposure, which did not meet the standard loss rate, and the specimen with a loss rate of 15.2% without UV exposure had a loss rate of 26.8% after UV exposure, which did not meet the standard loss rate. This is consistent with the reality that aggregate scattering from porous asphalt pavement increases with long-term use.

[0018] In contrast, in the case of the polymer-modified asphalt H type of the present invention, as shown in Table 8, when waste carbon black was not added, the test specimen with a loss rate of 7.8% without exposure to ultraviolet light had a loss rate of 19.3% after exposure to ultraviolet light, which was just barely clearing the standard loss rate, but when waste carbon black was added, the test specimen with a loss rate of 6.7% without exposure to ultraviolet light had a loss rate of 10.3% after exposure to ultraviolet light, which was a remarkable effect that it was able to greatly clear the standard loss rate. As a result, even if the standard loss rate of 20% was cleared in the Cantabro test of a test specimen not exposed to ultraviolet light, it was shown that wear was increased by exposure to ultraviolet light and aggregate scattering resistance was deteriorated, and the actual situation that aggregate scattering of the porous asphalt pavement is more than that of the dense-graded asphalt pavement shows that the Cantabro test of the test specimen after exposure to ultraviolet light is necessary.

[0019] In addition, there is a significant effect of enabling the recycling of waste carbon black or dry-distilled carbonized material containing moisture, and there is also an effect of preventing global warming since it is possible to prevent the large amount of CO2 that would be emitted into the atmosphere when waste carbon black is incinerated for disposal.

[0020] There was concern that a large amount of dust would be generated when carbon black was mixed with aggregate heated to 180°C and stone powder and then dry-mixed in a mixer, but in the case of waste carbon black or dry-distilled carbide containing moisture, there was a remarkable effect that no dust was generated. Since waste carbon black or dry-distilled carbide containing moisture contains moisture, it is thought that this moisture suppresses the generation of dust. This makes it possible to realize a safe and healthy environment where no dust-related accidents occur.

[0021] Furthermore, no steam explosion occurred. This is believed to be because the moisture contained in the waste carbon black or the dry-distilled carbide containing moisture was dispersed when the waste carbon black or the dry-distilled carbide containing moisture was put into a mixer together with aggregate and stone powder heated to 180°C and mixed dry.

[0022] Furthermore, compared to new carbon black, which costs more than 300,000 yen per ton, waste carbon black is cheaper because it is reused from waste materials that had been disposed of. Also, the amount of cheap waste carbon black added can be within the range of 0.01 to 10%, making it even cheaper than expensive carbon black.

[0023] Therefore, conventional porous asphalt road pavements have water permeability due to their high porosity, but their lifespan is only 60 to 70% compared to dense-graded asphalt road pavements. However, the porous asphalt road pavement of the present invention has the remarkable effect of being water permeable and having a lifespan equal to or greater than that of dense-graded asphalt road pavements even when exposed to ultraviolet rays. [Brief description of the drawings]

[0024] [Figure 1] FIG. 2 is a cross-sectional view illustrating the infiltration and flow of rainwater through a porous asphalt pavement. [Diagram 2] FIG. 2 is a cross-sectional view illustrating the flow of rainwater over the surface of a dense-graded asphalt pavement. [Diagram 3] FIG. 1 is an explanatory diagram of the deterioration state of the polymer-modified asphalt covering the aggregate in the surface layer of a porous asphalt pavement mixture, in which (a) is an explanatory diagram showing the state when the polymer-modified asphalt (polymer-modified asphalt H type) covers the aggregate surface at the start of construction, (b) is an explanatory diagram showing the state in which the polymer-modified asphalt H type has peeled off from the surface of the surface aggregate and the surface aggregate has been scattered in the case of a porous asphalt pavement mixture using conventional polymer-modified asphalt H type without carbon black (CB) several years later, and (c) is an explanatory diagram showing the state in which the polymer-modified asphalt H type still remains on the surface of the surface aggregate and covers the aggregate surface in the case of a porous asphalt pavement mixture using the polymer-modified asphalt H type containing carbon black (CB) of the present invention several years later. [Figure 4]FIG. 1 is an explanatory diagram comparing the asphalt in a porous asphalt pavement mixture when it is a polymer-modified asphalt type H that does not contain carbon black (CB) with the polymer-modified asphalt type H that contains the CB of the present invention, where (a) shows the relationship between performance deterioration, repair implementation, and the number of years that have passed, and (b) shows the relationship between construction and repair costs and the number of years that have passed, showing the difference in life cycle costs after 20 years. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Regarding the composition of the carbon black of the present invention, the composition of discarded carbon black is 88.9 to 96.1% carbon black, 0.3 to 11.0% moisture, and 0.1 to 2.1% impurities such as dust and fine particles, the composition of carbonized waste rubber is about 70% carbon black and about 30% lime-based impurities, the composition of carbonized waste tire containing moisture is 75 to 85% carbon black, about 15% impurities, and 5 to 10% moisture, the composition of carbonized waste tire is about 85% carbon black and about 15% impurities, and the composition of new carbon black is 100% carbon black.

