Paper base material for fibrous casing base material

JPWO2024232136A1Pending Publication Date: 2024-11-14
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2025519321
Authority / Receiving Office
JP · JP
Patent Type
Applications
Priority Date
2023-05-10
Filing Date
2024-02-15
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing paper base materials for fibrous casings lack sufficient wet strength and alkali resistance during viscose coating processing, especially when not pre-impregnated with viscose liquid, leading to potential breakage and inadequate properties.

Method used

A paper base material incorporating natural fibers, specifically hemp pulp, and a combination of cationic and anionic paper strength enhancers added both internally and externally, ensuring high wet strength and alkali resistance without pre-impregnation with viscose liquid.

Benefits of technology

The paper base material achieves excellent wet strength, alkali resistance, and wettability, preventing breakage during viscose coating and ensuring uniform coating, as demonstrated by the examples with hemp pulp and various pulp blends.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention addresses the problem of providing a paper base material for a fibrous casing base material. The paper base material does not require preliminary impregnation with a viscose liquid, and has sufficient alkali resistance and wet strength when undergoing viscose application. As a solution to the problem, provided is a paper base material for a fibrous casing base material, the paper base material comprising natural fibers and a paper-strengthening agent. Both a cationic paper-strengthening agent and an anionic paper-strengthening agent are added as the paper-strengthening agent by internal sizing and surface sizing.
Need to check novelty before this filing date? Find Prior Art

Description

Paper base material for fiber casing

[0001] The present invention relates to a paper substrate for a fibrous casing substrate.

[0002] Casings used in meat processing such as ham, sausage, and bacon include natural casings (animal intestines) and artificial casings (cellulose casing, collagen casing, plastic casing). Artificial casings are inexpensive and have the advantage of being hygienic and providing consistent product sizes. Fibre casings, which are classified as cellulose casings, are particularly widely used because they are strong and can be smoked.

[0003] Fibre casing is a paper base material made of cellulose pulp that has been impregnated with viscose, coagulated, and recycled. This paper base material is required to have wet strength and alkali resistance (resistance to alkaline solutions). Conventionally, to impart wet strength and alkali resistance to such paper base materials, they have been pre-impregnated with a low-concentration viscose solution and recycled. Patent Document 1 proposes a paper base material that is imparted with wet strength and alkali resistance by preparing and manufacturing a papermaking raw material from a pulp slurry containing guar gum and polyamide epichlorohydrin resin. Patent Document 2 proposes a paper base material that combines two types of pulp fibers specified by fiber coarseness, exhibiting good viscose impregnation during viscose processing, alkali resistance, and high wet strength. However, due to the high manufacturing costs of viscose processing and the need to address environmental issues caused by the generation of hydrogen sulfide, paper base material suppliers have been investigating alternative chemicals to viscose pre-impregnation.

[0004] JP-A-6-294094 JP-A-6-141760

[0005] As a paper base material for fibrous casing, instead of paper that has been pre-impregnated with viscose liquid and recycled, one that does not use viscose liquid has been proposed, but these have not provided sufficient wet strength and alkali resistance for the viscose coating process when used as a fibrous casing. Therefore, there has been a demand for a paper base material for fibrous casing that does not require pre-impregnation with viscose liquid and has sufficient wet strength and alkali resistance for the viscose coating process.

[0006] The means for solving the problems of the present invention are as follows: 1. A paper base material for a fibrous casing base material, comprising natural fibers and a paper strength agent, wherein the paper strength agent comprises both a cationic strength agent and an anionic strength agent, both internally and externally added. 2. The paper base material for a fibrous casing base material described in 1., wherein the blending amount of hemp pulp relative to the total natural fibers is 40 mass% or more. 3. The paper base material for a fibrous casing base material described in 1. or 2., wherein the natural fibers have an overall freeness (Canadian standard freeness) of 450 ml to 700 ml. 4. The paper base material for a fibrous casing base material described in any one of 1. to 3., wherein the wet tensile strength against a 5% sodium hydroxide aqueous solution measured in accordance with JIS P8135:1998 is 3.0 N / 15 mm or more. 5. The paper base material for a fibrous casing base material described in 1. to 4., wherein the contact angle after 20 seconds of 4 μl of ion-exchanged water being dropped thereon is 60° or less. The paper substrate for a fibrous casing substrate according to any one of the preceding claims.

[0007] According to the present invention, it is possible to provide a paper base material for a fibrous casing base material that does not require pre-impregnation with a viscose liquid and has sufficient wet strength and alkali resistance during viscose coating processing.

