Electromagnetic shielding material
Patent Information
- Application Number
- JP2024511528
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-01
- Filing Date
- 2023-03-01
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-03-01
AI Technical Summary
Conventional electromagnetic shielding materials fail to effectively shield high-frequency electromagnetic waves and are not suitable for the casings of smaller, lighter electronic devices due to poor workability and strength issues, particularly in the high frequency band of 10 MHz or more.
A laminated stainless steel foil with a structure comprising an austenite phase and a ferrite phase, where the austenite phase constitutes 75% or more of one region and the ferrite phase 95% or more of another region, is used to enhance electromagnetic shielding properties and workability, with the phases alternately laminated in the thickness direction to maximize reflection and absorption losses.
The solution provides effective electromagnetic shielding in the high frequency band while maintaining strength and workability, suitable for the housings of electronic devices, by utilizing the interphase reflection and absorption losses in the laminated structure, reducing electromagnetic wave penetration and improving ductility and corrosion resistance.
Abstract
Description
Electromagnetic wave shielding material
[0001] The present invention relates to an electromagnetic wave shielding material.
[0002] Currently, electromagnetic wave (EMC) countermeasures for electronic devices use sintered ferrite for absorbing electromagnetic waves, and electromagnetic wave shielding films and electromagnetic wave shielding coatings for shielding (electromagnetic wave shielding). Sintered ferrite has excellent electromagnetic wave absorption properties and is mixed with resins and applied to electronic device housings. It is effective in low-frequency bands below several tens of megahertz. Electromagnetic wave shielding films include those made by pressing a metal plate (metal foil) and a resin layer, or those made by applying a conductive material made by mixing metal or magnetic powder with resin to a resin or cloth substrate. For example, Patent Document 1 proposes an electromagnetic wave shielding film laminated with a protective layer, a metal layer, and an adhesive layer. Patent Document 2 proposes an electromagnetic wave shielding film laminated with conductive layers on both sides of a flame-retardant cloth and an anti-corrosion layer on top of that. Electromagnetic wave shielding coatings are applied to the housing of electronic devices to reflect electromagnetic waves and prevent electromagnetic wave interference from entering the housing. For example, Patent Document 3 proposes a spray coating agent for electromagnetic wave shielding, which contains silver particles dispersed in a solvent, a thermosetting resin, and a curing agent.
[0003] JP 2021-174948 A JP 2004-031589 A JP 2020-143225 A
[0004] In recent years, in response to the explosive increase in communication data volume and the need for faster communication speeds, carrier waves have been increasing in frequency as a means of increasing the volume and speed of data communication. Accordingly, the frequency band of electromagnetic waves that must be blocked in electronic devices that receive and transmit high-frequency radio waves has been increasing. Conventional electromagnetic wave shields in low-frequency bands below 10 MHz can cause electronic devices to malfunction, so recently, there has been a demand for electromagnetic wave shields in high-frequency bands of 10 MHz or higher.
[0005] Furthermore, as electronic devices become smaller and lighter, their shapes become more diverse. Conventional electromagnetic wave shielding films and coatings are difficult to apply, making it difficult to completely shield them. Therefore, there is a demand for the housings of electronic devices and components to be made of electromagnetic wave shielding materials. To be used in electronic device housings, they must be strong and workable when thinned to reduce size and weight. However, electromagnetic wave shielding films and coatings are not suitable for use as strong components. Aluminum foil also lacks strength, and when thinned, it breaks during drawing and other processes, making it unsuitable for housings.
[0006] Therefore, in order to meet the need to add electromagnetic wave shielding properties to the housings of electronic devices, an object of the present invention is to propose an electromagnetic wave shielding material that has electromagnetic wave shielding properties in the high frequency band of 10 MHz or more, while also maintaining strength and processability even when made thin.
[0007] The present inventors conducted extensive research to achieve the above-mentioned objectives and obtained the following findings. [a] Selection of a metal material suitable for electronic device and component housings. To meet the need for smaller and lighter electronic devices and components (hereinafter collectively referred to as electronic devices), they investigated metal materials that have strength and workability even when extremely thin. Metals with good electromagnetic shielding properties and high conductivity include silver, copper, and aluminum. However, these metals have low strength and are prone to breakage when processed into complex shapes, posing practical problems. Therefore, they came up with the idea of using stainless steel foil (hereinafter sometimes referred to as "stainless steel foil"), which has a certain degree of strength and workability even when made extremely thin, although its conductivity is inferior to that of aluminum, and they further investigated the possibility of realizing this idea.
[0008] [b] Improvement of Electromagnetic Wave Shielding Properties The electromagnetic wave shielding properties of stainless steel are based on the following two mechanisms: Electromagnetic wave energy is basically attenuated (lost) due to reflection by the outer surface of the metal material (external reflection loss).
[0009] Furthermore, electromagnetic waves that penetrate into metals are attenuated as their energy is absorbed within the metal (absorption loss). Electromagnetic wave absorption loss also occurs in stainless steel, and because ferritic stainless steel has better conductivity than austenitic stainless steel, the absorption loss effect is greater in the high frequency band above 10 MHz.
[0010] These external reflection losses and absorption losses occur in any metallic material and depend on the dielectric constant and magnetic permeability of the metal. Therefore, although stainless steel has inferior conductivity to copper and aluminum, the inventors of the present invention have conducted extensive research to improve the electromagnetic wave shielding properties of stainless steel, and have obtained the following findings.
[0011] - When austenite phase (sometimes called γ) and ferrite phase (sometimes called α) exist in stainless steel, the electromagnetic wave energy is attenuated due to reflection at the interface between them (interphase interface reflection loss).
[0012] - The attenuation effect is further enhanced by repeated reflection at multiple interfaces between the austenite and ferrite phases.