[0026] The porous asphalt pavement mixture of the present invention contains any one of new carbon black, waste carbon black, waste rubber carbonized carbonized waste tire carbonized carbonized waste tire carbonized water-containing waste tire carbonized carbonized water, and polymer modified asphalt H type.

[0027] The amount of carbon black added to the porous asphalt pavement mixture is 0.01 to 10%, preferably 0.1 to 5%, more preferably 0.1 to 3%, and even more preferably 0.1 to 0.5%. When the amount added is up to 5%, the brittleness of the porous asphalt pavement mixture is not noticeable, but when the amount added exceeds 10%, the porous asphalt pavement mixture becomes brittle.

[0028] An example of the blending ratio of the porous asphalt pavement mixture (c to d) of the present invention and the blending ratios of the comparative examples (a, b) are shown in Table 1. In Table 1, specimens a and b were polymer-modified asphalt type II used for indoor tests and actual plant tests, specimen c was polymer-modified asphalt type H used for indoor tests and actual plant tests, specimen d was polymer-modified asphalt type H used for actual plant tests, and specimen e was polymer-modified asphalt type H used for indoor tests.

[0029] [Table 1]

[0030] As shown in Table 1, the porous asphalt pavement mixture of the present invention contains polymer modified asphalt H type, waste carbon black, No. 6 crushed stone, crushed sand, and stone powder. Horn Health was used for the No. 6 crushed stone and crushed sand, and limestone powder was used for the stone powder.

[0031] First, quality tests were conducted on the asphalt pavement mixture in laboratory tests. Specifically, a Cantabro test was conducted to evaluate the aggregate scattering resistance of the asphalt pavement mixture, a wheel tracking test that has a good correlation with actual road rutting, and a Marshall stability test was conducted to evaluate the maximum load and deformation amount when the asphalt pavement mixture is destroyed by load.

[0032] In the Cantablo test, a specimen of porous asphalt pavement mixture was placed in a Los Angeles tester at room temperature, the drum was rotated 300 times without using steel balls, and the amount of loss of the specimen after the test was measured. The Cantablo test results were carried out on the porous asphalt pavement mixture of the present invention using polymer modified asphalt H type and the comparative example of porous asphalt pavement mixture using polymer modified asphalt II type, with different moisture contents relative to the waste carbon black. The results of the laboratory test are shown in Table 2.

[0033] [Table 2]

[0034] As can be seen from Table 2, in the case of porous asphalt pavement mixtures using polymer modified asphalt type II, the cantabro loss rate was 10.8% to 13.5%, and the cantabro loss rate increased as the moisture content relative to the waste carbon black increased, but all were significantly below the standard value of 20% for the cantabro loss rate.

[0035] Furthermore, in the case of a porous asphalt pavement mixture using polymer modified asphalt type H, a moisture content of 0% was used for the waste carbon black, but the Cantabro loss rate was 6.3%, while the Cantabro loss rate for a porous asphalt pavement mixture using polymer modified asphalt type II, which has a moisture content of 0% for the waste carbon black, was 10.8%. This shows that the Cantabro loss rate is roughly halved when using polymer modified asphalt type H compared to when using polymer modified asphalt type II.

[0036] In addition, when looking at polymer modified asphalt type II, the quality of the porous asphalt pavement mixture to which waste carbon black with a moisture content of 6% was added was almost the same as that with a moisture content of 0%, and no deterioration in quality due to moisture was observed.

[0037] Next, the wheel tracking test was performed by placing a small iron wheel (diameter 20 cm, width 5 cm, ground pressure 6.4 kg / cm) on a test piece of porous asphalt pavement mixture of a specified size (30 × 30 × 5 cm). 2 ) was repeatedly run back and forth at a specified temperature (60°C), for a specified time, and at a specified speed (21 round trips / min over a distance of 23 cm), and the dynamic stability (rounds / mm) was calculated from the amount of deformation (wheel rutting) per unit time. The wheel tracking test, which measures wheel rutting and indicates dynamic stability, confirmed the difference in the effect of adding waste carbon black (WCB) when comparing polymer modified asphalt type II and polymer modified asphalt type H. The results of this laboratory test are shown in Table 3.

