Dye-exchanged zeolite marker

A cation exchange reaction binds dyes to zeolite pores, enhancing stability and reducing dye requirements, addressing stability issues in existing markers for use in polymer processing and detection applications.

KR103046117B1Active Publication Date: 2026-11-10사에스게터스에스페아
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020257006100
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-29
Filing Date
2023-07-28
Publication Date
2026-11-10
Estimated Expiration
2043-07-28

AI Technical Summary

Technical Problem

Existing dye-based markers for zeolites suffer from low stability under thermal treatment and solvent exposure, requiring high dye-to-zeolite ratios for effective detection, which complicates their use in polymer processing.

Method used

A dye-exchanged zeolite marker is produced through a cation exchange reaction, where the dye is efficiently bound to the zeolite pores, enhancing stability and allowing for reduced dye-to-zeolite ratios without compromising detection efficacy.

Benefits of technology

The dye-exchanged zeolite marker maintains stability under high temperatures and solvent contact, enabling effective detection with a lower dye content, suitable for integration into polymer matrices and various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025021366492-PCT00011_ABST
    Figure 112025021366492-PCT00011_ABST
Patent Text Reader

Abstract

The present invention relates to a dye-exchanged zeolite marker characterized by a pore size of 4 Å to 12 Å for the zeolite, a dye being an organic cationic molecule, and an amount of dye being 0.05 wt% to 1 wt% relative to the weight of the zeolite, an optically active composition comprising said marker dispersed in a polymeric matrix, and the use of said markers as detectable markers.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a dye-exchanged zeolite marker and an optically active composition comprising said marker dispersed in a polymeric matrix. Background Technology

[0002] Numerous patent disclosures, such as EP1409997, EP1356478, WO2011045572, WO2021113377, or US20100003762, relate to the preparation of materials for manufacturing purposes, such as anti-counterfeiting objectives, inventory management or warranty purposes, detection of the presence of specific substances in specific media, or for a wide range of possible applications as packaging solutions. A well-known means of detecting specific substances is the use of colorimetric indicators that rely on the optical properties of reactive dyes or inks under specific conditions. Specifically, the dye may exist in at least two different chemical states in which each form of the dye absorbs light within a specific wavelength range. When such a reactive dye existing in its first form is exposed to a given substance, it is converted to a second form of the dye by reacting with the substance through a reversible chemical reaction. When the dye in its second form absorbs light at a different wavelength, the chemical reaction provides a visible—and thus detectable—color change.

[0003] The incorporation of the above molecules into a desired substrate, including the possibility of using zeolites, is typically realized by using an impregnation method as disclosed in WO2011045572 or by using a post-treatment method described in US11027241. Additionally, CN110903826 discloses the use of fluorescent molecules, such as Rhodamine, incorporated onto the surface of a metal-organic framework (MOF) type structure using a diffusive impregnation technique. On the other hand, WO2021113377 describes antimicrobial zeolite nanoparticles that may additionally include an optical tracer (e.g., a fluorescent dye) that is non-covalently or covalently bonded to the surface of the zeolite but not bonded within the pores of the nanoparticles, in addition to the metal species.

[0004] The main drawback of such an approach is related to the limited stability of the final system, which tends to easily release dye molecules and decompose when exposed to heat treatment, such as during an extrusion process in a thermoplastic matrix or in the presence of water or other solvents.

[0005] Another possible approach is based on the use of dyes as described in WO2005052069, in which a dye composition is realized through a substitution reaction using one or more cationic dye groups in the presence of a zeolite dye suspension. However, one of the negative consequences of using both organic and inorganic dyes as disclosed in WO2005052069 is related to the large amount of dye relative to the amount of zeolite, and consequently, the high dye / zeolite ratio value required to achieve the coloring purpose. The problem to be solved

[0006] Accordingly, there is still a need to develop novel chemical indicators, particularly markers, that provide simple, reliable, and cost-effective detection means exhibiting enhanced stability compared to those known in the relevant art, especially when subjected to thermal treatment or contact with solvents. Furthermore, there is a need to develop novel optically active compositions containing such markers that can be manufactured and processed using known polymer processing techniques while maintaining the efficacy and stability of the novel indicators. means of solving the problem

[0007] [Summary of the Invention]

[0008] The present invention overcomes the drawbacks of the aforementioned prior art by implementing a dye-exchanged zeolite marker prepared by a cation exchange reaction between a zeolite cation and one of the dye organic molecules.

[0009] In the context of the present disclosure, "dye-exchanged Zeolite Marker The term "..." should be interpreted as referring to what is generally recognized in the relevant technical field, specifically a marker or indicator based on zeolite and obtainable by a cation exchange reaction between a cationic dye and a zeolite. The short form "marker" refers to "dye-exchanged Zeolite marker It is used in a compatible way with ".

[0010] More specifically, with the goal of providing a marker species capable of overcoming the problems of the prior art related to low stability disclosed above, the inventors of the present invention have surprisingly discovered that when a cation exchange reaction occurs between a dye and a zeolite, the dye is more efficiently bound to the zeolite, particularly to the zeolite pores, and consequently is not released or decomposed when in contact with a solvent or high temperature conditions, that is to say, it is more stable than that known in the relevant art.

[0011] Accordingly, the present invention relates to a dye-exchanged zeolite marker comprising a zeolite and a dye organic molecule, obtainable through a cation exchange reaction between at least one cation of the zeolite and at least one cation of the dye organic molecule.