[0013] On the other hand, repeated random reflections at grain boundaries can cause electromagnetic waves to slip between the grains, penetrating the stainless steel foil and leaking into the housing. To prevent this, we came up with the idea of layering austenite-based regions (regions with an austenite area ratio of 75% to 100%, also known as austenitic stainless steel) and ferrite-based regions (regions with a ferrite area ratio of 95% to 100%, also known as ferritic stainless steel) in the thickness direction. This differs from the interfacial reflections that occur when one phase is the matrix and the other is the grains, as the interface between the two phases is always present in the thickness direction. Therefore, the reflected waves always collide with the interface between the two phases, resulting in reflection and attenuation. As a result, we found that the electromagnetic wave energy that ultimately passes through the stainless steel foil and reaches the housing interior is significantly reduced.
[0014] Furthermore, we discovered that when precipitates (such as oxides or nitrides) are present in the stainless steel foil, electromagnetic waves are reflected at the interface with the precipitates, resulting in attenuation (grain boundary interface reflection loss).
[0015] [c] Improved Workability Stainless steel foil has higher strength than aluminum foil, copper foil, or silver foil of a similar thickness, is resistant to damage (e.g., cracks, pinholes, etc.) caused by processing, and has excellent workability. Utilizing these properties, it has already been applied to electronic device housings and battery cases. It has been explained that laminating austenite and ferrite phases in layers is effective for improving electromagnetic wave shielding, and it has been discovered that this dual-phase laminated stainless steel foil also has advantages in terms of improved workability.
[0016] Typically, austenitic stainless steel has better workability than ferritic stainless steel. However, the ferrite phase has low work hardening, which causes strain to concentrate locally, reducing the ductility of the foil. Therefore, by stacking these two phases, the ferrite phase deforms following the austenite phase, which has excellent ductility, during deformation, dispersing strain and improving the ductility of the foil.
[0017] Furthermore, since general housing processing involves a lot of drawing and bending, maximum tensile stress occurs on the surface of the plate, making it prone to cracks. Therefore, it was discovered that making the surface austenite phase improves the applicability to housing processing.
[0018] [D] Manufacturing method of austenite and ferrite phase laminated stainless steel foil As explained above, there are various methods for manufacturing stainless steel foil laminated with austenite and ferrite phases. For example, a clad steel sheet is made by alternately laminating austenitic stainless steel sheets and ferritic stainless steel sheets, and a stainless steel foil laminated with both phases can be obtained by a conventional foil rolling process.
[0019] Furthermore, for example, stainless steel foil with a laminated austenite and ferrite phases can be obtained by nitriding a conventionally obtained ferritic stainless steel foil and incorporating nitrogen into the surface to convert it to an austenite phase. This method produces a stainless steel foil in which one or both surfaces are austenite phase and the center is ferrite phase. Furthermore, by controlling the heat treatment during the nitriding treatment, it is possible to control the precipitation of precipitates in the austenite phase in the surface layer. This method can be produced relatively easily by utilizing existing processes, as it only requires nitriding an existing ferritic stainless steel foil.
[0020] Based on the above findings, the inventors discovered that by using a multi-layer stainless steel foil in which austenite and ferrite phases are layered in the thickness direction, it is possible to obtain an electromagnetic wave shielding material that has an improved electromagnetic wave shielding effect and that has the same workability and strength as conventional stainless steel foils.
[0021] [1] An electromagnetic shielding material having a thickness of 5 to 200 μm, characterized in that a first region made of stainless steel having an austenite phase area ratio of 75% or more and a second region made of stainless steel having a ferrite phase area ratio of 95% or more are laminated in the thickness direction. The first region and the second region may be laminated alternately in the thickness direction, and the number of layers is not particularly limited. The first region and the second region may be a total of two layers, one layer each, or a three-layer structure with one layer on one side and two on the other, or even a multi-layer structure with more than one layer. [2] The electromagnetic shielding material according to [1], wherein at least one surface is the first region. [3] The electromagnetic shielding material according to [1], wherein both surfaces are the first region. [4] The electromagnetic shielding material according to [2] or [3], wherein the first region has precipitates containing at least one of carbide, oxide, and nitride, the precipitates having a particle size of 1 μm or less, and the precipitates having a particle size of 0.1 μm or more account for 10% or less in area ratio in the thickness direction cross section. [5] The electromagnetic shielding material according to any one of [1] to [4], having a thickness of 5 to 50 μm. [6] The electromagnetic shielding material according to any one of [1] to [5], wherein the total area ratio of the second regions in the cross section in the thickness direction is 15% or more. [7] The chemical composition of the second regions, in mass %, is: Cr: 20.00 to 26.00%, N: 0 to 0.10%, Si: 0 to 2.00%, C: 0 to 0.040%, P: 0.030% or less, S: 0.030% or less, Mn: 0 to 1.50%, Cu: 0 to 0.50%, Mo: 0 to 3.00%, Ni: 0 to 5.00%, Ca: 0 to 50 ppm, sol. The electromagnetic wave shielding material according to any one of [1] to [6] above, wherein Al is 0 to 300 ppm, and the balance is Fe and impurities.[8] The electromagnetic shielding material according to [7], wherein the first region has a chemical composition, in mass%, of Cr: 20.00 to 26.00%, N: 0.15 to 5.00%, Si: 0 to 2.00%, C: 0 to 0.040%, P: 0.030% or less, S: 0.030% or less, Mn: 0 to 1.50%, Cu: 0 to 0.50%, Mo: 0 to 3.00%, Ni: 0 to 5.00%, Ca: 0 to 50 ppm, sol. Al: 0 to 300 ppm, and the balance: Fe and impurities.
[0022] According to the present invention, it is possible to obtain an electromagnetic shielding material that has electromagnetic wave shielding properties against electromagnetic waves in the high-frequency band, while also having strength and processability. This electromagnetic shielding material can be used to manufacture housings (casings) for electronic devices and components that have electromagnetic shielding properties.
[0023] FIG. 1 is a flow diagram showing an example of a method for producing a stainless steel foil as an electromagnetic wave shielding material according to an embodiment of the present invention.
[0024] Hereinafter, an electromagnetic shielding material according to the present invention will be described using as an example an embodiment of the present invention having a three-layer structure of austenite phase (hereinafter sometimes referred to as γ)-ferrite phase (hereinafter sometimes referred to as α)-austenite phase (γ).
