Method for forming a composite substrate
The method of mixed gas plasma activation and UV surface modification addresses bonding issues in piezoelectric materials, achieving strong and stable bonds for piezoelectric wafers on support materials, enhancing the performance of thin-film surface acoustic wave devices.
Patent Information
- Application Number
- KR1020247035010
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2022-11-15
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2042-11-15
AI Technical Summary
Existing wafer bonding methods for piezoelectric materials suffer from issues such as bandpass shift with temperature, substrate deformation, thermal micro-voids, electrostatic charge breakdown, insufficient bonding strength, and increased SAW propagation loss in radio frequency filter devices.
A method involving mixed gas plasma activation using O2 and N2, combined with UV surface modification, followed by low-temperature thermal annealing, to form a stable bond between piezoelectric and support wafers, ensuring high bonding quality and strength without micro-pores or warping.
The method achieves strong adhesion between piezoelectric materials like lithium tantalate and lithium niobate on silicon, silicon oxide, silicon carbide, and diamond, with improved thermal stability and reduced defects, enabling the production of high-performance thin-film surface acoustic wave devices.
Smart Images

Figure 112024114153779-PCT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention generally relates to the field of forming composite substrates including a wafer bonding process. Background Technology
[0002] A surface acoustic wave (SAW) device is known to be a device that combines a piezoelectric substrate, which propagates surface acoustic waves, with a support substrate. It is known that by attaching a support substrate having a lower coefficient of thermal expansion than that of the piezoelectric substrate, changes in the size of the piezoelectric substrate during temperature changes are suppressed, and changes in the frequency characteristics of the surface acoustic wave device are reduced.
[0003] WO2017163722A1 discloses a surface acoustic wave device having a structure that bonds a piezoelectric substrate and a silicon substrate together using a multi-stage procedure, wherein in the first stage, a so-called bonding layer among different specific material groups is deposited on at least one bonding partner, and in the second stage, the surface of this layer and another bonding partner is activated by a direct bonding step followed by a plasma process and then by thermal annealing.
[0004] CN109786229B discloses a surface acoustic wave device for bonding piezoelectric wafers with different substrate materials for a limited wafer size of 0.051 m to 0.102 m using a wet chemical wafer bonding surface procedure followed by Ar / O2 mixed gas plasma activation.
[0005] CN109166793B discloses a two-step surface activation prior to the direct bonding step. Here, the first activation step is: placing a silicon wafer to be bonded with a lithium niobate wafer under a vacuum ultraviolet light source and activating it under humidity conditions of 20 to 80%. The second activation step is: placing the wafer activated by the vacuum ultraviolet light into an N2 plasma at a pressure of 10 to 80 Pa.
[0006] Known wafer bonding methods for bonding piezoelectric materials onto a support wafer often exhibit one or more of the following technical problems and / or issues with the final produced radio frequency filter device: namely, bandband shift of the SAW device with temperature, deformation of the substrate during annealing and thinning processes, thermal micro-voids (e.g., gas emission), breakdown of high electrostatic charge (e.g., warping and high bending), insufficient bonding strength for additional processes of the bonded wafer pair (e.g., thinning, dicing), and increased SAW propagation loss. The problem to be solved
[0007] The present invention aims to provide a method for forming a composite substrate including a wafer bonding process with improved performance. means of solving the problem
[0008] The above method for forming a composite substrate may include the features of claim 1. Additional embodiments are provided by the description in the dependent claims. The method provides for the efficient fabrication of thin film surface acoustic wave (also known as TF-SAW) and other related devices by efficiently forming a stable bond between a support wafer and a piezoelectric wafer.
[0009] For example, the above method considers a process flow for improving the wafer bonding of piezoelectric crystals onto supporting wafer materials that appear in known wafer bonding processes and the manufacture of SAW devices. For example, the following characteristics can be improved through the above method: bandpass shift of the SAW device with respect to temperature, substrate deformation during annealing and thinning processes, thermal micro-voids (e.g., gas emission), breakdown of high electrostatic charges (e.g., warping and high bending), insufficient bonding strength for additional processes of bonded wafer pairs (e.g., thinning, dicing), and SAW propagation loss.
[0010] In this way, a piezoelectric material with a large electromechanical coupling coefficient and excellent temperature stability can be provided. Brief explanation of the drawing
[0011] Similar reference characters in the drawings generally refer to the same parts throughout the drawings. Although not necessarily drawn to scale, the drawings generally focus on illustrating the principles of the invention. In the following description, various aspects of the invention are described with reference to the following drawings. Figure 1 shows a schematic cross-sectional view of a composite substrate. Figure 2 illustrates a flowchart of a method for manufacturing a composite substrate. FIGS. 3a to 3f are schematic drawings illustrating the above method for manufacturing a composite substrate. Figure 4 illustrates a schematic plasma system for the above method of manufacturing a composite substrate. FIGS. 5a to 5d show atomic force microscope images of the substrate surface constituting the composite substrate. FIGS. 6 to 10b show surface acoustic microscope (SAM) and infrared transmission images (IR) of the substrate surface constituting the composite substrate, and FIGS. 11a to 12b illustrate schematic cross-sectional views of a composite substrate in a substrate thinning process. Specific details for implementing the invention
[0012] The following detailed description refers to the attached drawings, which exemplarily illustrate specific details and aspects in which the present invention can be implemented.
[0013] For example, a method for wafer bonding piezoelectric materials onto a support substrate manufactured using mixed gas plasma activation is described. For example, the method includes mixed gas plasma activation of oxygen (O2) and nitrogen (N2), mixed gas of O2 and N2 including ultraviolet (UV) surface modification, for example, mixed gas using an excimer lamp, a bonding process in low vacuum, and thermal annealing at a low temperature of less than 200°C.
