Semiconductor substrate, Semiconductor device and Electronic device
The semiconductor substrate design addresses defects and cracks in GaN devices by using a mask layer and ELO method for lateral growth, resulting in reduced defects and improved reliability and efficiency.
Patent Information
- Application Number
- KR1020257013181
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-29
- Filing Date
- 2021-12-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-12-28
AI Technical Summary
Existing semiconductor devices using GaN face challenges in reducing defects and cracks due to lattice mismatch with heterogeneous substrates, leading to poor reliability and efficiency.
A semiconductor substrate design featuring a mask layer with controlled openings and a seed portion, utilizing the ELO method to grow a GaN-based semiconductor layer laterally, with a low-defect region and controlled gap formation to reduce stress and defects, followed by easy device separation and peeling from the template substrate.
The design significantly reduces defects and cracks, enhances film quality, and facilitates efficient device production with improved reliability and cost-effectiveness.
Smart Images

Figure 112025045419284-PAT00015_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a semiconductor substrate, a semiconductor device, and an electronic device. Background Technology
[0002] Semiconductor devices using GaN (gallium nitride) generally have higher power conversion efficiency than semiconductor devices made of Si (silicon). As a result, semiconductor devices using GaN have lower power loss than semiconductor devices made of Si, so energy saving effects are expected. Conventionally, research has been conducted on techniques for forming GaN-based semiconductor devices in order to manufacture semiconductor devices using GaN. For example, Patent Document 1 discloses a method of forming a GaN-based semiconductor layer on a GaN-based substrate or a heterogeneous substrate (e.g., a sapphire substrate) using the ELO (Epitaxial Lateral Overgrowth) method. Prior art literature
[0003] Japanese Patent Publication No. 2013-251304
[0004] A semiconductor substrate according to the present disclosure comprises a main substrate having a lattice constant different from that of a GaN-based semiconductor, a mask layer having an opening and a mask portion located on an upper layer above the main substrate, a seed portion overlapping with the opening in a planar view, and a semiconductor layer comprising a GaN-based semiconductor disposed on the seed portion and the mask portion, wherein the semiconductor layer comprises an effective portion located between the center of the opening and the mask portion in a planar view, and the upper surface of the effective portion comprises at least one low-defect region having a size of 10 μm in a first direction along the width direction of the opening and 10 μm in a second direction orthogonal to the first direction, and no line-shaped defects are measured by the CL method in the low-defect region. Brief explanation of the drawing
[0005] FIG. 1 is a plan view and a cross-sectional view showing the configuration of a semiconductor substrate according to the present embodiment. FIG. 2 is a cross-sectional view showing another configuration of a semiconductor substrate according to the present embodiment. FIG. 3 is a cross-sectional view showing another configuration of a semiconductor substrate according to the present embodiment. FIG. 4 is a plan view and a cross-sectional view showing different configurations of a semiconductor substrate according to the present embodiment. FIG. 5 is a plan view and a cross-sectional view showing different configurations of a semiconductor substrate according to the present embodiment. FIG. 6 is a cross-sectional view showing a device separation process according to the present embodiment. FIG. 7 is a plan view showing the device isolation process according to the present embodiment. Figure 8 is a cross-sectional view showing another example of a device isolation process. Figure 9 is a cross-sectional view showing another example of a device isolation process. Figure 10 is a cross-sectional view showing the device peeling process. Figure 11 is a cross-sectional view showing another example of a device peeling process. FIG. 12 is a schematic diagram showing the configuration of an electronic device according to the present embodiment. FIG. 13 is a schematic diagram showing another configuration of an electronic device according to the present embodiment. FIG. 14 is a cross-sectional view showing an example of the transverse growth of a semiconductor layer. FIG. 15 is a plan view and a schematic diagram showing the evaluation of the semiconductor substrate (configuration in which the ELO semiconductor layer has an edge surface on the mask). FIG. 16 is a plan view and a schematic diagram showing the evaluation of the semiconductor substrate (configuration in which the ELO semiconductor layer has an edge surface on the mask). FIG. 17 is a plan view and a schematic diagram showing the evaluation of the semiconductor substrate (configuration in which the ELO semiconductor layer has an edge surface on the mask). FIG. 18 is a plan view and a schematic diagram illustrating the evaluation of the semiconductor substrate (configuration in which the ELO semiconductor layer has an edge surface on the mask). FIG. 19 is a plan view and schematic diagram showing the evaluation of an integrated semiconductor substrate in which the ELO semiconductor layer does not have an edge surface on the mask. FIG. 20 is a plan view and schematic diagram illustrating the evaluation of an integrated semiconductor substrate in which the ELO semiconductor layer does not have an edge surface on the mask. FIG. 21 is a plan view and schematic diagram illustrating the evaluation of an integrated semiconductor substrate in which the ELO semiconductor layer does not have an edge surface on the mask. FIG. 22 is a plan view and schematic diagram illustrating the evaluation of an integrated semiconductor substrate in which the ELO semiconductor layer does not have an edge surface on the mask. FIG. 23 is a CL phase targeting the ELO semiconductor layer (8) of a semiconductor substrate (10) (the main substrate is a silicon substrate). FIG. 24 is a CL phase targeting the ELO semiconductor layer (8) of a semiconductor substrate (10) (the main substrate is a sapphire substrate). FIG. 25 is a CL phase on the back side (skinned side) of the ELO semiconductor layer of a semiconductor substrate (10). Figure 26 shows the CL phase on the surface of the GaN layer of the reference example. Figure 27 shows the CL phase on the surface of the GaN layer of the reference example. Figure 28 shows the CL phase on the surface of the GaN layer of the reference example. Figure 29 is a CL phase on the back side (exfoliation surface) of the GaN layer of the ELO method film of the reference example. Figure 30 is a CL phase on the back side (exfoliation surface) of the GaN layer of the ELO method film of the reference example. FIG. 31 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 1. FIG. 32 is a cross-sectional view showing an example of semiconductor layer peeling in Example 1. FIG. 33 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 2. FIG. 34 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 3. FIG. 35 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 4. FIG. 36 is a cross-sectional view showing an application example of Example 4. FIG. 37 is a cross-sectional view showing the configuration of Example 5. FIG. 38 is a cross-sectional view showing the configuration of Example 6. FIG. 39 is a cross-sectional view showing another configuration of Example 6. FIG. 40 is a block diagram showing an example of the configuration of a semiconductor substrate manufacturing apparatus. Specific details for implementing the invention
[0006] (Semiconductor substrate)
[0007] FIG. 1 is a plan view and a cross-sectional view showing the configuration of a semiconductor substrate according to the present embodiment. As shown in FIG. 1, the semiconductor substrate (10) (semiconductor wafer) according to the present embodiment comprises a main substrate (1), a lower layer (4) formed on the main substrate (1) and including a seed portion (3S), a mask layer (6) formed on the lower layer (4) and having an opening (KS) and a mask portion (5) that overlap with the seed portion (3S) in a planar view, and a semiconductor layer (8) comprising a nitride semiconductor (e.g., GaN-based semiconductor) disposed on the seed portion (3S) and the mask portion (5). The lower layer (4) may be the lower portion (4), the mask layer (6) may be the mask (6) (mask pattern), and the semiconductor layer (8) may be the semiconductor portion (8).
[0008] The opening (KS) of the mask layer (4) may be tapered (a shape in which the width narrows toward the lower layer (4)). In this case, the width of the opening (KS) and the width of the mask portion (5) may be indicated with respect to the upper surface of the mask layer. However, it is not limited to this.
[0009] Nitride semiconductors can be represented, for example, as AlxGayInzN (0≤x≤1; 0≤y≤1; 0≤z≤1; x+y+z=1), and specific examples include GaN-based semiconductors, AlN (aluminum nitride), InAlN (indium aluminum nitride), and InN (indium nitride). A GaN-based semiconductor is a semiconductor containing gallium atoms (Ga) and nitrogen atoms (N), and typical examples include GaN, AlGaN, AlGaInN, and InGaN. The semiconductor layer (8) may be a doped type (for example, an n-type containing a donor) or a non-doped type. A semiconductor substrate means a substrate containing a nitride semiconductor (for example, a GaN-based semiconductor), and the material of the main substrate (1) may be a semiconductor or a non-semiconductor. There are cases where it is called a base substrate including the main board (1) and the lower layer (4), and cases where it is called a template substrate (7) including the main board (1), the lower layer (4), and the mask layer (6).
