Microporous graphene oxide sheet, dispersion and membrane including the same

The method of producing microporous graphene oxide sheets through a carbon-zeolite composite process addresses the challenges of uniformity and scalability, enabling the creation of high-performance membranes with uniform nanopores for efficient separation and filtration.

KR103044983B1Active Publication Date: 2026-11-06KOREA ADVANCED INST OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020220152964
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-15
Publication Date
2026-11-06
Estimated Expiration
2042-11-15

AI Technical Summary

Technical Problem

Existing methods for manufacturing microporous graphene materials face challenges in achieving uniform pore size, high conductivity, and scalability due to issues with pore formation, stacking, and exfoliation, making them unsuitable for high-quality membranes.

Method used

A method involving the use of a carbon-zeolite composite, followed by oxidation and zeolite removal, and subsequent sonication in a solvent, allows for the production of microporous graphene oxide sheets with uniform nanopores and single-atom thickness, enabling their dispersion and layer-by-layer stacking to form defect-free membranes.

Benefits of technology

The resulting microporous graphene oxide sheets exhibit uniform pore size, regular spacing, and high density, facilitating mass production of high-performance membranes suitable for selective permeation and applications in separation and filtration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022121686642-PAT00001_ABST
    Figure 112022121686642-PAT00001_ABST
Patent Text Reader

Abstract

The invention relates to a microporous graphene oxide sheet having an average pore size of 0.1 nm to 2 nm, a pore spacing of 0.3 nm to 10 nm, a standard deviation of the pore spacing of 5 nm or less, and a thickness of 2 nm or less, a method for manufacturing the same, a dispersion containing the same, and a membrane containing a stack of the microporous graphene oxide sheets.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This relates to a microporous graphene oxide sheet, a dispersion containing the same, and a membrane. Background Technology

[0002] Graphene-based two-dimensional carbon materials are attracting attention in various fields, such as separators, electrochemical energy storage, and transistors, due to their unique physical and chemical stability. However, graphene is a densely arranged sp² 2 Since graphene is composed of a hybrid carbon framework and is impermeable to all molecules and ions, structural design that imparts permeability to target substances, such as by forming pores or channels, is essential for using graphene as a separation membrane material.

[0003] Conventional methods for manufacturing microporous graphene with nanometer-sized pores can be broadly classified into top-down and bottom-up methods. The top-down method involves forming defects in graphene using ion bombardment, UV, or plasma; however, this approach makes it impossible to obtain pores of uniform size, and the pore density is approximately 1 pore / 100 nm. 2 There are limitations, such as low conductivity and the difficulty of mass production. Additionally, there is an oxidative etching method that treats graphene with hydrogen peroxide; while this can form many pores, it results in the irregular formation of pores of non-uniform sizes and has limitations due to low conductivity caused by numerous defects. The bottom-up fabrication method involves synthesizing a precursor and then polymerizing it into microporous graphene; however, the process from precursor synthesis to graphene manufacturing is complex and uneconomical, and the defect density is too high to be used for large-area membranes.

[0004] Non-patent literature 1, etc., presents a method for manufacturing microporous carbon with a three-dimensional structure by depositing carbon onto a three-dimensional zeolite framework and then selectively removing the zeolite. Subsequently, studies on carbon materials using three-dimensional zeolite templates were presented, which involved synthesizing carbon materials with three-dimensional structures such as ribbon or tube shapes. However, these carbon materials have high aspect ratios and have limitations in being manufactured into membranes due to their three-dimensional shape.

[0005] In addition, even when manufacturing a microporous carbon material with a two-dimensional structure, strong π-π forces act between carbon sheets with an aromatic framework, resulting in a semi-permanently stacked form. To manufacture this into a defect-free membrane, a preliminary step is required to exfoliate it into single sheets of single-atom thickness and disperse them in a solution. However, because the forces between the sheets are too strong, exfoliation is difficult, and there is a problem with the sheets not dispersing in the solution; therefore, the introduction of a technology to weaken the forces between the carbon sheets is essential.

[0006] [Non-patent literature 1] T. Kyotani et al., Chem. Mater. 13, 4413 (2001) The problem to be solved

[0007] The present invention provides a microporous graphene oxide sheet having a single-atom thickness with regularly spaced nanopores of uniform size, a method for manufacturing the same, and a dispersion in which the sheets are dispersed. Furthermore, the present invention provides a membrane comprising a laminate in which the microporous graphene oxide sheets are interlocked and stacked in layers, and a method for manufacturing the same. means of solving the problem

[0008] In one embodiment, a microporous graphene oxide sheet is provided having an average pore size of 0.1 nm to 2 nm, a spacing between pores of 0.3 nm to 10 nm, a standard deviation of the spacing between pores of 5 nm or less, and a thickness of 2 nm or less.

[0009] In one embodiment, a method for manufacturing a microporous graphene oxide sheet is provided, comprising preparing a carbon-zeolite composite by depositing carbon on a zeolite template having a two-dimensional pore structure, oxidizing the carbon-zeolite composite, removing the zeolite from the oxidized carbon-zeolite composite to obtain microporous graphene oxide, and sonicating the obtained product in a solvent to obtain a microporous graphene oxide sheet having a thickness of 2 nm or less.

[0010] In one embodiment, a dispersion is provided comprising a solvent and a microporous graphene oxide sheet dispersed in the solvent and having a thickness of 2 nm or less.

[0011] In one embodiment, a membrane comprising a stack of the microporous graphene oxide sheets is provided.

