Film-like adhesive and method for manufacturing the same, dicing-die bonding integrated film, and semiconductor device and method for manufacturing the same

A film-like adhesive with a specific epoxy-to-hydroxyl group ratio and controlled molecular weight and glass transition temperature addresses adhesion and separability issues in semiconductor manufacturing, enhancing yield and efficiency.

JP7948305B2Active Publication Date: 2026-11-11RESONAC CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024501389
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-02-16
Filing Date
2023-02-14
Publication Date
2026-11-11
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing is maintaining adhesion of film-like adhesives during high-temperature processing and ensuring separability during cooled expansion, which affects yield and production efficiency.

Method used

A film-like adhesive composed of epoxy resin, phenolic resin, elastomer, and inorganic filler, with a specific ratio of epoxy groups to hydroxyl groups, and controlled molecular weight and glass transition temperature, enhances adhesion and separability.

Benefits of technology

The adhesive maintains sufficient adhesion during high-temperature processing and exhibits excellent detachability by cooling and expanding, improving yield and production efficiency in semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948305000002
    Figure 0007948305000002
  • Figure 0007948305000003
    Figure 0007948305000003
  • Figure 0007948305000004
    Figure 0007948305000004
Patent Text Reader

Abstract

The present invention discloses a film-like adhesive. The film-like adhesive contains an epoxy resin, a phenolic resin, an elastomer and an inorganic filler. The ratio of the epoxy groups in the epoxy resin to the hydroxyl groups in the phenolic resin is 1.2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a film-shaped adhesive and a method for producing the same, a dicing die-bonding integrated film, as well as a semiconductor device and a method for producing the same.

Background Art

[0002] In the semiconductor field represented by data storage media, integrated circuits (ICs) and the like, in recent years, along with higher functionality, semiconductor packages have been increasing in density and integration. Along with this, thinning of semiconductor wafers is progressing, and defects such as wafer cracking during processing are more likely to occur, which may lead to a problem of reduced yield. Therefore, as the thickness of semiconductor wafers decreases (for example, 50 μm or less), the transition from conventional physical grinding methods to new processing methods is advancing.

[0003] As one of the new processing methods, a method has been recently proposed in which a laser beam is irradiated to the inside of a semiconductor wafer on a planned cutting line to form a modified region, and then the semiconductor wafer is cut by expanding the outer peripheral portion (for example, Patent Documents 1 and 2). This method is called stealth dicing. With the development of new processing methods, it is necessary to develop semiconductor materials that can be adapted thereto. As such a semiconductor material, a dicing die-bonding integrated film having both the performances of a dicing film and a die-bonding film has been reported (for example, Patent Documents 3 and 4).

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Patent Document 2

Patent Document 3

Patent Document 4

[0005] Incidentally, in the manufacturing process of semiconductor devices, semiconductor elements and support members are bonded together via an adhesive layer (adhesive strip) made of a film-like adhesive. In the post-bonding process, the adhesive layer may be exposed to even higher temperatures, and it is required that the adhesive layer be able to maintain its adhesion even during high-temperature treatment (for example, 150°C for 6 hours or more).

[0006] Therefore, the main objective of this disclosure is to provide a film-like adhesive and a method for manufacturing the same that can maintain sufficient adhesiveness even during high-temperature processing. [Means for solving the problem]

[0007] Through diligent research, the inventors discovered that in a film-like adhesive containing epoxy resin, phenolic resin, elastomer, and inorganic filler, sufficient adhesiveness can be maintained even during high-temperature treatment by adjusting the ratio of epoxy groups of the epoxy resin to the hydroxyl groups of the phenolic resin within a specific range, thus completing the present invention.

[0008] One aspect of this disclosure relates to a film-like adhesive. The film-like adhesive contains an epoxy resin, a phenolic resin, an elastomer, and an inorganic filler. The ratio of epoxy groups of the epoxy resin to hydroxyl groups of the phenolic resin is 1.2 or more. This ratio of 1.2 or more makes it possible to maintain sufficient adhesion even during high-temperature processing.

[0009] The elastomer may include an elastomer that satisfies the following conditions (i) and (ii). In the manufacturing process of semiconductor devices, when a modified region is formed and separated by stealth dicing, expansion under cooling conditions (hereinafter sometimes referred to as "cooled expansion") may be performed. However, when a conventional dicing-die bonding integrated film is applied to cooled expansion, unseparation may occur in the adhesive layer made of film-like adhesive. If the adhesive layer is unseparated, it becomes a problem that the yield decreases and the production time efficiency for sorting unseparated products decreases. By including an elastomer that satisfies conditions (i) and (ii), the separability of the film-like adhesive by cooled expansion tends to improve. Condition (i): The glass transition temperature is 10°C or higher. Condition (ii): The weight-average molecular weight is 1 million or less.

[0010] The total content of epoxy resin and phenolic resin may be 5 to 25% by mass, based on the total amount of the film-like adhesive.

[0011] The average particle size of the inorganic filler may be 400 nm or less. The inorganic filler content may be 18 to 40% by mass, based on the total amount of the film-like adhesive.

[0012] The thickness of the film-like adhesive may be 25 μm or less.

[0013] The film-like adhesive may be used in the manufacturing process of a semiconductor device comprising multiple semiconductor elements stacked on top of each other. In this case, the semiconductor device may be a stacked MCP (Multi-Chip Package) in which semiconductor elements (semiconductor chips) are stacked in multiple layers, or it may be a three-dimensional NAND memory.

[0014] Another aspect of this disclosure relates to a method for producing a film-like adhesive. The method for producing the film-like adhesive comprises the steps of applying a varnish of an adhesive composition containing an epoxy resin, a phenolic resin, an elastomer, an inorganic filler, and a solvent to a support film, and removing the solvent from the applied varnish by heat drying to obtain a film-like adhesive. The ratio of epoxy groups of the epoxy resin to hydroxyl groups of the phenolic resin is 1.2 or more.

[0015] Another aspect of this disclosure relates to a dicing-die bonding integrated film. This dicing-die bonding integrated film comprises, in this order, a substrate layer, an adhesive layer, and an adhesive layer consisting of the above-mentioned film-like adhesive.

[0016] Another aspect of this disclosure relates to a semiconductor device. The semiconductor device comprises a semiconductor element, a support member on which the semiconductor element is mounted, and an adhesive member provided between the semiconductor element and the support member for bonding the semiconductor element and the support member. The adhesive member is a cured product of the above-mentioned film-like adhesive. The semiconductor device may further comprise other semiconductor elements laminated on the semiconductor element.

[0017] Another aspect of this disclosure relates to a method for manufacturing a semiconductor device. One embodiment of the method for manufacturing the semiconductor device comprises the step of interposing the above-mentioned film-like adhesive between a semiconductor element and a support member, or between a first semiconductor element and a second semiconductor element, to bond the semiconductor element and the support member, or the first semiconductor element and the second semiconductor element.

[0018] Another aspect of the method for manufacturing a semiconductor device includes a step of attaching the adhesive layer of the dicing-die bonding integrated film to a semiconductor wafer, a step of dicing the semiconductor wafer to which the adhesive layer is attached, a step of producing a plurality of singulated semiconductor elements with adhesive pieces by expanding the base material layer under cooling conditions, a step of picking up the semiconductor elements with adhesive pieces from the pressure-sensitive adhesive layer, and a step of bonding the picked-up semiconductor elements with adhesive pieces to a support member via the adhesive pieces. In this case, the method for manufacturing a semiconductor device may further include a step of bonding another semiconductor element with an adhesive piece to the surface of the semiconductor element bonded to the support member via the adhesive piece.

