Conductive material dispersed solution, electrode and lithium secondary battery prepared by using the same

A conductive dispersion with a controlled dispersion index using single-walled carbon nanotubes and a fluorine-based polymer addresses dispersibility issues, enhancing electrode conductivity and energy density in lithium secondary batteries.

KR103045766B1Active Publication Date: 2026-11-10LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020240120769
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-09-06
Filing Date
2024-09-05
Publication Date
2026-11-10
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Existing conductive material dispersions for single-walled carbon nanotubes suffer from poor dispersibility and high viscosity, leading to phase separation and nozzle clogging during the manufacturing of electrodes for lithium secondary batteries, particularly when using materials with large specific surface areas.

Method used

A conductive dispersion comprising single-walled carbon nanotubes and a fluorine-based polymer with a controlled dispersion index (D = [10^6 (1+Wu) / [Mw(1+Ws)(1+MH)]), where Wu is the weight fraction of unsaturated functional groups, Ws is the weight fraction of saturated residual compound units, and MH is the number of moles of heteroatoms, is used to enhance dispersibility and stability.

Benefits of technology

The dispersion achieves excellent dispersibility with low viscosity, improving electrode conductivity and energy density while reducing resistance, and maintaining stability over time.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a conductive material dispersion, an electrode manufactured using the conductive material dispersion, and a secondary battery. The conductive material dispersion comprises a single-walled carbon nanotube, a fluorinated polymer, and an organic solvent. The fluorinated polymer has a dispersion index (D) of 0.10 to 0.90 that reflects the characteristics of unsaturated functional groups, comonomers, or saturated functional groups within the polymer. The conductive material dispersion containing the fluorinated polymer has the advantage of having excellent dispersibility due to low viscosity and a small number of aggregated particles in the dispersed state, and excellent storage stability due to minimal change in viscosity over time.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a conductive dispersion comprising a fluorine-based polymer and a single-walled carbon nanotube, wherein the dispersion index defined by factors affecting dispersibility satisfies a specific value, and to an electrode and a lithium secondary battery to which the dispersion is applied. Background Technology

[0003] Due to the rapid increase in the use of fossil fuels, there is a growing demand for alternative or clean energy. As part of this effort, the fields of power generation and energy storage utilizing electrochemical reactions are the most actively researched.

[0004] Currently, a representative example of an electrochemical device utilizing such electrochemical energy is the secondary battery, and its scope of application is increasingly expanding. Recently, with the technological development and growing demand for portable devices such as portable computers, mobile phones, and cameras, the demand for secondary batteries as an energy source has been rapidly increasing. Among these secondary batteries, much research has been conducted on lithium secondary batteries, which have high energy density—that is, high capacity—and have been commercialized and are widely used.

[0005] The electrode of a secondary battery comprises an electrode active material, a conductive material, and a binder. Carbon nanotubes can be used as the conductive material to improve the conductivity of the electrode; in particular, when a material with a large specific surface area is applied, the conductivity improvement effect is excellent even when using a small amount.

[0006] Meanwhile, when single-walled carbon nanotubes are used instead of multi-walled carbon nanotubes, the resistance of the electrode can be further lowered, and since the specific surface area is relatively large, it is easy to secure conductivity with only a small amount. In order for the single-walled carbon nanotubes to be uniformly distributed within the electrode, when manufacturing the electrode, a conductive material dispersion in which the single-walled carbon nanotubes are dispersed is first formed, and then an electrode slurry is prepared using the conductive material dispersion.

[0007] A high-pressure homogenizer is used to prepare the above-mentioned conductive material dispersion. Specifically, within the high-pressure homogenizer, a pre-mixed solution containing bundled single-walled carbon nanotubes, a dispersant, and a dispersion medium is passed through a nozzle with a diameter of 80 μm to 800 μm under a high pressure of 100 bar to 2,500 bar, thereby applying a shear force to the bundled single-walled carbon nanotubes and causing the dispersion of the bundled single-walled carbon nanotubes.

[0008] Meanwhile, when a solution containing bundled single-walled carbon nanotubes, a dispersant, and a dispersion medium is pre-mixed, the bundled carbon nanotubes in the solution must be effectively de-bundled by the dispersant to enable a dispersion process using a high-pressure homogenizer, thereby finally producing a conductive material dispersion in which single-walled carbon nanotubes are uniformly dispersed. Conversely, if de-bundling is not smooth during the pre-mixing, phase separation occurs between the bundled carbon nanotubes and the dispersion medium in the solution, causing the nozzle of the high-pressure homogenizer to become clogged by the bundled carbon nanotubes, making the dispersion process using the high-pressure homogenizer impossible.

[0009] To address these dispersibility issues, conventional methods involve incorporating an auxiliary dispersant into the conductive material dispersion along with hydrogenated nitrile butadiene rubber, which acts as a dispersant. However, this problem becomes particularly pronounced when applying carbon nanotubes with large specific surface areas, such as single-walled carbon nanotubes, and causes various issues due to high viscosity. Therefore, there is a need for research on conductive material dispersions capable of improving the dispersibility of single-walled carbon nanotubes. The problem to be solved

[0011] One objective according to the present invention is to provide a conductive material dispersion with a controlled dispersion index by applying a dispersant with controlled weight-average molecular weight and functional group content to achieve excellent dispersibility and storage stability, while having a low content of large-sized carbon nanotubes.