[0010] The semiconductor layer (8) is formed by the ELO (Epitaxial Lateral Overgrowth) method starting from the seed portion (3S) exposed from the opening (KS). For this reason, the semiconductor layer (8) is sometimes referred to as the ELO semiconductor layer (8). The thickness direction of the semiconductor layer (8) is the Z direction (of the GaN-based crystal). <0001> The direction is. The opening (KS) is elongated, and its width direction is the X direction (the <11-20> direction of GaN-based crystals).
[0011] FIG. 2 is a cross-sectional view showing another configuration of a semiconductor substrate according to the present embodiment. As shown in FIG. 2, the semiconductor substrate (10) may be configured such that the main substrate (1), the lower layer (4), the mask layer (6), the semiconductor layer (8), and the functional layer (9) are formed in this order.
[0012] In the semiconductor substrate (10), a plurality of layers are stacked on the main substrate, and the stacking direction can be called the “upward direction.” In addition, viewing the semiconductor substrate (10) from a line of sight parallel to the normal direction of the semiconductor substrate (10) can be called the “planar view.”
[0013] (Main board)
[0014] For the main substrate (1), a heterogeneous substrate having a lattice constant different from that of a GaN-based semiconductor may be used. Examples of heterogeneous substrates include a silicon (Si) substrate, a sapphire (Al2O3) substrate, a silicon carbide (SiC) substrate, a ScAlMgO4 substrate, etc. The plane orientation of the main substrate (1) is, for example, the (111) plane of a silicon substrate, the (0001) plane of a sapphire substrate, and the 6H-SiC (0001) plane of a SiC substrate. These are examples, and any substrate and plane orientation capable of growing the semiconductor layer (8) by the ELO method may be used. The main substrate may be a self-supporting substrate (for example, a wafer cut from a bulk crystal).
[0015] (Lower body layer)
[0016] As a base layer (4), a buffer layer (2) (e.g., an AlN layer) and a seed layer (3) (e.g., a GaN-based semiconductor) can be formed sequentially from the main board side. The buffer layer (2) is a melting suppression layer that can reduce the melting of the main board (1) and the seed layer (3) by direct contact. It also has the effect of increasing the crystallinity of the seed layer (3). The AlN layer is formed, for example, using the MOCVD method, with a thickness of about 10 nm to about 5 μm. For example, if a main board (1) that does not melt with the seed layer (3), which is a GaN-based semiconductor, is used, it is possible to have a configuration in which the buffer layer (2) is not formed. When a silicon substrate or the like is used for the main board (1), the GaN-based semiconductor, melts with the seed layer, so by forming a buffer layer (2), such as an AlN layer, melting is reduced.
[0017] For example, an AlGaN layer may be used as the seed layer (3). The seed layer (3) includes a seed portion (3S) that overlaps with the opening (KS) of the mask layer (6). As the seed layer (3), a graded layer in which the Al composition is graded to approach GaN may be used. The graded layer is, for example, the first layer, Al, in order starting from the AlN layer side. 0.7 Ga 0.3 N layer and the second layer, Al 0.3 Ga 0.7 It is a laminated body having an N layer formed. In this case, the composition ratio of Ga (0.7 / 2=0.35) in the second layer (Al:Ga:N=0.3:0.7:1) is greater than the composition ratio of Ga (0.3 / 2=0.15) in the first layer (Al:Ga:N=0.7:0.3:1). The graded layer can be easily formed by the MOCVD method and may be composed of three or more layers. By using the graded layer in the seed layer (3), stress from the main substrate (1), which is a heterogeneous substrate, can be relieved. The seed layer (3) may be configured to include a GaN layer. In this case, the seed layer (3) may be a single GaN layer, or the uppermost layer of the graded layer, which is the seed layer (3), may be a GaN layer. The lower layer (4) may be composed of only the buffer layer (2) and the seed layer (3). In addition, a self-supporting SiC substrate (e.g., a single-crystal wafer cut from a bulk crystal) can be used on the main substrate (1), and a mask layer (6) can be formed on the SiC substrate without forming an underlayer, thereby serving as a template substrate.
[0018] (Mask layer)
[0019] A mask portion (5) and an opening (KS) are formed in the mask layer (6). The opening (KS) has the function of a growth initiation opening that exposes the seed layer (3) to initiate the growth of the semiconductor layer (8), and the mask portion (5) may have the function of a selective growth mask that grows the semiconductor layer (8) in the transverse direction. The opening (KS) is a portion (non-formed portion) in the mask layer (6) (mask pattern (6)) where the mask portion (5) is not present, and it does not need to be surrounded by the mask portion (5).
[0020] As a mask layer (6), an inorganic insulating film such as a silicon oxide (SiOx) film, a silicon nitride (SiNx) film, a silicon oxynitride (SiON) film, or a titanium nitride (TiNx) film may be used. For example, a silicon oxide film with a thickness of about 50 nm to about 4 μm (e.g., about 100 nm to about 2 μm) is formed over the entire surface of the silicon oxide film using a sputtering method on the lower layer (4), and a resist is applied to the entire surface of the silicon oxide film. Then, the resist is patterned using a photolithography method to form a resist having stripe-shaped openings. Then, a part of the silicon oxide film is removed to form an opening (KS) by a wet etchant such as hydrofluoric acid (HF) or buffered hydrofluoric acid (BHF), and the resist is removed by organic cleaning, thereby forming a mask layer (6) having openings (KS) and a mask portion (5). It is also possible to form a mask portion on the entire surface of a substrate using a photolithography method, then apply a resist to pattern it, remove the resist in the area that becomes the opening (KS), and form the opening (KS) using a dry etching method.
[0021] The opening (KS) has a long shape, and a plurality of openings (KS) are arranged periodically in the a-axis direction (first direction (X)) of the ELO semiconductor layer (8) with a first period.
[0022] The width of the opening (KS) is set to approximately 0.1㎛ to 20㎛. As the width of the opening (KS) decreases, the number of penetrating dislocations propagating from the opening (KS) to the ELO semiconductor layer (8) decreases. Additionally, peeling of the ELO semiconductor layer (8) in the subsequent process becomes easier. Furthermore, the area of the effective portion with fewer surface defects can be increased.
[0023] In the mask layer (6), a laminated film containing the above material may be used, for example, a laminated film containing a silicon oxide film and a silicon nitride film.
[0024] (Formation of ELO semiconductor layer)
[0025] As a semiconductor layer (8) (ELO semiconductor layer (8)), a GaN-based semiconductor layer is formed by the ELO method. The ELO semiconductor layer (8) may be composed of GaN, and the seed portion (3S) may also contain GaN. For example, a template substrate (7) including a main substrate (1), a sublayer (4), and a mask layer (6) is introduced into a MOCVD device, and a GaN layer is deposited on the template substrate (7). As an example of ELO deposition conditions, substrate temperature: 1120°C, growth pressure: 50kPa, TMG (trimethylgallium): 22sccm, NH3: 15slm, and V / III = 6000 (ratio of the supply amount of Group V raw material to the supply amount of Group III raw material) may be adopted.
[0026] In the formation of the semiconductor layer (8), it is desirable to reduce the mutual reaction between the semiconductor layer (8) and the mask portion (5) so that the semiconductor layer (8) and the mask portion (5) maintain a state in which they are in contact through van der Waals forces. That is, the semiconductor layer (8) and the mask portion (5) are in contact mainly through van der Waals forces.
[0027] The adjacent ELO semiconductor layers (8) grown from adjacent openings (KS) may be joined together, or they may not be joined together, thereby forming a gap near the center of the mask portion (5). If joined together, the entire surface of the substrate can form a flat surface. If not joined together, the stress (compressive stress or tensile stress) that occurs when using a main substrate (1) made of a material different from the nitride semiconductor can be more effectively relieved in the gap, thereby effectively suppressing the occurrence of defects or cracks.