[0019] The present disclosure provides [1] to

[15] . [1] An adhesive film comprising an epoxy resin, a phenol resin, an elastomer, and an inorganic filler, wherein the ratio of the epoxy groups of the epoxy resin to the hydroxyl groups of the phenol resin is 1.2 or more, the adhesive film. [2] The adhesive film according to [1], wherein the elastomer comprises an elastomer that satisfies the following condition (i) and the following condition (ii). Condition (i): The glass transition temperature is 10°C or higher. Condition (ii): The weight average molecular weight is 1,000,000 or less. [3] The adhesive film according to [1] or [2], wherein the total content of the epoxy resin and the phenol resin is 5 to 25% by mass based on the total amount of the adhesive film. [4] The adhesive film according to any one of [1] to [3], wherein the average particle diameter of the inorganic filler is 400 nm or less. [5] The adhesive film according to any one of [1] to [4], wherein the content of the inorganic filler is 18 to 40% by mass based on the total amount of the adhesive film. [6] The adhesive film according to any one of [1] to [5], wherein the thickness is 25 μm or less. ​​​​The film adhesive according to any one of [1] to [5]. [7] Used in a manufacturing process of a semiconductor device formed by stacking a plurality of semiconductor elements, The film adhesive according to any one of [1] to [6]. [8] The semiconductor device is a three-dimensional NAND memory, The film adhesive according to [7]. [9] A step of applying a varnish of an adhesive composition containing an epoxy resin, a phenol resin, an elastomer, an inorganic filler, and a solvent onto a support film, A step of removing the solvent from the applied varnish by heating and drying to obtain a film adhesive, comprising, The ratio of the epoxy groups of the epoxy resin to the hydroxyl groups of the phenol resin is 1.2 or more, A method for producing a film adhesive.

[10] Comprising a base material layer, a pressure-sensitive adhesive layer, and an adhesive layer composed of the film adhesive according to any one of [1] to [6] in this order, A dicing die-bonding integrated film.

[11] A semiconductor element, A support member on which the semiconductor element is mounted, An adhesive member provided between the semiconductor element and the support member, for bonding the semiconductor element and the support member, comprising, The adhesive member is a cured product of the film adhesive according to any one of [1] to [6], A semiconductor device.

[12] Further comprising another semiconductor element stacked on the semiconductor element, The semiconductor device according to

[11] .

[13] Comprising a step of interposing the film adhesive according to any one of [1] to [6] between a semiconductor element and a support member, or between a first semiconductor element and a second semiconductor element, and bonding the semiconductor element and the support member, or the first semiconductor element and the second semiconductor element, A method for manufacturing a semiconductor device. The process of attaching the adhesive layer of the dicing-die bonding integrated film described in

[14]

[10] to a semiconductor wafer, A step of dicing the semiconductor wafer to which the adhesive layer has been attached, A step of manufacturing a plurality of individualized semiconductor elements with adhesive pieces attached by expanding the substrate layer under cooling conditions, A step of picking up the adhesive-attached semiconductor element from the adhesive layer, A step of bonding the picked-up semiconductor element with adhesive piece attached to a support member via the adhesive piece, Equipped with, A method for manufacturing a semiconductor device.

[15] Further comprising the step of bonding another semiconductor element with adhesive piece to the surface of the semiconductor element bonded to the support member via the adhesive piece, A method for manufacturing a semiconductor device as described in

[14] . [Effects of the Invention]

[0020] This disclosure provides a film-like adhesive capable of maintaining sufficient adhesion even during high-temperature processing, and a method for manufacturing the same. Several forms of the film-like adhesive also exhibit excellent detachability by cooling and expanding. Furthermore, this disclosure provides a dicing-die bonding integrated film using such a film-like adhesive, as well as a semiconductor device and a method for manufacturing the same. Moreover, this disclosure provides a method for manufacturing a semiconductor device using such a dicing-die bonding integrated film. [Brief explanation of the drawing]

[0021] [Figure 1] Figure 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive. [Figure 2] Figure 2 is a schematic perspective view showing a sample fixed to a jig during a fracture test. [Figure 3] Figure 3 is a schematic cross-sectional view showing the state in which a load is applied to the sample using a pressing jig during a fracture test. [Figure 4] Figure 4 is a schematic graph showing an example of the results of a fracture test. [Figure 5] Figure 5 is a schematic cross-sectional view showing one embodiment of a dicing-die bonding integrated film. [Figure 6] Figure 6 is a schematic cross-sectional view showing one embodiment of a semiconductor device. [Figure 7] Figure 7 is a schematic cross-sectional view showing another embodiment of the semiconductor device. [Figure 8] Figure 8 is a schematic cross-sectional view showing another embodiment of the semiconductor device. [Modes for carrying out the invention]

[0022] Embodiments of the present disclosure will be described below with reference to the drawings as appropriate. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including steps, etc.) are not essential unless otherwise specified. The sizes of the components in each figure are conceptual, and the relative relationships of the sizes of the components are not limited to those shown in each figure.

[0023] The same applies to numerical values ​​and their ranges in this disclosure, and this disclosure is not limited. Numerical ranges indicated using "~" in this specification indicate a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In numerical ranges described in steps in this specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in steps. Also, in numerical ranges described in this specification, the upper or lower limit of that numerical range may be replaced with the values ​​shown in the examples.

[0024] In this specification, (meth)acrylate means acrylate or the corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl group and (meth)acrylic copolymer.

[0025] Unless otherwise specified, each component and material exemplified herein may be used alone or in combination of two or more.

[0026] [Film-type adhesive] The film-type adhesive contains epoxy resin (hereinafter sometimes referred to as "component (A)"), phenolic resin (hereinafter sometimes referred to as "component (B)"), elastomer (hereinafter sometimes referred to as "component (C)"), and inorganic filler (hereinafter sometimes referred to as "component (D)"). In addition to components (A), (B), (C), and (D), the film-type adhesive may further contain a coupling agent (hereinafter sometimes referred to as "component (E)"), a curing accelerator (hereinafter sometimes referred to as "component (F)"), and other components.

[0027] A film-like adhesive can be obtained by forming an adhesive composition containing components (A), (B), (C), and (D), as well as other components added as needed (components (E), (F), and other components, etc.), into a film. The film-like adhesive (adhesive composition) may undergo a semi-cured state (stage B) and then become fully cured (stage C) after a curing treatment.

[0028] (A) Component: Epoxy resin Component (A) can be used without particular limitations as long as it has an epoxy group in its molecule. Examples of component (A) include bisphenol A type epoxy resin; bisphenol F type epoxy resin; bisphenol S type epoxy resin; phenol novolac type epoxy resin; cresol novolac type epoxy resin; bisphenol A novolac type epoxy resin; bisphenol F novolac type epoxy resin; stilbene type epoxy resin; triazine skeleton-containing epoxy resin; fluorene skeleton-containing epoxy resin; triphenolmethane type epoxy resin; biphenyl type epoxy resin; xylylene type epoxy resin; biphenyl aralkyl type epoxy resin; naphthalene type epoxy resin; and diglycidyl ether compounds of polycyclic aromatics such as polyfunctional phenols and anthracenes. These may be used individually or in combination of two or more. Among these, component (A) may include cresol novolac type epoxy resin from the viewpoint of film tackiness, flexibility, etc.

[0029] The epoxy equivalent of component (A) is not particularly limited, but may be 90-300 g / eq, 100-290 g / eq, or 110-280 g / eq. When the epoxy equivalent of component (A) is in this range, better reactivity and fluidity tend to be obtained.