[0012] In addition, the aim is to provide a conductive material dispersion comprising a modified polysiloxane-based material capable of further maximizing such dispersibility in the dispersion with excellent dispersibility described above.

[0013] Another objective according to the present invention is to provide an electrode and a secondary battery manufactured using the conductive material dispersion solution. means of solving the problem

[0015] [1] According to one embodiment of the present invention, a conductive dispersion is provided comprising a single-walled carbon nanotube and a fluorine-based polymer, wherein the fluorine-based polymer has a dispersion index (D) defined by Formula 1 below of 0.10 to 0.90.

[0016] [Equation 1]

[0017] D = [10 6 (1+W u )] / [M w (1+W s )(1+M H )]

[0018] In Equation 1 above, Mw is the unitless number of the weight-average molecular weight (g / mol) of the fluorinated polymer, and W u is the weight fraction of unsaturated functional group units in the fluorinated polymer, and W s is the weight fraction of saturated residual compound units in the fluorinated polymer, and M H is the number of moles of heteroatoms in a saturated residual compound unit, where the saturated residual compound unit is one or more selected from a saturated functional group unit and a comonomer unit.

[0019] [2] In the above [1], the conductive material dispersion may further include a modified polysiloxane-based material.

[0020] [3] In the above [2], the modified polysiloxane-based material may have a molecular weight of 4,000 g / mol to 8,000 g / mol.

[0021] [4] In at least one of [2] and / or [3] above, the modified polysiloxane-based material may include a polydialkyl siloxane, and the alkyl may have 1 to 5 carbon atoms.

[0022] [5] In at least one of [1] to [4] above, the fluorine-based polymer may be polyvinylidene fluoride.

[0023] [6] In at least one of [1] to [5] above, the unsaturated functional group of the fluorinated polymer may include a carboxyl group.

[0024] [7] In at least one of [1] to [6] above, the saturated functional group may include an alkoxy group having 1 to 5 carbon atoms, and the comonomer unit may include a hexafluoropropylene unit.

[0025] [8] In at least one of [1] to [7] above, the unsaturated functional group of the fluorinated polymer may be included in an amount of 0.01% to 1.0% by weight relative to the total weight of the polymer.

[0026] [9] In at least one of [1] to [8] above, the saturated residual compound unit of the fluorinated polymer may be included in an amount of 0.01% to 5.0% by weight relative to the total weight of the polymer.

[0027]

[10] In at least one of [1] to [9] above, the fluorine-based polymer may have a weight-average molecular weight of 1,000,000 g / mol to 2,000,000 g / mol.

[0028]

[11] According to another embodiment of the present invention, an electrode is provided comprising an electrode active material, a single-walled carbon nanotube, and a fluorine-based polymer, wherein the fluorine-based polymer has a dispersion index (D) represented by the following formula 1 of 0.10 to 0.90.

[0029] [Equation 1]

[0030] D = [10 6 (1+W u )] / [M w (1+W s )(1+M H )]

[0031] In Equation 1 above, Mw is the unitless number of the weight-average molecular weight (g / mol) of the fluorinated polymer, and W u is the weight fraction of unsaturated functional group units in the fluorinated polymer, and W s is the weight fraction of saturated residual compound units in the fluorinated polymer, and M H is the number of moles of heteroatoms in a saturated residual compound unit, where the saturated residual compound unit is one or more selected from a saturated functional group unit and a comonomer unit.

[0032]

[12] According to another embodiment of the present invention, a lithium secondary battery is provided having a structure in which electrodes and separators are alternately stacked, and the electrodes are the aforementioned electrodes. Effects of the invention

[0034] The conductive material dispersion according to the present invention has excellent dispersibility with low viscosity and low content of large-sized carbon nanotubes by controlling the dispersion index defined from the relationship between factors affecting dispersibility in the fluorine-based polymer included as a dispersant, and can have excellent storage stability due to the small change in viscosity over time.

[0035] In addition, by including the above conductive material dispersion in the electrode slurry, the phase stability of the slurry can be improved, and sufficient conductivity can be secured with only a small amount of carbon nanotubes, thereby enabling the realization of an electrode with high energy density.

[0036] Furthermore, high-power batteries can be realized in that resistance can be improved despite reducing the content of conductive material in the slurry due to excellent dispersibility. Specific details for implementing the invention

[0038] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0039] In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and do not exclude the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0040] In this specification, "specific surface area" is measured by the BET method, and specifically, can be calculated from the amount of nitrogen gas adsorbed at a liquid nitrogen temperature (77K) using BEL SORP-mino II of BEL Japan.

[0041] D in this specification 10 , D 50 and D 90 In the particle size distribution curve of silver particles, they can be defined as the particle sizes corresponding to 50% and 90% of the cumulative volume, respectively. The above D 50 and D 90For example, it can be measured using the laser diffraction method. The laser diffraction method generally enables the measurement of particle sizes ranging from the submicron range to several millimeters, and can obtain results with high reproducibility and high resolution.

[0042] In this specification, "weight-average molecular weight (Mw)" refers to a converted value for standard polystyrene measured by gel permeation chromatography (GPC). Specifically, the weight-average molecular weight is a converted value obtained by measuring the value using GPC under the following conditions, and standard polystyrene from Agilent Systems was used for the calibration curve.