[0025] [First Region (Austenitic Stainless Steel)] The first region is stainless steel (austenitic stainless steel) mainly composed of austenite phase, and all phases detectable by EBSD (Electron Back Scattered Diffraction) (iron phases such as ferrite phase, austenite phase, martensite phase, Cr 2 The austenite phase is a region mainly composed of an austenite phase (area ratio of 75% to 100%) among the entire steel (including compound phases such as N and CrN, and passive films). The area ratio of the austenite phase is preferably 80% or more, 85% or more, or 90% or more.
[0026] [Second Region (Ferritic Stainless Steel)] The second region is stainless steel (ferritic stainless steel) mainly composed of ferrite phase. As with the first region, all phases detectable by EBSD (electron backscattered diffraction) (iron phases such as ferrite, austenite, and martensite, Cr 2 The area ratio of the ferrite phase is preferably 92% or more, 94% or more, or 95% or more.
[0027] [Laminated structure of first region and second region] The first region (austenitic stainless steel) and the second region (ferritic stainless steel) are each layered (layers parallel to the surface), and these regions are alternately laminated in the thickness direction of the plate-shaped electromagnetic shielding material (laminated structure). As long as the austenitic stainless steel is used, it belongs to the first region even if it is a different type of austenitic stainless steel. Similarly, as long as the ferritic stainless steel is used, it belongs to the second region even if it is a different type of ferritic stainless steel.
[0028] The laminated structure is not particularly limited in its configuration, as long as the first region and the second region are alternately laminated. For example, it may be a two-layer structure, with the first layer being the first region and the second layer being the second region. For example, it may be a three-layer structure with the order of first region-second region-first region. For example, it may be a multilayer structure with four or more layers, such as first region-second region-first region-second region-... In order to obtain the effect of interface reflection loss between the first region and the second region, a multilayer structure with three or more layers is preferable. Of course, the first region and the second region may be reversed in the layer order described above. On the other hand, since a multilayer structure complicates the manufacturing process, it is best to determine the number of layers by balancing the electromagnetic wave shielding effect and manufacturing costs.
[0029] [Divided Portions] It is preferable that each layer has fewer divided portions that penetrate the layer (portions that are not austenite phase in the first region and portions that are not ferrite phase in the second region; hereinafter, these will be referred to as divided portions). This is because if there are divided portions, electromagnetic waves will transmit through those portions. When each layer is viewed vertically from above, it is desirable that the area ratio of the divided portions be 30% or less, 20% or less, 10% or less, 5% or less, 3% or less, 2% or less, 1% or less, or 0% (none).
[0030] [At least one surface is the first region] Because the austenite phase has better corrosion resistance than the ferrite phase, if at least one of the front and back surfaces of the electromagnetic shielding material is covered with stainless steel (first region) mainly composed of austenite, better corrosion resistance can be ensured. Also, from the standpoint of workability, in bending and drawing, it is preferable that the outermost layer, where maximum stress occurs, is stainless steel (first region) mainly composed of austenite. Therefore, it is preferable that at least one surface portion (surface layer portion) of the surface of the electromagnetic shielding material, preferably both surface portions (both surface layer portions), be the first region.
[0031] [Thickness of Each Layer] The thickness of each layer is not particularly limited.
[0032] [Method of measuring layer thickness and cross-sectional area ratio] The method of measuring each layer thickness is described below. A test piece is taken from the electromagnetic shielding material so that the cross section in the plate thickness direction serves as the observation surface. The observation surface is polished and etched. The etching solution is not particularly limited as long as it is an etching solution for stainless steel, but an etching solution containing aqua regia and glycerin in a volume ratio of 4:1 can be preferably used.
[0033] The boundary between the first and second regions in the electromagnetic shielding material can be clearly identified by etching. The boundary between the first and second regions can also be confirmed by electron backscattered diffraction (EBSD). From the EBSD IPF map, the region (first region) mainly composed of the austenite phase (γ) and the region (second region) mainly composed of the ferrite phase (α) can be confirmed. After determining the boundary between the first and second regions by the above-mentioned method, the area of each layer is calculated using image analysis software.
[0034] For example, in the case of a three-layer structure consisting of the first region (γ) - the second region (α) - the first region (γ), if the area of the second region is A, the area of the first layer of the region other than the second region (i.e., the first region) is B1, and the area of the third layer is B2, the cross-sectional area ratio of the second region can be calculated from A / (A+B1+B2). Similarly, the cross-sectional area ratio of the first layer can be calculated from B1 / (A+B1+B2), and the cross-sectional area ratio of the third layer can be calculated from B2 / (A+B1+B2). Because the first and second regions are layered, the calculated cross-sectional area ratio is the ratio of the layer thicknesses. Therefore, the thickness of each layer can be calculated by multiplying the thickness of the electromagnetic shielding material by the cross-sectional area ratio.
[0035] In addition, when the electromagnetic shielding material is long, it is desirable to measure the cross-sectional area ratio of a plurality of cross sections (e.g., 10 cross sections) obtained by cutting the electromagnetic shielding material evenly and calculate the average. The area of the precipitates in the first region is obtained from the distribution of metal elements such as C, N, O, and Cr, and the proportion of the precipitates can be calculated from the area of the first region.
[0036] [Precipitates] One or more precipitates containing at least one of carbides, oxides, and nitrides may be dispersed in the first and second regions. Examples of precipitates include Cr nitrides, Cr oxides, Cr carbides, Fe oxides, and Fe carbides. The presence of precipitates is expected to reduce the reflection loss of electromagnetic wave energy at the interface. In particular, the presence of precipitates in the outermost layer (the layer on at least one side of the electromagnetic wave shielding material) can be expected to reduce reflection loss at the surface layer. Furthermore, the reflected waves are reflected by the interface between the first and second regions, preventing them from penetrating the shielding material.