[0030] (B) Component: Phenolic resin Component (B) may be a polycondensation product of phenols such as phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene, and aldehydes such as formaldehyde. Polycondensation is usually carried out in the presence of a catalyst such as an acid or a base. Phenolic resins obtained when an acid catalyst is used are in particular called novolac-type phenolic resins. Examples of novolac-type phenolic resins include phenol / formaldehyde novolac resin, cresol / formaldehyde novolac resin, xylenol / formaldehyde novolac resin, resorcinol / formaldehyde novolac resin, and phenol-naphthol / formaldehyde novolac resin. Furthermore, examples of phenolic resins include phenol aralkyl resins, naphthol aralkyl resins, biphenyl aralkyl type phenolic resins, and phenyl aralkyl type phenolic resins, which are synthesized from phenols and / or naphthols such as allylated bisphenol A, allylated bisphenol F, allylated naphthalenediol, phenol novolac, and phenol, and dimethoxyp-xylene or bis(methoxymethyl)biphenyl.

[0031] The hydroxyl group equivalent of component (B) may be 80-250 g / eq, 90-200 g / eq, or 100-180 g / eq. When the hydroxyl group equivalent of component (B) is 80 g / eq or higher, the storage modulus tends to improve further, and when it is 250 g / eq or lower, it is possible to prevent problems caused by foaming, outgassing, etc.

[0032] The softening point of component (B) may be 50-140°C, 55-115°C, or 60-100°C. The softening point refers to the value measured by the ring-and-ball method in accordance with JIS K7234.

[0033] The ratio (equivalent ratio) of epoxy groups of component (A) to hydroxyl groups of component (B) (number of epoxy groups of component (A) / number of hydroxyl groups of component (B)) is 1.2 or greater. This ratio (equivalent ratio) of 1.2 or greater allows the film adhesive to maintain sufficient adhesion even during high-temperature processing. This ratio (equivalent ratio) may be 1.3 or greater, 1.4 or greater, 1.5 or greater, 1.6 or greater, 1.8 or greater, or 2.0 or greater. The upper limit of this ratio (equivalent ratio) may be, for example, 5.0 or less, 4.5 or less, 4.0 or less, 3.8 or less, or 3.6 or less.

[0034] When using one component (A) and one component (B), the ratio of epoxy groups of component (A) to hydroxyl groups of component (B) can be calculated using the following formula. The ratio = [Amount of component (A) / Epoxy equivalent of component (A)] / [Amount of component (B) / Hydroxyl equivalent of component (B)]

[0035] When using component (A) of type m (m≧1) and component (B) of type n (n≧1), the ratio of epoxy groups of component (A) to hydroxyl groups of component (B) can be calculated from the following formula. The ratio = [((A1) amount / (A1) epoxy equivalent) + ... + ((Am) amount / (Am) epoxy equivalent)] / [((B1) amount / (B1) hydroxyl equivalent) + ... + ((Bn) amount / (Bn) hydroxyl equivalent)] Here, (A1), ..., (Am) represent m types of (A) components, and (B1), ..., (Bn) represent n types of (B) components.

[0036] The total content of component (A) and component (B) may be 5 to 25% by mass, based on the total amount of the film-like adhesive. When the total content of component (A) and component (B) is 5% by mass or more, based on the total amount of the film-like adhesive, the adhesion retention of the film-like adhesive during high-temperature treatment tends to be further improved. When the total content of component (A) and component (B) is 25% by mass or less, based on the total amount of the film-like adhesive, the handling properties or thin-film coating properties tend to be superior. The total content of component (A) and component (B) may be 8% by mass or more, 10% by mass or more, or 12% by mass or more, and may also be 22% by mass or less, 20% by mass or less, or 18% by mass or less, based on the total amount of the film-like adhesive.

[0037] (C) Ingredients: Elastomer Examples of component (C) include acrylic resin, polyester resin, polyamide resin, polyimide resin, silicone resin, butadiene resin; and modified versions of these resins. These may be used individually or in combination of two or more. Among these, component (C) may be an acrylic resin (acrylic rubber) having constituent units derived from (meth)acrylic acid ester as its main component, as it has fewer ionic impurities, superior heat resistance, easier connection reliability for semiconductor devices, and superior fluidity. The content of constituent units derived from (meth)acrylic acid ester in component (C) may be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total amount of constituent units. The acrylic resin (acrylic rubber) may contain constituent units derived from (meth)acrylic acid ester having crosslinkable functional groups such as epoxy groups, alcoholic or phenolic hydroxyl groups, or carboxyl groups.

[0038] Among these, component (C) may include an elastomer that satisfies conditions (i) and (ii) (hereinafter sometimes referred to as "component (C1)"). Condition (i): The glass transition temperature is 10°C or higher. Condition (ii): The weight-average molecular weight is 1 million or less.

[0039] Regarding condition (i), the glass transition temperature (Tg) of component (C1) may be 10°C or higher, and may be 12°C or higher, 15°C or higher, 18°C ​​or higher, or 20°C or higher. When the Tg of component (C1) is 10°C or higher, it is possible to further improve the adhesive strength of the film-like adhesive and, furthermore, it tends to prevent the film-like adhesive from becoming too flexible. Therefore, by using such a (C1) component, the cleavage of the film-like adhesive in the cooled expand can be further improved. There is no particular upper limit to the Tg of component (C1), but for example, it may be 55°C or lower, 50°C or lower, 45°C or lower, 40°C or lower, 35°C or lower, 30°C or lower, or 25°C or lower. When the Tg of component (C1) is 55°C or lower, it tends to suppress the decrease in flexibility of the film-like adhesive. As a result, it tends to be easier to adequately fill voids when attaching the film-like adhesive (adhesive layer) to the semiconductor wafer. Furthermore, it becomes possible to prevent chipping during dicing due to reduced adhesion to the semiconductor wafer. Here, the glass transition temperature (Tg) refers to the value measured using a DSC (Differential Scanning Calorimeter) (for example, Thermo Plus 2 manufactured by Rigaku Corporation). The Tg of component (C1) can be adjusted to a desired range by adjusting the type and content of the constituent units that make up component (if component (C1) is acrylic resin (acrylic rubber), the constituent units are derived from (meth)acrylic acid ester).

[0040] Regarding condition (ii), the weight-average molecular weight (Mw) of component (C1) may be 1 million or less, 900,000 or less, or 800,000 or less. The lower limit of Mw of component (C1) is not particularly limited, but may be, for example, 10,000 or more, 50,000 or more, 100,000 or more, 300,000 or more, or 500,000 or more. When the Mw of component (C1) is within this range, the fragmentation properties, film formation properties, film strength, flexibility, tackiness, etc. in the cooling and expanding of the film can be appropriately controlled, and the reflowability and embedding properties can be improved. Here, Mw refers to the value measured by gel permeation chromatography (GPC) and converted using a calibration curve with standard polystyrene.

[0041] The content of component (C1) may be 50-100% by mass, 70-100% by mass, 90-100% by mass, or 95-100% by mass, based on the total amount of component (C). The content of component (C1) may also be 100% by mass, based on the total amount of component (C).

[0042] Component (C) may include, in addition to component (C1), an elastomer that does not meet the requirements of component (C1) (hereinafter sometimes referred to as "component (C2)").

[0043] The content of component (C2) may be 0-50% by mass, 0-30% by mass, 0-10% by mass, or 0-5% by mass, based on the total amount of component (C). The content of component (C2) may also be 0% by mass, based on the total amount of component (C). In other words, component (C) may not contain component (C2).

[0044] The content of component (C) may be 40% by mass or more, 45% by mass or more, or 50% by mass or more, based on the total amount of the film-like adhesive. When the content of component (C) is within this range, the thin-film coating properties tend to be superior. The content of component (C) may be 80% by mass or less, 75% by mass or less, or 70% by mass or less, based on the total amount of the film-like adhesive. When the content of component (C) is within this range, the content of components (A) and (B) can be sufficiently ensured, and compatibility with other properties tends to be maintained.

[0045] (D) Ingredients: Inorganic filler Examples of inorganic fillers as component (D) include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, boron nitride, silica, etc. These may be used individually or in combination of two or more. Among these, silica may be used as the inorganic filler from the viewpoint of adjusting the melt viscosity. The shape of the inorganic filler is not particularly limited, but it may be spherical.