[0043] <Measurement Conditions>

[0044] Measuring instrument: Agilent GPC (Agilent 1200 series, USA)

[0045] Column: PL Mixed B 2 connected

[0046] Column temperature: 40℃

[0047] Eluent: Tetrohydrofuran

[0048] Flow rate: 1.0 mL / min

[0049] Concentration: ~1 mg / mL (100 μL injection)

[0051] The present invention will be described in detail below.

[0052] In this specification, each of the conductive material dispersion, electrode, and lithium secondary battery comprises one or more of the technical features and / or technical configurations described below, and these technical features and / or technical configurations may be combined in various ways.

[0054] Dispersed conductive material

[0055] A conductive material dispersion according to one embodiment of the present invention comprises a single-walled carbon nanotube and a fluorine-based polymer, wherein the fluorine-based polymer has a dispersion index (D) defined by Formula 1 below of 0.10 to 0.90.

[0056] [Equation 1]

[0057] D = [10 6 (1+W u )] / [M w (1+W s )(1+M H )]

[0058] In Equation 1 above, Mw is the unitless number of the weight-average molecular weight (g / mol) of the fluorinated polymer, and W u is the weight fraction of unsaturated functional groups in the fluorinated polymer, and W s is the weight fraction of saturated residual compound units in the fluorinated polymer, and M H is the number of moles of heteroatoms in a saturated residual compound unit, where the saturated residual compound unit is one or more selected from a saturated functional group unit and a comonomer unit.

[0060] (1) Single-walled carbon nanotube

[0061] Carbon nanotubes are graphite sheets that have a cylindrical shape with a nano-sized diameter and possess an sp2 bonding structure; they exhibit conductive or semiconductor properties depending on the rolling angle and structure of the graphite sheets. Carbon nanotubes can be classified into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT) based on the number of bonds forming the walls.

[0062] According to one embodiment of the present invention, the conductive material dispersion comprises single-walled carbon nanotubes. Since single-walled carbon nanotubes have a larger specific surface area compared to multi-walled carbon nanotubes, sufficient conductivity can be ensured even with only a small amount added, thereby significantly increasing the reduction in electrode resistance.

[0063] D of the above single-walled carbon nanotube 50 The size may be 2 μm to 8 μm, specifically 3 μm or more, or 4 μm or more, and also 7 μm or less, or 6 μm or less. D of the single-walled carbon nanotube above 90 The range may be 10 μm to 30 μm, specifically 12 μm or more, 14 μm or more, 16 μm or more, or 18 μm or more, and may also be 28 μm or less, 26 μm or less, 24 μm or less, or 22 μm. Satisfying the above range means that the bundled carbon nanotubes used as raw materials are effectively dispersed within the conductive material dispersion, and thus the electrode and battery resistance is effectively improved.

[0064] The carbon nanotubes may be included in an amount of 0.4 to 2.0 parts by weight per 100 parts by weight of the conductive material dispersion, specifically 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, or 0.8 parts by weight or more, and may also be included in an amount of 1.7 parts by weight or less, 1.5 parts by weight or less, 1.3 parts by weight or less, or 1.2 parts by weight or less. When the above ranges are satisfied, high productivity is maintained while the transfer and input of the electrode slurry are easy. In addition, since the solid content of the manufactured electrode slurry does not become excessively low, binder migration during electrode drying can be suppressed. Accordingly, electrode adhesion can be improved, and packing of the electrode active material layer is effectively achieved, allowing for the manufacture of a low-thickness electrode.

[0066] (2) Fluoropolymer

[0067] A conductive material dispersion according to one embodiment of the present invention comprises a fluorine-based polymer, wherein the fluorine-based polymer satisfies a dispersion index (D) defined by Formula 1 below of 0.10 to 0.90.

[0068] [Equation 1]

[0069] D = [10 6 (1+W u )] / [M w (1+W s )(1+M H )]

[0070] In Equation 1 above, Mw is the unitless number of the weight-average molecular weight (g / mol) of the fluorinated polymer, and W u is the weight fraction of unsaturated functional groups in the fluorinated polymer, and W s is the weight fraction of saturated residual compound units in the fluorinated polymer, and M H is the number of moles of heteroatoms in a saturated residual compound unit, where the saturated residual compound unit is one or more selected from a saturated functional group unit and a comonomer unit.

[0071] The above dispersion index establishes the relationship between factors that can influence the dispersion of single-walled carbon nanotubes when using a fluorinated polymer as a dispersant, taking into account the weight-average molecular weight of the fluorinated polymer, the content of unsaturated functional groups within the fluorinated polymer, and the content of saturated residual compound units.

[0072] How well a polymer used as a dispersant can disperse single-walled carbon nanotubes depends on how the polar and non-polar parts present within the polymer acting as the dispersant interact between the non-polar carbon nanotubes and the polar organic solvent.

[0073] The above dispersion index reflects the weight fraction of highly polar unsaturated functional groups within the fluorinated polymer, while also reflecting the weight fraction of saturated residual compound units that are polar but whose polarity is not relatively large compared to the unsaturated functional groups; however, it balances the influence of the unsaturated functional groups by considering that, in the case of saturated residual compound units, the number of moles of heteroatoms (e.g., F, N, P, or O) contained within the unit also has an effect.

[0074] It is difficult to accurately determine the degree of dispersion of single-walled carbon nanotubes using only these factors, and it may be necessary to reflect the influence of the polymer itself rather than just the units within the polymer; for example, the weight-average molecular weight was incorporated as a factor to account for the effects of steric hindrance or the overall molecular size.