[0028] (Shape of the ELO semiconductor layer)
[0029] The semiconductor layer (8) has an effective portion (YS) (a portion that constitutes the device portion in the post-processing stage) located between the opening (KS) and the center (5C) of the mask portion in the planar view. Among the semiconductor layer (8), the portion located on the seed portion (3S) (a portion with a high penetration potential) becomes a non-effective portion (NS). That is, the semiconductor layer (8) includes an effective portion (YS) with relatively low penetration potential and a non-effective portion (NS) with relatively high penetration potential. The non-effective portion (NS) is a potential succession portion and has a higher penetration potential than the effective portion (YS) (potential non-succession portion), but it may be used as part of the device. For example, if the functional layer (9) includes an active layer, the portion where electrons and holes combine (light-emitting portion) among the active layer may be formed to overlap with the effective portion (YS) in the planar view. The N-type electrode (cathode), etc., may be formed to overlap with the non-effective portion (NS) in the planar view.
[0030] The penetrating potential is in the thickness direction of the ELO semiconductor layer (8) <0001> It is a potential (defect) extending from the lower surface or interior of the semiconductor layer (8) along the direction (Z direction) to the surface or surface layer. The penetrating potential can be observed by performing a CL (Cathode Luminescence) measurement on the surface (parallel to the c-plane) of the semiconductor layer (8).
[0031] The semiconductor layer (8) of FIG. 1 has an edge surface (side) (8E) near the center of the mask portion (5) and does not associate with the semiconductor layer (8) grown from the adjacent seed portion (3S). Meanwhile, when the ELO semiconductor layer (8) of the c-plane is formed in an island shape, the side of the ELO semiconductor layer (8) is typically formed by a <1-10α> plane (α is any integer), a <11-2β> plane (β is any integer), or a plane crystallographically equivalent to these. That is, the edge surface (8E) of the semiconductor layer (8) may have an inclined surface (facet).
[0032] In this way, the semiconductor layers (8) grown laterally in the reverse direction from two adjacent seed portions (3S) do not come into contact (coordinate) on the mask portion (5) and have a gap (gap) (GP), thereby reducing the internal stress of the semiconductor layers (8). As a result, cracks and defects occurring in the semiconductor layers (8) can be reduced. This effect is particularly effective in the present embodiment where the main substrate (1) is a heterogeneous substrate. The width of the gap (GP) is preferably 4 μm or less, and more preferably 3 μm or less.
[0033] The semiconductor layer (8) may be an n-type GaN-based semiconductor (as a donor, for example, silicon). When a functional layer (9) including, for example, a p-type semiconductor layer is formed on a layer above the semiconductor layer (8) (see FIG. 2), if the semiconductor layer (8) has silicon or oxygen as an n-type dopant, the p-type dopant (magnesium, etc.) can be compensated for, so this phenomenon can be significantly reduced by suppressing the width of the gap (GP) to the above range.
[0034] FIG. 3 is a cross-sectional view showing another configuration of a semiconductor substrate according to the present embodiment. When forming a functional layer (9), an edge growth (9G) (corner portion) may occur as shown in FIG. 3. For example, this is the case where the functional layer (9) includes an AlGaN layer. The edge growth may have a width of 10 μm or more and a height of 200 to 300 nm, which may cause an obstacle to the post-processing, but by suppressing the width of the gap (GP) to the above range, the edge growth (9G) can be significantly reduced (for example, 100 nm or less).
[0035] FIGS. 4 and FIGS. 5 are a plan view and a cross-sectional view showing different configurations of a semiconductor substrate according to the present embodiment. The semiconductor layer (8) of FIG. 4 has a configuration in which semiconductor layers grown laterally in the reverse direction from two adjacent seed portions (3S) come together near the center (5C) of the mask portion to form an integrated structure. In this configuration, by appropriately setting the film formation conditions of the ELO semiconductor layer (8) and the width of the mask portion (5), a hollow portion (8C) may be formed near the center (5C) of the mask portion, which is the point of convergence, as shown in FIG. 5. The shape of the hollow portion (8C) is such that the width widens on the side of the mask portion (5) (for example, a cone shape or a teardrop shape in cross-section). In this case, the semiconductor layer (8) has a portion (ineffective portion (NS)) that overlaps with the hollow portion (8C) in plan view. That is, the semiconductor layer (8) has an effective portion (YS) and a non-effective portion (NS) adjacent to the effective portion (YS).
[0036] Silicon oxide, silicon nitride, and silicon oxynitride films used as materials for the mask layer (6) have a smaller coefficient of thermal expansion compared to GaN-based semiconductors. Therefore, when the ELO semiconductor layer (8) assembled at approximately 1000°C is cooled to room temperature, cracks may occur in the ELO semiconductor layer (8) due to the difference in the coefficient of thermal expansion. Since the hollow portion (8C) has the effect of significantly reducing internal stress in the semiconductor layer (8), the occurrence of such cracks can be effectively reduced. Additionally, the surface of the semiconductor layer (8) may have a depression (8D) in the portion corresponding to the upper part of the hollow portion (8C). This depression (8D) also has the effect of relieving internal stress in the semiconductor layer (8).
[0037] (Functional layer)
[0038] The semiconductor substrate (10) of FIG. 2 includes a functional layer (9) on a semiconductor layer (8). The functional layer (9) includes, for example, at least one of a GaN-based n-type semiconductor layer, a GaN-based non-doped semiconductor layer, a GaN-based p-type semiconductor layer, a conductive layer, and an insulating layer. Any film deposition method may be used for the GaN-based semiconductor layer of the functional layer (9). The functional layer (9) may be a compound semiconductor layer (compound semiconductor part). The compound semiconductor layer may be a nitride semiconductor layer (nitride semiconductor part), and in this case, the nitride semiconductor layer may include a p-type layer and an active layer (for example, a light-emitting layer), and the nitride semiconductor layer may include an n-type layer, an active layer, and a p-type layer.
[0039] The functional layer (9) may form a semiconductor device (e.g., LED, laser) together with the semiconductor layer (8), but is not limited to this. For example, it may only form a GaN-based n-type semiconductor layer.
[0040] (Device separation on a semiconductor substrate)
[0041] FIG. 6 is a cross-sectional view showing a device separation process according to the present embodiment. FIG. 7 is a plan view showing a device separation process according to the present embodiment. As shown in FIG. 6, in the semiconductor substrate (10), the region (AK) overlapping with the opening (KS) in the planar view is removed using vapor phase etching until it reaches the lower layer (4).
[0042] Here, a portion of each of the lower layer (4), mask layer (6), semiconductor layer (8), and functional layer (9) is to be removed, and the lower layer (4) and mask portion (5) are exposed within the trench (TR) (device separation groove) formed after removal. It is preferable that the opening width of the trench (TR) be larger than the opening (KS) of the mask layer. By the device separation process, the device portion (DS) can be separated from the semiconductor substrate (10). At this stage, the device portion (DS) is van der Waals bonded with the mask portion (5) of the template substrate and is part of the semiconductor substrate (10).
[0043] As shown in FIG. 7, the trench (TR) can be formed in a grid shape (lattice pattern) in a planar view. In this case, the configuration may include one element (DS) in the area surrounded by adjacent transverse trenches (extended in the X direction) and adjacent longitudinal trenches (extended in the Y direction).
[0044] Vapor etching is realized using a general photolithography method. After the etching is finished, it is necessary to remove the photoresist that served as the mask for the vapor etching. If organic cleaning is performed using weak ultrasound, there is less risk of the device part (DS) peeling off from the mask part (5).
[0045] FIG. 8 is a cross-sectional view showing another example of a device separation process. As shown in FIG. 8, the region overlapping with the opening (KS) and the region overlapping with the gap (GP) in the planar view of the semiconductor substrate (10) may be removed using vapor phase etching until it reaches the lower layer (4). By doing so, the meandering of the semiconductor layer (8) in the second direction (the length direction of the opening (KS), Y direction) is eliminated, and a device part (DS) with an aligned shape can be obtained.
[0046] FIG. 9 is a cross-sectional view showing another example of a device separation process. As shown in FIG. 9, in a semiconductor substrate (10), the region overlapping with the opening (KS) in a planar view and the region overlapping with the central part of the mask part (5) (ineffective part (NS)) can be removed using vapor phase etching until it reaches the lower layer (4).