[0038] [Table 3]

[0039] From Table 3, the dynamic stability (DS value) of the polymer modified asphalt type II was 5,730 times / mm to 6,300 times / mm, which was significantly higher than the standard value of 3,000 times / mm and was good. The dynamic stability (DS value) of the polymer modified asphalt type H was 15,750 times / mm, despite the small amount of waste carbon black (WCB) added of 1%, which is about three times higher than that of the polymer modified asphalt type II, indicating that the dynamic stability (DS value) performance has been significantly improved. In other words, it is shown that rutting hardly occurs even after long-term use.

[0040] In addition, when looking at polymer modified asphalt type II, the quality of the porous asphalt pavement mixture to which waste carbon black with a moisture content of 6% was added was almost the same as that with a moisture content of 0%, and no deterioration in quality due to moisture was observed.

[0041] Next, in the Marshall stability test, the sides of a cylindrical specimen (diameter 101.6 mm, thickness 63.5 mm) of porous asphalt pavement mixture were sandwiched between two arc-shaped loading heads, and a load was applied in the diameter direction at a specified temperature (60°C) and a specified loading rate (50 mm per minute), and the maximum load (stability kN) that the cylindrical specimen showed before it broke and the corresponding deformation amount (flow value 1 / 100 cm) were measured. A Marshall stability test was conducted to compare polymer modified asphalt type II and polymer modified asphalt type H to confirm the difference in the effect of adding waste carbon black (WC). The results of the laboratory test are shown in Table 4.

[0042] [Table 4]

[0043] Table 4 shows that polymer modified asphalt type H containing 1% waste carbon black has slightly higher stability and residual stability values ​​than polymer modified asphalt type II containing 3% waste carbon black, indicating that it has higher performance.

[0044] In addition, when looking at polymer modified asphalt type II, the quality of the porous asphalt pavement mixture to which waste carbon black with a moisture content of 6% was added was almost the same as that with a moisture content of 0%, and no deterioration in quality due to moisture was observed.

[0045] From the results of the above laboratory tests, the Cantabro test, the wheel tracking test and the Marshall stability test, firstly, porous asphalt pavement mixtures containing waste carbon black are effective for asphalt pavement, secondly, when polymer modified asphalt H type is used, the performance of the porous asphalt pavement mixture can be improved even if the ratio of waste carbon black added is significantly reduced, and thirdly, the water content The quality of the porous asphalt pavement mixture containing 6% waste carbon black was almost the same as that containing 0% moisture, indicating that no deterioration in quality due to moisture was observed.

[0046] Next, a porous asphalt pavement mixture was manufactured in an actual plant, and the manufactured porous asphalt pavement mixture was used as a test specimen to carry out a Cantabro test, a Marshall stability test, and a wheel tracking test. During the porous asphalt pavement mixture manufacturing process in an actual plant, even when a porous asphalt pavement mixture to which waste carbon black containing 6% moisture was added was mixed in a mixer in the actual plant, there was almost no dust being blown up, and no risk of a steam explosion was observed.

[0047] First, a wheel tracking test was conducted on the porous asphalt pavement mixture produced in the actual plant, and the results are shown in Table 5.

[0048] [Table 5]

[0049] Table 5 shows that the dynamic stability of polymer-modified asphalt type II is increased by 2,100 times / mm to 4,200 times / mm by adding 3% of waste carbon black, and that of polymer-modified asphalt type H is increased by about 1.3 to 2 times from 7,000 times / mm to 9,000 times / mm. It was also shown that the dynamic stability of polymer-modified asphalt type H (9,000 times / mm) with 0.5% of waste carbon black added is increased by about 2.1 times compared to polymer-modified asphalt type II (4,200 times / mm) with 3% of waste carbon black added. Polymer-modified asphalt type H with 0.5% of waste carbon black added has a dynamic stability of 9,000 times to create a 1 mm rut, and the coefficient of variation for evaluating the variation showed almost no change, indicating that a porous asphalt pavement mixture with extremely high dynamic stability can be produced.

[0050] Next, Marshall stability tests were conducted on the porous asphalt pavement mixture produced in the actual plant, and the results are shown in Table 6.