[0075] The dispersion index derived in this way can be viewed as an index that can more accurately determine how well single-walled carbon nanotubes can be dispersed, and the dispersion index is characterized by being 0.10 to 0.90. The dispersion index may preferably be 0.11 or higher, 0.12 or higher, or 0.13 or higher, and may also be 0.85 or lower, 0.80 or lower, 0.75 or lower, 0.70 or lower, or 0.68 or lower, and most preferably 0.14 to 0.67.

[0076] Since various factors are reflected in the above dispersion index, a conductive material dispersion with excellent dispersibility can be provided as the value becomes smaller; however, if it is less than 0.10, the weight-average molecular weight relative to the content of unsaturated functional groups is too large, so there is a concern that the contribution to the dispersion of carbon nanotubes will be small due to the attractive forces between the polymers, and as the influence of the saturated residual compound unit becomes greater than the influence of the unsaturated functional group, there is a concern that large aggregates will be formed in the dispersion even if the viscosity of the dispersion is lowered.

[0077] When the above dispersion index is greater than 0.90, it is difficult to consider that carbon nanotubes are properly dispersed, resulting in high viscosity and a problem where the content of large particles also increases.

[0078] The above-mentioned fluorine-based polymer may be one or more polymers selected from the group consisting of polyvinylidene fluoride (PVDF), polyperfluoroalkoxy (PFA), polytetrafluoroethylene (PTFE), and copolymers in which these are copolymerized with comonomers, and preferably may be polyvinylidene fluoride. When the above-mentioned polyvinylidene fluoride is applied in the dispersion of single-walled carbon nanotubes, it has excellent affinity with the organic solvent used, which enables the formation of a polymer solution, and thus has the advantage of excellent processability.

[0079] The above-mentioned fluorine-based polymer may include a carboxyl group as an unsaturated functional group, and the unsaturated functional group may be included in an amount of 0.01% to 1.00% by weight relative to the total weight of the polymer, preferably 0.02% or more, 0.03% or more, or 0.05% or more by weight, and 0.90% or less, 0.80% or less by weight, preferably 0.75% or less by weight. The unsaturated functional group is a major factor that causes polar properties, and it may be desirable to control the appropriate content to contribute to the dispersion of single-walled carbon nanotubes.

[0080] The above-mentioned fluorine-based polymer may include saturated residual compound units, and the saturated residual compound units may refer to saturated functional groups and / or comonomer units. In the present invention, the term "saturated residual compound unit" may refer to the remaining compound units excluding the main monomer unit and the unsaturated functional group. Among these saturated residual compound units, the saturated functional group may include an alkoxy group having 1 to 5 carbon atoms, and the comonomer unit may include one or more selected from the group consisting of hexafluoropropylene units and chlorotrifluoroethylene.

[0081] The above-mentioned saturated residual compound unit may be included in an amount of 0.01% to 5.0% by weight relative to the total weight of the polymer, preferably 0.02% or more, 0.03% or more by weight, and may also be included in an amount of 4.0% or less, 3.0% or less by weight, or 2.5% or less by weight. Furthermore, the number of moles of heteroatoms included in the saturated residual compound unit may be 1 to 6, and this is considered together with the content of the above-mentioned saturated residual compound unit so that the effect of the saturated residual compound unit on dispersibility is reflected in proportion to how much electronegative heteroatom is included.

[0083] The above fluorinated polymer may have a weight-average molecular weight of 1,000,000 g / mol to 2,000,000 g / mol. It may be desirable to control the weight-average molecular weight so that it is not too small or too large, thereby ensuring that the dispersion index satisfies the above-mentioned range.

[0084] In the above conductive material dispersion, the fluorine-based polymer may be included in an amount of 0.5 to 6.0 parts by weight per 100 parts by weight of the conductive material dispersion, specifically 0.8 parts by weight or more, 1.0 parts by weight or more, 1.5 parts by weight or more, 2.0 parts by weight or more, or 2.4 parts by weight or more, and may also be included in an amount of 5.0 parts by weight or less, 4.0 parts by weight or less, 3.0 parts by weight or less, or 2.6 parts by weight or less. When the above range is satisfied, the carbon-based conductive material can be smoothly dispersed in the conductive material dispersion, and the energy density of the electrode being manufactured can be improved and the resistance can be reduced.

[0086] The above conductive material dispersion may additionally include a dispersant in addition to the above fluorine-based polymer, and may, for example, include a hydrogenated nitrile-based copolymer. The hydrogenated nitrile-based copolymer may be a copolymer comprising α,β-unsaturated nitrile-derived structural units and hydrogenated conjugated diene-derived structural units, or a copolymer comprising α,β-unsaturated nitrile-derived structural units, conjugated diene-derived structural units, and hydrogenated conjugated diene-derived structural units. The hydrogenated nitrile-based copolymer may be hydrogenated nitrile butadiene rubber, specifically hydrogenated acrylonitrile-butadiene rubber, more specifically partially hydrogenated acrylonitrile-butadiene rubber.

[0088] (3) Modified polysiloxane-based material

[0089] A conductive material dispersion according to one embodiment of the present invention may further include a modified polysiloxane-based material. The modified polysiloxane-based material may have a molecular weight of 4,000 g / mol to 8,000 g / mol, and preferably 4,500 g / mol to 7,500 g / mol.