[0047] (Detachment of device from template substrate)
[0048] FIG. 10 is a cross-sectional view illustrating a device peeling process. Since the semiconductor layer (8) and the mask portion (5) are bonded by van der Waals forces (weak forces), as shown in FIG. 10, the functional layer (9) can be lifted by means of attractive forces (adhesive force, suction force, electrostatic force, etc.) such as a stamp device (ST), thereby allowing the device portion (DS) to be easily peeled from the template substrate and made into a semiconductor device (20). The ability to peel directly from the mask portion (5) using a viscoelastic elastomer stamp, an electrostatic adhesive stamp, etc., is a significant advantage in terms of cost and throughput. However, since peeling becomes difficult if there is adhesion between the mask portion (5) and the semiconductor layer (8), reducing such adhesion is of great significance (described later). After contacting the viscoelastic elastomer stamp, an electrostatic adhesive stamp, etc., with the semiconductor layer (8), vibrations such as ultrasonic waves may be applied, for example. Due to this vibration, etc., the semiconductor layer (8) can be peeled off more easily from the mask portion (5).
[0049] FIG. 11 is a cross-sectional view showing another example of a device peeling process. As shown in FIG. 11, the mask portion (5) is wet-etched, and after the device portion (DS) of the semiconductor layer (8) is connected only to the seed layer (3), the device portion (DS) may be mechanically peeled from the template substrate (7) by means of a tape (TP), etc. In this case, since there is no need to etch the opening (KS), a large semiconductor device (20) can be formed. This peeling method has the advantage of being able to omit the device separation process when the semiconductor layer (8) is of the separable type (when it has an edge surface on the mask portion). When the semiconductor layer (8) is of the integral type (when it does not have an edge surface on the mask portion), it is sufficient to form a cut-out portion (up to the lower layer) for etchant inflow, and there is the advantage that device peeling is easy.
[0050] (Semiconductor device)
[0051] As shown in FIGS. 10 and 11, the device portion (DS) peeled off from the template substrate (7) functions as a semiconductor device (20). Specific semiconductor devices (20) may include, for example, a light-emitting diode (LED), a semiconductor laser, a Schottky diode, a photodiode, a transistor (including a power transistor and a high electron mobility transistor).
[0052] (Electronic devices)
[0053] FIG. 12 is a schematic diagram showing the configuration of an electronic device according to the present embodiment. The electronic device (30) of FIG. 12 includes a semiconductor device (20) comprising a semiconductor layer (8) and a functional layer (9), a driving substrate (23) on which the semiconductor device (20) is mounted, and a control circuit (25) for controlling the driving substrate (23). FIG. 13 is a schematic diagram showing another configuration of an electronic device according to the present embodiment. The electronic device (30) of FIG. 13 includes a semiconductor substrate (10) comprising a semiconductor layer (8) and a functional layer (9), a driving substrate (23) on which the semiconductor substrate (10) is mounted, and a control circuit (25) for controlling the driving substrate (23). In this case, the main substrate (1) may be a substrate having light transmittance (e.g., a sapphire substrate).
[0054] Examples of electronic devices include display devices, laser emitting devices (including Fabry-Perot type and surface-emitting type), measuring devices, lighting devices, communication devices, information processing devices, and power control devices.
[0055] (Air gap on the back side of the ELO semiconductor layer)
[0056] Below, the back side (interface with the mask portion (5)) of the ELO semiconductor layer (8) in the semiconductor substrate (10) will be described.
[0057] When a heterogeneous substrate is used and the mask portion (5) is widened, a void may form on the back side of the ELO semiconductor layer (8). This void becomes the cause of surface defects in the ELO semiconductor layer (8) (for example, the starting point of defects when stress is applied to the semiconductor layer (8)), and causes deterioration of the characteristics and reduction of reliability of the device formed on the ELO semiconductor layer (8). In this embodiment, by increasing the transverse film deposition rate and reducing the mutual reaction between the ELO semiconductor layer (8) and the mask portion (5), the surface morphology of the mask portion (5) is improved, and as a result, it is successful to reduce the void on the back side of the ELO semiconductor layer (8) and adhesion with the mask portion (5).
[0058] Specifically, in order to reduce the deterioration of the mask portion (5), the transverse film deposition rate is increased, and the mask portion (5) is rapidly covered with a transverse growth film (ELO semiconductor layer (8)). This is because if the transverse film deposition rate is low during MOCVD, the mask portion (5) is exposed to hydrogen and nitrogen for a long time at high temperatures, and evaporation and decomposition of the mask portion (5) proceed, which may lead to deterioration of the surface morphology, the occurrence of pinholes, and the occurrence of pits.
[0059] A method for increasing the transverse film formation rate is as follows. First, a longitudinal growth layer growing in the c-axis direction is formed on a seed portion exposed from the opening (KS) of the mask layer (6), and then a transverse growth layer growing in the a-axis direction is formed. At this time, by making the thickness of the longitudinal growth layer 10 μm or less, preferably 5 μm or less, and more preferably 3 μm or less, the thickness of the transverse growth layer is kept low, thereby increasing the transverse film formation rate.
[0060] FIG. 14 is a cross-sectional view illustrating an example of lateral growth of a semiconductor layer. As shown in FIG. 14, it is preferable to form an initial growth layer (SL) on a seed portion (3S) that overlaps with an opening (KS), and then to grow the semiconductor layer (8) laterally from the initial growth layer (SL). The initial growth layer (SL) serves as the starting point for the lateral growth of the semiconductor layer (8). In the deposition of the semiconductor layer (8), it is preferable to stop the deposition of the initial growth layer (SL) at a timing just before the edge of the initial growth layer (SL) climbs over the upper surface of the mask portion (5) (a stage where it is in contact with the upper side of the mask portion (5)), or immediately after it climbs over the upper surface of the mask portion (5) (i.e., at this timing, switch the ELO deposition conditions from the c-axis direction deposition conditions to the a-axis direction deposition conditions). In this way, since the initial growth layer (SL) is slightly protruding from the mask portion (5) and transverse film formation is performed, the consumption of material for growth in the thickness direction of the semiconductor layer (8) is reduced, and the semiconductor layer (8) can be effectively grown transversely at high speed. The initial growth layer (SL) can be formed with a thickness of 50 nm to 5.0 μm (for example, 80 nm to 2 μm). The thickness of the initial growth layer (SL) may be 500 nm or less.
[0061] As shown in FIG. 14, by forming an initial growth layer (SL) and then growing a semiconductor layer (8) in the transverse direction, it is possible to increase the non-penetrating potential within the effective portion (YS) (reduce the penetration potential density on the surface of the effective portion (YS)). In addition, the distribution of impurity concentration (e.g., silicon, oxygen) within the effective portion (YS) can be controlled. Meanwhile, by appropriately controlling the conditions during the formation of the semiconductor layer (8), it is possible to control the growth of the semiconductor layer (8) in the Z direction (c-axis direction) or in the X direction (a-axis direction).
[0062] For the effective portion (YS) of the semiconductor layer (8) shown in FIG. 14, the ratio (W1 / d1) of the size (W1) in the X direction (first direction) to the thickness (d1) can be, for example, 2.0 or more. By using the method of FIG. 14, W1 / d1 can be 1.5 or more, 2.0 or more, 4.0 or more, 5.0 or more, 7.0 or more, or 10.0 or more. It can be seen that by making W1 / d1 1.5 or more, the splitting process as shown in FIG. 7 becomes easier. In addition, the internal stress of the semiconductor layer (8) is reduced, and the bending of the substrate is reduced. The aspect ratio of the semiconductor layer (8) (ratio of size in the X direction to thickness = WL / d1) can be 3.5 or more, 5.0 or more, 6.0 or more, 8.0 or more, 10 or more, 15 or more, 20 or more, 30 or more, or 50 or more. Additionally, by using the method of FIG. 14, the ratio (WL / WK) of the size (WL) in the X direction of the semiconductor layer (8) to the width (WK) of the opening (KS) can be 3.5 or more, 5.0 or more, 6.0 or more, 8.0 or more, 10 or more, 15 or more, 20 or more, 30 or more, or 50 or more, and the ratio of the effective portion can be increased. The semiconductor layer (8) shown in FIG. 14 can be a nitride semiconductor crystal (e.g., GaN crystal, AlGaN crystal, InGaN crystal, or InAlGaN crystal).