[0012] In one embodiment, a method for manufacturing a membrane is provided, comprising manufacturing a microporous graphene oxide sheet by the method described above and then laminating the sheet onto a substrate. Effects of the invention

[0013] A microporous graphene oxide sheet according to one embodiment is a microporous carbon material having uniform pore size, regular spacing between pores, and high pore density, and is an exfoliated graphene oxide sheet with a single-atom level thickness of 2 nm or less, which can exist in a dispersed state in a solution. These microporous graphene oxide sheets can be stacked layer by layer to interlock with each other to manufacture a membrane free of defects or pinholes. Furthermore, the microporous graphene oxide sheet, the dispersion containing it, and the membrane can be manufactured using a solution process, making it advantageous and economical for mass production. The membrane has excellent performance in selectively permeating target substances and can be used as various separation membranes or filters. In addition, the microporous graphene oxide sheet can be utilized in various fields, such as energy storage materials like electrode active materials, electronic materials like quantum dots, chemical detectors, and various catalysts. Brief explanation of the drawing

[0014] Figure 1 is a schematic diagram illustrating the shape of a membrane manufactured by stacking a carbon material that is not exfoliated (left) and an exfoliated carbon material (right) with a single atomic thickness. FIG. 2 is a schematic diagram illustrating a method for manufacturing a microporous graphene oxide sheet according to one embodiment and subsequently manufacturing a membrane. Figure 3 shows an image (top) of microporous graphene prepared in Reference Example 1 taken with an Atomic Force Microscopy (AFM) and a graph (bottom) analyzing its thickness. Figure 4 is a transmission electron microscope (TEM) image of the surface of the microporous graphene oxide sheet prepared in Example 1. Figure 5 is an atomic force microscope image (left) of the microporous graphene oxide sheet prepared in Example 1, and a graph (right) analyzing the thickness at positions 1 and 2. Figure 6 is a photograph of the membrane prepared in Example 1. Figure 7 is a scanning electron microscope (SEM) image of the surface of the carbon-coated portion of the membrane prepared in Example 1. Figure 8 is a scanning electron microscope image of a cross-section of the membrane prepared in Example 1. Figure 9 is a graph showing the organic solvent nanofiltration characteristics of the membrane prepared in Example 1, and the rejection rate according to the permeability of methanol and the molecular weight of organic dye molecules. Figure 10 is a graph showing the filtration rate of organic dye molecules and methanol permeability, comparing the performance of previously reported organic solvent nanofiltration membranes with the membrane prepared in Example 1. Specific details for implementing the invention

[0015] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0016] In the following, "combinations thereof" means mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.

[0017] The terms “include,” “have,” or “have,” etc., shall be understood as intending to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and shall not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0018] In the drawing, the thickness is enlarged to clearly represent various layers and regions. When a part such as a layer, film, region, or plate is described as being "on" or "on" another part, this includes not only cases where it is "immediately on" another part, but also cases where there is another part in between. Conversely, when a part is described as being "immediately on" another part, it means that there is no other part in between. Furthermore, when observed in a plan view, the term "layer" includes not only shapes formed on the entire surface but also shapes formed on a part of the surface.

[0019] Here, “or” is not interpreted in an exclusive sense; for example, “A or B” is interpreted to include A, B, A+B, etc.

[0020] Microporous graphene oxide sheet

[0021] In one embodiment, a microporous graphene oxide sheet is provided having an average pore size of 0.1 nm to 2 nm, a spacing between pores of 0.3 nm to 10 nm, a standard deviation of the spacing between pores of 5 nm or less, and a thickness of 2 nm or less.

[0022] The graphene oxide sheet described above can be described as an exfoliated graphene oxide sheet having a single atomic thickness. As shown in the left image of FIG. 1, even if a two-dimensional microporous carbon material is successfully manufactured, if it is not exfoliated to a single atomic thickness, it is difficult to stack the layers interlock during manufacturing into a membrane, and defects or pinholes may occur within the structure, making it impossible to manufacture a high-quality membrane. On the other hand, as shown in the right image of FIG. 1, according to one embodiment, graphene oxide sheets exfoliated to a single atomic thickness can form a membrane with a well-interlocked structure in a layer-by-layer assembly. Since such a membrane is free of defects or pinholes within the structure, it can exhibit excellent separation performance for target materials and high physical and chemical stability.

[0023] A microporous graphene oxide sheet according to one embodiment has a thickness of 2 nm or less, for example, 1.5 nm or less, 1 nm or less, or less than 1 nm, and for example, 0.1 nm to 2 nm, 0.1 nm to 1.5 nm, 0.3 nm to 1 nm, or 0.34 nm to 2 nm. A sheet having such a thickness can be interpreted as a single atomic layer, or a sheet having layers within 5 layers, or layers within 3 layers.

[0024] The lateral dimensions of the microporous graphene oxide sheet, i.e., the width and length, may be approximately 50 nm to 1,000 nm. In addition, the area of ​​the microporous graphene oxide sheet is 2,500 nm. 2 to 1,000,000 nm 2 It could be.

[0025] The microporous graphene oxide sheet may have an atomic ratio of oxygen to carbon of 0.1 to 1.0, for example, 0.2 to 0.9, 0.3 to 0.8, or 0.4 to 0.7. The graphene oxide sheet may be partially oxidized or completely oxidized graphene. Additionally, the microporous graphene oxide sheet may contain 10% to 60% by weight of oxygen relative to 100% by weight of the microporous graphene oxide sheet, for example, 25% to 55% by weight, or 30% to 50% by weight of oxygen. Such graphene oxide sheets may be dispersed in a solution, making them easily applicable to manufacturing processes and application processes.

[0026] In addition, the microporous graphene oxide sheet according to one embodiment is characterized by having uniform pore size, regular spacing between pores, and high pore density. While many porous graphene-based carbon materials have been previously reported that have non-uniform pore size, irregular pore distribution, or low pore density, these materials are unsuitable for use as high-quality membranes and are generally uneconomical and difficult to mass-produce. On the other hand, the microporous graphene oxide sheet according to one embodiment has nano-pores of uniform size existing regularly and at a high density, making it possible to use it as a high-quality membrane. Furthermore, since it is possible to perform a solution process, it has the advantages of a simple, economical manufacturing method and the ability to mass-produce.

[0027] Here, microporous can mean having pores of about 2 nm or less. That is, micro-pores can mean pores having a size of about 2 nm or less.