[0046] The average particle size of component (D) may be 400 nm or less, and may also be 350 nm or less, 300 nm or less, 250 nm or less, or 200 nm or less, from the viewpoint of thin film coating properties and adhesion. The average particle size of component (D) may be, for example, 10 nm or more, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more. When the average particle size of component (D) is 400 nm or less, it tends to have excellent thin film coating properties. When the average particle size of component (D) is 10 nm or more, it tends to have excellent adhesion properties. Here, the average particle size of component (D) can be determined by the following method. First, component (D) is dispersed in a solvent to prepare a dispersion. Next, the particle size distribution is obtained by applying the dynamic light scattering method to the prepared dispersion. Then, the average particle size of component (D) can be determined based on the obtained particle size distribution. The average particle size of component (D) can also be determined from a film-like adhesive containing component (D). In this case, a dispersion is prepared by dispersing the residue obtained by heating the film-like adhesive to decompose the resin components in a solvent. Next, the particle size distribution is obtained by applying dynamic light scattering to the prepared dispersion. Then, the average particle size of component (D) can be determined based on the obtained particle size distribution.

[0047] Component (D) may consist of, for example, one or more inorganic fillers with an average particle size of 400 nm or less, such as one or more inorganic fillers with an average particle size of 10-400 nm, 30-400 nm, 50-400 nm, 100-400 nm, 150-400 nm, 10-350 nm, 30-350 nm, 50-350 nm, 100-350 nm, 150-350 nm, 10-300 nm, and flat It may also be made from inorganic filler foundation with uniform particle size of 30-300 nm, average particle size of 50-300 nm, average particle size of 100-300 nm, average particle size of 150-300 nm, average particle size of 10-250 nm, average particle size of 30-250 nm, average particle size of 50-250 nm, average particle size of 100-250 nm, average particle size of 150-250 nm, average particle size of 10-200 nm, or average particle size of 150-200 nm.

[0048] The content of component (D) may be 18 to 40% by mass, based on the total amount of the film-like adhesive. When the content of component (D) is 18% by mass or more, there is a tendency for excellent separation by cooling and expanding. When the content of component (D) is 18% by mass or more, there is a tendency for adhesive strength to improve when it is 40% by mass or less. The content of component (D) may be 20% by mass or more, 22% by mass or more, or 24% by mass or more, and may be 38% by mass or less, 35% by mass or less, 32% by mass or less, or 30% by mass or less, based on the total amount of the film-like adhesive.

[0049] (E) Component: Coupling agent Component (E) may be a silane coupling agent. Examples of silane coupling agents include γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, 3-phenylaminopropyltrimethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane.

[0050] (F) Ingredient: Curing accelerator Examples of component (F) include imidazoles and their derivatives, organophosphorus compounds, secondary amines, tertiary amines, and quaternary ammonium salts. These may be used individually or in combination of two or more. Among these, from the viewpoint of reactivity, component (F) may be imidazoles and their derivatives.

[0051] Examples of imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole. These may be used individually or in combination of two or more.

[0052] The film-like adhesive may further contain other components. Examples of other components include pigments, ion capture agents, antioxidants, and so on.

[0053] The total content of component (E), component (F), and other components may be 0.01% by mass or more, 0.1% by mass or more, or 0.3% by mass or more, based on the total amount of the film adhesive, and may be 20% by mass or less, 10% by mass or less, 5% by mass or less, 3% by mass or less, or 1% by mass or less.

[0054] Figure 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive. The film-like adhesive 1 shown in Figure 1 is formed by molding an adhesive composition into a film. The film-like adhesive 1 is usually in a semi-cured (B stage) state and may become fully cured (C stage) after curing treatment. The film-like adhesive 1 can be formed by applying the adhesive composition to a support film. In forming the film-like adhesive 1, a varnish (adhesive varnish) of the adhesive composition may be used. The adhesive varnish can be prepared, for example, by mixing or kneading components (A), (B), (C), and (D), as well as components added as needed, in a solvent. In one embodiment, the film-like adhesive 1 can be manufactured by a method comprising the steps of applying a varnish (adhesive varnish) of an adhesive composition containing components (A), (B), (C), (D), and a solvent to a support film, and removing the solvent from the applied varnish (adhesive varnish) by heat drying. At this time, the ratio of epoxy groups of the epoxy resin to hydroxyl groups of the phenolic resin is 1.2 or more. The step of removing the solvent from the applied adhesive varnish by heat drying may be a step of removing at least a portion of the solvent from the applied adhesive varnish by heat drying. That is, a small amount of solvent may remain in the film-like adhesive 1 obtained after the step of removing the solvent from the applied adhesive varnish by heat drying.

[0055] The support film is not particularly limited as long as it can withstand the above-mentioned heat drying, but may be, for example, polyester film, polypropylene film, polyethylene terephthalate film, polyimide film, polyetherimide film, polyethylene naphthalate film, polymethylpentene film, etc. The support film may be a multilayer film made by combining two or more types, and its surface may be treated with a release agent such as silicone or silica. The thickness of the support film may be, for example, 10 to 200 μm or 20 to 170 μm.

[0056] Mixing or kneading can be carried out using conventional agitators, mixers, three-roll mills, ball mills, and other dispersers, in appropriate combinations.

[0057] The solvent used in the preparation of the adhesive varnish is not limited as long as it can uniformly dissolve, knead, or disperse each component, and conventionally known solvents can be used. Examples of such solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, as well as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, toluene, and xylene. From the viewpoint of drying speed and cost, the solvent may be methyl ethyl ketone or cyclohexanone.

[0058] Known methods can be used to apply the adhesive varnish to the support film, such as the knife coating method, roll coating method, spray coating method, gravure coating method, bar coating method, and curtain coating method. Heat drying is not particularly limited as long as the conditions allow the solvent used to evaporate sufficiently, but it can be carried out in the range of 50 to 150°C for 1 to 30 minutes. Heat drying can be carried out in stages with different heating temperatures and different heating times.

[0059] The thickness of the film-like adhesive may be 25 μm or less, and may be 22 μm or less, 20 μm or less, 18 μm or less, 15 μm or less, 12 μm or less, or 10 μm or less. The lower limit of the thickness of the film-like adhesive is not particularly limited, but may be, for example, 1 μm or more.

[0060] A film-like adhesive prepared on a support film may have a cover film on the side opposite to the support film to prevent damage or contamination. Examples of cover films include polyethylene film, polypropylene film, and surface release agent treated film. The thickness of the cover film may be, for example, 15 to 200 μm or 30 to 170 μm.

[0061] Because the film-like adhesive can be made into a thin film, it can be suitably used in the manufacturing process of semiconductor devices formed by stacking multiple semiconductor elements. In this case, the semiconductor device may be a stacked MCP or a three-dimensional NAND memory.

[0062] The film-like adhesive 1 may be a film-like adhesive in which the fracture coefficient m is 70 or less in a fracture evaluation method that utilizes the results of a fracture test performed under the following conditions (a method for evaluating the fracture properties of a film-like adhesive under low temperature conditions (e.g., in the range of -15°C to 0°C) in which cooling expansion is performed). <Condition> Sample width: 5 mm Sample length: 23 mm Relative speed between the pressing jig and the sample: 10 mm / min

[0063] The fracture test is described below. The fracture test is classified as a flexural strength test and includes the step of pressing the central part of the sample until it breaks while both ends of the sample are fixed. As shown in Figure 2, the sample S is subjected to the fracture test while fixed between a pair of sample fixing jigs 20. The pair of sample fixing jigs 20 are made of, for example, cardboard with sufficient strength and each has a rectangular opening 20a in the center. A load is applied to the central part of the fixed sample S using a pressing jig 21 (see Figure 3).