[0014] The above method achieves high bonding quality for piezoelectric substrates such as lithium tantalate (LT) and lithium niobate (LN) on silicon (Si), silicon oxide, silicon carbide (SiC), cubic boron nitride (c-BN), and diamond. The resulting bonded material (also referred to as a composite substrate) may be free of or substantially free of macroscopic and microscopic voids across the bonding interface. Alternatively, or additionally, the composite substrate may be free of creaking and warping of the bonded wafer. The initial pre-bonding state (also referred to as a precursor composite substrate) may exhibit higher bonding strength than that achieved using known bonding techniques. The composite structure can be used to achieve thin-film surface acoustic wave (also referred to as TF-SAW) devices in various applications, for example, as a filtering device in communications or as a pump or mixing device in fluid handling equipment.
[0015] Piezoelectric materials derived from material groups such as lithium tantalate (LT) and lithium niobate (LN) have large electromechanical coupling coefficients that are advantageous for achieving broadband filter characteristics. However, these materials have the disadvantage of poor stability with respect to temperature. The method of the present invention provides a permanent wafer direct bonding method (also referred to as fused bonding) by providing a composite substrate (also referred to as a cohesive composite substrate) having strong adhesion or strong bonding between the wafer and the piezoelectric material using a mixed gas plasma activation process and UV-surface modification. The composite substrate may not have micro-pores at the bonding interface for different material combinations such as LT / / Si, LN / / Si, LN / / SiO2, LT / / SiO2, quartz / / Si, LN / SiC, LT / / SiC, LN / / BN, LT / / BN, LT / / diamond, and LN / / diamond.
[0016] The above method may be configured such that a plasma activation process using a UV modification process forms an intermediate film (also referred to as a bonding layer) of a predetermined level. The characteristics of the intermediate film may be controlled by parameters of the plasma activation process and parameters of the UV modification process that affect the bonding surfaces of the piezoelectric substrate and the support substrate. The bonding layer may include components such as the plasma gas used, e.g., oxygen and nitrogen, and the same components from the materials of the two substrates to be bonded, e.g., a wafer and a piezoelectric material wafer.
[0017] The above intermediate layer may include one or more amorphous oxides and one or more amorphous nitrides. The amorphous oxide can improve the bonding quality, and the amorphous nitride can improve the bonding strength.
[0018] The above plasma activation process and mixed gas UV-surface modification process may be configured to clean the surfaces to be bonded by removing impurities and organic contaminants from the surfaces of the substrates. This improves the bonding quality and bonding strength between the piezoelectric substrate and the support substrate at low temperatures.
[0019] The above bonding process can be performed at a low vacuum, preferably 0.1 Pa or less. In this way, residues of the water film are removed from the surfaces of both substrates.
[0020] For example, the bonding process described above is a direct wafer bonding of different material combinations. As such, through material-related optimization of plasma activation parameters, efficient bonding at room temperature with high bonding strength of Si / / Si, Si / / SiO2, LT / / silicon dioxide, LT / / Si, LT / / quartz, and LT / / sapphire (Al2O3) is possible. Plasma activation parameters may include plasma power, plasma gas pressure, plasma duration, gas flow rate ratio (N2 to O2), pre-bonding process conditions (e.g., vacuum atmosphere and mechanical pressure), mixed gas UV-surface modification, and (post-)thermal annealing processes.
[0021] The above method provides surface activation using a gas mixture of O2 and N2 for plasma surface activation and mixed gas UV-surface modification of two wafers to be bonded, for example, a piezoelectric wafer (also referred to as the second substrate) and a support substrate wafer (also referred to as the first substrate).
[0022] The first substrate (support substrate) comprises, for example, silicon (Si), silicon oxide (SiO2), sapphire (Al2O3), silicon carbide (SiC), cubic boron nitride (c-BN), and diamond, or is formed from these. The second substrate (piezoelectric substrate) comprises, for example, lithium niobate (LN), lithium tantalate (LT), and quartz (SiO2), or is formed from these. The first substrate is directly bonded to the second substrate after the plasma activation process and the UV modification process. The mixed-gas plasma surface activation process can support the substrate by bonding the piezoelectric lithium niobate (LN) surface or the piezoelectric lithium tantalate (LT) surface together with the mixed-gas UV-radiation modification process. The bonding process can be used to bond heterogeneous materials, such as LN wafers or LT wafers, to any one of Si, SiO2, c-BN, SiC, and diamond wafers at room temperature under vacuum conditions.
[0023] The above plasma activation process may be performed in a plasma chamber accommodating the first electrode and the second electrode, having a controllable gas flow between the first electrode and the second electrode. The power at the first electrode and the second electrode may be controlled independently of each other (also indicated as being separated). The potential between the first electrode and the second electrode may form a plasma from gas molecules flowing between the first electrode and the second electrode. Accordingly, the power supplied to the first electrode and the second electrode may also be indicated as a plasma power. The plasma power of the first electrode, which may be the upper electrode of the plasma chamber, may be, for example, 10 W to 150 W. The plasma power of the second electrode, which may be the lower electrode of the plasma chamber, may be, for example, 10 W to 75 W.
[0024] The processing time of the plasma activation process of the first substrate and / or the second substrate (also indicated as plasma activation time) may be about 5 seconds to about 180 seconds, for example, about 10 seconds to about 120 seconds.
[0025] The plasma operating pressure of the plasma activation process of the first substrate and / or the second substrate may be about 10 Pa to about 300 Pa, for example, about 20 Pa to about 100 Pa.
[0026] The thermal annealing of the bonded precursor composite substrate can be performed at a temperature of about 80°C to about 190°C, for example, about 100°C to about 175°C, under a forming gas atmosphere.
[0027] The direct covalent junction between the crystalline piezoelectric material of the second substrate and the material of the first substrate is approximately 0.5 J / m 2 Up to about 2.5 J / m 2 , for example, 0.5 J / m 2 , 0.8 J / m 2 , 1.0 J / m 2 , 1.2 J / m 2 , 1.5 J / m 2 , 1.8 J / m 2 , or 2.0 J / m 2 Adjustable bonding strength can be achieved.
[0028] The above composite substrate may be one of various material combinations that are covalently bonded and have high bond strength, for example, LT / / Si, LT / / SiO2, LT / / SiC, LT / / c-BN, LT / / Diamond, LN / / Si, LN / / SiO2, LN / / SiC, LN / / c-BN, LN / / Diamond, or a combination thereof.