[0028] A microporous graphene oxide sheet according to one embodiment may be a graphene oxide sheet having pores of a size of 0.1 nm to 2 nm. The average size of the pores may be, for example, 0.1 nm to 1.9 nm, 0.1 nm to 1.8 nm, 0.1 nm to 1.7 nm, 0.1 nm to 1.6 nm, 0.1 nm to 1.5 nm, 0.1 nm to 1.4 nm, 0.1 nm to 1.3 nm, 0.1 nm to 1.2 nm, 0.1 nm to 1.1 nm, 0.2 nm to 1.0 nm, 0.3 nm to 0.9 nm, or 0.4 nm to 0.8 nm. When the average size of the pores satisfies these ranges, the microporous graphene oxide sheet is advantageous for selectively permeating molecules or ions and can be utilized in various fields.

[0029] The above pore is a two-dimensional pore and may be in the shape of a circle, ellipse, polygon, etc., and, for example, may be substantially close to a circle. The size of the above pore may refer to the diameter if the pore is circular, and may refer to the longest length among the lengths corresponding to the diameter or the length of the longest axis if the pore is not circular. In addition, the size of the above pore may be measured through an electron microscope image, such as a scanning electron microscope or a transmission electron microscope. The above average size may be the arithmetic mean of the sizes measured in the electron microscope image. For example, the average size of the pore can be derived by measuring the sizes of approximately 50 random pores in the electron microscope image and calculating their arithmetic mean.

[0030] A microporous graphene oxide sheet according to one embodiment has very uniform pore sizes. For example, the standard deviation of the average pore size may be 1 nm or less, and may be, for instance, 0.9 nm or less, 0.8 nm or less, 0.7 nm or less, 0.6 nm or less, 0.5 nm or less, 0.4 nm or less, 0.3 nm or less, 0.2 nm or less, 0.1 nm or less, 0.09 nm or less, or 0.08 nm or less, or may be 0.001 nm or more, or 0.01 nm or more. When the standard deviation of the average pore size is small in this way, that is, when the pore size is very uniform, the performance of selectively permeating molecules or ions is excellent, and accordingly, it is advantageous for application to various membranes or electrode materials.

[0031] A microporous graphene oxide sheet according to one embodiment has pore spacing that is not too narrow or too far apart, but within an appropriate range, and the spacing is very regular. Specifically, the average spacing between pores is 0.3 nm to 10 nm, and the standard deviation thereof is 5 nm or less. Here, the spacing between pores may refer to the distance from the center of a pore to the center of an adjacent pore. The average spacing between pores may be the arithmetic mean of the spacing measured by electron microscope images, etc. For example, the average spacing between pores can be derived by measuring the spacing between approximately 50 randomly selected pores in an electron microscope image and calculating their arithmetic mean and standard deviation. Alternatively, the spacing between pores may be measured through X-ray diffraction (XRD).

[0032] The spacing between the pores may be, for example, 0.3 nm to 10 nm, 0.3 nm to 9 nm, 0.3 nm to 8 nm, 0.3 nm to 7 nm, 0.3 nm to 6 nm, 0.4 nm to 5 nm, 0.5 nm to 4 nm, 0.6 nm to 3 nm, 0.8 nm to 2 nm, or 1.0 nm to 1.5 nm. A microporous graphene oxide sheet having a spacing between pores that satisfies these ranges has an appropriate pore density, is effective in selectively permeating various molecules or ions, and is therefore advantageous for application in various fields.

[0033] The standard deviation for the interpore spacing may be, for example, 5 nm or less, 4 nm or less, 3 nm or less, 2 nm or less, 1 nm or less, 0.5 nm or less, 0.1 nm or less, or 0.08 nm or less, or 0.001 nm or more, or 0.01 nm or more. When the standard deviation for the interpore spacing is small in this way, it means that the spacing between pores is very regular, and such graphene oxide sheets are effective in selectively permeating molecules or ions, so they can be used in various fields such as separators or electrode materials.

[0034] The above microporous graphene oxide sheet can exhibit a high pore density, for example, a pore density of 10 pores / 100 nm 2 Up to 100 pores / 100 nm 2 It can be, for example, 20 to 100 pores / 100 nm 2 , 30 to 100 pores / 100 nm 2 , 40 to 90 pores / 100 nm 2 , or 50 to 80 pores / 100 nm 2It is possible. If the pore density satisfies this range, the graphene oxide sheet is effective for selectively permeating molecules or ions and is suitable for application in various separation membranes or electrode materials.

[0035] The microporous graphene oxide sheet may exhibit peaks in X-ray spectroscopy (XRD) at 2θ values ​​of 7.2° and / or 7.6°. The interlayer spacing (d-spacing) at 2θ values ​​of 7.2° and 7.6° may be 1.23 nm and 1.16 nm, respectively. These peaks demonstrate that nanopores of uniform size are regularly formed in the graphene oxide sheet.

[0036] The above-mentioned microporous graphene oxide sheet has many edge sites, and accordingly, it is possible to introduce various functional groups. Depending on the type and amount of functional groups introduced, the size of effective pores and the polarity of the surface can be controlled.

[0037] A microporous graphene oxide sheet according to one embodiment may be doped with sulfur, nitrogen, or a combination thereof. Here, the doping amount may be 0.1 wt% to 20 wt% with respect to 100 wt% of the microporous graphene, for example, 1 wt% to 10 wt%. That is, the microporous graphene oxide sheet may contain 0.1 to 20 wt% of nitrogen and 0.1 to 20 wt% of sulfur. By doping the microporous graphene oxide sheet with sulfur, nitrogen, or a combination thereof, the effective pores may be reduced and the surface polarity may be increased. Conversely, the edge sites of the microporous graphene oxide sheet may be substituted with hydrogen, in which case the effective pores may be increased and the surface polarity may be reduced. It is possible to adjust the pore size and surface polarity, etc., in various ways to suit the desired characteristics in the application field.