[0037] On the other hand, if precipitates are present in stainless steel, strain concentrates around the precipitates during processing, becoming the starting point for fracture. In particular, coarse crystal grains not only become the starting point for stress concentration, but also reduce the effective thickness of the stainless steel foil, causing fracture. Therefore, from the perspective of workability, it is preferable that precipitates are absent. Considering workability, it is preferable that the precipitates have a particle size of 1.0 μm or less. Smaller precipitates are preferable, with particle sizes of 0.8 μm or less, 0.6 μm or less, 0.4 μm or less, 0.2 μm or less, or 0.1 μm or less being preferred. Furthermore, the density of the precipitates should be 10% or less, 7% or less, 5% or less, or 3.5% or less, in terms of the area ratio of precipitates with a particle size of 0.1 μm or more in the thickness direction cross section of the electromagnetic shielding material.
[0038] The lower limit of the precipitate density (area ratio) is preferably 0%, but in the case of the outermost layer (surface layer), since a reflection loss effect can also be expected at the precipitate interface, the area ratio of precipitates with a grain size of 0.1 μm or more may be 0.1% or more, 0.2% or more, 0.3% or more, 0.4% or more, or 0.5% or more. Note that the grain size of the precipitates here refers to the diameter of a circle equivalent to the area of the precipitate observed in a cross section in the plate thickness direction of the electromagnetic shielding material.
[0039] [Components] The electromagnetic shielding material according to this embodiment may have any component. The first region may have any component as long as it is made of stainless steel mainly composed of austenite phase. The second region may also have any component as long as it is made of stainless steel mainly composed of ferrite phase.
[0040] [Thickness] The thickness of the electromagnetic wave shielding material according to this embodiment is not particularly limited. However, if the thickness is too thin, it becomes difficult to roll the material while maintaining its shape, and it also becomes difficult to ensure foil flatness. Therefore, the thickness should be 5 μm or more. Preferably, it should be 7 μm or more, 8 μm or more, 9 μm or more, or 10 μm or more. On the other hand, if the thickness is too thick, it becomes difficult to perform fine processing as a shielding material for small electronic components such as sensors, and the weight of the electronic device increases, making it unsuitable for practical use. Therefore, the thickness should be 200 μm or less. Preferably, the thickness should be 150 μm or less, 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 20 μm or less, or 10 μm or less.
[0041] [Manufacturing method] The electromagnetic wave shielding material according to the present invention can be manufactured by any method as long as it has the above-described structure. For example, a clad steel sheet can be manufactured by laminating an austenitic stainless steel sheet and a ferritic stainless steel sheet, and a stainless steel foil in which both phases are laminated can be obtained by a conventional foil rolling process.
[0042] Furthermore, for example, stainless steel foil with austenite and ferrite phases laminated together can be obtained by nitriding ferritic stainless steel foil and allowing nitrogen to penetrate through the surface to convert the surface layer to austenite. This method produces stainless steel foil with austenite (γ) on one or both surfaces and ferrite (α) in the center (γ-α two-layer or γ-α-γ three-layer stainless steel foil). Since existing ferritic stainless steel foil can be nitrided, this method can be produced relatively easily using existing equipment.
[0043] Alternatively, the two methods may be combined. For example, a ferritic stainless steel sheet, an austenitic stainless steel sheet, and a ferritic stainless steel sheet may be laminated to form an α-γ-α clad steel sheet, which may then be nitrided. This allows for the production of a γ-α-γ-α-γ five-layer stainless steel foil.
[0044] As one embodiment of the manufacturing method, a manufacturing method for nitriding a ferritic stainless steel foil serving as a base material will be described below. FIG. 1 is a flow diagram showing an example of a manufacturing method for stainless steel foil as an electromagnetic wave shielding material according to this embodiment. This manufacturing method is merely exemplary, and the manufacturing method of stainless steel sheet according to this embodiment is not limited to this method. This manufacturing method includes a step of preparing a slab (step S1), a step of hot-rolling and cold-rolling the slab to obtain a rolled steel sheet with a thickness of 5 to 200 μm (step S2), and a step of annealing (nitriding) the rolled steel sheet in a nitrogen-containing gas atmosphere and cooling it (step S3). Each step is described in detail below.
[0045] [Slab Preparation Step] Step S1: A slab having the chemical composition of a ferritic stainless steel base material is prepared (Step S1). For example, the chemical composition of the ferritic stainless steel according to one embodiment is, in mass %, 20-26% Cr, 0.1% or less N, 2.0% or less Si, 0.040% or less C, 0.030% or less P, 0.030% or less S, 1.5% or less Mn, 0.50% or less Cu, 3.00% or less Mo, 5.00% or less Ni, less than 50 ppm Ca, less than 300 ppm sol. Al, and the balance being Fe and impurities. The N content of the slab is set to 0.1% or less because a N content exceeding 0.1% increases deformation resistance, making it difficult to produce a steel sheet by rolling. The upper limit of the N content of the slab is preferably 0.05%.
[0046] The chemical composition of the ferritic stainless steel base material according to the embodiment will be described below. In the following description, "%" and "ppm" for the content of elements mean mass % and mass ppm, respectively, unless otherwise specified.
[0047] (Cr: 20.00 to 26.00%) Chromium (Cr) is the metal that forms on the surface of stainless steel. 2 O 3Cr has the effect of forming a passive film and improving corrosion resistance. If the Cr content is low, the austenitized structure due to nitrogen absorption may contain a large amount of martensite phase. Furthermore, if the Cr content is low, severe deformation may result in the formation of a deformation-induced martensite phase. Therefore, the lower limit of Cr is set to 20.00%. On the other hand, as the Cr content increases, the deformation resistance increases. Therefore, to ensure more stable manufacturability (especially the flatness of thin steel sheets), the upper limit of the Cr content is set to 26.00%. The lower limit of the Cr content is preferably set to 21.00%, 22.00%, or 23.00%. The upper limit of the Cr content is preferably set to 25.00% or 24.00%.
[0048] (N in the second region: 0.10% or less) In this embodiment, a ferritic stainless steel base material is used, and the surface layer is converted into an austenitic stainless steel (first region) by surface nitriding. Therefore, the ferritic stainless steel base material remains as the second region. Nitrogen (N) is also an element that promotes the austenitization of stainless steel. To obtain a structure primarily composed of ferrite phase in Fe—Cr—N stainless steel, the nitrogen (N) content should be 0.10% or less. Furthermore, when the ferritic stainless steel base material is rolled to a predetermined thickness and then the first region is formed by surface nitriding, if the N content in the base material exceeds 0.10%, the deformation resistance increases, making it difficult to form the steel plate by rolling. For these reasons, the N content of the ferritic stainless steel base material should be 0.10% or less, and preferably 0.09% or less, 0.08% or less, 0.07% or less, 0.06% or less, or 0.05% or less.