[0064] The sample S can be any piece cut from the film-like adhesive to be evaluated, and it is not necessary to prepare the sample by laminating multiple adhesive pieces cut from the film-like adhesive. In other words, the thickness of the sample S may be the same as the thickness of the film-like adhesive. The width of the sample S (Ws in Figure 2) may be, for example, 1 to 30 mm, or 3 to 8 mm. It should be set to an appropriate width depending on the condition of the measuring device. The length of the sample S (Ls in Figure 2) may be, for example, 5 to 50 mm, or 10 to 30 mm or 6 to 9 mm. The length of the sample S depends on the size of the opening 20a of the sample fixing jig 20. Note that the shape of the sample fixing jig 20 and the size of the sample S may be other than those described above, as long as the cleavage test can be performed.

[0065] The push-in jig 21 consists of a cylindrical member having a conical tip portion 21a. The diameter of the push-in jig 21 (R in Figure 3) is, for example, 3 to 15 mm, or it may be 5 to 10 mm. The angle of the tip portion 21a (θ in Figure 3) is, for example, 40 to 120°, or it may be 60 to 100°.

[0066] The cleavage test is performed in a constant temperature chamber set to a predetermined temperature. The constant temperature chamber should be set to a constant temperature in the range of -15°C to 0°C (the temperature of the expected cooled expander). For example, the TLF-R3-FW-PL-S manufactured by ITEC Corporation can be used as the constant temperature chamber. An autograph (for example, AZT-CA01 manufactured by A&D Corporation, load cell 50N, compression mode) is used to obtain the cleavage work W, cleavage strength P, and cleavage elongation L.

[0067] The relative speed between the indentation jig 21 and the sample S is, for example, 1 to 100 mm / min, or 5 to 20 mm / min. If this relative speed is too fast, sufficient data on the fracture process tends not to be obtained, and if it is too slow, the stress tends to relax and fracture does not occur easily. The indentation distance of the indentation jig 21 is, for example, 1 to 50 mm, or 5 to 30 mm. If the indentation distance is too short, fracture tends not to occur. It is preferable to prepare multiple samples of the film-like adhesive to be evaluated and perform fracture tests multiple times to confirm the stability of the test results.

[0068] Figure 4 is a graph showing an example of the results of a fracture test. As shown in Figure 4, the work of fracture W is the area enclosed when a graph is created with the load on the vertical axis and the amount of indentation until the sample S fractures on the horizontal axis. The fracture strength P is the load at which the sample S fractures. The elongation at fracture L is the amount of elongation of the sample S at the time of fracture. The elongation at fracture L can be calculated using trigonometric functions from the indentation distance at the time of fracture of the sample S and the width of the opening 20a of the sample fixing jig 20.

[0069] From the values ​​of the cutting work W (N·mm), cutting strength P (N), and cutting elongation L (mm) obtained by the cleavage test, the cleavage coefficient m (dimensionless) and cleavage resistance R (N / mm) can be determined from equations (1) and (2). 2 ) m = W / [1000 × (P × L)] (1) R = P / A (2)

[0070] According to our research, when a cleavage test is conducted under the following conditions, film-like adhesives with a cleavage coefficient m of 70 or less tend to exhibit superior cleavage performance when actually subjected to cooling and expanding in stealth dicing. <Condition> Sample width: 5 mm Sample length: 23 mm Relative speed between the pressing jig and the sample: 10 mm / min

[0071] [Dicing and die bonding integrated film] Figure 5 is a schematic cross-sectional view showing one embodiment of a dicing-die bonding integrated film. The dicing-die bonding integrated film 10 shown in Figure 5 comprises, in this order, a base layer 2, an adhesive layer 3, and an adhesive layer 1A consisting of a film-like adhesive 1 (adhesive composition). The base layer 2 and the adhesive layer 3 may be dicing films 4. Using such a dicing-die bonding integrated film 10 allows for a single lamination process to the semiconductor wafer, thereby improving work efficiency. The dicing-die bonding integrated film may be in the form of a film, sheet, tape, or the like.

[0072] The dicing film 4 comprises a base layer 2 and an adhesive layer 3 provided on the base layer 2.

[0073] Examples of the base layer 2 include plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, and polyimide film. These base layer 2 may be subjected to surface treatments such as primer application, UV treatment, corona discharge treatment, polishing treatment, and etching treatment as needed.

[0074] The adhesive layer 3 is a layer made of adhesive. The adhesive is not particularly limited as long as it has sufficient adhesive strength to prevent the semiconductor elements from scattering during dicing and low enough adhesive strength to avoid damaging the semiconductor elements during the subsequent semiconductor element pickup process. Adhesives conventionally known in the field of dicing films can be used. The adhesive may be either radiation-curable or non-radiation-curable. A radiation-curable adhesive is an adhesive that has the property of decreasing in adhesiveness upon irradiation with radiation (e.g., ultraviolet light). A radiation-curable adhesive may be, for example, an ultraviolet-curable adhesive. On the other hand, a non-radiation-curable adhesive is an adhesive that exhibits a certain level of adhesiveness with short-term pressure.

[0075] The thickness of the dicing film 4 (base layer 2 and adhesive layer 3) may be 60 to 150 μm or 70 to 130 μm from the viewpoint of economy and ease of handling of the film.

[0076] The dicing-die bonding integrated film 10 can be obtained, for example, by preparing a film-like adhesive 1 and a dicing film 4, and bonding the film-like adhesive 1 and the adhesive layer 3 of the dicing film 4. Alternatively, the dicing-die bonding integrated film 10 can also be obtained, for example, by preparing a dicing film 4 and applying an adhesive composition (adhesive varnish) onto the adhesive layer 3 of the dicing film 4, similar to the method for forming the film-like adhesive 1 described above.

[0077] When bonding the film-like adhesive 1 to the adhesive layer 3 of the dicing film 4, the integrated dicing-die bonding film 10 can be formed by bonding the film-like adhesive 1 to the dicing film 4 under predetermined conditions (for example, at room temperature (25°C) or in a heated state) using a roll laminator, vacuum laminator, etc. Since the integrated dicing-die bonding film 10 can be manufactured continuously and is highly efficient, it may also be formed using a roll laminator in a heated state.

[0078] The film-like adhesive and the dicing / die bonding integrated film may be used in the manufacturing process of semiconductor devices, and may also be used in the manufacturing process of semiconductor devices comprising multiple semiconductor elements stacked on top of each other.

[0079] Film-type adhesives are also suitable for use as adhesives to bond semiconductor elements to support members on which they are mounted.

[0080] Furthermore, film-type adhesives are also suitably used as adhesives for bonding semiconductor elements together in stacked MCPs (for example, three-dimensional NAND memory), which are semiconductor devices formed by stacking multiple semiconductor elements.

[0081] Film-type adhesives can also be used, for example, as protective sheets to protect the back surface of semiconductor elements in flip-chip semiconductor devices, or as sealing sheets to seal the space between the surface of semiconductor elements in flip-chip semiconductor devices and the adherend.

[0082] A semiconductor device manufactured using a film-like adhesive and a dicing / die bonding integrated film will be described in detail below with reference to the drawings. It should be noted that various structures of semiconductor devices have been proposed in recent years, and the applications of the film-like adhesive and dicing / die bonding integrated film of this embodiment are not limited to the semiconductor device with the structure described below.

[0083] [Semiconductor device] Figure 6 is a schematic cross-sectional view showing one embodiment of a semiconductor device. The semiconductor device 100 shown in Figure 6 comprises a semiconductor element 11, a support member 12 on which the semiconductor element 11 is mounted, and an adhesive member 15. The adhesive member 15 is provided between the semiconductor element 11 and the support member 12 and adheres the semiconductor element 11 and the support member 12 together. The adhesive member 15 is a cured product of an adhesive composition (a cured product of a film-like adhesive). The connection terminal (not shown) of the semiconductor element 11 is electrically connected to an external connection terminal (not shown) via a wire 13 and sealed by a sealing material 14.