[0012] Furthermore, it has been demonstrated that even when using a reduced amount of dye molecules relative to the zeolite, the detectable properties of the resulting marker can still be measured without altering the surface properties of the zeolite or its suitability for different applications. Accordingly, the present invention also relates to a dye-exchanged zeolite marker comprising a zeolite and a dye organic molecule, advantageously comprising a weight ratio between the dye and the zeolite of 0.05 wt% to 1 wt%, preferably 0.1 wt% to 0.5 wt% relative to the weight of the zeolite. In other words, unlike that disclosed in the prior art, the marker of the present invention does not require a high dye / zeolite ratio value to achieve coloring purposes.

[0013] As will be revealed in the experimental section of this disclosure, the dimensions of the zeolite pores can play an important role in the manufacture of the dye-exchanged zeolite markers of the present invention, at least in terms of process yield. It has been found that zeolite dye-exchanged zeolites having pore sizes ranging from 4 Å to 12 Å are particularly advantageous.

[0014] The present invention also relates to an optically active composition comprising a dye-exchanged zeolite marker and a polymeric matrix disclosed herein, preferably wherein the marker is dispersed within the polymeric matrix.

[0015] Furthermore, the present invention relates to the use of the dye-exchanged zeolite or composition disclosed herein as a detectable marker comprising, or in which the dye-exchanged zeolite or composition according to the present invention is embedded or (at least partially) coated therewith, as well as as a detectable article. Brief explanation of the drawing

[0016] Fig. 1: A graph showing thermogravimetric analysis (TG-MS) combined with mass spectrometry to evaluate organic vapor generation during process simulations in samples C2 and S2. During the slope at 250 °C, slight organic material generation due to decomposition initiation was clearly observed in the case of sample C2, whereas the absence of random organic material generation (continued at level 0) in the case of sample S2 confirmed that the decomposition process is not induced in such samples due to the stability of the dye-zeolite bond. Specific details for implementing the invention

[0017] As predicted above, the inventors of the present invention, after intensive experimentation, discovered that a dye-exchanged zeolite marker obtained through a cation exchange reaction between a zeolite and a dye is more stable than other zeolite-based markers already known in the relevant art field in which the dye is simply adsorbed onto the zeolite.

[0018] Accordingly, the present invention relates to a dye-exchanged zeolite marker comprising a zeolite and an organic cationic dye, obtainable through a cation exchange reaction between at least one cation of the zeolite and at least one cation of the organic cationic dye.

[0019] As will be revealed in the experimental section of this disclosure, the inventors have discovered zeolites having pore sizes ranging from 4 Å to 12 Å, which are particularly advantageous in that they allow dyes to bind more efficiently to the zeolite, as well as enable superior process yields. Surface area and porosity analysis were performed using a Micromeritics BET instrument. Prior to analysis, the samples were pre-conditioned by degassing at 180 °C in a turbo vacuum, which made it possible to remove physically bound impurities from the material being analyzed. Subsequently, analysis was continued using CO2 for LTA (-20 °C) or Ar for other zeolites (-186 °C). The micropore surface area was calculated using the Dubinin-Astakhov model, while the pore size was calculated using the Saito-Foley or NLDFT models.

[0020] Another important feature of the marker obtainable according to the present invention is that it enables effective detection despite a relatively low dye / zeolite weight ratio value (see samples S1-S4 in Table 1). Surprisingly, even at a weight ratio between dye and zeolite of 0.05 wt% to 1 wt%, preferably 0.1 wt% to 0.5 wt% (including extremes) relative to the weight of zeolite, the marker still enables effective detection without altering the surface characteristics of the zeolite.

[0021] Accordingly, the present invention provides a dye-exchanged zeolite marker comprising a zeolite and a dye, wherein

[0022] - The zeolite is characterized by a pore size included in the range of 4 Å to 12 Å, and

[0023] - The dye is an organic cationic molecule, and

[0024] - The amount of dye is included in an amount of 0.05% to 1% by weight relative to the weight of the zeolite

[0025] This relates to dye-exchanged zeolite markers.

[0026] A zeolite suitable for the purposes of the present invention is a zeolite generally known in the relevant art, provided that it has a pore size included in 4 Å to 12 Å. Preferably, the zeolite is a Faujasite-type zeolite (FAU) or a Mordenite zeolite (MOR).

[0027] The dye is a colorimetric dye as generally known in the relevant art, preferably an organic cationic dye. Preferably, the dye is rhodamine or a derivative thereof, and more preferably, the dye is selected from the group consisting of rhodamine B, tetramethyl rhodamine isothiocyanate-dextran, rhodamine 6G, rhodamine B isothiocyanate, rhodamine 19 perchlorate, and other rhodamine derivatives.

[0028] In any embodiment of the present invention, the zeolite is preferably X, which is 0.5 to 20 μm. 90 Value - here X 90 It exists in the form of a powder having an average particle size characterized by 90% of the particles in the sample having a spherical diameter that falls within a given volume reference range of 0.5 to 50 μm.

[0029] Since the dye is efficiently bound to the internal portion of the zeolite, one of the additional advantages associated with the marker is the possibility of utilizing the zeolite surface for further functionalization and activation.

[0030] In fact, in a preferred embodiment of the present invention, the zeolite surface of the marker is, for example, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, N-trimethoxysilylpropyl-N,N,N-trimethylammonium chloride, octadecyldimethyl(3-trimethoxysilylpropyl)ammonium chloride, tetradecyldimethyl(3-trimethoxysilylpropyl)ammonium chloride, n,n-didecyl-N-methyl-N-(3-trimethoxysilylpropyl)ammonium chloride, s-(trimethoxysilylpropryl)isothiouronum chloride, 3-(trihydroxysilyl)propyldimethyloctadecylammonium chloride, silsesquioxane 3-(dimethyloctadecylammonio)propyl, hydroxy-terminated chloride, and (3-glycidoxypropyl)trimethoxysilane. It is modified by an alkoxysilane. The modification is carried out through hydrolysis and condensation by the alkoxysilane. Preferably, the alkoxysilane derivative or alkoxysilane moiety is present in an amount of 1 to 40 weight percent relative to the weight of the zeolite. The silane moiety can later be utilized according to its inherent properties or as a linker for additional reaction or polymerization steps.