[0051] [Table 6]

[0052] From Table 6, when comparing with 0% waste carbon black content, the stability of Polymer Modified Asphalt Type II is 4.68kN compared to Polymer Modified Asphalt Type H at 6.42kN, and the residual stability of Polymer Modified Asphalt Type II is 90.4% compared to Polymer Modified Asphalt Type H at 92.4%. Therefore, without the addition of waste carbon black, Polymer Modified Asphalt Type H has slightly higher performance than Polymer Modified Asphalt Type II in both stability and residual stability.

[0053] In addition, when looking at the effect of adding waste carbon black in terms of stability, for polymer modified asphalt type II, the strength increased from 4.68 kN with 0% waste carbon black to 6.05 kN with the addition of 3% waste carbon black, and for polymer modified asphalt type H, the strength increased slightly from 6.42 kN with 0% waste carbon black to 6.79 kN with the addition of 0.5% waste carbon black, indicating that the addition of waste carbon black increases stability.

[0054] Regarding residual stability, for polymer modified asphalt type II, the 90.4% with 0% waste carbon black was reduced to 82.5% with the addition of 3% waste carbon black, and for polymer modified asphalt type H, the 92.4% with 0% waste carbon black was reduced slightly to 90.1% with the addition of 0.5% waste carbon black. In the case of polymer modified asphalt type H, the reduction was slight and the standard value was cleared by a large margin, so there is no problem.

[0055] Next, a Cantablo test was conducted on the porous asphalt pavement mixture produced in the actual plant, and the results are shown in Table 7.

[0056] [Table 7]

[0057] From Table 7, in the case of polymer modified asphalt type II with 3% added waste carbon black, the Cantabro loss rate was reduced from 19.6% without added waste carbon black to 15.2%, and in the case of polymer modified asphalt type H with 0.5% added waste carbon black, the Cantabro loss rate was reduced from 7.8% without added waste carbon black to 6.7%. It is also shown that the Cantabro loss rate is extremely small at 6.7%, even though only 0.5% waste carbon black was added to polymer modified asphalt type H.

[0058] Next, a Candabro test was conducted on the porous asphalt pavement mixture produced in the actual plant after exposure to ultraviolet light, since roads are always exposed to sunlight. A Candabro test was conducted on the porous asphalt pavement mixture of the present invention using polymer modified asphalt H type and the comparative example of the porous asphalt pavement mixture using polymer modified asphalt II type, with the moisture content of the waste carbon black set at 6%. The results are shown in Table 8.

[0059] The Cantabro test shown in Table 8 shows the results after a weathering test in which the material was exposed to UV rays for 40 days. The amount of UV rays from this 40-day continuous exposure is equivalent to the amount of UV rays that an actual road receives from sunlight for 20 years.

[0060] [Table 8]

[0061] Table 8 shows that the cantabro loss rate increases when all test specimens are exposed to UV rays. For example, the cantabro loss rate when polymer modified asphalt type II is used without adding waste carbon black is 19.6%, but increases to 42.5% after UV exposure.

[0062] In addition, the Cantabro loss rate is smaller when polymer modified asphalt type H is used than when polymer modified asphalt type II is used. Also, when comparing cases where waste carbon black (WCB) is not included, the Cantabro loss rate is 19.6% when polymer modified asphalt type II is used, while when polymer modified asphalt type H is used it is 7.8%, which is about one-third the rate.

[0063] In addition, when the effect of waste carbon black (WCB) was confirmed, the cantabro loss rate when polymer modified asphalt type II was used was 19.6% without UV exposure when no waste carbon black was added, but 42.5% after UV exposure, a change of 22.9%, and when 3% waste carbon black was added, the cantabro loss rate was 15.2% without UV exposure, but 26.8% after UV exposure, a change of 11.6%. In addition, when polymer modified asphalt type H was used, the cantabro loss rate was 7.8% without UV exposure when no waste carbon black was added, but 19.3% after UV exposure, a change of 11.5%, and when 0.5% waste carbon black was added, the cantabro loss rate was 6.7% without UV exposure, but 10.3% after UV exposure, a change of 3.6%, a remarkable effect.

[0064] In addition, when the effect of waste carbon black was confirmed by the cantabro loss rate after exposure to ultraviolet rays, the cantabro loss rate when polymer modified asphalt type II was used was 42.5% without the addition of waste carbon black, which decreased to 26.8% with the addition of 3% waste carbon black, and the cantabro loss rate when polymer modified asphalt type H was used was 19.3% without the addition of waste carbon black, which decreased to 10.3% with the addition of 0.5% waste carbon black.