[0049] (N in the first region: 0.15 to 5.00%) In this embodiment, the surface of the ferritic stainless steel base material is nitrided to convert the surface layer to austenite. Therefore, in the Fe-Cr-N stainless steel, the N content required to obtain a structure (first region) mainly composed of an austenite phase in the surface layer should be 0.15% or more. On the other hand, Cr in the grains 2Since the formation of nitrides such as N and CrN deteriorates workability, the upper limit of the N content is set to 5.00% to suppress this. Therefore, the nitrogen (N) content of the first region is set to 0.15% or more and 5.00% or less. The lower limit of the N content of the first region can be preferably set to 0.17%, 0.19%, 0.21%, 0.23%, 0.25%, 0.27%, 0.29%, 0.31%, 0.33%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, or 0.60%. The upper limit of the N content may be preferably 4.75%, 4.50%, 4.25%, 4.00%, 3.75%, 3.50%, 3.25%, 3.00%, 2.80%, 2.60%, 2.40%, 2.20%, 2.00%, 1.80%, 1.60%, 1.50%, 1.40%, 1.30%, or 1.20%. Naturally, in this embodiment, the N content of the first region is higher than the N content of the second region (base metal).
[0050] (Si: 0 to 2.00%) Silicon (Si) does not necessarily have to be contained. Si is an element that deteriorates the workability of stainless steel, so it is not usually an element that is actively added. On the other hand, when stainless steel is exposed to a transpassive corrosive environment, Si forms SiO 2 and Cr 2 O 3 It acts to cover and protect the passive film. On the other hand, if the Si content is high, workability deteriorates and a brittle σ phase is more likely to precipitate during manufacturing, which can cause cracks during the steel sheet processing step or result in poor flatness and a shape that is not suitable for press processing. Therefore, when Si is contained, the upper limit of the Si content is set to 2.00%. The upper limit of the Si content is preferably 1.90%, 1.80%, 1.70%, 1.60%, or 1.50%. The preferred lower limit of the Si content is more than 0%, and more preferably 0.10% or more.
[0051] (C: 0 to 0.040%) Carbon (C) does not necessarily need to be contained. Since the stainless steel sheet of this embodiment contains a certain amount of N or more, solid solution strengthening by N is sufficient, and C does not need to be added. On the other hand, C is a solid solution strengthening element and contributes to improving the strength of stainless steel. However, if the C content is too high, many carbides are generated during the manufacturing process, and these carbides become the origin of fracture, reducing the formability of the steel. Therefore, the C content is set to 0.040% or less. The upper limit of the C content is preferably 0.038%, 0.036%, 0.034%, 0.032%, or 0.030%. The preferred lower limit of the C oil content is greater than 0%, and more preferably 0.001%.
[0052] (P: 0.030% or less) Phosphorus (P) is an impurity. P segregates at grain boundaries during solidification and increases solidification cracking susceptibility. Therefore, it is preferable that the P content be as low as possible. Therefore, the P content is set to 0.030% or less. The lower limit of the P content is 0%, but an excessive decrease requires an increased load during refining or the use of expensive raw materials, so in reality, 0.001% may be sufficient.
[0053] (S: 0.030% or less) Sulfur (S) is an impurity. S segregates at grain boundaries during solidification and increases solidification cracking susceptibility. Therefore, it is preferable that the S content is as low as possible. Therefore, the S content is set to 0.030% or less. The lower limit of the S content is 0%, but an excessive decrease requires an increased load during refining or the use of expensive raw materials, so in reality, 0.001% may be sufficient.
[0054] (Mn: 0 to 1.50%) Manganese (Mn) does not necessarily need to be contained. On the other hand, Mn suppresses the deterioration of hot workability due to S. Mn also deoxidizes stainless steel. However, an increase in Mn content promotes the precipitation of intermetallic compound phases such as the σ phase. The precipitation of the σ phase reduces structural stability and also reduces the toughness and ductility of the stainless steel. Therefore, the Mn content is set to 1.50% or less. The upper limit of the Mn content is preferably 1.40%, 1.30%, 1.20%, 1.10%, 1.00%, 0.90%, 0.80%, 0.70%, 0.60%, or 0.50%. The lower limit of the Mn content is preferably more than 0%, and more preferably 0.01%, 0.05%, or 0.10%.
[0055] (Cu: 0 to 0.50%) Copper (Cu) does not necessarily need to be contained. Cu tends to segregate at grain boundaries and is an austenite stabilizing element. Cu acts as a solid solution strengthening element and contributes to increasing the high-temperature strength required for structural materials, so it may be contained as needed. A high Cu content suppresses ferrite formation during solidification during casting, increasing solidification cracking susceptibility. Furthermore, a high Cu content may degrade hot workability. Therefore, the Cu content is set to 0.50% or less. The upper limit of the Cu content is preferably 0.47%, 0.43%, 0.40%, 0.37%, 0.33%, 0.30%, 0.27%, 0.23%, or 0.20%. The lower limit of the Cu content is preferably greater than 0%, and more preferably 0.01%.
[0056] (Mo: 0 to 3.00%) Molybdenum (Mo) does not necessarily have to be contained. On the other hand, when it is particularly desired to improve corrosion resistance, Mo has the effect of increasing the corrosion resistance of stainless steel. However, Mo is an expensive element classified as a rare metal, and is not preferable from the viewpoint of providing an economically excellent material. Furthermore, if the Mo content is too high, hot workability decreases and a structure mainly composed of an austenite phase may not be obtained in the surface layer. Therefore, the Mo content is set to 3.00% or less. The upper limit of the Mo content is preferably 2.75%, 2.50%, 2.25%, 2.00%, 1.80%, 1.60%, 1.50%, 1.30%, 1.10%, 1.00%, 0.90%, 0.80%, 0.70%, 0.60%, or 0.50%. The lower limit of the Mo content is preferably more than 0%, and more preferably 0.01%, 0.05%, 0.10%, 0.20%, or 0.30%.