[0031] A dye-exchanged zeolite marker according to any of the embodiments disclosed herein may be dispersed in a polymer matrix to achieve an optically active composition.

[0032] Accordingly, the present invention also relates to a composition comprising a dye-exchanged zeolite marker and a polymer or polymer matrix according to any of the embodiments disclosed herein. The polymer matrix should be characterized by not having excitation and emission features (peaks as a generalized increase in absorption and / or emission and / or more complex spectral features) at a level that could perturb the excitation or emission of the marker. More specifically, since the dye excitation and emission peaks of rhodamine or rhodamine derivatives are centered at 560 nm and 580 nm, respectively, considering a buffer spectral region identified as ±100 nm, a suitable polymer matrix is ​​characterized by not having excitation and emission features in the range included in 460 to 680 nm.

[0033] In a preferred embodiment, the polymeric matrix is ​​polyethylene (PE), polypropylene (PP), polystyrene (PS), polyethylene terephthalate (PET), acrylonitrile butadiene styrene (ABS) and copolymers and functionalized polymers thereof, acrylic, acrylic-styrene, vinyl and alkyl copolymers, urethane-acrylic, aliphatic-urethane, urethane, polyurethane, epoxy, siloxane and polysiloxane, phenolic resins, poly[ethene-co-(vinyl alcohol)] (EVOH), poly(vinyl alcohol) (PVAL), poly(lact-co-glycolic acid) (PLGA), polyethylene glycol (PEG), poly(vinyl acetate) (PVAC), water-based or water-reducible latex, polylactic acid (PLA), aliphatic / aromatic co-polyester, preferably polybutylene adipate terephthalate (PBAT) and poly(butylene It is selected from the group consisting of sebacate-co-terephthalate (PBSeT), poly(butylene succinate-co-butylene terephthalate) (PBST), aliphatic co-polyesters from 1,4-butanediol and carboxylic acid, preferably poly(butylene succinate) (PBS) and polybutylene succinate adipate (PBSA), polyhydroxyalkanoate (PHA), preferably polyhydroxybutyrate (PHB), poly(hydroxybutyrate-co-hydroxyvalerate) (PHBV), polyhydroxybutyrate-hexanoate (PHBH), natural polymers, in particular polysaccharide polymers such as chitosan, sodium alginate and starch or modified starch, and mixtures thereof. Preferred examples of polymer blends are as follows: a blend of polylactic acid (PLA) and polyhydroxybutyrate / polyhydroxyvalerate (PHBV) or a blend of polyvinyl alcohol (PVOH) and hydroxypropylated starch ether (STARCH).

[0034] In the active composition obtained, the dye-exchanged zeolite marker is preferably present in an amount of 0.1 to 10 weight percent with respect to the weight of the polymeric matrix.

[0035] In other embodiments, one or more additional components, such as fillers, are added to the composition in an amount preferably contained in 0.1 to 20 weight percent with respect to the polymeric matrix. The additional components may be selected from the group consisting of, for example, hydrotalcite, zirconium phosphate, porphyrin, graphene and other two-dimensional crystals, zeolites, halloysite, graphene oxide, metal-organic frameworks (MOFs), organic beads, cellulose and antioxidant capsules, self-assembling proteins, ester-terminated polyamides, tertiary amide-terminated polyamides, polyether polyamides, polyalkyleneoxy-terminated polyamides, and mixtures thereof.

[0036] As will be revealed in the following non-limiting examples, the dye-exchanged zeolite of the present invention, as well as the polymeric composition containing it, is provided to have effective optical activity.

[0037] Accordingly, the present invention also relates to the use of the dye-exchanged zeolite or a polymeric composition containing it as a detectable marker.

[0038] As would be known to a person skilled in the art, the dye-exchanged zeolite or polymeric composition of the present invention can be embedded or coated onto an article, such as packaging, fabric, or general plastic article, thereby making the article itself or at least a part thereof detectable.

[0039] Accordingly, the present invention also relates to an item or article selected from packaging, fabrics, clothing, devices, such as medical devices, optical tags, marking components, and anti-counterfeiting elements, which at least partially comprises, is embedded in, or is coated with a dye-exchanged zeolite or polymeric composition according to any one of the embodiments disclosed herein.

[0040] As seen above, a composition comprising a dye-exchanged zeolite according to any embodiment of the present invention may be processed into a coating, film, lacquer, framework, three-dimensional element, pellet or sheet, or any other form generally suitable for the intended purpose.

[0041] The above marker may be used as is, or included in a polymeric matrix as disclosed above to obtain an optically active composition.

[0042] Several methods can be used to manufacture polymer / zeolite composites, such as in situ polymerization, polymer dissolution and mixing, extrusion, melt-blending, or other molding processes (e.g., injection, transfer, compression, foaming, thermoforming, film blowing).

[0043] As will be revealed in the experimental section below, the present invention also relates to a method for preparing a polymeric composition comprising a dye-exchanged zeolite marker according to any of the embodiments disclosed herein through in situ polymerization, polymer dissolution and mixing or melt-blending, as well as to the composition obtainable thereby.