[0038] Method for manufacturing microporous graphene oxide sheets

[0039] In one embodiment, a method for manufacturing a microporous graphene oxide sheet is provided, comprising preparing a carbon-zeolite composite by depositing carbon on a zeolite template having a two-dimensional pore structure, oxidizing the carbon-zeolite composite, removing the zeolite from the oxidized carbon-zeolite composite to obtain microporous graphene oxide, and sonicating the obtained product in a solvent to obtain a microporous graphene oxide sheet having a thickness of 2 nm or less. According to the manufacturing method, it is possible to manufacture graphene oxide with uniform pore size, regular inter-pore spacing, and high pore density, and it is possible to manufacture a microporous graphene oxide sheet with a single atomic layer thickness. Furthermore, the manufacturing method is capable of a solution process, making it simple, economical, and capable of mass production.

[0040] In the above manufacturing method, it is possible to obtain a two-dimensional graphene material having uniform nanopores by removing the zeolite template from a carbon-zeolite composite using a zeolite template with a two-dimensional pore structure. However, the two-dimensional graphene obtained in this way has a thickness of several nanometers to tens of nanometers and has a structure in which more than 10 single atomic layers are stacked. Strong π-π forces act between carbon sheets having an aromatic framework, so the sheets are manufactured in a semi-permanently stacked form.

[0041] However, as mentioned above, such two-dimensional stacked structures are prone to defects or pinholes when manufactured into membranes. Therefore, to produce membranes or the like, it is essential to exfoliate the microporous two-dimensional graphene stack into single-atom-thick sheets. It can be said that the success of membrane manufacturing is determined by whether exfoliation is possible. However, because the attractive forces between the stacked sheets are too strong, exfoliation is impossible using the conventional method of dispersing microporous graphene in a solvent and applying sonication. If strong energy exceeding the π-π attractive force is provided—for example, when horn-type ultrasonication is applied—a problem arises where the graphene sheets split during exfoliation due to the excessive energy.

[0042] In one embodiment, a partially oxidized graphene stack was obtained by preparing a zeolite-carbon composite, performing an oxidation treatment, and then removing the zeolite template, and the stack was successfully exfoliated into single-atom-thick microporous graphene oxide sheets by sonicating it in a solution. When the zeolite-carbon composite is oxidized, oxygen functional groups such as O, OH, and COOH are formed in the carbon layer, and due to their electrostatic repulsion, the zeolite can be removed and then exfoliated into single-atom-thick graphene oxide sheets solely through sonicating. The oxidation treatment can be carried out using an oxidation solution in a low-irritant manner, the zeolite removal can also be performed using a leaching solution, and the sonicating treatment does not require the use of high energy; thus, the entire process can be carried out as a mild chemical / physical treatment, and is simple and economical, making it advantageous for mass production.

[0043] In the above manufacturing method, the zeolite template is characterized by having a two-dimensional pore structure. Since the diffusion of the carbon precursor is disadvantageous in a two-dimensional pore structure compared to a three-dimensional pore structure, it is important to select a zeolite template when synthesizing two-dimensional microporous graphene. That is, for uniform carbon deposition, it is necessary to use a two-dimensional zeolite template having micropores of an appropriate size.

[0044] The zeolite template used in one embodiment has a two-dimensional pore structure, and the pores may have a size of 10 memberd-rings (MR) or larger. When using a zeolite template having two-dimensional pores smaller than a 10 memberd-ring, sp 2 Hybridized carbon bonds can be disadvantageous for growth, but conversely, if a zeolite template having two-dimensional pores larger than 10-membered rings is used, microporous graphene with regular nanopores can be effectively synthesized.

[0045] In the above zeolite template, the size of the two-dimensional pores may be 10-sided rings or more, 11-sided rings or more, or 12-sided rings or more, and may be 30-sided rings or less, or 20-sided rings or less. When using a zeolite template in which the pore size satisfies the above range, a microporous graphene oxide sheet with a two-dimensional structure can be successfully synthesized.

[0046] Specifically, the above zeolite mold is, * CTH, EWS, IWV, MWW, NES, OKO, * It may be at least one selected from the group consisting of PCS, SEW, SFG, SFS, SSF, TER, USI, and UTL. That is, when using a zeolite template of the structure exemplified, microporous graphene oxide sheets can be effectively synthesized.

[0047] The carbon may be deposited, for example, by chemical vapor deposition. For example, carbon may be deposited by supplying a carbon precursor comprising acetylene, ethylene, propylene, ethanol, or a combination thereof to the zeolite template. In this case, the carbon precursor may be supplied together with helium gas. That is, the carbon deposition may be performed in a helium gas atmosphere. In addition, the carbon deposition may be carried out, for example, in a temperature range of 573 K to 1273 K and for 1 hour to 48 hours.

[0048] Meanwhile, when depositing carbon onto a zeolite mold, a nitrogen precursor and / or a sulfur precursor may be additionally supplied. In this case, it is possible to manufacture microporous graphene oxide sheets doped with nitrogen and / or sulfur.

[0049] The nitrogen precursor may include, for example, ammonia, methylamine, ethylamine, propylamine, butylamine, acetonitrile, pyrrole, pyridine, or a combination thereof. The sulfur precursor may include hydrogen sulfide, thiophene, thiophenol, mercaptoethanol, thioacetic acid, methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, or a combination thereof. Further supplying the nitrogen precursor and / or sulfur precursor may be in a content range such that the content of each nitrogen and / or sulfur is 0.1 to 20 weight% with respect to 100 weight% of the microporous graphene oxide sheet.

[0050] After depositing carbon on the zeolite mold, a heat treatment may be optionally performed. This can be described as a type of carbonization process. The heat treatment may be performed, for example, in a temperature range of 773K to 1323K, for 30 minutes to 10 hours, or for 30 minutes to 5 hours, and may be performed in a helium atmosphere.