[0008] The paper base material for the fibrous casing base material of the present invention (hereinafter also referred to as paper base material) contains natural fibers and a paper strength agent, and both a cationic strength agent and an anionic strength agent are added as paper strength agents by internal and external addition. The paper base material of the present invention can be produced by adding the cationic strength agent and the anionic strength agent to a pulp slurry containing natural fiber pulp, making the resulting paper into a papermaking raw material, and further adding the cationic strength agent and the anionic strength agent by size press coating, and can be produced using a papermaking machine used in known papermaking applications.

[0009] (Natural Fibers) Natural fibers include wood pulps such as softwood pulp and hardwood pulp; bast fibers such as flax, ramie, jute, kenaf, hemp, paper mulberry, and mitsumata; hard fibers such as bagasse, bamboo, and esparto; seed fiber fibers such as cotton pulp; and non-wood pulps such as leaf sheath and leaf fibers such as abaca and sisal. One or more of these cellulosic fibers can be used. To ensure the wet strength and breathability required for the paper base, hemp pulp and softwood pulp, which have relatively long fiber lengths, are preferred as natural fibers. A mixture of these fibers can also be used. The amount of hemp pulp relative to the total natural fibers is preferably 40% by mass or more. If the amount of hemp pulp is less than 40% by mass, the paper base may lack sufficient wet strength and alkali resistance during viscose coating, resulting in breakage. The amount of hemp pulp relative to the total natural fibers is more preferably 45% by mass or more. As the hemp pulp, any pulp used in the papermaking field, such as flax, ramie, jute, kenaf, hemp, abaca, sisal, etc., can be used without any particular limitation.

[0010] The paper base material of the present invention may also contain non-natural fibers such as regenerated cellulose fibers, provided that the effects of the present invention are not impaired. However, the proportion of natural fibers relative to all papermaking fibers is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, even more preferably 99% by mass or more, and most preferably 100% by mass. In the present invention, the Canadian Standard Freeness (hereinafter also referred to as freeness) of the natural fibers used alone, measured in accordance with JIS P8121-2:2012, is preferably 450 ml to 800 ml. Furthermore, the freeness of all papermaking fibers contained in the paper stock (when two or more natural fibers are used in combination, this is the freeness after mixing the natural fibers in a predetermined ratio; hereinafter also referred to as total freeness) is preferably 450 ml to 700 ml. If the total freeness is less than 450 ml, the breathability may be impaired, which may result in poor viscose impregnation during viscose coating. If the total freeness is higher than 700 ml, the paper base may break due to insufficient wet strength and alkali resistance during viscose coating processing on the paper base.

[0011] (Paper Strength Agent) The paper base material of the present invention is provided with both a cationic paper strength agent and an anionic paper strength agent by internal and external addition. Furthermore, a neutral paper strength agent can also be used in combination. Commonly used paper strength agents include polyamide epichlorohydrin resins, polyamine epichlorohydrin resins, polyamide polyamine epichlorohydrin resins, melamine formaldehyde resins, urea formaldehyde resins, glyoxal-modified polyacrylamides, Hoffman-modified polyacrylamides, anionic-modified polyacrylamides, dialdehyde starch, polyethyleneimine, and epoxidized polyamides. These agents can be used singly or in combination, without any restrictions on whether they are cationic or anionic.

[0012] The paper base material of the present invention contains at least four types of paper strength agents: cationic and anionic internal strength agents, and cationic and anionic external strength agents. The internal strength agents and external strength agents may be the same or different. As the internal strength agents, it is preferable to use a cationic polyamine epichlorohydrin resin as the cationic strength agent and an anionic polyacrylamide resin as the anionic strength agent, since this can uniformly improve the wet resistance of the entire paper base material. Furthermore, it is preferable to use a cationic polyamide epichlorohydrin resin as the cationic strength agent and an anionic polyacrylamide resin as the anionic strength agent, since this improves wettability with the viscose liquid during the viscose coating process and prevents a decrease in wet strength due to penetration of the viscose liquid. The amount of each strength agent is not particularly limited, but is preferably 0.1% by mass or more and 5.0% by mass or less, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, and more preferably 4.0% by mass or less, and even more preferably 3.0% by mass or less, relative to the natural fiber. The amount of all strength agents is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less, relative to the natural fiber. The amounts of each strength agent may be the same or different.