[0044] [ Examples ]

[0045] Experimental section

[0046] The present invention will be described in more detail below with reference to the following non-limiting embodiments. Variations or changes to the embodiments exemplified herein that are obvious to those skilled in the art are encompassed by the appended claims.

[0047] Rhodamine-exchanged zeolite marker's Manufacturing (Samples S1-S6 and Relative example C1)

[0048] A quantity of 0.05 to 1.25 g of Rhodamine B (RhB) or RhB-dextran (both from Sigma Aldrich) was dissolved in 100 mL of distilled water. Next, 5 g of zeolite was added to the mixture, and the pH of the mixture was adjusted to 6 using an HCl (1 M) solution. The mixture was stirred using a laboratory magnetic stirrer at RT for 24 hours while protected from light. Next, the complex obtained by filtration was purified. Purification involved intensive washing of the powder with distilled water until the collected filtrate appeared completely clear. The resulting Rhodamine-exchange complex was dried overnight in an oven at 80 °C.

[0049] Table 1

[0050]

[0051] The ion exchange reaction using 0.25 g of RhB and LTA zeolite (C1) resulted in a very low Rhodamine B content (0.02 wt%) in the LTA zeolite, making the sample unsuitable for use as a marker.

[0052] Relative example Manufacturing of C2

[0053] By mechanically mixing 0.25 g of Rhodamine B (RhB) with 5 g of zeolite, efficient dispersion of different materials in powder form was ensured. The resulting mixture was dried overnight in an oven at 80°C.

[0054] Relative example C3 manufacturing

[0055] 0.25 g of 9-(diethylamino)-5H-benzo[a]phenoxazine-5-one (alternative marker NR) was dissolved in 100 mL of dimethyl sulfoxide. Next, 5 g of zeolite was added to the mixture. The mixture was stirred using a laboratory magnetic stirrer at RT for 24 hours while protected from light. Next, the complex obtained by filtration was purified. Purification involved intensive washing of the powder with distilled water until the collected filtrate appeared completely clear. The resulting exchange complex was dried overnight in an oven at 80 °C.

[0056] Relative example C4 manufacturing

[0057] 0.25 g of the fluorescent substance 5(6)-isothiocyanate (an alternative marker, FITC) was dissolved in 100 mL of distilled water. Next, 5 g of zeolite was added to the mixture. The mixture was stirred using a laboratory magnetic stirrer at RT for 24 hours while protected from light. Next, the complex obtained by filtration was purified. Purification involved intensive washing of the powder with distilled water until the collected filtrate appeared completely clear. The resulting exchange complex was dried overnight in an oven at 80 °C.

[0058] Relative example C5 manufacturing

[0059] Prior to its binding to the zeolite surface, a 3-aminopropyl)triethoxysilane-rhodamine (APTES-RhB) molecule was prepared. Its synthesis is described in the literature [ T. Nedelcev et al. / Dyes and Pigments 76 (2008) 550e556The protocol described in ] was followed. Briefly, Rhodamine B (0.002 mol, 0.96 g) was dissolved in chloroform (30 ml). The solution was heated to the boiling point of chloroform (61.2 °C) while stirring. Next, APTES (ABCR) (0.002 mol, 0.465 ml) was added dropwise to the Rhodamine B solution under stirring. After 30 minutes, the reaction was stopped, and the chloroform was removed from the reaction mixture using rotavapor. The remaining material (silanized Rhodamine, approximately 1.3 g) was dried in an oven at 60 °C.

[0060] Samples S1-S6 and Relative example Emission test in C1-C4

[0061] To demonstrate that the dye in the dye-exchanged zeolite marker is efficiently bound to the zeolite and, consequently, is not released when in contact with a solvent or applied at a higher temperature, the marker dispersion can be directly investigated. 22.4 mg of selected samples (S1-S6) or corresponding examples (C1-C4) were dispersed in 20 g of solvent. The samples were vigorously stirred at room temperature (RT) and subsequently allowed to settle for 24 hours. As described below, the supernatant was analyzed for its appearance by simple visual inspection and compared with a reference color sample (R1) obtained by dissolving 1.12 mg (2,34E-06 mol) of RhB powder in 20 g of solvent. The list of solvents adopted includes distilled water, acetone, dimethyl sulfoxide, tetrahydrofuran, chloroform, and dichloromethane (DCM). In all adopted solvents, the absence of released dye was confirmed by a completely transparent dispersion, as recorded in Table 2.

[0062] As an additional test, the prepared sample dispersion was vigorously stirred for 10 minutes under heating at 50°C and then allowed to settle for 24 hours. In this case as well, the supernatant of the sample was analyzed for its appearance through simple visual observation as described below and compared with a dye sample of a reference color. A completely transparent dispersion confirmed the absence of released dye, and the absence of spectrophotometric signals indicating dye confirmed the absence of release. As recorded in Table 2, the stability results observed for the room temperature sample after heat treatment were confirmed.

[0063] The dispersion prepared as described above was further analyzed using UV-Vis spectrophotometry. A calibration curve was defined for each solvent, and a detection limit (DL) of 1 ppm was determined. The influence of some parameters, such as solvent characteristics, temperature, and stirring time, was investigated. The results are recorded in Table 3, where no absorption peak was detected, a detection limit was determined for each solvent, and the calculated relative error was 15%.

[0064] Table 2. Solubilization of sample markers in selected solvents ( × = No dye released; ∨ = dye released). Tested at both RT and 50 ℃ after 10 minutes; observed after 24 hours.