[0065] In addition, it was shown that the cantabro loss rate after exposure to ultraviolet light for polymer modified asphalt type II, which contained 3% added waste carbon black, was 26.8%, while the cantabro loss rate after exposure to ultraviolet light for polymer modified asphalt type H, which contained only 0.5% added waste carbon black, was extremely small at 10.3%.

[0066] In addition, the results of the Cantabro test after exposure to ultraviolet light when 0.5% recycled carbon black (WCB) was added to polymer modified asphalt type H showed that the Cantabro loss rate was reduced to 10.3%, which is smaller than the Cantabro loss rate (26.8%) when 3% recycled carbon black (WCB) was added to polymer modified asphalt type II. This indicates that the effect of adding recycled carbon black (WCB) in preventing ultraviolet degradation is greater for polymer modified asphalt type H than for polymer modified asphalt type II.

[0067] From the above-mentioned laboratory test and actual plant test, the quality of the porous asphalt pavement mixture containing waste carbon black with a moisture content of 6% was not deteriorated by moisture content compared to that with a moisture content of 0%. It was also shown that the polymer modified asphalt type H can obtain higher quality than the polymer modified asphalt type II.

[0068] Based on the above, in the porous asphalt pavement mixture 10 using the polymer-modified asphalt 40b containing carbon black (CB) of the present invention, it can be expected that the aggregate 30 will be firmly covered with the polymer-modified asphalt 40b even after approximately 20 years, as shown in Figures 3(c) and 4(a).

[0069] As a result, as shown in Fig. 4(a), in the case of the polymer-modified asphalt H type 40a in which the asphalt of the porous asphalt pavement mixture 20 does not contain carbon black (CB), two repairs are required in about 20 years, whereas in the case of the polymer-modified asphalt H type 4b in which the CB of the porous asphalt pavement mixture 10 of the present invention is contained, the asphalt 40b will not peel off for about 20 years, and the surface layer does not need to be repaired. The reason why no repair is required for 20 years is that the performance standard is satisfied in the Cantabro test of a test specimen exposed to ultraviolet rays equivalent to the amount of ultraviolet rays irradiated from sunlight for 20 years.

[0070] As a result, as shown in Figure 4 (b), although the initial construction cost of porous asphalt pavement 10 using H-type polymer modified asphalt containing CB of the present invention is only about 1% higher than that of porous asphalt pavement 20 using H-type polymer modified asphalt not containing CB, the life cycle cost (construction and repair costs) over 20 years is expected to be reduced by more than 40%.

[0071] The above tests were conducted using discarded carbon black. However, because the effects are due to carbon black, the same effects as those of discarded carbon black can be expected from new carbon black, carbonized waste rubber, carbonized waste tire, or carbonized water-containing waste tire, which contain carbon black. [Explanation of symbols]

[0072] 1. Porous asphalt pavement (surface layer) 2 Dense-grained asphalt pavement (surface layer) 3 Impermeable layer 4 Rainfall 5a Rainwater infiltration flow 5b Rainwater flow on pavement surface 10 Porous asphalt paving mixture 20 Porous asphalt paving mixture 30 Aggregate 40a Polymer modified asphalt H type 40b Polymer modified asphalt H type + CB (carbon black)

Claims

1. Polymer modified asphalt H type; A porous asphalt pavement mixture characterized by being composed of waste carbon black having a composition of 88.9 to 96.1% by weight of carbon black, 0.3 to 6% by weight of moisture, and 0.1 to 2.1% by weight of impurities such as dust and fine particles, crushed stone, crushed sand, and stone powder.

2. The waste carbon black has a composition of 88.9 to 96.1% by weight of carbon black, 0.3 to 6% by weight of moisture, and 0.1 to 2.1% by weight of impurities such as dust and fine particles. The amount of the waste carbon black added to the porous asphalt pavement mixture is 0.01 to 10% by weight. Porous asphalt pavement mixture according to claim 1.

Citation Information

Patent Citations

  • Asphalt composition

    JP2000265069A

  • Asphalt mixture

    JP2004292796A

  • Synthetic hollow spheres

    JP2005536333A

  • Recycled aggregate manufacturing method and recycled porous asphalt mixture manufacturing method

    JP2008208606A

  • Method of manufacturing asphalt pavement mixture

    JP2009068218A