[0090] The above modified polysiloxane-based material may be affected by the dispersion index of the aforementioned fluorine-based polymer. When added together with a fluorine-based polymer whose dispersion index does not fall within the range of 0.10 to 0.90, a viscosity reduction effect can be expected, but the content of large particles may increase, leading to a problem of deteriorating dispersibility. However, when added together with a fluorine-based polymer that satisfies the dispersion index, a viscosity reduction effect can be expected without deteriorating dispersibility, and thus the effect of adding the modified polysiloxane-based material can be maximized. Therefore, it is desirable to add the above modified polysiloxane-based material to reduce viscosity by considering the dispersion index.

[0091] The polysiloxane portion of the above modified polysiloxane material may include dialkyl siloxane as a monomer unit, and in the case of the dialkyl siloxane, the alkyl group may have 1 to 5 carbon atoms. For example, the polysiloxane portion may include polydimethyl siloxane, polymethylethyl siloxane, polymethylpropyl siloxane, etc.

[0092] Preferably, the modified polysiloxane-based material may be a polyether-based modified polysiloxane-based material modified by a polyether-based material, in which case the polyether-based material may be modified in a form in which the polyether-based material is bonded to the alkyl group. The polyether-based material may include homopolymers such as polyethylene glycol, propoxylated polyethylene glycol, polypropylene glycol, and ethoxylated polypropylene glycol; random copolymers thereof; or block copolymers thereof.

[0093] The above-mentioned polyether-modified polysiloxane-based material may be in the form of, for example, a block copolymer of a polyether-based material and a polysiloxane-based material. The above-mentioned modified polysiloxane-based material may be in the form where the polyether-based material is distributed on one side and the polysiloxane-based material is distributed on the other side, and these two materials are connected by covalent bonds.

[0094] For example, the weight ratio of the polysiloxane-based material and the polyether-based material of the modified polysiloxane-based material may be about 95:5 to 5:95, preferably 70:30 to 10:90, 60:40 to 10:90, 50:50 to 10:90, 40:60 to 10:90, and more preferably 30:70 to 10:90.

[0095] As the above-described modified polysiloxane-based material is modified in this manner, it possesses both polar and non-polar parts within the molecule, which can further enhance interactions with fluorinated polymers and conductive materials, and further improve dispersibility. In particular, since it can significantly influence the dispersion index through interactions with the functional groups of fluorinated polymers, a substantial synergistic effect can be expected.

[0097] (4) Organic solvent

[0098] The above organic solvent may be an organic solvent comprising one or more heteroatoms selected from the group consisting of nitrogen atoms (N) and oxygen atoms (O) having non-covalent electron pairs.

[0099] Specifically, the organic solvent is an amide-based polar organic solvent such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc), or N-methylpyrrolidone (NMP); alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol, or octanol; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, or hexylene glycol; and polyhydric alcohols such as glycerin, trimethylolpropane, pentaerythritol, or sorbitol. Examples include glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, or tetraethylene glycol monobutyl ether; ketones such as acetone, methyl ethyl ketone, methylpropyl ketone, or cyclopentanone; esters such as ethyl acetate, γ-butyl lactone, and ε-propiolactone, and any one or a mixture of two or more of these may be used. N-methylpyrrolidone (NMP) is particularly preferred when considering miscibility with the electrode slurry.

[0101] In the above conductive material dispersion, the solid content of the conductive material dispersion may be 1% to 10% by weight, specifically 2% to 8% by weight, and more specifically 3.5% to 5.5% by weight. When the above range is satisfied, the viscosity of the conductive material dispersion can be maintained at a low level, while the dispersion of the conductive material dispersion can be effectively achieved. Here, solid content may refer to single-walled carbon nanotubes and fluorinated polymers contained in the conductive material dispersion.

[0103] The conductive material dispersion described above can be prepared by mixing single-walled carbon nanotubes, a fluorinated polymer, and an organic solvent. At this time, the mixing can be performed using conventional mixing methods, specifically using a mixing device such as a homogenizer, a bead mill, a ball mill, a basket mill, an attrition mill, a universal stirrer, a clear mixer, a spike mill, or a TK mixer, and the order of mixing of each component is not particularly limited. That is, the conductive material dispersion according to the present invention may be prepared by adding single-walled carbon nanotubes to an organic solvent and then adding and mixing a fluorinated polymer; by adding a fluorinated polymer to an organic solvent first and then mixing the single-walled carbon nanotubes; or by adding both single-walled carbon nanotubes and a fluorinated polymer to an organic solvent together and then mixing.

[0104] Meanwhile, cavitation dispersion treatment may be performed to enhance the dispersibility of single-walled carbon nanotubes during the above mixing process. The cavitation dispersion treatment is a dispersion method that utilizes shock waves generated by the rupture of vacuum bubbles formed in water when high energy is applied to a liquid, and this method allows for dispersion without damaging the properties of single-walled carbon nanotubes. Specifically, the cavitation dispersion treatment may be performed by ultrasound, a jet mill, or shear dispersion treatment.

[0106] electrode

[0107] An electrode according to another embodiment of the present invention comprises an electrode active material, a single-walled carbon nanotube, and a fluorine-based polymer, wherein the dispersion index of the fluorine-based polymer is as described above.

[0108] The above electrode may include a current collector and an electrode active material layer disposed on the current collector, and the electrode active material layer may include an electrode active material, a single-walled carbon nanotube, and a fluorine-based polymer.