[0013] (Manufacturing Method) The paper base material of the present invention can be manufactured using a method known in the art for papermaking. Specifically, it can be manufactured using a Fourdrinier paper machine, a cylinder paper machine, a short wire paper machine, a twin-wire paper machine, an on-top hybrid paper machine, a gap former machine, etc. The internal paper strength enhancer is incorporated into the papermaking raw materials, while the external paper strength enhancer can be applied to the base paper by impregnation processing using a mangle, size press, etc., or surface coating using a gate roll coater, blade coater, bar coater, gravure coater, die coater, curtain coater, spray coater, etc., as appropriate.

[0014] The basis weight of the paper base material is 15 g / m 2 30g / m or more 2 A basis weight of 15 g / m or less is preferred.2 If the basis weight is less than 30 g / m, sufficient alkali resistance may not be obtained. 2 If the dry tensile strength is higher than this, the viscose impregnation may be poor during the viscose coating process. The paper substrate preferably has a dry tensile strength in the machine direction of 7.0 N / 15 mm or more, measured in accordance with JIS P8113:2006, and a wet tensile strength in the machine direction of 4.0 N / 15 mm or more, measured in accordance with JIS P8135:1998. If the tensile strength (dry, wet) of the paper substrate is less than the above-mentioned values, the paper substrate may break during the viscose coating process. The dry tensile strength in the machine direction of the paper substrate is more preferably 10.0 N / 15 mm or more, and even more preferably 14.0 N / 15 mm or more. The wet tensile strength in the machine direction of the paper substrate is more preferably 4.5 N / 15 mm or more, and even more preferably 5.0 N / 15 mm or more. The ratio of the wet tensile strength in the machine direction of the paper substrate (machine direction / machine direction) is preferably 50% or more. If this ratio is less than 50%, the bag may break during the meat stuffing process. This ratio is more preferably 60% or more, and even more preferably 70% or more.

[0015] The alkali resistance of a paper substrate can be evaluated by measuring the tensile strength (longitudinal direction) after immersion in a 5% sodium hydroxide aqueous solution instead of water for 30 seconds using a method in accordance with JIS P8135:1998. The alkali resistance of a paper substrate is preferably such that the tensile strength is 3.0 N / 15 mm or more. If this value is less than 3.0 N / 15 mm, the paper substrate may break during viscose coating. The tensile strength is more preferably 3.1 N / 15 mm or more, and even more preferably 3.2 N / 15 mm or more.

[0016] The paper substrate preferably has a contact angle of 60° or less 20 seconds after 4 μl of ion-exchanged water is dropped onto it. If this contact angle exceeds 60°, the wettability of the coating liquid during the viscose coating process may be insufficient, making it difficult to achieve uniform coating. This contact angle is more preferably 56° or less, and even more preferably 52° or less.

[0017] Example 1: 750 ml of hemp pulp (abaca pulp, produced in Ecuador) and 500 ml of hemp pulp (abaca pulp, produced in the Philippines) with a Canadian Standard Freeness (CSF) were separately prepared. 50 parts by mass of each pulp was mixed to obtain a natural fiber slurry with a total freeness of 625 ml. To this slurry, 0.7% solids of an anionic paper strength agent (polyacrylamide resin (Hercobond 2515AP, 15% nonvolatile content, pH 6.5-7.5 / 25°C, manufactured by Riken Green Co., Ltd.) based on the dry weight of the natural fibers were added, and 0.65% solids of an aqueous aluminum sulfate solution (liquid aluminum sulfate, 27% nonvolatile content, pH 2.1 / 20°C, manufactured by Asahi Chemical Industry Co., Ltd.) based on the dry weight of the natural fibers were added with stirring. To this, a cationic paper strength agent, polyamine epichlorohydrin resin (WS4010, nonvolatile content 20%, pH 2.5-5.0, manufactured by Seiko PMC Corporation) activated with caustic soda was added while stirring in an amount of 1.0% in solid content relative to the natural fiber (dry mass) to prepare a papermaking raw material. Using this papermaking raw material, a papermaking machine with a target basis weight of 18 g / m was prepared. 2 Next, a cationic paper strength agent, polyamide epichlorohydrin resin (WS4035, nonvolatile content 25%, pH 2.5 to 4.5, manufactured by Seiko PMC Corporation) and an anionic paper strength agent, polyacrylamide resin (Hercobond 2515AP, manufactured by Riken Green Co., Ltd.) were mixed in water at a solids ratio of 8:13 to prepare a 2.1% aqueous solution. This external coating solution was then impregnated and coated onto the base paper using a Hishira copier, and the paper substrate was then dried at a drying temperature of 105°C for 2 minutes to obtain a paper base material.