[0057] (Ni: 0 to 5.00%) Nickel (Ni) does not necessarily need to be contained. On the other hand, Ni is an element that promotes the austenitization of stainless steel and also contributes to improving corrosion resistance. Therefore, Ni may be contained when it is particularly desired to enhance corrosion resistance or improve workability. However, Ni is a rare metal element, and is therefore undesirable from the perspective of providing an economically superior material. Furthermore, elution of Ni ions may reduce the oxygen reduction reaction rate at the interface between the platinum catalyst and the polymer electrolyte membrane. Therefore, the Ni content is set to 5.0% or less. The upper limit of the Ni content is preferably 4.50%. It is preferably set to 4.00%, 3.50%, 3.00%, 2.50%, 2.00%, 1.50%, 1.00%, 0.80%, 0.70%, 0.6%, 0.5%, 0.4%, 0.3%, or 0.2%. The lower limit of the Ni content is preferably more than 0%, and more preferably 0.01%, 0.05%, or 0.10%.
[0058] (Ca: 0 to less than 50 ppm) Calcium (Ca) is an impurity and is therefore preferably not contained. CaS and MnS are generally known non-metallic inclusions that can serve as starting points for corrosion of stainless steel. In order to prevent the formation of large amounts of CaS, which can serve as starting points for corrosion, the Ca content should be less than 50 ppm.
[0059] (sol. Al: 0 to less than 300 ppm) Aluminum (Al) does not necessarily need to be contained. On the other hand, Al deoxidizes stainless steel. However, if the Al content is too high, the cleanliness of the steel decreases, and the workability and ductility of the stainless steel decrease. Therefore, the Al content is less than 300 ppm. A preferred lower limit of the Al content is more than 0%, and more preferably 1 ppm, 10 ppm, 50 ppm, or 100 ppm. In this specification, the Al content means the content of acid-soluble Al (sol. Al).
[0060] The balance of the chemical composition of the stainless steel sheet according to this embodiment is Fe and impurities. The impurities referred to here refer to elements that are unintentionally mixed in from ores or scrap used as raw materials for steel, or elements that are mixed in from the environment during the manufacturing process, etc.
[0061] The process for preparing a slab can be, but is not limited to, the following: Melting raw materials. Examples of raw materials include ferrochrome and ferrosilicon for stainless steel production, cast iron, and ferritic stainless steel scrap. Melting is typically performed in an electric furnace. At the laboratory level, it can also be performed in a vacuum induction furnace. Refining is performed to reduce carbon content, gas components, and metal inclusions. Refining methods that can be used include argon-oxygen decarburization (AOD), vacuum-oxygen decarburization (VOD), and V-AOD. The slab is then cast into a continuous casting machine or case to form a slab suitable for rolling. The chemical composition of the slab can be adjusted by adjusting the raw material composition and refining conditions.
[0062] [Rolling Process] Step S2 The slab is hot-rolled and cold-rolled to obtain a rolled steel sheet having a thickness of 5 to 200 μm (Step S2). Hot rolling and cold rolling may be repeated, and intermediate heat treatment such as annealing or pickling may be performed as needed. In addition to hot rolling and cold rolling, hot forging and cutting may also be performed as needed.
[0063] The rolling process is not limited to this, but can be, for example, as follows: The slab is hot-rolled using a tandem mill or a Steckel mill to form a hot coil. This hot coil is annealed and pickled. It is further cold-rolled using a multi-roll cold rolling mill to form a rolled steel sheet with a thickness of 5 to 200 μm.
[0064] [Annealing (nitriding) process] Step 3: The rolled steel sheet is annealed in a nitrogen-containing gas atmosphere and cooled (Step S3). This process allows nitrogen to penetrate from the surface of the steel sheet, converting the structure of the surface layer on both or either one of the surfaces of the steel sheet into a structure (first region) mainly composed of austenite phase. If only the surface layer on one surface is to be converted into austenite phase, for example, the opposite surface (the surface not to be converted into austenite phase) may be masked before nitriding.
[0065] The N content in the surface layer portion (first region) of the steel sheet after the annealing step can be adjusted by the N content of the slab, the annealing conditions, etc. Specifically, the N content in the surface layer portion (first region) of the steel sheet can be increased by increasing the N content of the slab, increasing the nitrogen partial pressure during annealing, increasing the annealing temperature, or lengthening the annealing holding time, or controlling the steel sheet passing speed.
[0066] The ratio of the nitrogen partial pressure to the total pressure of the processing gas is preferably 0.2 to 0.9. If the ratio of the nitrogen partial pressure to the total pressure is less than 0.2, nitrogen is not sufficiently supplied from the surface, and when the steel sheet is thick, it becomes difficult to form a first region that covers the entire front and back surfaces of the steel sheet. On the other hand, if the ratio of the nitrogen partial pressure to the total pressure of the processing gas is higher than 0.9, Cr nitrides are excessively formed on the surface, which may become the starting point for cracking during processing. The upper limit of the ratio of the nitrogen partial pressure to the total pressure of the processing gas is preferably 0.75. Hydrogen is preferably used as the gas to be mixed with nitrogen to prevent oxidation of the steel sheet. Argon may be used instead of or in addition to hydrogen.
[0067] The annealing temperature is preferably 950 to 1200° C. If the annealing temperature is less than 950° C., not only the austenite phase but also Cr phase will remain in the equilibrium state. 2Due to the presence of the N phase, it may be difficult to increase the austenite phase fraction in the first region. On the other hand, if the annealing temperature exceeds 1200°C, a liquid phase may be generated near the grain boundaries, melting the grains and causing embrittlement, especially when Si is contained. The annealing temperature varies depending on the Cr content, but is more preferably 1050 to 1150°C.