[0051] Subsequently, a step of oxidizing the prepared carbon-zeolite composite is carried out. Through this step, it is possible to exfoliate it into a single-atom-thickness graphene oxide sheet. The method of oxidation is not particularly limited, but, for example, a mild oxidation method using an oxidation solution may be used. That is, the carbon-zeolite composite can be oxidized by adding the carbon-zeolite composite and an oxidizing agent to a solvent and mixing them. Here, the solvent is referred to as the first solvent to distinguish it from the solvent in the sonication step described later. The carbon-zeolite composite may be dispersed in the first solvent, and an oxidizing agent may be added thereto. The oxidizing agent may include, for example, KMnO4, H2O2, HNO3, NaNO3, H2SO4, or a combination thereof, and may be an aqueous solution containing such. The first solvent may be, for example, a water-based solvent, and may include water, an alcohol-based solvent, or a combination thereof.

[0052] Subsequently, it is possible to selectively remove only the zeolite template by placing the oxidized carbon-zeolite composite into a leaching solution and stirring. The leaching solution may include, for example, HCl, NaOH, KOH, HF, NaF, NH4F, AlF3, or a combination thereof. The leaching solution may be an aqueous solution containing at least one of the exemplified compounds in an amount of 0.1% to 5% by weight. The stirring may be carried out for, for example, 10 minutes to 120 minutes. By selectively removing the zeolite template in this way, microporous graphene oxide with uniform nanopores can be obtained. The microporous graphene oxide obtained here has a thickness of about 10 nm or more and can be described as having a structure in which more than 10 single-atom layers are stacked, and accordingly, it can be referred to as a microporous graphene oxide stack.

[0053] After separating the zeolite template by introducing a leaching solution, the precipitate is recovered by methods such as centrifugation, thereby obtaining a solvent-removed microporous graphene oxide stack. Subsequently, a drying process of the obtained product may be additionally performed optionally.

[0054] The obtained microporous graphene oxide stack can be redispersed in a solvent and then subjected to sonication. Here, the solvent may be referred to as a second solvent to distinguish it from a first solvent. The first solvent and the second solvent may be the same or different from each other. The second solvent may include, for example, N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), toluene, acetone, water, methanol, ethanol, isopropyl alcohol, dimethyl sulfoxide (DMSO), propylene glycol methyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), ethyl-3-ethoxypropionate (EEP), butyl carbitol (BC), or a combination thereof.

[0055] The above sound wave treatment may be carried out for, for example, at conditions of 20 kHz to 100 kHz for 1 hour to 20 hours. Through this process, microporous graphene oxide sheets having a thickness of 2 nm or less can be successfully exfoliated.

[0056] Microporous graphene oxide sheets, consisting of a single atomic layer or a very small number of layers, may be dispersed in the solution in which the above-mentioned sonic treatment has been performed. Optionally, after centrifugation, the supernatant may be recovered to obtain a dispersion in which microporous graphene oxide sheets having a thickness of 2 nm or less are dispersed in a solvent.

[0057] Specifically, a method for manufacturing a microporous graphene oxide sheet according to one embodiment may include: (i) preparing a carbon-zeolite composite by depositing carbon on a zeolite template having a two-dimensional pore structure; (ii) dispersing the carbon-zeolite composite in a first solvent and then oxidizing it by adding an oxidizing agent; (iii) removing the zeolite from the oxidized carbon-zeolite composite by adding a leaching solution thereto; (iv) obtaining a precipitate of microporous graphene oxide through centrifugation; (v) redispersing the obtained product in a second solvent and then ultrasonically treating it; and (vi) recovering the supernatant by centrifugation.

[0058] The finally obtained microporous graphene oxide sheet is a porous sheet with uniform pore size, regular spacing between pores, and high pore density, and is a single-atom layer sheet with a thickness of 2 nm or less. The physical properties of the microporous graphene oxide sheet, such as pore characteristics and thickness, are as described above.

[0059] Meanwhile, after obtaining a microporous graphene oxide sheet, a drying step may be included, and subsequently, oxygen (O2) or hydrogen (H2) gas treatment may be additionally performed. In this case, microporous graphene oxide in which edge sites are substituted with oxygen or hydrogen, or reduced graphene oxide, can be produced, and accordingly, the size of the effective pores and surface polarity can be appropriately controlled.

[0060] dispersion

[0061] In one embodiment, a dispersion is provided comprising a solvent and a microporous graphene oxide sheet dispersed in the solvent and having a thickness of 2 nm or less. Here, microporous means having pores of about 2 nm or less, and a thickness of 2 nm or less may mean the thickness of a single atomic layer. That is, the dispersion may be a microporous structure having nanopores of 2 nm or less, in which exfoliated graphene oxide sheets with a single atomic thickness are dispersed in a solvent. In addition, the sheets may be partially or completely oxidized graphene, and the atomic ratio of oxygen to carbon may be 0.1 to 1.0, or 0.2 to 0.9, or 0.3 to 0.8.

[0062] Various methods have been studied for synthesizing graphene-based carbon materials having a porous structure and a single atomic thickness, but most of them were not economical or impossible to mass-produce because they were not obtained in a dispersed state in a solvent. A microporous graphene oxide sheet according to one embodiment is exfoliated to a single atomic thickness with a uniform pore distribution and can be synthesized and stored in a dispersed state in a solution, making it economical, convenient, and usable in various fields, and it is possible to manufacture it into high-performance carbon materials or membranes.

[0063] The above solvent is not particularly limited but may include, for example, N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), toluene, acetone, water, methanol, ethanol, isopropyl alcohol, dimethyl sulfoxide (DMSO), propylene glycol methyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), ethyl-3-ethoxypropionate (EEP), butyl carbitol (BC), or a combination thereof.

[0064] In the above dispersion, the microporous graphene oxide sheet may, for example, have an average pore size of 0.1 nm to 2 nm, a spacing between pores of 0.3 nm to 10 nm, and a standard deviation of the spacing between pores of 5 nm or less. That is, it may be a dispersion in which microporous graphene oxide sheets, in which very small pores are distributed very regularly, are exfoliated to a single atomic layer thickness and dispersed. Detailed information regarding the pore distribution, characteristics, thickness, etc. of the microporous graphene oxide sheet is omitted as it is as described above.