[0029] The bonding interface of the above composite substrate may be a high-quality bond, for example, the interface may be free of micro-pores, free of gas emission, and free of damage to the surface structure.
[0030] The bonding interface of the above composite substrate may have excellent thermal stability against high temperatures of up to 200°C.
[0031] The above method can bond first and second substrates of various commercially available wafer formats, for example, the support wafer size may be 0.051 m, 0.102 m, 0.153 m and 0.204 m, or larger.
[0032] FIG. 1 illustrates a schematic cross-sectional view of a composite substrate (100) comprising a first substrate (102) bonded to a second substrate (106) through a bonding layer (104). The second substrate (106) may include a piezoelectric material or be formed of a piezoelectric material as described above. The first substrate (102) and the second substrate (106) are directly bonded. Accordingly, the bonding layer (104) may include a combination of materials of the first substrate, the second substrate (106), oxygen and / or nitrogen.
[0033] For example, the bonding layer (104) may be divided into oxide amorphous domains, nitride amorphous domains, and metal amorphous domains at the directly bonded interface(s) and sub-bonding interface(s).
[0034] The above composite substrate (100) can be used, for example, to form a TF-SAW device.
[0035] The method of forming the above composite substrate (100) can be improved or even optimized by varying the following plasma conditions: plasma power, plasma duration, plasma gas pressure of less than 200 Pa, mixed gas flow rate and flow ratio of the two gases, and exposure to UV light (e.g., in the range of about 150 nm to 500 nm) at low power under a mixed gas (O2+N2) atmosphere.
[0036] The composite substrate (100) of various material combinations may have high bonding strength, no or substantially no thermal gas emission, and low electrostatic charge (e.g., the bow of the composite substrate (100) may be less than 20 μm), the bonded first and second substrates are not damaged during thermal annealing at a temperature of up to 200 °C, and no damage occurs to different wafer sizes (e.g., up to 0.153 m wafer for the first substrate (102) and second substrate (106)) even during selective mechanical thinning of the LT / LN bonded wafer portion to a film thickness of about 250 μm to about 2 μm.
[0037] FIG. 2 shows a flowchart of a method (200) for forming a composite substrate (100) illustrated in FIG. 1. The method (200) may include a plasma activation process (202) comprising the step of exposing a first surface of a first substrate in a plasma system. The plasma is a mixed gas plasma of oxygen and nitrogen at a first ambient pressure. The first ambient pressure may be lower than or equal to atmospheric pressure.
[0038] The above method (200) may include a plasma activation process (204) comprising the step of exposing a second surface of a second substrate. The plasma system may be a radio frequency system having plasma between a first electrode and a second electrode (e.g., a plasma chamber including radio frequency or microwave generators for generating gas plasma from a gas flowing through the plasma chamber). The first electrode and the second electrode may be configured to be powered and controlled separately. The plasma is a mixed gas plasma of oxygen and nitrogen at a first ambient pressure. The first ambient pressure may be at or below atmospheric pressure.
[0039] The above plasma system is illustrated in more detail in Fig. 4.
[0040] The above method (200) may also include a surface modification process (206) comprising the step of exposing a plasma-activated first surface to ultraviolet radiation in an atmosphere of oxygen and nitrogen at atmospheric pressure. The above method (200) may also include a surface modification process (208) comprising the step (208) of exposing a plasma-activated second surface to ultraviolet radiation in an atmosphere of oxygen and nitrogen at atmospheric pressure.
[0041] The above method (200) may also include a process (210) of forming a precursor composite substrate by placing the first surface of the first substrate on the second surface of the second substrate.
[0042] The above method (200) may include a process (212) of bonding the first substrate to the second substrate by applying a mechanical load to the precursor composite substrate at a second ambient pressure.
[0043] The above method may also include a process (214) of thermally annealing the bonded precursor composite substrate.
[0044] Here, the first substrate is a wafer configured to support the second substrate, which is single-crystal and non-crystalline. The second substrate is a wafer of piezoelectric material.
[0045] FIGS. 3a through 3f are schematic drawings illustrating the method of FIG. 2 for manufacturing a composite substrate. For example, the method includes a general process flow of directly wafer-bonding the second substrate (106) to the first substrate (102). The method may generally include the following steps: exposing the first substrate (102) and the second substrate (106) to excimer light (306, 308) emitted by excimer lamp(s) (302, 304) in an atmospheric atmosphere, as illustrated in FIG. 3a. The excimer lamp (302, 304) may provide electromagnetic radiation (also referred to as light) having a wavelength or wavelength spectrum in a wavelength range of about 150 nm to about 500 nm (also referred to as UV light). The excimer light (306, 308) may be the same or different for the first substrate (102) and the second substrate (106). Thus, organic and non-organic contamination may be reduced or even eliminated.
[0046] FIG. 3b illustrates that the first substrate (102) is exposed to a mixed gas plasma activation (310) at room temperature, and the second substrate (106) is exposed to a mixed gas plasma activation (312) at room temperature. In this way, the surface species of the material of the first substrate and the material of the second substrate can be reduced, and the bonding layer (104) can be formed on the first surface and the second surface.
[0047] The above method may include rinsing processes (314, 316) of the plasma-activated first substrate (102) and the plasma-activated second substrate (106), as illustrated in FIG. 3C. The rinsing processes (314, 316) may include an ultrasonic-assisted deionized (DI)-water rinsing step and a drying step of the rinsed first substrate and the rinsed second substrate. In this way, particles and organic contaminants can be removed from the first surface and the second surface.
[0048] In other words, after surface activation, the first substrate (102) and the second substrate (106) can be sequentially cleaned using an ultrasonic cleaning nozzle (wherein the ultrasonic may correspond to an acoustic signal having a frequency in the range of 700 kHz to 5 MHz) and a DI-water cleaning nozzle. The cleaned substrates (102, 106) can be placed in a spinner. The spinner can spin the cleaned substrates to dry the substrates. The cleaning using the ultrasonic cleaning nozzle, the DI-water cleaning nozzle, and the spinner can be integrated into a single wafer cleaning system.