[0084] Figure 7 is a schematic cross-sectional view showing another embodiment of a semiconductor device. In the semiconductor device 110 shown in Figure 7, the first-stage semiconductor element 11a is bonded to a support member 12 on which terminals 16 are formed by adhesive member 15a (cured product of adhesive composition (cured product of film-like adhesive)), and the second-stage semiconductor element 11b is further bonded to the first-stage semiconductor element 11a by adhesive member 15b (cured product of adhesive composition (cured product of film-like adhesive)). The connection terminals (not shown) of the first-stage semiconductor element 11a and the second-stage semiconductor element 11b are electrically connected to an external connection terminal via wire 13 and sealed by a sealing material 14. The semiconductor device 110 shown in Figure 7 can also be described as the semiconductor device 100 shown in Figure 6, further comprising another semiconductor element (11b) stacked on top of the semiconductor element (11a).

[0085] Figure 8 is a schematic cross-sectional view showing another embodiment of the semiconductor device. The semiconductor device 120 shown in Figure 8 comprises a support member 12 and semiconductor elements 11a, 11b, 11c, and 11d stacked on the support member 12. The four semiconductor elements 11a, 11b, 11c, and 11d are stacked at positions offset from each other in the lateral direction (direction perpendicular to the stacking direction) for connection to connection terminals (not shown) formed on the surface of the support member 12 (see Figure 8). Semiconductor element 11a is bonded to the support member 12 by an adhesive member 15a (cured product of an adhesive composition (cured product of a film-like adhesive)), and adhesive members 15b, 15c, and 15d (cured product of an adhesive composition (cured product of a film-like adhesive)) are also interposed between the three semiconductor elements 11b, 11c, and 11d, respectively. The semiconductor device 120 shown in Figure 8 can also be described as the semiconductor device 100 shown in Figure 6, further comprising other semiconductor devices (11b, 11c, 11d) stacked on top of the semiconductor device (11a).

[0086] Although the semiconductor device (package) has been described in detail above in relation to embodiments of the present disclosure, the present disclosure is not limited to the above embodiments. For example, Figure 8 illustrates a semiconductor device in which four semiconductor elements are stacked, but the number of stacked semiconductor elements is not limited to this. Also, Figure 8 illustrates a semiconductor device in which the semiconductor elements are stacked at positions offset from each other in the lateral direction (direction perpendicular to the stacking direction), but a semiconductor device in which the semiconductor elements are stacked at positions not offset from each other in the lateral direction (direction perpendicular to the stacking direction) may also be used.

[0087] [Manufacturing method for semiconductor devices] The semiconductor device (semiconductor package) shown in Figures 6, 7, and 8 can be obtained by a method comprising the step of interposing the above-mentioned film-like adhesive between a semiconductor element (semiconductor chip) and a support member, or between a semiconductor element (first semiconductor element) and a semiconductor element (second semiconductor element), and bonding the semiconductor element and the support member, or the semiconductor element (first semiconductor element) and the semiconductor element (second semiconductor element). More specifically, the above-mentioned film-like adhesive can be interposed between a semiconductor element and a support member, or between a semiconductor element (first semiconductor element) and a semiconductor element (second semiconductor element), and these can be bonded together by heating and pressing, and then, if necessary, the semiconductor device can be obtained by going through a wire bonding step, a sealing step with a sealing material, a heating and melting step including reflow with solder, etc.

[0088] As a method for interposing a film-like adhesive between a semiconductor element and a support member, or between a semiconductor element (first semiconductor element) and a semiconductor element (second semiconductor element), as described later, a semiconductor element with adhesive attached may be manufactured in advance and then attached to the support member or semiconductor element.

[0089] Next, an embodiment of a method for manufacturing a semiconductor device using the dicing-die bonding integrated film shown in Figure 5 will be described. Note that the method for manufacturing a semiconductor device using the dicing-die bonding integrated film is not limited to the method described below.

[0090] A semiconductor device can be obtained, for example, by a method comprising: a step of attaching the adhesive layer of the above-described dicing-die bonding integrated film to a semiconductor wafer (laminating step); a step of dicing the semiconductor wafer to which the adhesive layer has been attached (dicing step); a step of producing a plurality of individualized semiconductor elements with adhesive pieces (semiconductor chips with adhesive pieces) by expanding the substrate layer under cooling conditions (cooling and expanding step); a step of picking up the semiconductor elements with adhesive pieces from the adhesive layer (picking step); and a step of bonding the picked-up semiconductor elements with adhesive pieces to a support member via adhesive pieces (first bonding step). The method for manufacturing a semiconductor device may further include a step of bonding other semiconductor elements with adhesive pieces to the surface of a semiconductor element bonded to a support member via adhesive pieces (second bonding step).

[0091] The lamination process involves pressing the adhesive layer 1A of the dicing / die bonding integrated film 10 onto the semiconductor wafer and then bonding and holding it in place. This process may be performed while pressing with a pressing means such as a pressure roll. The semiconductor wafer can be exemplified by the same semiconductor wafer as described above.

[0092] Examples of semiconductor wafers include single-crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide.

[0093] The dicing process is the process of dicing a semiconductor wafer. Dicing can be performed, for example, from the circuit side of the semiconductor wafer according to conventional methods. In this process, methods such as half-cutting, which involves making a half-cut incision in the semiconductor wafer, or stealth dicing, which involves forming a modified region with a laser and dividing the wafer, can be employed. Since the adhesive layer of the above-mentioned dicing-die bonding integrated film exhibits excellent divisibility by cooling and expanding, it is preferable to employ stealth dicing. The dicing apparatus used in this process is not particularly limited, and conventionally known apparatuses can be used.

[0094] The cooling and expanding process is a process of expanding a substrate layer under cooling conditions. This allows for the production of multiple individual semiconductor elements with adhesive pieces attached. The expansion conditions under cooling can be set arbitrarily, but for example, the cooling temperature can be -30 to 5°C, the cooling time can be 30 seconds to 5 minutes, the push-up amount can be 5 to 15 mm, and the push-up speed can be 50 to 300 mm / second.

[0095] Examples of semiconductor elements (semiconductor chips) include ICs (integrated circuits). Examples of support members include lead frames such as 42 alloy lead frames and copper lead frames; plastic films such as polyimide resin and epoxy resin; modified plastic films obtained by impregnating and curing a substrate such as glass nonwoven fabric with plastics such as polyimide resin and epoxy resin; and ceramics such as alumina.

[0096] The pickup process is a process of picking up semiconductor elements with adhesive pieces attached to a dicing-die bonding integrated film while separating the semiconductor elements with adhesive pieces from each other in order to detach them. The method for separating the semiconductor elements with adhesive pieces is not particularly limited, and various conventionally known methods can be used. The method for picking up the semiconductor elements with adhesive pieces is not particularly limited, and various conventionally known methods can be used. For example, such a method may involve pushing up individual semiconductor elements with adhesive pieces from the dicing-die bonding integrated film side with a needle, and then picking up the pushed-up semiconductor elements with adhesive pieces using a pickup device.

[0097] In this case, if the adhesive layer is radiation-curable (e.g., ultraviolet light), the pickup process can be performed after irradiating the adhesive layer with radiation. This reduces the adhesive strength of the adhesive layer to the adhesive piece, making it easier to peel off the semiconductor element with the adhesive piece attached. As a result, pickup becomes possible without damaging the semiconductor element with the adhesive piece attached.