[0065] Membrane

[0066] In one embodiment, a membrane comprising a stack of the microporous graphene oxide sheets is provided. The stack may be a thin film or a coating layer having a structure in which single-atom thickness microporous graphene oxide sheets are stacked layer by layer in a well-interlocked manner. Such a stack may be a high-quality lamellar structure without internal defects or pinholes.

[0067] The above membrane comprises, for example, a substrate and a carbon coating layer located on the substrate, wherein the carbon coating layer may be a stack of the aforementioned microporous graphene oxide sheets. Such a membrane can be described as a two-dimensional planar sheet-shaped TFC (Thin Film Composite) membrane. By including a carbon coating layer in which defect-free and uniform nanopores are regularly formed, the membrane exhibits excellent performance in selectively permeating various molecules and ions, and thus can be applied as a separation membrane or filter in various fields.

[0068] The thickness of the carbon coating layer may be 10 nm to 50 μm, for example 10 nm to 40 μm, 10 nm to 30 μm, 10 nm to 20 μm, 10 nm to 10 μm, 10 nm to 5 μm, 15 nm to 1 μm, or 100 nm to 900 nm, and the thickness can be appropriately adjusted according to the application.

[0069] The type of the above-mentioned substrate is not particularly limited and can be appropriately selected and used according to the application; for example, a porous substrate may be used when used as a separator. For example, the above-mentioned substrate may include glass fiber, cellulose fiber, nylon, polycarbonate, polyethersulfone, polyester, polyethylene, polypropylene, polytetrafluoroethylene, polyethylene terephthalate, polyacrylate, polyimide, polystyrene, polyethylene naphthalate, aluminum oxide, silicon oxide, or a combination thereof. As an example, the above-mentioned substrate may include nylon, PCTE (Polycarbonate Track Etched), AAO (Anodic Aluminum Oxide), or a combination thereof.

[0070] Method for manufacturing a membrane

[0071] In one embodiment, a method for manufacturing the membrane is provided. The method for manufacturing the membrane comprises obtaining a microporous graphene oxide sheet having a thickness of 2 nm or less by the method described above, and then stacking the microporous graphene oxide sheets on a substrate.

[0072] Methods for laminating microporous graphene oxide sheets on a substrate may include, but are not limited to, vacuum filtration, spin coating, doctor-blade coating, and roll-to-roll methods. For example, a membrane in which microporous graphene oxide sheets are laminated on a substrate can be manufactured by vacuum filtration of a dispersion in which microporous graphene oxide sheets are dispersed. This method of manufacturing the membrane is a solution process, which is simple, economical, and advantageous for commercialization.

[0073] FIG. 2 is a schematic diagram illustrating a method for manufacturing a microporous graphene oxide sheet according to one embodiment and subsequently manufacturing a membrane to aid understanding.

[0074] As mentioned above, even if a two-dimensional microporous carbon material is successfully manufactured, if it is not exfoliated to a single atomic thickness, it is difficult to interlock and stack layers when manufacturing a membrane, and defects or pinholes occur within the structure, making it difficult to manufacture a high-quality membrane. On the other hand, in one embodiment, a two-dimensional microporous graphene having uniform nanopores was obtained by using a zeolite template having a two-dimensional pore structure, and the microporous graphene was strategically designed to be easily separated to a single atomic layer thickness, and by stacking them on a substrate, a non-bonding membrane with interlocked layers was successfully manufactured.

[0075] Specifically, partially oxidized two-dimensional microporous graphene can be obtained by depositing carbon onto a zeolite template having a two-dimensional pore structure, oxidizing it, and then removing the template. In this oxidized graphene, electrostatic repulsion of oxygen functional groups acts, and accordingly, it is possible to easily exfoliate it into single-atom-thick microporous oxidized graphene sheets through sonication. By stacking the exfoliated sheets onto a substrate using various conventional methods such as vacuum filtration, a defect-free high-performance membrane according to one embodiment can be manufactured.

[0076] Examples, comparative examples, and evaluation examples of the present invention are described below. The following examples are merely illustrative of the present invention, and the present invention is not limited to the examples described below.

[0077] Reference Example 1

[0078] An IWV zeolite template having a two-dimensional pore structure composed of 12-membered rings (12MR) is injected into a quartz reactor and heated to 773 K while supplying helium gas. Carbon is deposited on the zeolite template by chemical vapor deposition by supplying a mixed gas of ethylene and helium (ethylene: 20 vol%) at a rate of 200 mL / min for 2 hours. Subsequently, the mixture is heated to 1273 K while flowing helium gas at a rate of 200 mL / min, and a heat treatment process is carried out for 2 hours after the temperature stabilizes. Afterward, the mixture is cooled to room temperature in a helium atmosphere to obtain a carbon-zeolite composite. The composite is stirred in an aqueous solution of 1.1 wt% HCl and 0.8 wt% HF for 1 hour to remove the zeolite template, and then dried at 373 K for 24 hours. Through this process, microporous graphene with a two-dimensional structure in which nanopores of uniform size are regularly formed is synthesized.

[0079] The microporous graphene prepared in Reference Example 1 was imaged using an atomic force microscope (AFM), and its thickness was analyzed and is shown in Fig. 3. As a result of the analysis in Fig. 3, the average thickness of the prepared graphene was confirmed to be approximately ~15 nm, which is identified as a structure consisting of about 40 stacked single-atom layers. After dispersing this microporous graphene in an NMP solvent and performing bath sonication, the π-π forces between the stacked sheets were too strong, so the sheets did not delaminate at all. Consequently, when treated with strong energy exceeding the π-π forces (e.g., horn-type ultrasonication), the problem occurred in which the delaminated graphene sheets split.