[0049] The surface modification process of the method illustrated in FIG. 3d may include the step of exposing the first substrate (102) and the second substrate (106) to light (318, 320) emitted by one or more excimer lamp(s) (322, 324). The excimer light (318, 320) may be the same or different for the first substrate (102) and the second substrate (106). The first surface of the first substrate (102) and the second surface of the second substrate (106) may be exposed to a mixture (334) of radicals and other reactive atoms or molecules (N2 and O2) during the UV-light exposure. The mixtures (332, 334) may be the same or different for the first substrate (102) and the second substrate (106). The first surface of the first substrate (102) and the second surface of the second substrate (106) may be exposed to a low temperature (e.g., less than 100°C) during the UV-light exposure. In this way, any contamination can be removed from the first surface and the second surface. Additionally, the surface energy and polarity of the first surface and the second surface can be adjusted to match chemical reactions at the atomic or molecular level. In this way, functional groups for the dangling bonds are reinforced. Thus, the bond strength at room temperature can be improved.
[0050] The process of forming the precursor composite substrate (330) may include, for example, a flat-to-flat or notch-to-notch mechanical alignment of the first surface to the second surface, as illustrated in FIG. 3e. The bonding process may be performed at room temperature in a vacuum atmosphere with a process gas pressure of less than 0.1 Pa. The bonding process may be performed under a mechanical pressure of up to 5 kN. The mechanical pressure is oriented in a direction that compresses the first substrate and the second substrate. That is, the mechanical pressure is oriented to compress the first substrate toward the second substrate, or vice versa.
[0051] That is, in the process of forming the precursor composite substrate, the first substrate (102) having the first surface and the second substrate (106) having the second surface can be positioned to face each other through mechanical alignment (326) (e.g., wafer flat of the first substrate versus wafer flat of the second substrate) in a standard wafer-bonding system. The standard wafer-bonding system can utilize a mechanical pressure of up to 5 kN in a vacuum atmosphere of approximately 0.1 Pa. Thus, the van der Waals force bringing the first substrate and the second substrate into contact is up to 0.8 J / m² at room temperature. 2 A bonding strength of 1.2 J / m is obtained. In this way, thermal annealing is applied for several hours at a predetermined temperature between 100 ℃ and 190 ℃ to obtain a bonding strength of 1.2 J / m 2 Greater bonding strength can be improved.
[0052] The above thermal annealing (also referred to as post-thermal annealing) process (328) can be performed at one or more temperature(s) of up to 200°C in one or more temperature ranges on such a standard forming gas atmosphere furnace and / or hot plate as illustrated in FIG. 3f. In this way, bonding strength, such as the cohesion of the bonding layer (104) (see FIG. 1), can be improved.
[0053] The surface modification process including the above ambient UV-light exposure step may be an additional process applied to clean the first surface and the second surface from most organic contamination. The UV-light exposure may include, for example, excimer light having a wavelength of less than 400 nm.
[0054] The above UV-light exposure may be performed in a normal atmospheric environment. The UV-light exposure may be configured to break or destroy the molecular bonds of the organic material. In this way, the UV-light exposure may reduce various hydrocarbons on the first surface and / or the second surface, for example, prior to plasma activation.
[0055] FIG. 4 illustrates a schematic diagram of a dual RF-capacitive coupled plasma system (400) that can be used for the activation of the mixed gas plasma on wafer surfaces.
[0056] The plasma system (400) may have a conventional horizontal capacitive parallel dual electrode comprising a first electrode (404) and a second electrode (406). The first electrode (404) and the second electrode (406) may be individually powered and / or controlled by one or more RF power supplies (408, 410) and one or more controllers (not shown). The RF power supplies (408, 410) may provide RF power having different frequencies in the kHz range to the electrodes (404, 406). The plasma power may be in the range of about 10 W to 300 W for the first electrode (404) and the second electrode (406). The plasma power may have slight variations depending on the process gas mixture.
[0057] For example, a single wafer of the first substrate (102) and the second substrate (106) may be positioned on the second electrode (406) of the plasma system (400) inside the plasma chamber (402), for example, the lower electrode (406). A mixture (418) of gaseous oxygen (412) and gaseous nitrogen (414) is provided to the plasma chamber through an adjustable valve system (416) that provides flow rate control of oxygen (412) and nitrogen (414), respectively. The RF power at the electrodes (404, 406) adjustably forms a plasma (310 and / or 312) from the gas mixture (418). The surface of the substrate (102, 106) to be bonded (e.g., the first surface of the first substrate or the second surface of the second substrate) may be exposed to the plasma mixture (310 and / or 312) of oxygen (412) and nitrogen (414) for a short period of time. The period of time may range from about 5 seconds to about 120 seconds. The duration of time may vary according to the best-known method recipes (BKM).
[0058] Mixing of gases, e.g., oxygen (412) and nitrogen (414), within the plasma chamber (402) can be performed by controlling the flow rate of each gas (412, 414) to form the gas mixture (418) through the valve system (416). The flow rates of oxygen (412) and nitrogen (414) may be in the range of about 5 standard cubic centimeters (sccm) per minute to about 100 sccm. At the same time, the gas pressure within the plasma chamber (402) may be controlled during plasma activation, for example, by a suction capacity throttle valve in a vacuum pumping system (not shown). The gas pressure may be in the range of about 10 Pa to about 300 Pa. The concentration of the above N2-gas to O2-gas flow rate ratio may be in the range of about 5% to about 95%, for example, 10%, 15%, 20%, 25%, 30%, 50%, 75%, and 95%, depending on the materials of the first substrate and the second substrate.