[0063] Non-penetrating dislocations are dislocations observed in a cross-section by a plane parallel to the c-axis (a plane parallel to the thickness direction), and are mainly base plane (c-plane) dislocations. The plane parallel to the c-axis may be a plane parallel to the (1-100) plane (a plane with the normal in the Y direction) or a plane parallel to the (11-20) plane (a plane with the normal in the X direction).
[0064] The non-penetrating dislocation density of the effective portion (YS) of the semiconductor layer (8) is greater than the penetrating dislocation density of the effective portion (YS). In other words, the effective portion (YS) of the semiconductor layer (8) can be described as a GaN-based crystal (GaN-based layer) in which the non-penetrating dislocation density is greater than the penetrating dislocation density. In this case, the non-penetrating dislocation density can be at least 10 times, for example, at least 20 times, the penetrating dislocation density. The penetrating dislocation density is, for example, 5×10 6 [pieces / cm 2 ] It can be made less than. The width (length in the X direction) of the effective portion (GaN-based crystal) can be, for example, 10 μm or more. In addition, the effective portion (GaN-based crystal) can be made into a long shape in which the size in the Y direction (m-axis direction) is larger than the size in the X direction (a-axis direction). For the effective portion (GaN-based crystal), the non-penetrating dislocation density in the cross-section by the plane parallel to (11-20) plane may be greater than the non-penetrating dislocation density in the cross-section by the plane parallel to (1-100) plane. In addition, since the effective portion (GaN-based crystal) is formed by transverse (X-direction) growth, with respect to the X direction, the other end corresponding to the end of growth may have a lower concentration of impurities (atoms included in the mask layer (6), for example, silicon, oxygen) than the one end corresponding to the beginning of growth.
[0065] The quality of the mask portion (5) (uniformity of thickness, film quality, etc.) is influenced by the surface flatness, crystallinity, and material of the underlying layer on which the mask portion (5) is formed. If there is a defect in the underlying layer, the reaction between the mask portion (5) and the underlying layer proceeds from the defect, causing the quality of the mask portion (5) to deteriorate. As a result, the reaction between the mask portion (5) and the ELO semiconductor layer (8) deposited thereon is accelerated, and voids may occur on the back side of the ELO semiconductor (the boundary surface with the mask portion (5)). In the ELO method, since film deposition proceeds from both sides of the mask portion (5) toward the center, voids are likely to form in the part closer to the center (the part where the time to film deposition is long).
[0066] Regarding the deposition temperature of the ELO semiconductor layer (8), a temperature of 1150°C or lower is preferable to a high temperature exceeding 1200°C. It is possible to form the ELO semiconductor layer (8) at a low temperature below 1000°C, and this can be considered more desirable from the perspective of reducing mutual reactions. In such low-temperature deposition, it was found that when trimethylgallium (TMG) is used as the gallium raw material, the raw material is not sufficiently decomposed, and gallium atoms and carbon atoms enter the ELO semiconductor layer (8) in greater quantities than usual. It is thought that this is because, in the ELO method, deposition in the a-axis direction is fast and deposition in the c-axis direction is slow, so a large amount enters during the c-axis deposition.
[0067] It was found that carbon (carbon) included in the ELO semiconductor film reduces the reaction with the mask portion (5), thereby reducing mutual reaction with the mask portion (5) and preventing adhesion with the mask portion (5). Therefore, in the low-temperature deposition of the ELO semiconductor layer (8), the amount of ammonia supplied is reduced so that the film is deposited at a low V / III (<1000) level, allowing the ELO semiconductor layer (8) to accept carbon elements from the raw material or chamber atmosphere, thereby reducing the reaction with the mask portion (5). In this case, the semiconductor layer (8) is configured to include carbon (carbon).
[0068] In addition, for low-temperature film deposition below 1000°C, it is preferable to use triethylgallium (TEG) as the gallium source gas. Compared to TMG, TEG can increase the transverse film deposition rate because organic raw materials decompose efficiently at low temperatures.
[0069] An InGaN layer may be formed as the ELO semiconductor layer (8). The transverse deposition of the InGaN layer is performed at a low temperature, for example, below 1000°C. This is because at high temperatures, the vapor pressure of indium increases, so it does not effectively penetrate into the film. By making the deposition temperature low, the mutual reaction between the mask portion (5) and the InGaN layer is reduced. Additionally, the InGaN layer has the effect of having lower reactivity with the mask portion (5) than the GaN layer. It is desirable that the InGaN layer contains more than 1% of indium at the In composition level, as this further reduces reactivity with the mask portion (5). It is preferable to use triethylgallium (TEG) as the gallium source gas.
[0070] Since the mutual reaction between the mask portion (5) and the ELO semiconductor layer (8) is caused by a combination of various factors, the above-described measures may be combined.
[0071] By suppressing the occurrence of voids on the back side of the ELO semiconductor layer (8), linear defects on the surface (surface layer) of the ELO semiconductor layer (8) can be reduced. The m-plane of the ELO semiconductor layer (8) is vulnerable to stress and is prone to defects. These linear defects are thought to be caused by the slip of crystals along the m-plane. In a specific cross-section parallel to the c-plane, dislocations extending in the direction of the m-axis (presumed to be mixed dislocations combining blade-shaped dislocations and spiral dislocations) may be observed as linear defects, but the linear defects must disappear (not be observed) in a cross-section (parallel to the c-plane) cut from the surface layer than this specific cross-section.
[0072] (Adhesion on the back side of the ELO semiconductor layer)
[0073] When a heterogeneous substrate is used and the mask portion (5) is widened, adhesion may occur between the mask portion (5) and the back surface of the ELO semiconductor layer (8). If this adhesion is present, it becomes difficult to relieve stress caused by the difference in the coefficient of thermal expansion between the ELO semiconductor layer (8) and the heterogeneous substrate, which becomes a cause of surface defects. Additionally, when peeling the ELO semiconductor layer (8) from the template substrate (7), it worsens the peeling yield.
[0074] In this embodiment, the adhesion between the ELO semiconductor layer (8) and the mask portion (5) is reduced by reducing the mutual reaction between the ELO semiconductor layer (8) and the mask portion (5). Specifically, the material and thickness of the mask portion (5) are optimized, and the film density of the mask portion (5) is increased. When the film density of the mask portion (5) is low, the film evaporates quickly or the etching rate increases with respect to the film formation in the high temperature, hydrogen atmosphere of the MOCVD apparatus. When the ELO semiconductor layer (8) growing laterally covers such a mask portion (5), the mask portion (5) and the ELO semiconductor layer (8) adhere to each other. This is thought to be because a reaction layer formed by mixing the mask portion (5) and the ELO semiconductor layer (8) is generated, causing the ELO semiconductor layer (8) to become fixed to the mask portion (5).
[0075] When the ELO semiconductor layer (8) and the mask portion (5) are bonded together, an intermediate layer (a layer in which the mask portion (5) and the semiconductor layer (8) react or are mixed) is formed on the back side of the ELO semiconductor layer (8). This intermediate layer (bonding layer) is not removed even when the mask portion (5) is removed using an etchant such as hydrofluoric acid, and remains on the back side of the ELO semiconductor layer (8). Therefore, when the intermediate layer is formed, the surface morphology of the back side of the ELO semiconductor layer (8) after peeling from the template substrate (7) deteriorates. The effect of bonding is minimal when the arithmetic mean surface roughness Ra is 10 nm or less in an AFM (Atomic Force Microscope), and preferably about 1 nm. In addition, the effect of bonding is significant when Ra is about 13 nm. By using the peeling method described later (see Example 1) and measuring the surface roughness of the back side of the ELO semiconductor layer (8) with an AFM, the state of bonding can be determined.
[0076] (Desirable composition of the mask layer)
[0077] As a mask layer, the silicon oxide film (SiO₂) described above is used. x In addition to ), examples include a single layer made of any one of titanium nitride film (TiN, etc.), silicon nitride film (SiN, etc.), silicon oxynitride film (SiON), and high melting point metal film, or a multilayer film made of two or more.