[0068] The annealing holding time needs to be controlled within a narrow range depending on the thickness and nitrogen partial pressure of the steel sheet. Austenitization due to nitrogen absorption progresses from the surface to the interior of the sheet over time, but in the manufacturing of the stainless steel sheet according to this embodiment, it is necessary to stop the progress of austenitization midway. If the holding time is too short, there is a risk that ferrite phase will remain on the surface even if the sheet thickness is thin. On the other hand, if the holding time is too long, there is a risk that the cross-sectional area ratio of the second region will be too low.
[0069] When cooling annealed steel sheet, controlled cooling according to the temperature range is recommended. If the annealed steel sheet is slowly cooled, the austenite phase formed by absorbing nitrogen will change into a two-phase structure of ferrite and Cr nitride. On the other hand, if the cooling rate is too fast, it will be impossible to form an austenite phase in the surface layer, which has a structure in which one or more precipitates consisting of carbides, oxides, and nitrides are dispersed. Specifically, controlled cooling is recommended, in which the steel sheet is cooled from the annealing temperature to approximately 500°C at a fast cooling rate (10 to 15°C / min), and then cooled from 500°C to 300°C at a relatively slow cooling rate (5 to 8°C / sec). Alternatively, the steel sheet may be cooled to 500°C at a fast cooling rate (10 to 15°C / sec), held at 500°C ± 10°C for approximately 1 to 30 seconds, and then cooled at a fast cooling rate (10 to 15°C / sec).
[0070] The annealing step may be performed in any form using an annealing furnace as long as the above annealing conditions are satisfied. For example, the annealing step may be performed by passing the steel sheet through an annealing line called a continuous bright annealing line.
[0071] This annealing step forms a first region mainly composed of an austenite phase in the surface layer of the steel sheet. The surface layer of the steel sheet after the annealing step is adjusted so that the N content is 0.15 to 5.0 mass % and the cross-sectional area ratio of the second region is 15% or more.
[0072] [Test Materials] Eight types of steel having the chemical compositions shown in Table 1 were melted in a 30 kg vacuum melting furnace using a high-frequency induction heating system to produce cast ingots having a generally truncated cone shape with a diameter of 125 to 115 mm and a height of 320 mm. The surface black scale on the side of the truncated cone shape of these cast ingots was ground using a grinder, and after grinding, the ingots were heated and held at 1250°C for 3 hours, followed by hot forging to a finished thickness of 25 mm and grinding to a thickness of 20 mm to produce slabs.
[0073] The slab was then held at 1200°C for 2 hours and hot rolled to a thickness of 4 mm to obtain a hot-rolled steel sheet. To remove the black scale after rolling, the hot-rolled steel sheet was ground to a thickness of 3 mm, and then cold-rolled to a thickness of 0.5 mm to obtain a cold-rolled steel sheet. The obtained cold steel sheet was repeatedly subjected to intermediate annealing in an argon atmosphere at 800°C for 10 minutes and cold rolling to obtain test materials with the thicknesses shown in Table 2.
[0074] [Annealing Treatment (Nitriding Treatment)] Test specimens measuring 70 mm wide x 200 mm long were cut out from each test material and subjected to annealing treatment in a continuous annealing simulator under the annealing treatment (nitriding treatment) conditions shown in Table 2, thereby carrying out nitrogen absorption treatment (nitriding treatment) in the solid phase. The total pressure was 1 atmosphere. After annealing, the specimens were cooled under the cooling conditions shown in Table 2. Some test materials (TP7 and 8 in Table 2) were held at 500°C for 10 seconds, and then cooled to 300°C at an average cooling rate of 14°C / second. Stainless steel plates (test materials) were obtained from the above process.
[0075] [Investigation of Structure, etc.] (1) Measurement of N Content in Stainless Steel Plate The N content in the steel after nitriding treatment was measured by an inert gas conveying fusion thermal conductivity method using an analytical sample taken from the entire thickness of each test piece.
[0076] (2) Confirmation of the Presence of the First and Second Regions A sample was taken from each test piece so that the cross section perpendicular to the rolling direction (cross section in the plate thickness direction) served as the observation surface, embedded in resin, mirror-polished, and then etched using an etching solution of aqua regia and glycerin in a volume ratio of 4:1 until the metal structure appeared. When the test material had the first and second regions, the boundary between them could be clearly distinguished by etching.
[0077] The region mainly composed of ferrite phase (second region) was etched more deeply than the region mainly composed of austenite phase (first region). In the region mainly composed of ferrite phase, the difference in etching between crystal grains was small, the etching at the grain boundaries was thin, and the etching within the grains was relatively smooth. This is thought to be because no nitrogen penetration occurred, and the original ferrite phase remained, only being subjected to the thermal history of high-temperature annealing.
[0078] In contrast, the region mainly composed of austenite (region 1) was etched more shallowly than the region mainly composed of ferrite (region 2). In the region mainly composed of austenite, the etching differed greatly among grains, with the grain boundaries being etched relatively clearly and the grain interiors being etched relatively coarsely. This is thought to be due to the accumulation of strain within the grains as the ferrite phase transformed to the austenite phase due to nitrogen enrichment caused by nitrogen penetration while the surroundings were constrained in the solid state.
[0079] Furthermore, it was confirmed by the EBSD orientation map that the surface layer is a region (first region) mainly composed of austenite phase (γ) (γ area ratio of 75% or more), and the central part is a region (second region) mainly composed of ferrite phase (α) (α area ratio of 95% or more). The cross-sectional structure of the sample taken out of the test material was also analyzed by EBSD (Electron Back Scattered Diffraction, JEOL JSM-7001F). Measurements were performed using an accelerating voltage of 15 kV, a measurement field of view of 150 μm (horizontal) × 50 μm (vertical), and a step size of 0.01 μm, using a TSL Solutions HIKARI (high-speed detector) and OIM DATA COLLECTION (measurement software), and analysis was performed using OIM Analysis (analysis software). From the EBSD IPF map, it was confirmed that the surface layer was a region (first region) mainly composed of the austenite phase (γ), and the center portion was a region (second region) mainly composed of the ferrite phase (α). The "Layer Structure" column in Table 2 lists the phases in order from the surface layer.