[0109] The electrode active material layer may be formed from an electrode slurry composition comprising an electrode active material, a conductive material dispersion, and a binder. Specifically, the electrode comprises an electrode current collector and an electrode active material layer formed on the electrode current collector, and the electrode active material layer may be formed by an electrode slurry composition comprising an electrode active material, a conductive material dispersion, and a binder.

[0110] At this time, the conductive material dispersion is the conductive material dispersion according to the present invention described above. Since the details regarding the conductive material dispersion are the same as those described above, a detailed explanation is omitted, and the remaining components are described below.

[0112] The above electrode current collector is not particularly limited as long as it is a material that is conductive without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, alloys thereof, materials surface-treated with carbon, nickel, titanium, silver, etc., or calcined carbon, etc. may be used.

[0113] The above electrode current collector can typically have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to strengthen the bonding force of the negative active material. In addition, the above electrode current collector can be used in various forms, such as, for example, a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.

[0114] Meanwhile, the electrode active material (a) included in the electrode active material layer may be a positive electrode active material or a negative electrode active material commonly used in the relevant technical field, and its type is not particularly limited.

[0115] For example, as the positive electrode active material, a lithium oxide containing lithium and one or more metals such as cobalt, manganese, nickel, or aluminum may be used. More specifically, the lithium oxide is a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), or a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y1 Mn Y1 O2(here, 0 <Y1<1), LiNi Z1 Mn 2-Z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y2 Co Y2 O2(here, 0 <Y2<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y3 Mn Y3 O2(here, 0 <Y3<1), LiMn 2-Z2 Co Z2 O4 (where 0 < Z2 < 2), etc.), lithium-nickel-cobalt-manganese oxides (e.g., Li(Ni P1 Co Q1 Mn R1 )O2(where, 0<P1<1, 0<Q1<1, 0<R1<1, P1+Q1+R1=1) or Li(Ni P2 Co Q2 Mn R2 )O4 (where 0<P2<2, 0<Q2<2, 0<R2<2, P2+Q2+R2=2), etc.), or lithium-nickel-cobalt-manganese-other metal (M) oxide (e.g., Li(Ni P3 Co Q3 Mn R3 M 1 S )O2(here, M 1The elements are selected from the group consisting of Al, Cu, Fe, V, Cr, Ti, Zr, Zn, Ta, Nb, Mg, B, W, and Mo, and P3, Q3, R3, and S are each atomic fractions of independent elements, such as 0 < P3 < 1, 0 < Q3 < 1, 0 < R3 < 1, 0 < S < 1, P3 + Q3 + R3 + S = 1), etc., and any one or more of these compounds may be included.

[0116] Meanwhile, as the negative electrode active material, carbonaceous materials such as, for example, artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic materials capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; SiO v (0 <v<2), SnO2, 바나듐 산화물, 리튬 바나듐 산화물과 같이 리튬을 도프 및 탈도프할 수 있는 금속산화물; 또는 Si-C 복합체 또는 Sn-C 복합체과 같이 상기 금속질 화합물과 탄소질 재료를 포함하는 복합물 등을 들 수 있으며, 이들 중 어느 하나 또는 둘 이상의 혼합물이 사용될 수 있다. 또한, 상기 음극활물질로서 금속 리튬 박막이 사용될 수도 있다. 또, 탄소재료는 저결정 탄소 및 고결정성 탄소 등이 모두 사용될 수 있다.

[0117] The above electrode active material may be included in an amount of 90% to 99% by weight, preferably 95% to 99% by weight, based on the total solid content in the electrode slurry composition. When the content of the electrode active material satisfies the above range, excellent energy density, electrode adhesion, and electrical conductivity can be achieved.

[0119] The above binder is intended to secure adhesion between electrode active materials or between electrode active materials and current collectors, and general binders used in the relevant technical field may be used, and the type thereof is not particularly limited. Examples of the above binders include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.

[0120] The binder may be included in an amount of 5% by weight or less based on the total solid content in the electrode slurry composition, and preferably in an amount of 1% to 3% by weight. When the binder content satisfies the above range, excellent electrode adhesion can be achieved while minimizing the increase in electrode resistance.

[0121] Meanwhile, the electrode slurry composition may additionally include a solvent as needed to control viscosity, etc. In this case, the solvent may be water, an organic solvent, or a mixture thereof. Examples of the organic solvents include amide-based polar organic solvents such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP); and alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol, or octanol. Glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, or hexylene glycol; polyhydric alcohols such as glycerin, trimethylolpropane, pentaerythritol, or sorbitol; glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, or tetraethylene glycol monobutyl ether; Examples include ketones such as acetone, methyl ethyl ketone, methylpropyl ketone, or cyclopentanone; esters such as ethyl acetate, γ-butyl lactone, and ε-propiolactone; any one or more of these may be used, but are not limited thereto.

[0122] The solvent may be included in an amount such that the solid content in the electrode slurry is 60% to 85% by weight, preferably 65% ​​to 80% by weight. When the above range is satisfied, binder migration is suppressed, so electrode adhesion can be improved, the drying temperature can be lowered to improve coating properties, and the coating speed can be increased to improve productivity.

[0124] An electrode according to the present invention can be manufactured by applying an electrode slurry composition containing the above-mentioned components and drying it to form an electrode active material layer. Specifically, the electrode active material layer can be formed by a method of applying an electrode slurry onto an electrode current collector and then drying it, or by applying an electrode slurry onto a separate support and then laminating a film obtained by peeling it off from the support onto an electrode current collector. If necessary, after forming the electrode active material layer through the above-mentioned method, a rolling process may be additionally performed. At this time, drying and rolling may be performed under appropriate conditions considering the physical properties of the electrode to be finally manufactured, and are not particularly limited.