[0080] Example 1

[0081] 1. Fabrication of Microporous Graphene Oxide Sheets

[0082] 1 g of the carbon-zeolite composite prepared in Reference Example 1 is prepared and added to 100 mL of distilled water and mixed for 30 minutes. Then, 41 g of KMnO4 is added as an oxidizing agent and the mixture is mixed at 60 °C for 2 hours to carry out the oxidation treatment. Afterward, 50 mL of a 2.0 M HCl aqueous solution is added as a leaching solution and stirred at 60 °C for 2 hours, and then 50 mL of a 2.0 M HF aqueous solution is added and stirred at room temperature (25 °C) for 2 hours to remove the zeolite template. Subsequently, the mixture is centrifuged at 9000 rpm and the precipitate is recovered to obtain partially oxidized microporous graphene.

[0083] The prepared oxidized microporous graphene is redispersed in 100 mL of NMP solvent and subjected to sonication at 40 kHz for 6 hours. Afterward, the supernatant is recovered by centrifugation at 9000 rpm.

[0084] 2. Manufacture of Membranes

[0085] The obtained supernatant is vacuum filtered to form a carbon coating layer in which single-atom thickness microporous graphene oxide sheets are interlocked and stacked on a porous nylon substrate, thereby manufacturing a TFC membrane (Thin Film Composite Membrane).

[0086] Evaluation Example 1: Pore distribution and thickness analysis of graphene oxide sheets

[0087] After recovering the supernatant in Example 1, the solvent is removed and the sheet is dried at 373 K for 24 hours to obtain a microporous graphene oxide sheet.

[0088] Figure 4 is a transmission electron microscope (TEM) image of this, confirming that two-dimensional pores are formed very regularly in the obtained microporous graphene oxide sheet. Analysis of Figure 4 indicates that the pore density in the synthesized graphene oxide sheet is approximately 70 pores / 100 nm. 2 It is confirmed that...

[0089] In the TEM image of Fig. 4, about 50 random pores were selected and the size of each pore was measured to obtain an arithmetic mean of 0.68 nm, and the standard deviation of the pore size was calculated to be 0.063 nm. In addition, in the TEM image of Fig. 4, about 50 distances from the center of a pore to the center of an adjacent pore were randomly measured and the arithmetic mean was calculated to be 1.23 nm, and the standard deviation of the pore spacing was calculated to be 0.062 nm.

[0090] The left image of Fig. 5 is an atomic force microscope (AFM) image of the obtained dried microporous graphene oxide sheet. Here, the thickness of the graphene oxide sheet at positions 1 and 2 was analyzed, and the results are shown on the right side of Fig. 5. Referring to Fig. 5, the thickness of the obtained graphene oxide sheet is analyzed to be about 1 nm or less. Accordingly, it can be confirmed that a microporous graphene oxide sheet exfoliated to a single atomic thickness was successfully prepared by the method of Example 1.

[0091] Evaluation Example 2: Membrane Analysis

[0092] FIG. 6 is a photograph of the membrane prepared in Example 1, FIG. 7 is an SEM image of the surface of the carbon coating portion, and FIG. 8 is an SEM image of the cross-section of the membrane. Referring to FIG. 6 to 8, it can be seen that a carbon coating layer with a lamellar structure was formed on the surface of a porous nylon substrate, and a two-dimensional flat sheet TFC membrane was successfully prepared.

[0093] To evaluate the organic solvent nanofiltration properties of the fabricated membranes, various molecular weights (260 to 10¹⁸ g mol -1 The performance of the membrane was analyzed using a solution in which organic dye molecules carrying ) and charges (+ / -) were dispersed in a methanol solvent. For all nanofiltration tests, the transmembrane pressure was fixed at 1 bar, and the methanol permeability and the rejection rate of solutes (organic dye molecules) were measured 30 minutes after the start of nanofiltration.

[0094] FIG. 9 shows the organic solvent nanofiltration results of the membrane prepared in Example 1 (CG: Chrysoidine G, MR: Methyl Red, MB: Methylene Blue, CV: Crystal Violet, BB: Brilliant Blue G, RB: Rose Bengal). Referring to FIG. 9, the membrane according to one embodiment is 408 g mol -1 It exhibits an effective filtration performance of over 90% for all dye molecules with molecular weights above. In particular, despite the varying charges of organic dye molecules, the rejection curve appears as a function of molecular weight, which implies that the molecular sieving role of the carbon sheets forming the active layer is dominant in the separation mechanism of this membrane.

[0095] Figure 10 compares the organic solvent nanofiltration performance of the membrane prepared in Example 1 with that of existing state-of-the-art organic solvent nanofiltration membranes and is a graph showing the rejection rate of the organic dye molecule CV (Crystal Violet) and methanol permeability. Referring to Figure 10, it can be confirmed that the membrane according to one embodiment exhibits superior solvent permeability and solute filtration characteristics compared to other existing membranes. This is attributed to the unique pore structure of the membrane; the high density of micropores results in high solvent permeability, and the uniform size of micropores results in a high solute rejection rate. In particular, considering that the active layer thickness (200 nm) of the present membrane is much thicker than the active layer thickness (<80 nm) of existing commercial membranes, yet exhibits superior membrane performance, the 2D microporous graphene oxide sheet according to one embodiment can be considered a very excellent membrane material.

[0096] Although preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concepts defined in the following claims are also included within the scope of the present invention.

Claims

Claim 1 A two-dimensional microporous graphene oxide sheet having an average pore size of 0.1 nm to 2 nm, a pore spacing of 0.3 nm to 10 nm, a standard deviation of the pore spacing of 5 nm or less, and a thickness of 2 nm or less. Claim 2 In claim 1, a two-dimensional microporous graphene oxide sheet having an atomic ratio of oxygen to carbon of 0.1 to 1.