[0078] The mask portion (5) may be a silicon nitride film or a silicon oxynitride film. Although a silicon oxide film may decompose and evaporate in small amounts during the formation of the ELO semiconductor layer (8) and enter the ELO semiconductor layer (8), silicon nitride films and silicon oxynitride films have the advantage of being difficult to decompose and evaporate at high temperatures. Meanwhile, even when a general silicon oxide film is used as the mask layer in the ELO method, the mutual reaction between the mask portion (5) and the ELO semiconductor layer (8) can be effectively reduced by optimizing the film formation conditions of the mask layer and the film formation conditions of the ELO semiconductor layer (8).
[0079] Accordingly, the mask layer may be a single layer of silicon nitride or silicon oxynitride, a multilayer film formed by forming a silicon oxide film and a silicon nitride film in this order on the underlying layer, a multilayer film formed by forming a silicon nitride film and a silicon oxide film in this order on the underlying layer, or a multilayer film formed by forming a silicon nitride film, a silicon oxide film, and a silicon nitride film in this order on the underlying layer.
[0080] Defective parts such as pinholes in the mask portion (5) may be eliminated by performing organic cleaning after film formation and then introducing it back into the film formation device to form the same type of film. A high-quality mask layer may also be formed using a general silicon oxide film and the above-mentioned re-film formation method.
[0081] (Evaluation of the semiconductor substrate)
[0082] Below, the evaluation of the semiconductor substrate (10) is described. FIGS. 15 to 18 are plan and schematic diagrams illustrating the evaluation of the semiconductor substrate (configured such that the ELO semiconductor layer has an edge surface on the mask). Regarding the back surface of the semiconductor layer (8) (the boundary surface (8R) with the mask portion), the evaluation may be performed in the state of the boundary surface in contact with the mask portion (5), or the semiconductor layer (8) may be peeled off from the mask portion (5) and the peeled surface may be evaluated. In this case, the semiconductor layer (8) can be peeled off by removing the mask portion (5) by wet etching, etc. (Also, if the semiconductor layer (8) is an integral type, pre-excavation up to the underlying layer (4) may be performed).
[0083] With respect to the semiconductor substrate (10), the surface of the ELO semiconductor layer (8) was measured by the CL (cathode luminescence) method, and the upper surface (8F) of the effective portion (YS) included at least one low-defect region (AL) having a size of 10 μm in the first direction (X) (a-axis direction) along the width direction of the opening (KS) and 10 μm in the second direction (Y) (m-axis direction) orthogonal to the first direction, and in the low-defect region (AL), no linear defect (a linear defect that is inclined toward the first direction (X) and is thought to be caused by m-plane slippage) was measured (see FIG. 15, evaluation criterion 1). More specifically, the upper surface of the effective portion (YS) included a plurality of low-defect regions (AL) arranged in the first direction (X) and a plurality of low-defect regions (AL) arranged in the second direction (Y) (see FIG. 15, evaluation criterion 2). The size of the first direction of the effective portion (YS) was larger than the width of the opening (KS) (see Fig. 15, evaluation criterion 3).
[0084] The effective portion (YS) had a first region (A1) having a size of 10 μm in the first direction (X) and 10 μm in the second direction (Y) at the boundary surface (8R) with the mask portion (5), and a second region (A2) having the same size as the first region (A1), located closer to the center of the mask portion (5) than the first region (A1), and having a gap (PT) from the center (5C) of the mask portion (5) that is 30% or less of the width of the mask portion (5). Then, the effective portion (YS) was peeled off from the mask portion (5), and the first region (A1) and the second region (A2) were observed using AFM. As a result, the number of concave portions with a major axis of 0.1 μm or more in the first region (A1) was less than the number of concave portions with a major axis of 0.1 μm or more in the second region (A2) (see FIG. 16, evaluation criterion 4). In addition, the major axis of the concave portion in the first region (A1) was 1㎛ or less (hereinafter, evaluation criterion 5).
[0085] In addition, regarding the effective portion (YS) before peeling from the mask portion (5), cross-sectional observation of the first region (A1) and the second region (A2) was performed using AFM, and the number of voids with a major axis of 0.1 [㎛] or larger in the first region (A1) was less than the number of voids with a major axis of 0.1 [㎛] or larger in the second region (A2) (see FIG. 16, evaluation criterion 6).
[0086] The effective portion (YS) had a third region (A3) having a size of 10 μm in the first direction (X) and 10 μm in the second direction (Y) at the interface (8R) with the mask portion (5), and a fourth region (A4) having the same size as the first region and located on the central side of the mask portion (5) compared to the third region (A3). Then, the effective portion (YS) was peeled off from the mask portion (5), and the first region (A3) and the second region (A4) were observed using AFM. As a result, the adhesion area of the third region (A3) was smaller than the adhesion area of the fourth region (A4) (see FIG. 17, evaluation criterion 7). In addition, the third region (A3) was a non-adhesion area where adhesion with the mask portion (5) was not substantially visible (hereinafter, evaluation criterion 8). Meanwhile, the fourth region (A4) was a position where the gap (PT) with the center (5C) of the mask portion was 30% or less of the width of the mask portion (5).
[0087] The effective portion (YS) includes a first portion (P1) and a second portion (P2) that is farther from the opening (KS) than the first portion (P1) and has a gap (KT) from the opening (KS) of 10 μm or more. The surface roughness (Ra) of the peeled surface (F1) when the first portion (P1) is peeled from the mask portion (5) is the first surface roughness, and the surface roughness (Ra) of the peeled surface (F2) when the second portion (P2) is peeled from the mask portion (5) is the second surface roughness, so that the first surface roughness is less than or equal to the second surface roughness (see FIG. 18, evaluation criterion 9). Here, the arithmetic mean roughness (Ra) for a 5 μm × 5 μm range of each peeled surface can be represented as an average value by taking a portion of the roughness curve measured by AFM as a reference length. In addition, the value of the ratio of the second surface roughness to the first surface roughness was 1.0 to 10 (Evaluation Criterion 10). In addition, when the effective portion (YS) was peeled off from the mask portion (5), the peeled surface (including F1 and F2) had a size of 10 μm in the first direction and 10 μm in the second direction, and included a flat area in which no concave portion with a major axis of 0.1 μm or more existed (Evaluation Criterion 11). In addition, the second surface roughness was less than 10 nm (Evaluation Criterion 12). In addition, in the planar view, the first portion (P1) was adjacent to the opening (KS), and the gap (PT) between the second portion (P2) and the center (5C) of the mask portion was 30% or less of the width of the mask portion (5) (Evaluation Criterion 13). In addition, the ratio of the area occupied by a concave portion with a major axis of 0.1 μm or more included in the peeling surface (F1) of the first part (P1) to the area occupied by a concave portion with a major axis of 0.1 μm or more included in the peeling surface (F2) of the second part to the area occupied by a concave portion with a major axis of 0.1 μm or more included in the peeling surface is the first concave portion ratio, and the first concave portion ratio is less than or equal to the second concave portion ratio (evaluation criterion 14). Here, the concave portion (void region) can be measured by AFM for a 5 μm × 5 μm range of each peeling surface to obtain its major axis, ratio, etc.
[0088] In addition, the impurity concentration in the peeled surface (F1) of the first part (P1) was greater than the impurity concentration in the peeled surface (F2) of the second part (P2) (evaluation criterion 15).
[0089] In addition, the penetration potential density on the upper surface (8R) of the effective portion (YS) is 5×10 6 [pieces / cm 2 ] was below (evaluation criterion 16).
[0090] As described above, in order to reduce surface defects of the semiconductor layer (8), it is important to reduce adhesion with the mask portion (5) to relieve stress, and at the same time reduce the occurrence of voids that cause surface defects (m-surface slippage).
[0091] The crystallinity of the ELO semiconductor layer (8) growing laterally on the mask (5) from the opening (KS) of the mask (5) is extremely high. In the semiconductor substrate (10), by reducing the mutual reaction between the mask portion (5) and the semiconductor layer (8), the voids and adhesions occurring on the back side of the semiconductor layer (8) are reduced, and the stress from the main substrate (1) can be effectively relieved. As a result, it can be seen that defects occurring in the effective portion (YS) do not penetrate to the surface of the semiconductor layer (8) but are trapped inside it.
[0092] FIGS. 19 to 22 are plan and schematic diagrams illustrating the evaluation of a semiconductor substrate with a different configuration (an integrated type in which the ELO semiconductor layer does not have an edge surface on the mask). In this case as well, it was found that evaluation criteria 1 to 16 were satisfied.