[0126] lithium secondary battery

[0127] A lithium secondary battery according to another embodiment of the present invention has a structure in which electrodes and separators are alternately stacked, and the electrodes include the aforementioned electrodes. Specifically, the secondary battery according to the present invention may include a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode may be the electrode of the above-described embodiment.

[0128] As the electrode according to the present invention has been described above, a detailed explanation is omitted, and only the remaining components will be described below.

[0129] The above separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions; any separator typically used in secondary batteries can be used without any special restrictions. Specifically, as the separator, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.

[0131] Examples of the above electrolytes that can be used in the manufacture of lithium secondary batteries include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., but are not limited to these.

[0132] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0133] As the above-mentioned non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyl lactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolone, formamide, dimethylformamide, dioxolan, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolan derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, ethyl propionate, etc. may be used.

[0134] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.

[0135] The metal salt mentioned above may be a lithium salt, and the lithium salt is a substance that dissolves well in the non-aqueous electrolyte; for example, as the anion of the lithium salt, F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 -, CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more types selected from the group consisting of can be used.

[0136] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride.

[0138] Examples

[0139] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0141] Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3

[0142] 2.0 parts by weight of polyvinylidene fluoride (PVDF), 1.0 parts by weight of single-walled carbon nanotubes (Tuball, OcSiAl), and 97 parts by weight of N-methylpyrrolidone were mixed as fluorine-based polymers having the characteristics described in Table 1 below, and then mixed for 180 minutes using a mixer (BTM-50, disper 1000 rpm / anchor 100 rpm). The mixed mixture was stirred for 30 minutes using a high-pressure homogenizer (Micronox, Picomax MN230A, pressure: 1,500 bar) to obtain conductive material dispersions.

[0143] M W (g / mol x10 6 ) Main monomer unit (weight fraction) Unsaturated functional groups (weight fraction) Saturated residual compound unit (weight fraction) Diversification index Saturated functional group comonomer unit Heteroatom moles Example 1-1 1.5 0.995 0.005 0 0 0 0.67 Examples 1-2 1.0 0.998 0.0015 0.0005 0 1 0.50 Examples 1-3 1.0 0.970 0.005 0 0.025 6 0.14 Comparative Example 1-1 1.0 0.995 0.005 0 0 0 1.01 Comparative Example 1-2 0.9 1.000 0 0 0 0 1.11 Comparative Examples 1-3 2.0 0.900 0.02 0 0.08 6 0.067

[0144] Experimental Example 1: Particle Size Analysis

[0145] The particle size of each conductive material dispersion of the Examples and Comparative Examples was analyzed using laser diffraction and is shown in Table 2. Specifically, after dispersing the conductive material dispersion in a solvent, it was introduced into a laser diffraction particle size measuring instrument (Malvern Mastersizer 3000) to calculate the particle size distribution by measuring the difference in diffraction patterns according to particle size as the particles passed through the laser beam. By confirming the particle size at the points corresponding to 10%, 50%, and 90% of the cumulative volume distribution according to particle size, D 10 , D 50 and D 90 Measured.

[0147] Experimental Example 2: Viscosity Analysis (Immediately after preparation of conductive material dispersion)

[0148] The viscosity of the conductive material dispersion prepared according to the above examples and comparative examples was measured at 25°C and 12 rpm using a viscometer (Brookfield, viscometer DV2T, LV) and is shown in Table 2.

[0150] Experimental Example 3: Confirmation of viscosity increase during long-term storage

[0151] For the conductive material dispersions prepared according to the examples and comparative examples, the viscosity increase rate (%) according to the following formula was determined.

[0152] Viscosity increase rate (%) = {(Viscosity of conductive material dispersion measured after 4 weeks of storage at 25℃ - Viscosity of conductive material dispersion immediately after manufacturing) / Viscosity of conductive material dispersion immediately after manufacturing} × 100

[0153] Entry to the island Viscosity (cp) Viscosity (cp) after 4 weeks of storage Viscosity increase rate (%) D 10 (㎛) D 50 (㎛) D 90 (㎛) Example 1-1 1.39 9.66 36.2 6,090 6,608 8.5 Examples 1-2 1.48 11.10 37.4 7,620 8,542 12.1 Examples 1-3 2.05 13.80 43.6 5,940 6,605 11.2 Comparative Example 1-1 2.70 15.00 48.5 9,600 11,060 15.2 Comparative Example 1-2 1.99 13.30 45.9 9,120 10,960 20.2 Comparative Examples 1-3 3.00 17.10 51.2 12,050 14,580 21.0

[0154] Referring to Table 1 above, in the case of Examples 1-1 to 1-3, in which the dispersion index falls within the range of 0.1 to 0.9, the viscosity is low and the change over time is small, and the average particle size at 90% cumulative volume is relatively smaller compared to the comparative examples.

[0156] Experimental Example 4: Evaluation of Addition of Modified Polysiloxane-Based Material

[0157] In the conductive material dispersions of Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3 above, 0.5 parts by weight of a modified polysiloxane-based material with a molecular weight of 6,000 g / mol (modified by combining about 0.15 parts by weight of polydimethylsiloxane (PDMS) and about 0.85 parts by weight of polyethylene glycol) and 1.5 parts by weight of polyvinylidene fluoride were added instead of 2.0 parts by weight of polyvinylidene fluoride, which is the dispersant, to prepare the conductive material dispersions of Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-3, and the viscosity and particle size characteristics were evaluated in the same manner as in Experimental Examples 1 to 3 above, and the results are shown in Table 3 below.