0. Claim 3 A two-dimensional microporous graphene oxide sheet according to claim 1, comprising 10% to 60% by weight of oxygen with respect to 100% by weight of the two-dimensional microporous graphene oxide sheet. Claim 4 A two-dimensional microporous graphene oxide sheet having a standard deviation of the average size of the pores of claim 1 nm or less. Claim 5 In claim 1, the pore density is 10 pores / 100 nm 2 Up to 100 pores / 100 nm 2 Microporous graphene oxide sheet with a two-dimensional structure. Claim 6 A method for manufacturing a microporous graphene oxide sheet, comprising: preparing a carbon-zeolite composite by depositing carbon on a zeolite template having a two-dimensional pore structure; oxidizing the carbon-zeolite composite; removing the zeolite from the oxidized carbon-zeolite composite to obtain microporous graphene oxide; and sonicating the obtained product in a solvent to obtain a microporous graphene oxide sheet having a two-dimensional structure with a thickness of 2 nm or less. Claim 7 A method for manufacturing a microporous graphene oxide sheet according to claim 6, wherein the obtained two-dimensional structured microporous graphene oxide sheet has an average pore size of 0.1 nm to 2 nm, a pore spacing of 0.3 nm to 10 nm, and a standard deviation of the pore spacing of 5 nm or less. Claim 8 A method for manufacturing a microporous graphene oxide sheet according to claim 6, wherein the zeolite template has a two-dimensional pore structure having a size of 12 membered rings or larger. Claim 9 In paragraph 6, the zeolite mold is * CTH, IWV, OKO, * A method for manufacturing a microporous graphene oxide sheet, at least one selected from PCS, SEW, SFS, SSF, USI, and UTL. Claim 10 A method for manufacturing a microporous graphene oxide sheet according to claim 6, wherein the carbon is deposited via chemical vapor deposition using a carbon precursor comprising acetylene, ethylene, propylene, ethanol, or a combination thereof. Claim 11 A method for manufacturing a microporous oxidized graphene sheet according to claim 6, wherein oxidizing the carbon-zeolite composite comprises adding and mixing the carbon-zeolite composite and an oxidizing agent in a solvent, wherein the oxidizing agent comprises KMnO4, H2O2, HNO3, NaNO3, H2SO4, or a combination thereof. Claim 12 A method for preparing a microporous oxidized graphene sheet according to claim 6, wherein removing the zeolite from the oxidized carbon-zeolite composite comprises mixing the leaching solution with the oxidized carbon-zeolite composite, and the leaching solution comprises HCl, NaOH, KOH, HF, NaF, NH4F, AlF3, or a combination thereof. Claim 13 A method for manufacturing a microporous graphene oxide sheet according to claim 6, further comprising removing the zeolite from the oxidized carbon-zeolite composite, obtaining a precipitate of microporous graphene oxide through centrifugation, and dispersing the obtained product in a solvent. Claim 14 A method for manufacturing a microporous graphene oxide sheet according to claim 6, wherein the sound wave treatment is carried out for 1 hour to 20 hours under conditions of 20 kHz to 100 kHz. Claim 15 A method for manufacturing a microporous graphene oxide sheet according to claim 6, comprising, after sonication, performing centrifugation and recovering the supernatant to obtain a dispersion in which two-dimensional microporous graphene oxide sheets having a thickness of 2 nm or less are dispersed in a solvent. Claim 16 A dispersion comprising a solvent and a two-dimensional structured microporous graphene oxide sheet dispersed in the solvent and having a thickness of 2 nm or less. Claim 17 In claim 16, the microporous graphene oxide sheet of the two-dimensional structure is a dispersion having an average pore size of 0.1 nm to 2 nm, a spacing between pores of 0.3 nm to 10 nm, and a standard deviation of the spacing between pores of 5 nm or less. Claim 18 In claim 16, the microporous graphene oxide sheet of the two-dimensional structure has a pore density of 10 pores / 100 nm 2 Up to 100 pores / 100 nm 2 Phosphorus dispersion. Claim 19 In claim 16, the microporous graphene oxide sheet of the two-dimensional structure is a dispersion having an atomic ratio of oxygen to carbon of 0.1 to 1.

0. Claim 20 In claim 16, the solvent is a dispersion comprising N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), tetrahydrofuran (THF), toluene, acetone, water, methanol, ethanol, isopropyl alcohol, dimethyl sulfoxide (DMSO), propylene glycol methyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), ethyl-3-ethoxypropionate (EEP), butyl carbitol (BC), or a combination thereof. Claim 21 A membrane comprising a laminate of two-dimensional microporous graphene oxide sheets according to any one of claims 1 to 5. Claim 22 A membrane according to claim 21, wherein the membrane comprises a substrate and a carbon coating layer positioned on the substrate, and the carbon coating layer comprises a stack of two-dimensional microporous graphene oxide sheets according to any one of claims 1 to 5. Claim 23 In paragraph 22, the membrane having a carbon coating layer thickness of 10 nm to 50 μm. Claim 24 In paragraph 22, the above description comprises a membrane comprising glass fiber, cellulose fiber, nylon, polycarbonate, polyethersulfone, polyester, polyethylene, polypropylene, polytetrafluoroethylene, polyethylene terephthalate, polyacrylate, polyimide, polystyrene, polyethylene naphthalate, aluminum oxide, silicon oxide, or a combination thereof. Claim 25 A method for manufacturing a membrane comprising manufacturing a two-dimensional microporous graphene oxide sheet with a thickness of 2 nm or less according to the method of claim 6, and stacking the two-dimensional microporous graphene oxide sheets with a thickness of 2 nm or less on a substrate.

Citation Information

Patent Citations

  • Method for separation of mixed gas containing ethane by ethane-selective adsorption using porous carbon structure having micropores with uniform distribution

    KR1020200120029A

  • MFI zeolite with hierarchical structure having micropores and mesopores, a preparation method thereof, and catalytic use thereof

    KR102035397B1

  • Perforated sheets of graphene-based material

    US20170036911A1

  • Graphene / polymer nanofiber membranes with a nanofilament network structure and their preparation method