[0098] The first bonding step is to bond the picked-up semiconductor element with adhesive piece attached to a support member for mounting the semiconductor element via the adhesive piece. The process may also include, if necessary, a second bonding step (a step in which other semiconductor elements with adhesive pieces attached are bonded to the surface of the semiconductor element bonded to the support member via the adhesive piece). Both bonding steps can be performed by compression. The compression conditions are not particularly limited and can be set as appropriate. For example, the compression conditions may be a temperature of 80-160°C, a load of 5-15N, and a time of 1-10 seconds. The support member may be similar to the one described above.

[0099] A method for manufacturing a semiconductor device may optionally include a step of thermal curing an adhesive piece. By thermal curing the adhesive piece that adheres the semiconductor element and the support member, or the semiconductor element (first semiconductor element) and the semiconductor element (second semiconductor element), a stronger bond can be achieved. When thermal curing is performed, pressure may be applied simultaneously to cure the adhesive. The heating temperature in this step can be appropriately changed depending on the components of the adhesive piece. The heating temperature may be, for example, 60 to 200°C. The temperature or pressure may be changed in stages.

[0100] A method for manufacturing a semiconductor device may, if necessary, include a step (wire bonding step) of electrically connecting the tip of the terminal portion (inner lead) of the support member to the electrode pad on the semiconductor element with a bonding wire. Examples of bonding wires include gold wire, aluminum wire, copper wire, etc. The temperature when performing wire bonding (setting the bonding wire) may be in the range of 80 to 250°C or 80 to 220°C. The heating time may be several seconds to several minutes. When setting the bonding wire, it may be done by combining ultrasonic vibration energy and applied pressure to create a crimping energy while the device is heated within the above temperature range.

[0101] A method for manufacturing a semiconductor device may optionally include a step of sealing a semiconductor element with a sealing material (sealing step). This step is performed to protect the semiconductor element or bonding wire mounted on a support member. This step can be performed by molding a sealing resin (sealing resin) in a mold. The sealing resin may be, for example, an epoxy resin. The heat and pressure during sealing embed the support member and residue, preventing delamination due to air bubbles at the adhesive interface.

[0102] The method for manufacturing a semiconductor device may, if necessary, include a step (post-curing step) to completely cure the sealing resin that is not sufficiently cured in the sealing step. Even if the adhesive piece is not heat-cured in the sealing step, in this step, the adhesive piece can be heat-cured along with the curing of the sealing resin, enabling adhesive fixation. The heating temperature in this step can be appropriately set depending on the type of sealing resin, and may be in the range of 165 to 185°C, for example, and the heating time may be about 0.5 to 8 hours.

[0103] The method for manufacturing a semiconductor device may, if necessary, include a step (heating and melting step) of heating the semiconductor element with adhesive pieces attached to a support member using a reflow oven. In this step, the resin-encapsulated semiconductor device may be surface-mounted on the support member. Examples of surface mounting methods include reflow soldering, in which solder is supplied onto a printed circuit board in advance, then heated and melted with hot air or the like to perform soldering. Examples of heating methods include hot air reflow and infrared reflow. Furthermore, the heating method may involve heating the entire device or heating only a specific area. The heating temperature may be, for example, in the range of 240 to 280°C. [Examples]

[0104] The present disclosure will be described below in detail based on examples, but the present disclosure is not limited to these examples.

[0105] [Preparation of film-like adhesives] (Examples 1-5 and Comparative Examples 1-4) <Preparation of adhesive varnish> Cyclohexanone was added to a mixture of components (A), (B), and (D) in the quantities and amounts (parts by mass) shown in Table 1, and stirred. Then, component (C) was added in the quantities and amounts (parts by mass) shown in Table 1, and stirred. Further, components (E) and (F) were added, and the mixture was stirred until all components were homogeneous to prepare the adhesive varnish. Note that the components shown in Table 1 refer to the following, and the values ​​shown in Table 1 refer to the solid content in parts by mass.

[0106] (A) Component: Epoxy resin (A-1) N-500P-10 (Product name, manufactured by DIC Corporation, o-cresol novolac type epoxy resin, epoxy equivalent: 203g / eq) (A-2) YDF-8170C (Product name, manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., bisphenol F type epoxy resin, epoxy equivalent: 159 g / eq)

[0107] (B) Component: Phenolic resin (B-1) MEH-7800M (product name, manufactured by Meiwa Chemical Co., Ltd., phenol novolac type phenolic resin, hydroxyl group equivalent: 175 g / eq, softening point: 61~90°C) (B-2) GPH-103 (Trade name, manufactured by Nippon Kayaku Co., Ltd., biphenyl aralkyl type phenolic resin, hydroxyl group equivalent: 230 g / eq, softening point: 99~106°C)

[0108] (C) Ingredients: Elastomer (C1-1) Acrylic rubber solution (Cyclohexanone solution of acrylic rubber, measured Tg of acrylic rubber: 20℃, weight-average molecular weight of acrylic rubber: 800,000) (C1-2) Acrylic rubber solution (Cyclohexanone solution of acrylic rubber, measured Tg of acrylic rubber: 12℃, weight-average molecular weight of acrylic rubber: 300,000) (C1-3) Acrylic rubber solution (Cyclohexanone solution of acrylic rubber, measured Tg of acrylic rubber: 12℃, weight-average molecular weight of acrylic rubber: 800,000)

[0109] (D) Ingredients: Inorganic filler (D-1) Silica filler dispersion (manufactured by Admatex Co., Ltd., cyclohexanone dispersion of silica filler, average particle size: 180 nm) (D-2) Silica filler dispersion (manufactured by Admatex Co., Ltd., cyclohexanone dispersion of silica filler, average particle size: 50 nm)

[0110] (E) Component: Coupling agent (E-1) A-189 (Product name, manufactured by Nippon Unicar Co., Ltd., γ-mercaptopropyltrimethoxysilane)

[0111] (F) Ingredient: Curing accelerator (F-1)2PZ-CN (product name, manufactured by Shikoku Chemicals, Inc., 1-cyanoethyl-2-phenylimidazole)

[0112] <Preparation of film-like adhesives> The prepared adhesive varnish was filtered through a 500-mesh filter and degassed under vacuum. A 38 μm thick polyethylene terephthalate (PET) film with a release treatment was prepared as a support film, and the degassed adhesive varnish was applied to the PET film. The applied adhesive varnish was heated and dried in two stages: 90°C for 5 minutes, followed by 130°C for 5 minutes, to obtain the film-like adhesives of Examples 1-5 and Comparative Examples 1-4 in the B-stage state. Two different thicknesses (10 μm and 20 μm) of the film-like adhesive were prepared for each example and comparative example. The thickness of the film-like adhesive was adjusted by the amount of adhesive varnish applied.

[0113] [Evaluation of fragmentation using a cooled expander] Adhesive strips (10 μm thick, 5 mm wide x 100 mm long) were cut from the film-like adhesives (10 μm thick) of Examples 1-5 and Comparative Examples 1-4. The adhesive strips were fixed to a pair of jigs (cardboard), and any portion of the adhesive strip protruding from the jigs was removed. This obtained the samples to be evaluated (5 mm wide x 23 mm long). A fracture test was performed in a constant temperature bath (ITEC Corporation, TLF-R3-FW-PL-S) set to 0°C. Specifically, a fracture test was performed using an Autograph (A&D Corporation, AZT-CA01, load cell 50N) in compression mode, at a speed of 10 mm / min, and with a pressing distance of 5 mm, and the work of fracture W, fracture strength P, and fracture elongation L when the film-like adhesive fractured were determined. Furthermore, the fracture coefficient m and fracture resistance R were calculated from the above equations (1) and (2). The fracture coefficient m and fracture resistance R are the average values ​​obtained by conducting eight or more fracture tests for each example and comparative example. As the fracture coefficient m decreases, the performance of fracture by cooling and expanding tends to improve. Cases with a fracture coefficient m of 70 or less were evaluated as "A" for excellent fracture by cooling and expanding, and cases with a fracture coefficient m greater than 70 were evaluated as "B". The results are shown in Table 1.