[0158] Entry to the island Viscosity (cp) Viscosity (cp) after 4 weeks of storage Viscosity increase rate (%) D 10 (㎛) D 50 (㎛) D 90 (㎛) Example 2-1 1.51 12.4 39.6 5,910 6,560 11.2 Example 2-2 1.60 11.7 42.0 4,800 5,424 13.1 Examples 2-3 1.60 17.1 41.0 4,750 5,370 13.0 Comparative Example 2-1 1.86 14.3 57.1 7,140 8,211 15.1 Comparative Example 2-2 1.58 14.0 55.0 7,320 8,200 12.1 Comparative Example 2-3 1.53 14.0 54.0 7,000 7,800 11.5

[0159] Referring to Table 3 above, it can be confirmed through Examples 2-1 to 2-3 that when a modified polysiloxane-based material is added to Examples 1-1 to 1-3, which have a dispersion index of 0.10 to 0.90, there is an effect of lowering viscosity, and it can be seen that this effect is also observed in Comparative Examples 2-1 to 2-3, which are cases where the material is added to Comparative Examples 1-1 to 1-3, which do not satisfy the dispersion index.

[0160] However, in the case of Comparative Examples 2-1 to 2-3, D 90 It can be confirmed that this has increased significantly, and through this, it can be seen that if the dispersion index is not satisfied, adding modified polysiloxane-based materials may actually have an adverse effect on dispersibility.

Claims

Claim 1 A conductive dispersion comprising single-walled carbon nanotubes and a fluorinated polymer, wherein the fluorinated polymer has a dispersion index (D) defined by the following Formula 1 of 0.10 to 0.90: [Formula 1] D = [10 6 (1+W u )] / [M w (1+W s )(1+M H In the above Equation 1, Mw is the unitless number of the weight-average molecular weight (g / mol) of the fluorinated polymer, and W u is the weight fraction of unsaturated functional group units in the fluorinated polymer, and W s is the weight fraction of saturated residual compound units in the fluorinated polymer, and M H is the number of moles of heteroatoms in a saturated residual compound unit, wherein the saturated residual compound unit is one or more selected from a saturated functional group unit and a comonomer unit, the saturated functional group includes an alkoxy group having 1 to 5 carbon atoms, and the comonomer unit includes one or more selected from the group consisting of a hexafluoropropylene unit and a chlorotrifluoroethylene. Claim 2 A conductive dispersion according to claim 1, wherein the conductive dispersion further comprises a modified polysiloxane-based material. Claim 3 In claim 2, the modified polysiloxane-based material is a conductive material dispersion having a molecular weight of 4,000 g / mol to 8,000 g / mol. Claim 4 A conductive material dispersion according to claim 2, wherein the modified polysiloxane-based material comprises a polydialkyl siloxane, and the alkyl has 1 to 5 carbon atoms. Claim 5 A conductive material dispersion according to claim 1, wherein the fluorine-based polymer is polyvinylidene fluoride. Claim 6 A conductive material dispersion according to claim 1, wherein the unsaturated functional group of the fluorinated polymer comprises a carboxyl group. Claim 7 delete Claim 8 A conductive material dispersion according to claim 1, wherein the unsaturated functional groups of the fluorinated polymer are included in an amount of 0.01% to 1.0% by weight based on the total weight of the polymer. Claim 9 A conductive material dispersion according to claim 1, wherein the saturated residual compound unit of the fluorinated polymer is included in an amount of 0.01% to 5.0% by weight based on the total weight of the polymer. Claim 10 The conductive material dispersion of claim 1, wherein the fluorine-based polymer has a weight-average molecular weight of 1,000,000 g / mol to 2,000,000 g / mol. Claim 11 The electrode comprises an electrode active material, a single-walled carbon nanotube, and a fluorinated polymer, wherein the fluorinated polymer has a dispersion index (D) represented by the following Formula 1 of 0.05 to 0.95: [Formula 1] D = [10 6 (1+W u )] / [M w (1+W s )(1+M H In the above Equation 1, Mw is the unitless number of the weight-average molecular weight (g / mol) of the fluorinated polymer, and W u is the weight fraction of unsaturated functional group units in the fluorinated polymer, and W s is the weight fraction of saturated residual compound units in the fluorinated polymer, and M H is the number of moles of heteroatoms in a saturated residual compound unit, wherein the saturated residual compound unit is one or more selected from a saturated functional group unit and a comonomer unit, the saturated functional group includes an alkoxy group having 1 to 5 carbon atoms, and the comonomer unit includes one or more selected from the group consisting of a hexafluoropropylene unit and a chlorotrifluoroethylene. Claim 12 A lithium secondary battery having a structure in which electrodes and separators are alternately stacked, wherein the electrodes are the electrodes of claim 11.

Citation Information

Patent Citations

  • Electrode, secondary battery comprising the same, and method for preparing the electrode

    KR1020190117387A

  • Active material-conductive material composite material for lithium secondary battery

    KR1020230087677A

  • Slurry composition for secondary battery electrodes, and secondary battery electrodes using the same

    KR1020220003984A

  • Electrode and secondary battery comprising the same

    KR1020220131200A