[0093] FIG. 23 shows a CL (cathode luminescence) image of an ELO semiconductor layer (8) of a semiconductor substrate (10) (the main substrate is a silicon substrate). No dark spots or dark lines are observed in the effective portion (YS). Only in the ineffective portion (NS) is a penetrating dislocation originating from the lattice integer difference between the silicon substrate and GaN 10 19 / cm 2There is a certain degree of existence.
[0094] FIG. 24 is a CL (cathode luminescence) image of an ELO semiconductor layer (8) of a semiconductor substrate (10) (the main substrate is a sapphire substrate). Since the ELO semiconductor layer (8) is mechanically peeled off from the template substrate, the non-effective portion (NS) is slightly damaged and the peeling surface is not flat, so the CL image is slightly distorted, but no dark spots or dark lines of penetrating dislocations are visible in the effective portion (YS), or a low dislocation density can be realized.
[0095] FIG. 25 is a CL image of the back side (peeled side) of the ELO semiconductor layer of the semiconductor substrate (10). It can be seen that no voids or adhesions are visible in the effective portion (YS).
[0096] (Reference example of the Tabernacle of ELO)
[0097] FIG. 26 shows the CL phase on the surface of the GaN layer of a reference example. In this reference example, sapphire is used as the substrate, and a GaN layer is deposited by the ELO method. On the opening, there are dark spots (10) which are high-density penetrating dislocations. 18 ~10 19 / cm 2 Both ) and dark lines exist. In addition, dark spots and dark lines are observed on the mask portion as well, although the density is lower than on the aperture portion.
[0098] FIG. 27 shows the CL phase on the surface of the GaN layer of the reference example. In this reference example, silicon is used as the main substrate, and a GaN layer is deposited by the ELO method. On the opening, 10 19 / cm 2 Dark spots are observed to a certain degree, and dark lines are also observed on the mask portion.
[0099] FIG. 28 shows the CL phase on the back side of the GaN layer of the reference example. In this reference example, silicon is used as the main substrate, and a GaN layer is deposited by the ELO method. A number of voids are observed at the ends of the mask portion.
[0100] FIG. 29 is an optical microscope image of the back side (peeling side) of the GaN layer of the ELO method film of the reference example. The adhesion (NL) (reaction layer) between the mask portion and the GaN layer can be seen. When this GaN layer is mechanically peeled from the mask portion (e.g., using a diamond pen), the GaN layer and the mask portion are peeled together from the template substrate, as shown in the peeling area (NA) of FIG. 30.
[0101] From the reference example, it can be seen that using the ELO method does not eliminate voids and adhesions, nor does it significantly reduce surface defects on the mask portion. Regarding dark lines (line-shaped defects), since their occurrence causes widespread effects, their reduction is of great significance.
[0102] (Example 1)
[0103] FIG. 31 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 1. A silicon substrate having a (111) plane was used for the main substrate (1). The buffer layer (2) of the lower layer (4) was made of an AlN layer (e.g., 30 nm). The seed layer (3) of the lower layer (4) is the first layer, Al 0.6 Ga 0.4 The N layer (e.g., 300 nm) and the second layer, a GaN layer (e.g., 1 to 2 μm), were formed in this order to form a graded layer. That is, the composition ratio of Ga (1 / 2=0.5) in the second layer (Ga:N=1:1) is greater than the composition ratio of Ga (0.6 / 2=0.3) in the first layer (Al:Ga:N=0.6:0.4:1).
[0104] A laminate formed by forming a silicon oxide film (SiO2) and a silicon nitride film (SiN) in this order was used for the mask layer (6). The thickness of the silicon oxide film is, for example, 0.3 μm, and the thickness of the silicon nitride film is, for example, 70 nm. A plasma chemical vapor deposition (CVD) method was used for forming the silicon oxide film and the silicon nitride film, respectively.
[0105] The semiconductor layer (8) was a GaN layer, and an ELO film was formed using an MOCVD apparatus. First, the ELO semiconductor layer (8) was selectively grown on the surface of the seed layer (3) (the second layer GaN layer) exposed to the opening (KS), and then subsequently grown laterally on the mask portion (5). At this time, growth was stopped before the semiconductor layers growing laterally from both sides on the mask portion (5) came together. At this time, the width of the gap (GP) was 2 μm.
[0106] The width (WM) of the mask portion (5) was 50㎛, the width of the opening portion (KS) was 5㎛, the width (WL) of the ELO semiconductor layer (8) was 53㎛, and the width (size in the X direction) of the effective portion (YS) was 24㎛. In addition, the layer thickness of the ELO semiconductor layer (8) was 5㎛, and the aspect ratio of the ELO semiconductor layer (8) was 53㎛ / 5㎛=10.6, so a very high aspect ratio was realized.
[0107] As a result of evaluating the semiconductor substrate (10) obtained in Example 1, it was found that the above-described evaluation criteria 1 to 16 were satisfied.
[0108] The peeling of the semiconductor layer (8) during the back-side evaluation of the semiconductor layer (8) can be performed as follows. For example, when the mask layer (6) is formed as a silicon oxide film, nitride film, or oxynitride film, the semiconductor substrate (10) that has undergone the device separation process (see FIG. 8 and FIG. 9) can be immersed in a hydrofluoric acid etchant for about 10 to 60 minutes so that the mask layer (6) dissolves in the etchant and the semiconductor layer (8) can be peeled from the template substrate (7).
[0109] As another peeling method, as shown in FIG. 32, the semiconductor substrate (10) is immersed in a hydrofluoric acid etchant to dissolve the mask layer (6), and then an adhesive tape (e.g., an adhesive dicing tape used when dicing a semiconductor wafer) is attached to the surface of the semiconductor layer (8). Then, using a Peltier element, the semiconductor substrate (10) with the adhesive tape attached may be lowered to a low temperature. At this time, the adhesive tape, which generally has a coefficient of thermal expansion greater than that of the semiconductor, shrinks significantly and applies stress to the semiconductor layer (8). Since the semiconductor layer (8) is bonded to the template substrate (7) only within the opening (KS) and the mask portion (5) is removed, the stress from the adhesive tape is effectively applied to the bonding portion with the template substrate (7), allowing the bonding portion to be mechanically cleaved or destroyed. That is, the bonding portion does not need to be removed by dry etching.
[0110] (Example 2)
[0111] FIG. 33 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 2. In Example 2, an integral type is adopted in which the ELO semiconductor layer (8) on the mask portion (5) does not have an edge surface. The width of the mask portion (5) is 50 μm, and the width of the opening (KS) is 5 μm. From the perspective of relieving film stress, the height of the hollow portion (8C) is preferably 1 μm or more. The width of the bottom surface of the hollow portion (8C) is also preferably 1 μm or more, and more preferably 2 μm or more.
[0112] As a result of evaluating the semiconductor substrate (10) obtained in Example 2, it was found that the above-described evaluation criteria 1 to 16 were satisfied.
[0113] (Example 3)
[0114] FIG. 34 is a cross-sectional view showing the configuration of a semiconductor substrate of Example 3. In Example 3, the width of the aperture (KS) is 700 nm, which is 1 μm or less, and the width of the mask portion (5) is 100 μm. In Example 3, since the width of the effective portion (YS) can be taken widely, it is desirable for high-power laser semiconductor devices (with a ridge width of about 40 μm), etc. FIG. 34 shows a structure in which the semiconductor layer (8) has an edge surface on the mask portion (5), but it may be an integrated type that does not have an edge on the mask portion (5).
[0115] As a result of evaluating the semiconductor substrate (10) obtained in Example 3, it was found that the above-described evaluation criteria 1 to 16 were satisfied.
[0116] (Example 4)
[0117] FIG. 35 is a cross-sectional view showing the configuration of Example 4. In Example 4, a functional layer (9) constituting an LED is formed on a semiconductor layer (8). The semiconductor layer (8) is an n-type semiconductor doped with, for example, silicon. The functional layer (9) includes, in order from the lower side, an active layer (34), an electron blocking layer (35), and a GaN-based p-type semiconductor layer (36). The active layer (34) is a Multi-Quantum Well (MQW) and includes an InGaN layer and a GaN layer. The electron blocking layer (35) is, for example, an AlGaN layer. The GaN-based p-type semiconductor layer (36) is, for example, a GaN layer. An anode (38) is formed to contact the GaN-based p-type semiconductor layer (36), and a cathode (39) is formed to contact the semiconductor layer (8).