[0059] UV-light exposure under the presence of a mixed gas (318) can be used to improve bond strength at room temperature and reduced annealing temperature. The exposure to the UV-light (e.g., having a wavelength in the range of about 150 nm to about 500 nm) can be performed, for example, using an excimer lamp under an atmosphere of atmospheric pressure and a mixed gas (N2 / O2) (e.g., 50% / 50% - note that this ratio may vary depending on the situation). In this case, the mixed gases can provide oxygen and nitrogen as one agent in the reaction between the piezoelectric material of the second substrate and the material of the first substrate. Thus, activated groups, for example, hydroxyl groups (-OH), can be generated on the surfaces of the first substrate and the second substrate. Thus, the polarity and surface energy of the first surface of the first substrate and the second surface of the second substrate can be increased. The UV-light exposure can be performed in a process chamber at atmospheric pressure.
[0060] Infrared analysis and scanning acoustic microscopy of the above-mentioned bonded precursor composite substrate generally show a bonding interface without detectable voids (also called micropores) typically caused by thermal gas emission, for example, the bonding layer mentioned above.
[0061] FIGS. 5a through 5d show AFM images (500, 502, 508, 510) including linear scan height profiles (504, 506, 512, 514) for materials shown after mixed gas (O2+N2) plasma activation (310 or 312) of FIG. 3b, for example, the surface of silicon (Si) shown in FIG. 5a, the thermal silicon dioxide (SiO2) film (0.5 μm thickness) on the Si wafer shown in FIG. 5b, the lithium tantalate surface shown in FIG. 5c, and the quartz surface using the BKM recipe per individual material after mixed gas (O2+N2) plasma activation shown in FIG. 5d. Despite individual scratches, the RMS roughness of all substrates can be much lower than 0.5 nm, as indicated by the linear scan height profiles (504, 506, 512, 514). A smooth surface having a mean squared roughness (RMS, Rq) of about 0.5 nm or less may be more suitable for bonding.
[0062] FIG. 6 shows a scanning acoustic microscopy (SAM) image of a first embodiment of a composite substrate. The first embodiment comprises Si / / Si wafer bonding of 0.204 m wafers. Here, the Si / / Si wafer bonding is plasma activated with a mixed gas concentration using a BKM recipe, with a gas flow rate of less than 100 sccm, a gas pressure of up to 100 Pa, and a plasma power of less than 50 W for the first electrode and the second electrode. The processes prior to the bonding process (also referred to as pre-bonding processes) can be performed in a vacuum under conditions equivalent to a mechanical pressure of 5 kN (piston drop) at room temperature, followed by post-bonding annealing at 300 °C for 2 hours. FIG. 6 shows a SAM image of a composite wafer pre-bonded in a vacuum. In contrast to pre-bonding in an atmospheric pressure environment, this forms a high-quality bonding interface free of micro-pores and thermal gas release across the entire bonding interface, with a bonding strength of 2.0 J / m 2 It can increase up to.
[0063] FIG. 7 shows a scanning acoustic microscope (SAM) image of a second embodiment of a composite substrate. The second embodiment comprises Si / / SiO2 wafers (both with a diameter of 0.204 m) bonded by the mixed-gas plasma activation processes using a BKM recipe, wherein a low plasma is used in which the plasma process gas pressure is less than 50 Pa and the plasma power of the first electrode and the second electrode is less than 100 W each, and after pre-bonding in vacuum under the same conditions at room temperature, post-bonding annealing is performed at 300 °C for 2 hours. There are almost no micropores or thermal gas emissions across the entire interface of the two bonded wafers (e.g., the first substrate and the second substrate), and there are only some small handling particles across the edge bonding region. The bonding strength is 1.6 J / m² after the post-thermal annealing. 2It can increase.
[0064] FIG. 8 shows a scanning acoustic microscope (SAM) image of a third embodiment of a composite substrate. The composite substrate comprises LiTaO3(LT) as a second substrate and Si as a first substrate. The illustrated image shows the composite substrate after thermal annealing at 175 °C. The composite substrate can be prepared and evaluated according to the same procedure as in Example 1. The precursor composite substrate can be bonded at 0.1 Pa in a vacuum atmosphere under a mechanical pressure of 2.0 kN at room temperature. The entire region of LiTaO3(LT) can be completely bonded. A void-free interface can be observed after annealing at 175 °C for 2 hours. The bonding strength is 1.27 J / m² after post-annealing at 175 °C for 5 hours. 2 The second substrate may be thinned to a thickness of about 250 μm to about 400 μm, in the range of about 1 μm to about 250 μm, for example, in the range of about 2 μm to about 10 μm.
[0065] FIG. 9 shows a scanning acoustic microscope (SAM) image of a fourth embodiment of a composite substrate (900). The composite substrate comprises a silicon wafer as a second substrate and a first substrate having a thermal oxide (e.g., 500 nm thick) after thermal annealing at 150 °C. In the fourth embodiment, the bonded 0.153 wafer of the first substrate and the second substrate can be manufactured and evaluated according to the same procedure as in the second embodiment. Here, the material of the piezoelectric single crystal substrate (second substrate) may be lithium tantalate (LT), and the Si-handle wafer may be prepared to be covered with a 500 nm thermal oxide (first substrate) so as to be used as a support material for an RF-velocity layer. FIG. 9 shows a scanning acoustic microscope (SAM) image of the bonded interface of the LT / / SiO2 junction at room temperature (RT) and an image after thermal annealing at 150 °C for 2 hours. The entire area of the above wafer pair can be completely bonded. The measured bonding strength is 1.1 J / m 2 It may be possible. From inspection by SAM measurement of such bonded interfaces, many small microbubbles may be observed, and the same is true when thermal oxide wafer bonding is performed in a vacuum. However, in the case of a Si wafer (thickness of 100 nm to 1000 nm) having sputter-deposited oxide, it can be observed that there is no gas emission and no gas bubbles after thermal annealing at 150°C for 5 hours. The second substrate may be thinned to a thickness of about 250 μm to about 400 μm, in the range of about 1 μm to about 250 μm, for example, in the range of about 2 μm to about 10 μm.