[0114] [Evaluation of adhesive retention during high-temperature processing] <Production of integrated dicing and die bonding films> First, dicing films having an adhesive layer consisting of a film-like adhesive (20 μm thick) and an ultraviolet-curing adhesive were prepared for Examples 1-5 and Comparative Examples 1-4. Next, the dicing-die bonding integrated films of Examples 1-5 and Comparative Examples 1-4 were fabricated by bonding the film-like adhesive to the adhesive layer of the dicing film.

[0115] <Preparation of evaluation samples> The adhesive retention during high-temperature processing was evaluated using the dicing-die bonding integrated film prepared as described above. Evaluation samples for evaluating adhesive retention during high-temperature processing were prepared as follows: A semiconductor wafer with a thickness of 75 μm was prepared, and the film-like adhesive side of the dicing-die bonding integrated film was bonded to the semiconductor wafer at a stage temperature of 70°C to prepare a dicing sample. The obtained dicing sample was cut using a fully automatic dicer DFD-6361 (manufactured by DISCO Corporation). Cutting was performed using a step-cut method with two blades, using dicing blades ZH05-SD2000-N1-70-FF and ZH05-SD4000-N1-70-EE (both manufactured by DISCO Corporation). The cutting conditions were: blade rotation speed: 4000 rpm, cutting speed: 50 mm / sec, chip size: 7.5 mm × 7.5 mm. The cutting process involved a first stage of cutting, leaving approximately 200 μm of the semiconductor wafer intact, followed by a second stage of cutting, creating a 20 μm incision in the dicing film. Next, the adhesive layer, made of UV-curable adhesive, was irradiated with ultraviolet light to cure the adhesive layer, and the semiconductor element with adhesive flakes attached was picked up. Subsequently, using a die bonder (Besi, Esec 2100 sD PPP Plus), the picked-up semiconductor element with adhesive flakes attached was pressed onto the stepped portion of a support member (substrate) with a 6 μm step on its surface, via the adhesive flakes, under conditions of 120°C, 0.1 MPa, and 1.0 second, to prepare an evaluation sample.

[0116] <Preparation of evaluation packages and evaluation of adhesion retention during high-temperature processing> At least four support members (substrates) for each dicing / die bonding integrated film were prepared for the evaluation samples created as described above, and these were placed on a hot plate. The hot plate was heated to 150°C, and evaluation samples were obtained with heat histories of 3 hours, 4 hours, 5 hours, and 6 hours. Subsequently, evaluation packages were obtained by sealing each evaluation sample with a molding sealant (Showa Denko Materials Co., Ltd., product name "CEL-9750ZHF10") using a mold molding machine (Apic Yamada Co., Ltd.). The sealing conditions for the sealant were 175°C / 6.8 MPa / 120 seconds. Next, the evaluation packages were observed using an ultrasonic imaging device (SAT) to check for delamination between the support member (substrate) and the adhesive piece. If no delamination was observed after heating at 150°C for 6 hours, it was evaluated as "A" indicating excellent adhesion retention during high-temperature processing, and if delamination was observed after heating at less than 150°C for 6 hours, it was evaluated as "B". The results are shown in Table 1.

[0117] [Table 1]

[0118] As shown in Table 1, the film adhesives of Examples 1 to 5 were superior to the film adhesives of Comparative Examples 1 to 4 in both cooling-induced fragmentation and adhesion retention during high-temperature processing. These results confirm that the film adhesive of this disclosure exhibits excellent fragmentation properties by cooling-induced expansion and can maintain sufficient adhesion even during high-temperature processing. [Explanation of symbols]

[0119] 1...Film-type adhesive, 1A...Adhesive layer, 2...Substrate layer, 3...Adhesive layer, 4...Dicing film, 10...Dicing / die bonding integrated film, 11,11a,11b,11c,11d...Semiconductor element, 12...Support member, 13...Wire, 14...Sealing material, 15,15a,15b,15c,15d...Adhesive member, 16...Terminal, 20...Sample fixing jig, 20a...Opening, 21...Pushing jig, 21a...Tip, 100,110,120...Semiconductor device.

Claims

1. It contains epoxy resin, phenolic resin, elastomer, and inorganic filler. The ratio of epoxy groups of the epoxy resin to hydroxyl groups of the phenolic resin is 1.5 or more. Film-type adhesive.

2. The elastomer includes an elastomer that satisfies the following conditions (i) and (ii): The film-like adhesive according to claim 1. Condition (i): The glass transition temperature is 10°C or higher. Condition (ii): The weight-average molecular weight is 1 million or less.

3. The total content of the epoxy resin and the phenolic resin is 5 to 25% by mass, based on the total amount of the film-like adhesive. The film-like adhesive according to claim 1.

4. The average particle size of the inorganic filler is 400 nm or less. The film-like adhesive according to claim 1.

5. The inorganic filler content is 18 to 40% by mass, based on the total amount of the film-like adhesive. The film-like adhesive according to claim 1.

6. The thickness is 25 μm or less. The film-like adhesive according to claim 1.

7. Used in the manufacturing process of semiconductor devices that are made by stacking multiple semiconductor elements, The film-like adhesive according to claim 1.

8. The semiconductor device is a three-dimensional NAND type memory. The film-like adhesive according to claim 7.

9. A step of applying a varnish of an adhesive composition containing epoxy resin, phenolic resin, elastomer, inorganic filler, and solvent to a support film, A step of removing the solvent from the applied varnish by heat drying to obtain a film-like adhesive, Equipped with, The ratio of epoxy groups of the epoxy resin to hydroxyl groups of the phenolic resin is 1.5 or more. A method for manufacturing film-like adhesives.

10. The device comprises, in this order, a base layer, an adhesive layer, and an adhesive layer made of a film-like adhesive according to any one of claims 1 to 6. Dicing and die bonding integrated film.

11. Semiconductor elements and A support member on which the semiconductor element is mounted, An adhesive member is provided between the semiconductor element and the support member to bond the semiconductor element and the support member, Equipped with, The adhesive member is a cured product of a film-like adhesive according to any one of claims 1 to 6. Semiconductor equipment.

12. The semiconductor element further comprises other semiconductor elements stacked on the aforementioned semiconductor element. The semiconductor device according to claim 11.

13. The method comprises the step of interposing a film-like adhesive according to any one of claims 1 to 6 between a semiconductor element and a support member, or between a first semiconductor element and a second semiconductor element, to bond the semiconductor element and the support member, or the first semiconductor element and the second semiconductor element. A method for manufacturing a semiconductor device.

14. A step of attaching the adhesive layer of the dicing-die bonding integrated film according to claim 10 to a semiconductor wafer, A step of dicing the semiconductor wafer to which the adhesive layer has been attached, A step of manufacturing a plurality of individualized semiconductor elements with adhesive pieces attached by expanding the substrate layer under cooling conditions, A step of picking up the adhesive-attached semiconductor element from the adhesive layer, A step of bonding the picked-up semiconductor element with adhesive piece attached to a support member via the adhesive piece, Equipped with, A method for manufacturing a semiconductor device.

15. The process further includes bonding another semiconductor element with adhesive pieces to the surface of the semiconductor element bonded to the support member via the adhesive pieces. The method for manufacturing a semiconductor device according to claim 14.

Citation Information

Patent Citations

  • Laser beam machining method

    JP2002192370A

  • Method for cutting semiconductor substrate

    JP2003338467A

  • Film for semiconductor and semiconductor device manufacturing method

    JP2012060038A

  • Adhesive sheet

    JP2012246461A

  • Method for manufacturing semiconductor device

    JP2015211080A