[0065]

[0066] Table 3. Release of sample dyes in selected solvents

[0067]

[0068] To confirm the increased stability of the marker prepared according to the present invention, trace amounts of organic material originating from Rhodamine B degradation were identified by further exposing samples C2 and S2 to a heat treatment simulating a polymer process characterized by a rapid gradient (50 °C / min) at 250 °C and a 5-minute isotherm in a Thermal Gravimetric Mass Spectrometry (TG-MS) instrument. As recorded in Fig. 1, when sample C2 was subjected to the above-mentioned treatment, a small amount of organic material was clearly identified, whereas in the case of sample S2, the organic material remained at a zero level for the entire time.

[0069] contact angle test

[0070] Contact angle measurement is a technique used to measure the infiltration characteristics of liquid droplets on a solid surface. The contact angle is the angle formed between the tangent at the three-phase contact line of the droplet and the solid surface.

[0071] First, prepare the relevant solid substrate to measure the infiltration behavior. In this case, the substrate is a zeolite powder ring. Next, carefully place a small droplet of the liquid under investigation onto the solid surface using a syringe, micropipette, or other precise dispensing method.

[0072] Finally, an image of the droplet on the solid surface is captured at a suitable angle using a high-resolution camera. Compared to standard protocols, for zeolite rings, capture must be very fast, taking less than 1 second. Next, the shape of the droplet is analyzed and the contact angle is measured by processing the captured image using special software.

[0073] When water is used as a liquid probe, if the contact angle is <90°, the sample is labeled as hydrophilic (polar surface, strong interaction with H2O), whereas if the result is >90°, it is labeled as hydrophobic.

[0074] While the surface of a typical zeolite is hydrophilic, if the powder surface is functionalized by organic molecules, it can become hydrophobic.

[0075] Contact angle analysis was performed on Sample S2 and Relative Example C5, and the relative results recorded in Table 4 demonstrate that it is possible to retain rhodamine in the pores of the zeolite only according to the procedure of the present invention, whereas according to the procedure known in the relevant art, rhodamine is bound to the outer surface.

[0076] Consequently, the present disclosed zeolite containing rhodamine within its pores is easier to incorporate into an additional matrix / composition than hydrophobic zeolites such as C5, and additionally, the zeolite is characterized by the possibility of exhibiting additional interactions or functionalization with respect to the surface.

[0077] Table 4. Contact angle values

[0078]

[0079] Polymer Dye-exchanged zeolite in the matrix marker Manufacturing method for obtaining an optically active composition by dispersion

[0080] Several methods can be used to manufacture polymer / zeolite composites, such as in-situ polymerization, polymer dissolution and mixing, or melt-blending.

[0081] Preparation via in situ polymerization is based on a first step involving the formulation of polymer precursors and the introduction of dyes using efficient techniques to obtain a subsequent fine dispersion. After obtaining a homogeneous dispersion, the liquid formulation is applied onto a support, whereby the polymerization process is promoted through initiator activation. Different activation fields may be adopted depending on the initiator characteristics and the chemical composition of the formulation. Conventional approaches are based on thermal treatment or UV irradiation.

[0082] The solution mixing method comprises the following four steps: solubilization of the polymer matrix in a suitable solvent at room temperature or elevated temperature, dispersion of the zeolite in the solvent, mixing of the two solutions by mechanical stirring or tip / tub ultrasonic treatment, and finally, precipitation or casting of the mixture to obtain a film after solvent evaporation.

[0083] Melt blending is a commonly used technique for manufacturing thermoplastic / zeolite composites. It utilizes high temperatures and high shear forces to disperse the zeolite and is compatible with industrial processes. Depending on the desired final structure / shape of the composite, the bulk material can be processed by different post-extrusion techniques such as film formation, injection molding, compression molding, and melt-turning.

[0084] The following different embodiments are described for different manufacturing methods according to the present invention:

[0085]

[0086] Sample AC 1.A film of the active composition was prepared by mixing 1.5 g of polyethylene glycol dimethacrylate (PEGDMA) with 0.07 g of IGM Resins’ ESACURE ONE (a difunctional oligomeric alpha-hydroxy ketone) as a free-radical generating photoinitiator. After complete dissolution of the photoinitiator, 0.015 g of Rhodamine-Zeolite Sample S2 was added to the mixture at room temperature, and mechanical mixing was applied for 30 minutes. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and 100 mW / cm² with a 365 nm focus was applied. 2 The polymerization process was promoted by using a UV lamp for 15 seconds at an irradiation level (radiation dose 1.5 J / cm² 2 The polymerization process was carried out in a glove box environment under an inert gas flow. A marker-free reference PEGDMA (UV-cured) film was also prepared by adopting the same experimental protocol.

[0087] Sample AC 2. A film of the active composition was prepared by mixing 1.5 grams of polyethylene glycol dimethacrylate with 0.07 grams of Sigma Aldrich azobisisobutyronitrile (AIBN) as a free-radical generating thermal initiator. After complete dissolution of the initiator, 0.015 g of Rhodamine-Zeolite sample S2 was added to the mixture at room temperature and mechanically mixed for 30 minutes. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and the polymerization process was promoted by heating the sample at 80 °C for 30 minutes. The polymerization process was carried out in a glove box environment under an inert gas flow.

[0088] A markerless reference PEGDMA (thermocuring) film was also prepared by adopting the same experimental protocol.