[0080] (3) Measurement of the cross-sectional area ratio of the second region (ferritic stainless steel) After defining the boundary between the first region and the second region, the areas of the first and second regions were determined using image analysis software. The area of the second region was designated A, and the area of the region other than the second region was designated B. The cross-sectional area ratio of the second region was calculated from A / (A+B).
[0081] (4) Identification of precipitates dispersed in the first region (austenitic stainless steel) Identification of precipitates dispersed in the first region was carried out by XRD. When the thickness of the test material was thicker than 30 μm, XRD measurement was carried out while polishing about 10 μm from one side. The precipitates formed in the first region were identified from the obtained XRD peaks.
[0082] (5) Measurement of the Proportion of Dispersed Precipitates in the First Region The cross-sectional structure of the test material was analyzed using an FE-EPMA (JXA-8530F manufactured by JEOL Ltd.). Details of the analysis method are as follows. In the first region of the test material, elemental mapping of nonmetallic elements (e.g., C for carbides, N for nitrides, and O for oxides) corresponding to the type of precipitate identified by XRD and alloy elements contained in the substrate was performed, and the distribution of each precipitate was identified from the overlap of nonmetallic elements and metallic elements and the XRD analysis results. From the obtained mapping data, the area of each precipitate with a particle size (diameter equivalent to an area-equivalent circle) of 0.1 μm or more was calculated using image analysis software. The area of the first region was defined as A, the area of the precipitate as C, and the area ratio of the precipitate was calculated from C / A.
[0083] [Evaluation of Test Material Properties] For each test material, the electromagnetic wave shielding properties in the high frequency range, as well as the formability (elongation) and strength (tensile strength) were investigated, and the evaluation results are shown in Table 2. In each TP, the maximum diameter of the precipitates was 1.0 μm or less.
[0084] (1) Evaluation of electromagnetic shielding properties at high frequencies. The higher the magnetic permeability of a material at the test frequency, the better the electromagnetic shielding properties. To evaluate the magnetic permeability in the high-frequency band, the test frequency was set to 100 MHz, and the electromagnetic shielding properties of each test material were evaluated by comparing the magnetic permeability at 100 MHz. Each test material was punched using a mold to an outer diameter of 6.93 to 6.96 mm and an inner diameter of 3.06 to 3.10 mm to prepare a test piece (TP). The magnetic permeability of each TP was measured at 100 MHz. The magnetic permeability was measured using a vector network analyzer (Keysight ENA E5071C) in the frequency range of 100 kHz to 8.5 GHz. The measured magnetic permeability was measured as complex permeability, and a complex permeability (imaginary part) of 0.5 or more at 100 MHz was considered to have excellent electromagnetic shielding properties (◯: excellent). As shown in Table 2, TP1 had a low Cr concentration, so the surface layer was not austenite but had a structure of ferrite and martensite (α'), and therefore the electromagnetic wave shielding properties were unacceptable.
[0085] (2) Evaluation of Formability and Strength The formability (elongation) and strength (tensile strength) of each test material were evaluated. ASTM half test pieces (parallel portion; 6.25 mm wide, 32 mm long) were subjected to tensile tests at room temperature at 2 mm / min. The elongation value (EL) was used as a representative value of ductility. For reference, the characteristic evaluations of aluminum foil and SUS304 stainless steel foil are listed in Table 2. Since a measured EL of 5% or more indicates a satisfactory level of formability, those between 5% and 7% were rated as having good formability (△; good), and those with an EL of 7% or more were rated as having excellent formability (〇: excellent). TP16, TP17, and TP19 were rated as having good formability (△) because their elongation values (EL) were smaller than those of the other TPs due to increased precipitate density. Strength (tensile strength) of 500 MPa or more was rated as having excellent strength (〇: excellent). The strength of the aluminum foil was only about 100 MPa at most, and therefore it was rated as inferior (x: insufficient strength).
[0086]
[0087]
[0088] The present invention can be used as an electromagnetic wave shielding material in all industrial fields, and in particular, can be used for housings of electronic devices and electronic equipment.
Claims
1. An electromagnetic shielding material having a plate-like shape with a thickness of 5 to 200 μm, characterized in that a first region made of stainless steel having an austenite phase of 75% or more in area ratio and a second region made of stainless steel having a ferrite phase of 95% or more in area ratio are laminated in the plate thickness direction.
2. The electromagnetic shielding material according to claim 1 , wherein at least one surface is the first region.
3. 3. The electromagnetic shielding material according to claim 2, wherein the first region has precipitates including at least one of carbides, oxides, and nitrides, the precipitates having a grain size of 1.0 μm or less, and precipitates having a grain size of 0.1 μm or more account for 10% or less in area ratio in a cross section in the sheet thickness direction.
4. 4. The electromagnetic shielding material according to claim 1, having a plate thickness of 5 to 50 μm.
5. 4. The electromagnetic shielding material according to claim 1, wherein the sum of the area ratios of the second regions in a cross section in the sheet thickness direction is 15% or more.
6. The chemical composition of the second region is, in mass%, Cr: 20.00-26.00%, N: 0 to 0.10%, Si: 0-2.00%, C: 0 to 0.040%, P: 0.030% or less, S: 0.030% or less, Mn: 0 to 1.50%, Cu: 0 to 0.50%, Mo: 0-3.00%, Ni: 0-5.00%, Ca: 0-50ppm, sol. Al: 0 to 300 ppm, 4. The electromagnetic shielding material according to claim 1, wherein the balance is Fe and impurities.
7. The chemical composition of the first region is, in mass%, Cr: 20.00-26.00%, N: 0.15-5.00%, Si: 0-2.00%, C: 0 to 0.040%, P: 0.030% or less, S: 0.030% or less, Mn: 0 to 1.50%, Cu: 0 to 0.50%, Mo: 0-3.00%, Ni: 0-5.00%, Ca: 0-50ppm, sol. Al: 0 to 300 ppm, The electromagnetic shielding material according to claim 6 , wherein the balance is Fe and impurities.
8. An electromagnetic wave shielding material as described in claim 4, wherein the sum of the area ratios of the second regions in the cross section in the thickness direction of the plate is 15% or more.