[0018] (Example 2) A paper base material was obtained in the same manner as in Example 1, except that a natural fiber slurry having a total freeness of 675 ml was used, which was obtained by mixing 750 ml of hemp pulp (abaca pulp, produced in Ecuador) and 500 ml of hemp pulp (abaca pulp, produced in the Philippines) in a mass ratio of 70:30, having a Canadian Standard Freeness (CSF).

[0019] (Example 3) Hemp pulp (abaca pulp, produced in Ecuador) with a Canadian Standard Freeness (CSF) of 750 ml and 500 ml of bleached softwood kraft pulp (NBKP) were separately prepared. 50 parts by mass of each of the pulps were mixed to obtain a natural fiber slurry with an overall freeness of 625 ml. A paper base was obtained in the same manner as in Example 1, except that this natural fiber slurry was used. (Example 4) A paper base with a target basis weight of 21 g / m 2 A paper base was obtained in the same manner as in Example 3, except that only NBKP having a Canadian Standard Freeness (CSF) of 500 ml was used as the natural fiber.

[0020] (Comparative Example 1) A paper base material was obtained in the same manner as in Example 1, except that no internally added paper strength agent or fixing agent was added. (Comparative Example 2) A paper base material was obtained in the same manner as in Example 1, except that no externally added paper strength agent was applied. (Comparative Example 3) A paper base material was obtained in the same manner as in Example 3, except that no externally added paper strength agent was applied.

[0021] The obtained paper substrate was evaluated as follows. The results are shown in Table 1. (Evaluation Method) (1) Basis Weight Measured in accordance with JIS P 8124:2011. (2) Thickness Measured in accordance with JIS P 8118:2014. (3) Density Calculated from the basis weight and thickness. (4) Tensile Strength Dry tensile strength was measured in accordance with JIS P8113:2006. Wet tensile strength was measured in accordance with JIS P8135:1998.

[0022] (5) Alkali Resistance: Using a method in accordance with JIS P8135:1998, samples were immersed in a 5% aqueous sodium hydroxide solution instead of water for 30 seconds, and the tensile strength was measured and evaluated according to the following criteria: ○: 3.0 N / 15 mm or more △: More than 2.5 N / 15 mm and less than 3.0 N / 15 mm ×: 2.5 N / 15 mm or less (6) Wettability (Contact Angle): Using a dynamic contact angle absorption tester (FIBRO 1100 DAT MKII: manufactured by FIBRO System AB), 4 μl of ion-exchanged water was dropped onto the sample measurement surface, and the contact angle was measured 20 seconds after the drop. The average value of three measurements was calculated and evaluated according to the following criteria: ○: 60° or less ×: More than 60°

[0023]

[0024] Results The paper base materials obtained in Examples 1 to 5 of the present invention were excellent in wet strength, alkali resistance, and wettability, making them suitable for use as fibrous casing base materials. In particular, the paper base materials obtained in Examples 1 to 4, which contained hemp pulp, were superior in alkali resistance. The paper base material obtained in Comparative Example 1, which did not contain an internal paper strength enhancer, had a low tensile strength value after alkali immersion and was poor in alkali resistance. The paper base materials obtained in Comparative Examples 2 and 3, which did not contain an external paper strength enhancer, had a large contact angle and were poor in wettability when coated with viscose liquid.

Claims

1. A paper base material for a fibrous casing base material, comprising natural fibers and a paper strength enhancer, wherein the paper strength enhancer includes both a cationic paper strength enhancer and an anionic paper strength enhancer, both of which are added internally and externally.

2. The paper base material for a fibrous casing base material according to claim 1, characterized in that the amount of hemp pulp relative to the total natural fibers is 40% by mass or more.

3. The paper base material for a fibrous casing base material according to claim 1 or 2, characterized in that the total freeness (Canadian standard freeness) of the natural fibers is 450 ml or more and 700 ml or less.

4. The paper base material for a fibrous casing according to claim 1 or 2, characterized in that the wet tensile strength in a 5% aqueous sodium hydroxide solution measured in accordance with JIS P8135:1998 is 3.0 N / 15 mm or more.

5. The paper base material for a fibrous casing according to claim 1 or 2, characterized in that the contact angle after 20 seconds from the application of 4 μl of ion-exchanged water is 60° or less.