[0089] Sample AC 3. A film of the active composition was prepared by mixing 0.9 grams of Hexion’s Epikote™ 862 (bisphenol F resin) with 0.15 grams of Hexion’s Epon 8111 (epoxy acrylate resin) and 0.38 grams of Epikote™ 03161 (rubber-modified bisphenol A resin). To obtain a homogeneous solution, the resulting mixture was vigorously stirred by mechanical mixing for 1 hour. Next, 0.08 grams of iriarylsulfonium hexafluoroantimonate salt as a cationic initiator were added and dissolved by mechanical stirring for 30 minutes. After the initiator was completely dissolved, 0.015 g of Rhodamine-Zeolite Sample S2 was added to the mixture at room temperature and mechanical mixing was applied for an additional 30 minutes. The obtained mixture is applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and 100 mW / cm² is applied for 120 seconds at λ = 365 nm. 2 The polymerization process was accelerated by applying UV treatment at the irradiation level.

[0090] A film based on the diglycidyl ether (DGEBF) of bisphenol F, a reference without a marker, was also prepared by adopting the same experimental protocol.

[0091] Sample AC 4.A film of the active composition was prepared by mixing 1.35 g of Dow Sylgard™ Part A (polydimethylsiloxane, PDMS) with 0.15 g of Dow 184 Part B (dimethyl, methylhydrosiloxane copolymer) as a crosslinking agent for 10 minutes. Next, 0.015 g of Rhodamine-Zeolite Sample S2 was added to the mixture at room temperature, and mechanical mixing was applied for an additional 10 minutes. After obtaining a homogeneous dispersion, a de-airing process under vacuum was applied for 15 minutes. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and the polymerization process was promoted by heating the sample at 100°C for 30 minutes.

[0092] A markerless reference PDMS film was also prepared by adopting the same experimental protocol.

[0093] Sample AC 5. A film of the active composition was prepared by mixing 1.45 g of SunChemical COMPOST LAM ADH (aliphatic polyisocyanate-based polyurethane, PU) with 0.05 g of alcohol dehydrogenase catalyst. Next, 0.015 g of Rhodamine-Zeolite Sample S2 was added at room temperature, and the dispersion was stirred by mechanically mixing for 15 minutes. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and a crosslinking reaction was promoted at room temperature.

[0094] A markerless reference PU film was also prepared by adopting the same experimental protocol.

[0095] Sample AC 6.1.5 g of LyondellBasell low-density polyethylene (LDPE) grade Lupolen® 2420 was dissolved in 8.5 g of toluene at a boiling temperature of 110 °C. After dissolving the polymer, 0.015 g of Rhodamine-Zeolite sample S2 was added to the polymeric solution at room temperature, and the dispersion was mixed for 30 minutes by ultrasonic treatment at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour.

[0096] The obtained formulation was applied to a thickness of 50 micrometers on Teflon foil using a doctor blade, and solvent evaporation was accelerated at 50°C. A composite film containing 1 wt% of marker in the polymer matrix was obtained. A reference LDPE film without a marker was also prepared by adopting the same experimental protocol.

[0097] Sample AC 7. 1.5 g of Versalis hybridized polystyrene (PS) grade EDISTIR® N1910 (ENI) was dissolved in 8.5 g of toluene at the boiling temperature of 110 °C. After dissolving the polymer, 0.015 g of Rhodamine-Zeolite sample S2 was added to the polymeric solution at room temperature, and the dispersion was mixed for 30 minutes by crude sonication at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour. The resulting mixture was applied to a thickness of 50 micrometers on Teflon foil using a doctor blade, and solvent evaporation was accelerated at 50 °C. A composite film containing 1 wt% of the marker in the polymer matrix was obtained. A markerless reference PS film was also prepared by adopting the same experimental protocol.

[0098] Sample AC 8.1.0 g of GoodFellow’s polylactic acid (PLA) (MFR=8) was dissolved in 9.0 g of chloroform at the boiling temperature of 61 °C. After dissolving the polymer, 0.01 g of Rhodamine-Zeolite sample S2 was added to the polymeric solution at room temperature. The dispersion was mixed for 30 minutes by crude sonication at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour. The resulting mixture was applied to a thickness of 50 micrometers on Teflon foil using a doctor blade, and solvent evaporation was accelerated at 40 °C. A composite film containing 1 wt% of the marker in the polymer matrix was obtained. A markerless reference PLA film was also prepared by adopting the same experimental protocol.

[0099] Sample AC 9. 1.0 g of Goodfellow’s polyhydroxybutyrate (PHB) was dissolved in 20.0 g of chloroform at the boiling temperature of 61 °C. After dissolving the polymer, 0.03 g of Rhodamine-Zeolite sample S2 was added to the polymeric solution at room temperature. The dispersion was mixed for 30 minutes by crude sonication at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour. The resulting mixture was applied to a thickness of 50 micrometers on Teflon foil using a doctor blade, and solvent evaporation was accelerated at 40 °C. A composite film containing 3 wt% of the marker in the polymer matrix was obtained. A markerless reference PHB film was also prepared by adopting the same experimental protocol.

[0100] Sample AC 10.1.0 g of Goodfellow’s polyhydroxybutyrate / polyhydroxyvalerate 2% (PHBV) was dissolved in 20.0 g of chloroform at the boiling temperature of 61 °C. After dissolving the polymer, 0.03 g of Rhodamine-Zeolite sample S2 was added to the polymeric solution at room temperature, and the dispersion was mixed for 30 minutes by crude sonication at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour. The resulting mixture was applied to a thickness of 50 micrometers on Teflon foil using a doctor blade, and solvent evaporation was accelerated at 40 °C. A composite film containing 3 wt% of the marker in the polymer matrix was obtained. A markerless reference PHBV film was also prepared by adopting the same experimental protocol.