[0066] FIGS. 10a and FIG. 10b show infrared (IR) transmission images of a bonded composite substrate comprising a LiTaO3 wafer as a second substrate bonded to a quartz wafer (Fig. 10a) and a sapphire wafer (Fig. 10b), respectively, as a first substrate. The bonded 0.102 m wafer can be manufactured and evaluated according to the same procedure as in Example 3. In this example, the piezoelectric material of the second substrate may be a 0.204 m single-crystal lithium tantalate (LT) wafer, and the first substrate may be 0.204 m quartz (fused silica) and 0.204 m sapphire (Al2O3). The composite substrates were pre-bonded at room temperature under a mechanical pressure of 2 kN in a vacuum atmosphere, followed by thermal annealing at less than 200 °C for 5 hours. The bonded composite substrates exhibit high bonding quality and are free of macroscopic voids and thermal microvoids formed before and after annealing. The above bonding strength is 1.3 J / m 2 The second substrate may be thinned to a thickness of about 250 μm to about 400 μm, for example, in the range of about 1 μm to about 250 μm.
[0067] FIGS. 11a and FIGS. 11b schematically illustrate a method for manufacturing a piezoelectric material on a SiC wafer composite substrate prior to a thinning and polishing process (1120) (Fig. 11a). Here, the second substrate (106) has a first thickness (1110). The thickness (1110) of the second substrate (106) can be reduced to a second thickness (1112) as shown in FIG. 11b by the thinning and polishing process (1120). The second thickness (1112) may be about 1 μm to about 250 μm, for example, about 2 μm to about 10 μm. The thinned composite substrate (1100) may contain a piezoelectric material on silicon carbide (SiC) in which the bonded surface may include a Si-plane. The wafer bonding can be manufactured and evaluated according to the same procedure as in Example 3 described above. However, the material of the piezoelectric single crystal substrate may include a lithium tantalate (LT) single crystal, and the material of the first substrate (102) may include a 4H-SiC substrate.
[0068] FIGS. 12a and 12b schematically illustrate a method for manufacturing a piezoelectric material on a thin film c-BN or diamond wafer composite substrate prior to a thin film forming and polishing process (1120) (Fig. 12a) (e.g., comprising a first substrate made of silicon and a thin film layer of c-BN or diamond). Here, the second substrate (106) has a first thickness (1210). The thickness (1210) of the second substrate (106) can be reduced to a second thickness (1212) as shown in FIG. 12b by the thin film forming and polishing process (1120). The second thickness (1212) may be about 1 μm to about 250 μm, for example, about 2 μm to about 10 μm.
[0069] The composite substrate (100) may include a piezoelectric material of the second substrate (106) bonded to the first substrate, for example, a c-BN layer (1204) or a thin diamond layer (1204) (e.g., with a thickness of less than 1 μm). That is, the composite substrate (100) may include a thin film of a c-boron nitride layer (1204) or a diamond layer (1204). The c-BN layer (1204) may be deposited using a physical vapor deposition (PVD) method, wherein the c-BN layer (1204) may be deposited by radio frequency magnetron sputtering (RFMS). A c-BN film having a thickness of about 1.1 μm may be deposited on the first substrate (102), for example, a Si substrate, with a very smooth surface. The composite substrate (100) can be manufactured and evaluated according to the same procedure as in Example 2, wherein the mixed gas plasma can be activated based on a high plasma power at a ratio of 1:1 (O2:N2) with a total gas flow rate of less than 50 sccm in a nitrogen / oxygen gas mixture. The bonding layer (104) can be very uniform and can have a thickness in the range of 10.0 nm. The bonding layer (104) can contain a large amount of amorphous nitride generated from the mixed gas activation process and mixed gas UV surface modification, thereby achieving a bonding strength of 0.8 J / m² without using heating after post-bonding. 2 It can be improved to a range of 1.8 J / m 2 Post-thermal annealing at a temperature higher than 200°C can be used to improve it up to 200°C.
[0070] The diamond layer (1204) may be deposited on a silicon substrate (102) by a PVD method. The diamond film (1204) may have a layer thickness of approximately 2.0 μm or more. The diamond layer (1204) may be polished using ion beam trimming to achieve a surface roughness (RMS) of less than 0.5 nm. The wafer bonding may be fabricated and evaluated according to the same procedure as in the above-described embodiment. The mixed gas plasma may be activated based on a high plasma power and may be activated for long-term plasma activation in a 1:1 (O2:N2) ratio nitrogen / oxygen gas mixture having a total gas flow rate of less than 75 sccm and a duration of less than 120 s by mixed gas UV surface modification. The bonding layer (104) may be very uniform and may have a thickness of approximately 15.0 nm or more. The bonding layer (104) may contain a large amount of amorphous nitride according to the mixed gas plasma activation of the first surface and the second surface to be bonded in order to improve bonding strength without using any heating. Here, the bonding strength can be improved by using post-thermal annealing at a temperature of 200°C or higher.
[0071] For example, lithium tantalate and lithium niobate single-crystal substrates can be used in elastic wave filters that may have low thermal conductivity. A surface activation process and a method for manufacturing a thin-film bonded wafer using a mixed gas (O2+N2) plasma and UV-surface modification under a mixed gas atmosphere (O2+N2) can exhibit an excellent bonding layer between bonded wafers of a composite substrate. The plasma activation method and the UV surface modification method may be used when a first substrate, such as silicon (Si), silicon oxide (SiO2), sapphire (Al2O3), silicon carbide (SiC), cubic boron nitride (c-BN), or diamond, is directly bonded to a second substrate, such as lithium niobate (LN), lithium tantalate (LT), or quartz (SiO2).
[0072] The above plasma surface activation process can be used to bond lithium tantalate (LT) and lithium niobate (LN) surfaces to various substrates.
[0073] The above bonding method can be used to bond heterogeneous materials of LN-wafers and LT-wafers to Si, SiO2, sapphire, c-BN, and SiC substrates (e.g., diameters 0.051 m, 0.102 m, 0.153 m, 0.204 m) in a vacuum atmosphere at room temperature.
[0074] The above mixed gas plasma process can be used for surface activation of all second substrates and first substrates with a plasma power source for the first electrode of a plasma system in the range of 10 W to 150 W and a plasma power source for the second electrode of a plasma system in the range of 10 W to 150 W.