[0118] Voids on the back side of the semiconductor layer cause surface defects (linear shape defects) and degrade the characteristics of the semiconductor device. Additionally, if the semiconductor device is a light-emitting element, voids on the back side of the semiconductor layer reduce the in-plane uniformity of the emitted light. In Example 6, since a device part (light-emitting element part) (DS) is formed on the ELO semiconductor layer (8) and the semiconductor device (20) which is a light-emitting element can be obtained by peeling it off, these problems can be improved. Specifically, no defects were observed in the light-emitting region of the semiconductor device (20).
[0119] FIG. 36 is a cross-sectional view showing an application example of Example 4. By Example 4, a red micro LED (20R), a green micro LED (20G), and a blue micro LED (20B) can be obtained, and by mounting these on a driving substrate (TFT substrate) (23), a micro LED display (30D) (electronic device) can be constructed. As an example, the red micro LED (20R), the green micro LED (20G), and the blue micro LED (20B) are mounted on a plurality of pixel circuits (27) of the driving substrate (23) by interposing a conductive resin (24) (e.g., anisotropic conductive resin), and then a control circuit (25) and a driver circuit (29), etc. are mounted on the driving substrate (23). A part of the driver circuit (29) may be included in the driving substrate (23).
[0120] (Example 5)
[0121] FIG. 37 is a cross-sectional view showing the configuration of Example 5. In Example 5, a functional layer (9) constituting a semiconductor laser is formed on a semiconductor layer (8). The functional layer (9) includes, in order from the bottom side, an n-type optical clad layer (41), an n-type optical guide layer (42), an active layer (43), an electron blocking layer (44), a p-type optical guide layer (45), a p-type optical clad layer (46), and a GaN-based p-type semiconductor layer (47). An InGaN layer may be used for each guide layer (42 and 45). A GaN layer or an AlGaN layer may be used for each clad layer (41 and 46). An anode (48) is formed to be in contact with the GaN-based p-type semiconductor layer (47).
[0122] In Example 5, as shown in FIG. 37, a cathode (49) is formed on the back side of the semiconductor layer (8) after the device portion (DS) is peeled off. Therefore, the quality of the back side of the semiconductor layer (8) affects the device characteristics.
[0123] (Example 6)
[0124] FIG. 38 is a cross-sectional view showing the configuration of Example 6. FIG. 39 is a cross-sectional view showing another configuration of Example 6. In Example 6, a sapphire substrate with surface roughness processing is used on the main substrate (1). The underlayer (4) has a buffer layer (2) and a seed layer (3). The semiconductor layer (8) may be in the form having an edge surface on the mask (5) (Fig. 38), or it may be an integral type without an edge surface on the mask (Fig. 39). In Example 6, a GaN layer having (20-21) planes can be deposited on the main substrate (1) as the underlayer (4). In this case, the ELO semiconductor layer (8) becomes the (20-21) planes, which are the crystal main surface of the underlayer (4), and an ELO semiconductor layer (8) with semipolar planes can be obtained. By forming a functional layer for a laser or LED on the semipolar planes, there are advantages such as a low piezoelectric field and a higher probability of electron-hole recombination in the active layer. Meanwhile, by using a sapphire substrate with surface roughness processing, a GaN layer having (11-22) planes can be formed as a lower layer (4) on the main substrate (1).
[0125] (Manufacturing device)
[0126] The method for manufacturing a semiconductor substrate (10) includes a process of forming a semiconductor layer (8) on at least a template substrate (7) using the ELO method. It may also include a process of forming an underlayer (4) and a mask layer (6) on a main substrate (1).
[0127] A semiconductor substrate (10) can be manufactured, for example, by a semiconductor substrate manufacturing apparatus described in FIG. 40. The semiconductor substrate manufacturing apparatus (70) includes at least a semiconductor layer forming unit (71) that performs a process of forming a semiconductor layer (8) on a template substrate (7) using the ELO method, and a control unit (72) that controls the semiconductor layer forming unit (71). The semiconductor layer forming unit (71) may include an MOCVD device, and the control unit (72) may include a processor and a memory. The control unit (72) may be configured to control the semiconductor layer forming unit (71) by executing a program stored on, for example, an internal memory, a communication device capable of communication, or an accessible network, and the program and a recording medium containing the program are also included in this embodiment. The semiconductor substrate manufacturing apparatus (70) may include a template substrate forming unit that performs a process of forming a lower layer (4) and a mask layer (6) on a main substrate (1), a functional layer forming unit that performs a process of forming a functional layer (9) on a semiconductor layer (8), etc. Additionally, a semiconductor device manufacturing apparatus that performs a device peeling process may be configured. The semiconductor device manufacturing apparatus may perform a device separation process. The semiconductor device manufacturing apparatus may include the semiconductor substrate manufacturing apparatus (70).
[0128] (Supplementary Note)
[0129] The invention of the present disclosure has been described above based on various drawings and embodiments. However, the invention of the present disclosure is not limited to each of the embodiments described above. That is, the invention of the present disclosure is capable of various modifications within the scope indicated in the present disclosure, and embodiments obtained by appropriately combining the technical means disclosed in each other embodiments are also included within the technical scope of the invention of the present disclosure. In other words, those skilled in the art should note that it is easy to make various modifications or variations based on the present disclosure. Furthermore, it should be noted that such modifications or variations are included within the scope of the present disclosure. Explanation of the symbols
[0130] *1; Main board 2; buffer layer 3; Seed layer 3S; Seed 4; Lower extremity layer 5; Mask part 6; Mask layer 8; semiconductor layer 9; Functional layer 10; semiconductor substrate 20; semiconductor device 30; electronic devices 70; Manufacturing apparatus for a semiconductor substrate KS; opening YS; Valid part
Claims
Claim 1 A semiconductor comprising a GaN-based semiconductor and a main substrate having different lattice constants, a first seed portion and a second seed portion located on an upper layer above the main substrate and adjacent to each other, a non-seed portion located between the first seed portion and the second seed portion, a first semiconductor portion including a GaN-based semiconductor and extending upward from the first seed portion to the non-seed portion, and a second semiconductor portion including a GaN-based semiconductor and extending upward from the second seed portion to the non-seed portion, wherein the first and second semiconductor portions are aligned with each other or adjacent with a gap, and the first semiconductor portion has a region in which the non-penetrating dislocation density is greater than the penetrating dislocation density, and the upper surface of the region includes a low-defect region in which line-shaped defects are not measured by the CL method, and wherein, in the region, one end that is closer to the first seed portion in the a-axis direction of the GaN-based semiconductor has a higher silicon concentration than the other end in the a-axis direction. Substrate. Claim 2 In claim 1, the above portion is elongated, and the size in the m-axis direction of the GaN-based semiconductor is larger than the size in the a-axis direction of the GaN-based semiconductor, the semiconductor substrate. Claim 3 In claim 1, the low-defect region is elongated, and the size in the m-axis direction of the GaN-based semiconductor is larger than the size in the a-axis direction of the GaN-based semiconductor, the semiconductor substrate. Claim 4 A semiconductor substrate according to claim 1, wherein the low-defect region overlaps the non-seed portion when viewed in a planar view. Claim 5 In claim 4, the semiconductor substrate comprises a non-seed portion including a mask portion formed from a silicon-based compound. Claim 6 In claim 1, the above portion is a semiconductor substrate in which the ratio of the length in the a-axis direction to the thickness in the c-axis direction of the GaN-based semiconductor is 5.0 or greater. Claim 7 In claim 1, the first and second semiconductor portions are adjacent semiconductor substrates spaced apart. Claim 8 In claim 7, the above gap is 4 μm or less, a semiconductor substrate. Claim 9 delete Claim 10 In claim 1, the above-mentioned portion is a semiconductor substrate that constitutes a part of the device portion in a post-processing step. Claim 11 A semiconductor substrate according to claim 1, wherein the non-seed portion is a mask layer, and the mask layer is a film comprising silicon oxide or silicon nitride.
Citation Information
Patent Citations
Semiconductor element and method of manufacturing the same
JP2012114263A