[0101] Sample AC 11. 1.0 g of Kuraray’s polyvinyl alcohol (PVOH): Grade Exceval® AQ-4104 was dissolved in 9.0 g of distilled water at the boiling temperature of 100 °C. After dissolving the polymer, 0.01 g of Rhodamine-Zeolite Sample S2 was added to the polymeric solution at room temperature, and the dispersion was mixed for 30 minutes by crude sonication at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and water evaporation was accelerated at 50 °C. A composite film containing 1 wt% of the marker in the polymer matrix was obtained. A markerless reference PVOH film was also prepared by adopting the same experimental protocol.

[0102] Sample AC 12.1.0 g of SOLAM hydroxypropylated starch ether (STARCH): Grade SOLCOAT P85 was dissolved in 9.0 g of distilled water at the boiling temperature of 100 °C. After dissolving the polymer, 0.01 g of Rhodamine-Zeolite Sample S2 was added to the polymeric solution at room temperature. The dispersion was mixed for 30 minutes by ultrasonic treatment at room temperature, followed by vigorous stirring by mechanical mixing for 1 hour. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and water evaporation was accelerated at 40 °C. A composite film containing 1 wt% of the marker in the polymer matrix was obtained. A markerless reference STARCH film was also prepared by adopting the same experimental protocol.

[0103] Examples AC 13 ( blend 1) 0.7 g of Goodfellow’s polylactic acid (PLA) (MFR=8) and 0.3 g of Goodfellow’s polyhydroxybutyrate / polyhydroxyvalerate 2% (PHBV) were dissolved in 18.0 g of chloroform at the boiling temperature of 61 °C. After dissolving the polymer, 0.05 g of Rhodamine-Zeolite sample S2 was added to the polymeric solution at room temperature, and the dispersion was mixed by ultrasonic treatment at room temperature for 30 minutes, followed by vigorous stirring by mechanical mixing for 1 hour. After solution casting, a composite film containing 3 wt% of the marker in the polymer matrix was obtained. A marker-free reference PLA / PHBV film was also prepared by adopting the same experimental protocol.

[0104] Examples AC 14 ( blend 2)0.7 g of Kuraray's polyvinyl alcohol (PVOH): Grade Exeval® AQ-4104 and 0.3 g of Solram's hydroxypropylated starch ether (STARCH): Grade Solcoat P85 were dissolved in 9.0 g of distilled water at 90 °C under vigorous stirring. After complete dissolution of the polymer, 0.01 g of Rhodamine-Zeolite Sample S2 was added to the polymeric solution at room temperature (RT), and the dispersion was mixed for 30 minutes by crude sonication at RT, followed by vigorous stirring by mechanical mixing at RT for 1 hour. The resulting mixture was applied to a glass substrate to a thickness of 50 micrometers using a doctor blade, and water evaporation was promoted at 50 °C. A marker-free reference PVOH / starch film was also prepared by adopting the same experimental protocol.

[0105] Examples AC 15 49 g of ≤400 micrometer low-density polyethylene powder purchased from Alfa Aesar was compounded with 1 g of Rhodamine-Zeolite (Sample S2) via melt-blending using a laboratory 2-roll open-mixing mill (Battaggion) for 5 minutes. The conditions for the rolling process were as follows: temperature of the front roller = 130 °C; temperature of the rear roller = 80 °C; rolling speed = 33 rpm. The resulting compounded material was compression-molded using a laboratory press (Gibitre Instruments) at P=230 bar and T=175 °C for 5 minutes to produce a sheet containing 2 wt% of marker (thickness 200 μm) was obtained. A markerless reference polyethylene sheet was also prepared according to the same experimental protocol.

[0106] Examples AC 16. Using a laboratory 2-roll open-mixing mill (Vatazion), 49 g of polylactic acid (Grade NatureWorks 2003D) was compounded with 1 g of rhodamine-zeolite (Sample S2) via melt-blending for 5 minutes. The conditions for the rolling process were as follows: temperature of the front roller = 155 °C; temperature of the rear roller = 125 °C; rolling speed = 33 rpm. By compression molding the resulting compounded material using a laboratory press (Givitre Instruments) at P=230 bar and T=190 °C for 5 minutes, a sheet containing 2 wt% of marker (thickness 200 μm) was obtained. A markerless reference polylactic acid sheet was also prepared according to the same experimental protocol.

[0107] Examples AC 17 . Using a laboratory 2-roll open-mixing mill (Vatazion), 48.5 g of Goodfellow’s polyhydroxybutyrate / polyhydroxyvalerate 2% (PHBV) was compounded with 1.5 g of rhodamine-zeolite (Sample S2) via melt-blending for 5 minutes. The conditions for the rolling process were as follows: temperature forward roller = 170 °C; temperature rear roller = 145 °C; rolling speed = 33 rpm. By compression molding the resulting compounded material using a laboratory press (Givitre Instruments) at P=230 bar and T=190 °C for 5 minutes, a sheet containing 3 wt% marker (thickness) was produced. 200 μm) was obtained. A markerless reference PHBV sheet was also prepared according to the same experimental protocol.

[0108] Examples AC 18Using a laboratory benchtop 2-roll mill (LabTech Engineering), 98 g of acrylonitrile butadiene styrene ABS (Grade Terluran® GP-22 manufactured by INEOS STYROLUTION) was compounded with 2 g of rhodamine-zeolite (Sample S5) via melt-blending for 5 minutes. The conditions of the rolling process were as follows: temperature forward roller = 175 °C; temperature rear roller = 170 °C; rolling speed = 10 rpm. The resulting compounded material containing 2 wt% of marker S5 was formed into a sheet (thickness 500 μm). A reference ABS sheet without a marker was prepared according to the same manufacturing protocol.