[0075] The above mixed gas plasma process for surface activation can be used on all second substrates and first substrates having a plasma duration (time) of 5 seconds to 180 seconds.
[0076] A mixed gas plasma process for surface activation of the second substrates and the first substrates can be used with a gas pressure plasma of 10 Pa to 200 Pa.
[0077] The mixed gas plasma process for surface activation of all second substrates and first substrates can be used with post-thermal annealing under a forming gas atmosphere of 100°C to 200°C.
[0078] The above method provides a composite substrate with a high-quality bonding interface free of macro- and micro- pores, strong bonding, no thermal gas emission, and no damage to the surface structure.
[0079] The above composite material can have excellent thermal stability at high temperatures up to 250°C. Therefore, it is possible to provide an efficiently manufactured thin-film surface acoustic wave (TF-SAW) device.
[0080] The above method can bond wafers of different sizes to almost the entire wafer of the first substrate and the second substrate. In other words, the composite substrate forming method may include a plasma activation process in which a first surface of the first substrate and a second surface of the second substrate are each exposed in a plasma system, wherein the plasma system may be a radio frequency system having plasma between a first electrode and a second electrode that can be supplied with power separately, and wherein the plasma may be a mixed gas plasma of oxygen and nitrogen at a first atmosphere below atmospheric pressure, and the surface modification process may include a step of exposing the plasma-activated first surface and the plasma-activated second surface to ultraviolet light in an atmosphere of oxygen and nitrogen at atmospheric pressure, and may include a process of forming a precursor composite substrate by placing the first surface of the first substrate on the second surface of the second substrate, a process of bonding the first substrate to the second substrate by applying a mechanical load at a second atmosphere on the precursor composite substrate, and a process of thermally annealing the bonded precursor composite substrate. The first substrate may be a wafer configured to support a second substrate, which may be single crystal or non-crystalline, and the second substrate may be a wafer of piezoelectric material.
[0081] The second ambient pressure may be atmospheric pressure. The second ambient pressure is approximately 0.1 Pa to approximately 10 -3 It can be a vacuum pressure in the Pa range.
[0082] The method may additionally include a step of polishing the first surface and the second surface so that the first surface and the second surface each have an average squared roughness of less than 0.5 nm.
[0083] The above method may include a plasma power supply for the first electrode in the range of about 10 W to about 300 W. The above method may include a plasma power supply for the second electrode in the range of about 10 W to about 300 W. One or more plasma activation time periods may be time periods of about 5 seconds to about 180 seconds.
[0084] The mixed gas plasma may include a gas flow ratio of nitrogen flow to oxygen flow in the range of about 0.01 to about 0.99. The gas flow of the mixed gas plasma may be about 5 sccm to about 100 sccm. The first ambient pressure may be about 10 Pa to about 200 Pa. The method may further include a rinsing process of rinsing and drying the plasma-activated first surface and second surface with ultrasonic-assisted deionized (DI) water. The surface modification process may include the rinsing process. Exposure to ultraviolet radiation may be performed prior to the rinsing process. Alternatively, exposure to ultraviolet radiation may be performed after the rinsing process.
[0085] The above ultraviolet radiation may include electromagnetic radiation having a wavelength in the range of about 150 nm to about 500 nm.
[0086] During the above ultraviolet radiation, the temperature of the first surface and the second surface may be less than about 100°C.
[0087] The above mechanical load may include a piston downward mechanical pressure of 5 kN or less.
[0088] The above thermal annealing process may include the temperature of the bonded precursor composite substrate in one or more temperature ranges at temperatures of 100 ℃, 120 ℃, 150 ℃, 175 ℃, 190 ℃, and 250 ℃.
[0089] The piezoelectric material wafer of the second substrate may include a piezoelectric single crystal selected from the group comprising lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof.
[0090] The above method may additionally include a third substrate bonded to the first substrate in addition to the second substrate, and the third substrate may be a wafer of a piezoelectric material different from the piezoelectric material of the second substrate. The wafer of the piezoelectric material of the third substrate may include a piezoelectric single crystal selected from the group comprising lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof.
[0091] The wafer of the first substrate may include a material substrate selected from the group consisting of silicon (Si), silicon oxide (SiO2), silicon carbide (SiC), cubic boron nitride (c-BN), sapphire, diamond, and any combination thereof.
[0092] In this specification, the term “one embodiment” is used to mean “functioning as an example, case, or illustration.” Any aspect or design described as “one embodiment” in this specification is not necessarily to be interpreted as being more desirable or advantageous than other aspects or designs. The word “exemplary” is used in this specification to mean “functioning as an example, case, or illustration.” Any embodiment or design described as “exemplary” in this specification is not necessarily to be interpreted as being more desirable or advantageous than other embodiments or designs.
[0093] In the detailed description or claims, the words “plural” and “multiple” explicitly mean one or more quantities. In the detailed description or claims, terms such as “group,” “set,” “set,” “sequence,” “sequence,” and “grouping” mean one or more quantities. Any term expressed in a plural form that does not explicitly indicate “plural” or “multiple” likewise means one or more quantities.
[0094] As used herein, the terms “processor” or “controller” may be understood as any kind of technical entity that enables, for example, the processing of data. Data may be processed according to one or more specific functions executed by the processor or controller. Additionally, as used herein, the processor or controller may be understood as any kind of circuit, for example, any kind of analog or digital circuit. Thus, the processor or controller may be an analog circuit, a digital circuit, a mixed-signal circuit, a logic circuit, a processor, a microprocessor, a central processing unit (CPU), a graphics processing unit (GPU), a digital signal processor (DSP), a field programmable gate array (FPGA), an integrated circuit, an application-specific integrated circuit (ASIC), or any combination thereof. Any other kind of implementation of each function may be understood as a processor, a controller, or a logic circuit. It should be understood that any two (or more) processors, controllers, or logic circuits described above in this specification may be realized as a single entity having equivalent functions, etc., and conversely, any single processor, controller, or logic circuit described above in this specification may be realized as two (or more) separate entities having equivalent functions, etc.