[0109] Preparation examples are summarized in Table 4 below:

[0110]

[0111] Marker and matrix optical characterization

[0112] Equipment description. A Horiba FluoroMax® Plus spectrofluorometer was used for the measurements. A continuous light source P focused on the entry slit of the excitation monochromator. oA 150 W ozone-free xenon arc lamp was employed. The instrument is based on two Czerny-Turner monochromators that disperse incident light by their reflective diffraction gratings. Optical spectra were obtained by rotating the diffraction gratings and recording intensity values ​​at each wavelength. The entry and exit ports of each monochromator included continuously adjustable slits to control spectral resolution and the intensity of the fluorescence signal recorded by a photomultiplier tube. A solid sample holder mounted on an adjustable protractor was used to test polymer products in the form of marker-added films or plaques. By using a sample setup with a 60° angle between the incident and mirror-reflected beams, the excitation beam was prevented from entering the emission slit, thereby avoiding interference from stray light. Data was acquired and processed using FluorEssence™ analysis management software.

[0113] Description of the sample characterization protocol

[0114] To detect the presence of dye within the polymeric matrix, the marker excitation and emission peaks in the polymeric matrix were compared with those of a reference sample (a polymeric matrix without a marker) and a pure marker excitation and emission peak. Considering dye fluorescence, sample performance was studied as the ratio between the fluorescence intensity I of the active composition applied at 540 nm and the fluorescence intensity I0 of the pure polymeric matrix without a dye. According to the adopted protocol, the presence of the marker was considered detectable if the I / I0 ratio was determined to be greater than 2. Table 5 below records the values ​​for all tested samples.

[0115] Table 5

[0116]

Claims

Claim 1 A dye-exchanged zeolite marker comprising a zeolite and a dye, wherein a) X in which the zeolite is contained in the range of 0.5 to 50 μm 90 A dye-exchanged zeolite marker comprising: a) a powder having an average particle size characterized by a value and a pore size included in 4 Å to 12 Å; b) a dye being an organic cationic molecule selected from the group consisting of Rhodamine B, tetramethyl rhodamine isothiocyanate-dextran, Rhodamine 6G, Rhodamine B isothiocyanate, and Rhodamine 19 perchlorate; and c) an amount of dye included in 0.05 wt% to 1 wt% relative to the weight of the zeolite. Claim 2 A dye-exchanged zeolite marker according to claim 1, wherein the zeolite is a fauzacite zeolite (FAU) or a mordenite zeolite (MOR). Claim 3 A dye-exchanged zeolite marker according to claim 1, wherein the amount of dye is included in an amount of 0.1% to 0.5% by weight relative to the weight of the zeolite. Claim 4 In claim 1, X having an average particle size included in the range of 0.5 to 20 μm. 90 Dye-exchanged zeolite marker characterized by a value. Claim 5 A dye-exchanged zeolite marker according to claim 1, wherein the zeolite comprises a surface modified or functionalized by an alkoxysilane derivative. Claim 6 A dye-exchanged zeolite marker according to claim 5, wherein the alkoxysilane derivative moiety is present in an amount of 1 to 40 weight percent relative to the weight of the zeolite. Claim 7 A dye-exchanged zeolite marker obtained through a cation exchange reaction between at least one cation of the zeolite and at least one cation of the dye, in claim 1. Claim 8 A composition comprising a dye-exchanged zeolite marker according to claim 1 dispersed in a polymeric matrix, wherein the polymeric matrix is ​​selected from polyethylene (PE), polypropylene (PP), polystyrene (PS), polyethylene terephthalate (PET), acrylonitrile butadiene styrene (ABS) and copolymers and functionalized polymers thereof, acrylic, acrylic-styrene, acryl-vinyl and alkyl copolymers, urethane-acrylic, urethane, polyurethane, epoxy, siloxane and polysiloxane, phenolic resins, poly[ethene-co-(vinyl alcohol)] (EVOH), poly(vinyl alcohol) (PVAL), poly(lact-co-glycolic acid) (PLGA), polyethylene glycol (PEG), poly(vinyl acetate) (PVAC), water-based or water-reducible latex, polylactic acid (PLA), aliphatic or aromatic co-polyesters and natural polymers. Claim 9 A composition according to claim 8, wherein the dye-exchanged zeolite marker is present in an amount of 0.1 to 10 weight percent with respect to the polymeric matrix. Claim 10 A composition according to claim 8, further comprising an amount of filler of 0.1 to 20 weight percent with respect to the polymeric matrix. Claim 11 A composition according to claim 10, wherein the filler is selected from the group consisting of hydrotalcite, zirconium phosphate, porphyrin, graphene and other two-dimensional crystals, zeolite, halloysite, graphene oxide, metal-organic framework (MOF), organic beads, cellulose and antioxidant capsules, self-assembling proteins, ester-terminated polyamides, tertiary amide-terminated polyamides, polyether polyamides, polyalkyleneoxy-terminated polyamides and mixtures thereof. Claim 12 A composition according to claim 8, wherein the polymeric matrix is ​​processed into the form of a coating, film, lacquer, framework, three-dimensional element, pellet, or sheet. Claim 13 delete Claim 14 delete

Citation Information

Patent Citations

  • Damage self-warning anticorrosive coating doped with zeolite-loaded fluorescent probe and preparation method of damage self-warning anticorrosive coating

    CN114574070A

  • Permanent heat activated electrographic printing process and composition

    EP0802861B1

  • Antimicrobial compositions and methods of using thereof

    WO2021113377A1