[0095] The term "connected" can be understood in the sense of direct or indirect connections and / or interactions (e.g., mechanical and / or electrical). For example, multiple elements may be physically held together (e.g., a plug connected to a socket) and mechanically connected to have an electrically conductive path (e.g., a signal path existing along a communication chain).
[0096] Although the foregoing description and associated drawings depict electronic device components as distinct elements, those skilled in the art will understand the various possibilities for combining or integrating distinct elements into a single element. Such may include combining two or more circuits in a single circuit, mounting two or more circuits on a common chip or chassis to form an integrated element, or running distinct software components on a common processor core. Conversely, those skilled in the art will understand the possibilities for separating a single element into two or more distinct elements, such as dividing a single circuit into two or more distinct circuits, separating a chip or chassis into the originally provided distinct elements, separating software components into two or more sections, or running each on a distinct processor core. Furthermore, specific embodiments of hardware and / or software components are merely exemplary, and other combinations of hardware and / or software performing the methods described herein should be understood to be within the scope of this disclosure.
[0097] It should be understood that embodiments of the method described in detail in this specification are illustrative in nature and may be implemented in the device. Likewise, it should be understood that embodiments of the device described in detail in this specification may be implemented in the method. Accordingly, it should be understood that the device corresponding to the method described in detail in this specification may include one or more components configured to perform each aspect of the relevant method.
[0098] All abbreviations defined in the above description are additionally included in all claims contained in this specification.
[0099] Although the present disclosure has been specifically illustrated and described with reference to specific embodiments, those skilled in the art will understand that various changes in form and detail may be made without departing from the spirit and scope of the present disclosure as defined by the appended claims. Accordingly, the scope of the present disclosure is defined by the appended claims, and all changes within the equivalent scope of the claims are intended to be comprehensive.
Claims
Claim 1 A method for forming a composite substrate comprising: a step of activating the surface of a support wafer and the surface of a piezoelectric material wafer in a plasma system utilizing a plasma generated from a gas mixture of oxygen (O2) and nitrogen (N2); then, a step of performing a surface modification process in which the plasma-activated surface of the support wafer and the plasma-activated surface of the piezoelectric material wafer are exposed to ultraviolet radiation in an atmosphere containing oxygen and nitrogen; then, a step of contacting the surface of the support wafer with the surface of the piezoelectric material wafer in a vacuum environment having a pressure of 0.1 Pa or less and applying a mechanical load to the contacted wafers; and a step of thermally annealing the contacted wafers at a temperature not exceeding 200°C; wherein the support wafer is configured to support the piezoelectric material wafer. Claim 2 A method for forming a composite substrate according to claim 1, further comprising the step of polishing the surface of the wafer and the surface of the piezoelectric material wafer such that the root-mean-square roughness of the surface of the wafer and the surface of the piezoelectric material wafer is each less than 0.5 nm. Claim 3 A method for forming a composite substrate according to claim 1, wherein the atmosphere has a gas flow rate ratio of nitrogen flow rate to oxygen flow rate of 0.01 to 0.
99. Claim 4 A method for forming a composite substrate according to claim 1, wherein the gas flow rate of the atmosphere is 5 sccm to 100 sccm. Claim 5 A method for forming a composite substrate according to claim 1, wherein the plasma activation comprises an ambient pressure in the range of 10 Pa to 200 Pa. Claim 6 A method for forming a composite substrate according to claim 1, wherein the rinsing process further includes a rinsing process, said rinsing process includes megagasonic assisted deionized water for rinsing and drying the plasma-activated surface of the wafer and the plasma-activated surface of the piezoelectric material wafer. Claim 7 A method for forming a composite substrate according to claim 6, wherein the surface modification process includes the rinsing process. Claim 8 A method for forming a composite substrate according to claim 6, wherein the exposure to the ultraviolet radiation is performed prior to the rinsing process. Claim 9 A method for forming a composite substrate according to claim 6, wherein the exposure to the ultraviolet radiation is performed after the rinsing process. Claim 10 A method for forming a composite substrate according to any one of claims 1 to 9, wherein the ultraviolet radiation comprises electromagnetic radiation having a wavelength in the wavelength range of 150 nm to 500 nm. Claim 11 A method for forming a composite substrate according to any one of claims 1 to 9, wherein, during ultraviolet radiation, the temperatures of the surface of the wafer and the surface of the piezoelectric material wafer are less than 100°C. Claim 12 A method for forming a composite substrate according to any one of claims 1 to 9, wherein the mechanical load comprises a piston downward mechanical pressure of up to 5 kN. Claim 13 A method for forming a composite substrate according to any one of claims 1 to 9, wherein the piezoelectric material wafer comprises a piezoelectric single crystal selected from the group consisting of lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof. Claim 14 A method for forming a composite substrate according to any one of claims 1 to 9, further comprising the step of bonding an additional piezoelectric material wafer to a support wafer on the opposite side of the piezoelectric material wafer, wherein the piezoelectric material of the additional piezoelectric material wafer is different from the piezoelectric material of the piezoelectric material wafer. Claim 15 A method for forming a composite substrate according to claim 14, wherein the piezoelectric material of the additional piezoelectric material wafer comprises a piezoelectric single crystal selected from the group consisting of lithium niobate (LN), lithium tantalate (LT), quartz, and any combination thereof. Claim 16 A method for forming a composite substrate according to any one of claims 1 to 9, wherein the wafer comprises a material selected from the group consisting of silicon (Si), silicon oxide (SiO2), silicon carbide (SiC), cubic boron nitride (c-BN), sapphire, diamond, and any combination thereof.
Citation Information
Patent Citations
A method for directly bon a lithium niobate wafer to a silicon wafer by two-step activation using vacuum ultraviolet light followed by nitrogen plasma
CN109166793A
A joint of a piezoelectric material substrate and a support substrate and a method for manufacturing the same
KR1020200100133A
Bonded substrate, surface acoustic wave element, surface acoustic wave element device, and method for manufacturing bonded substrate
US20210108338A1
Substrate bonding method
KR1020090096126A
A joint of a piezoelectric material substrate and a support substrate and a method for manufacturing the same
KR1020200033326A