Anti-slip thermal spray coating structure and forming method thereof

The thermal spray coating method with inorganic materials forms a durable anti-slip surface using zigzag or coil patterns, addressing wear and sunlight issues, ensuring consistent anti-slip performance in high-friction environments.

KR103046457B1Active Publication Date: 2026-11-10KOREA INST OF MATERIALS SCI +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020240104764
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2026-11-10
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

Existing anti-slip coatings, such as those using epoxy-based resins with silica-based sand or oxide particles, are prone to wear, brittle, and degrade under sunlight, leading to inconsistent anti-slip functionality and reduced durability in environments with frequent friction and wear.

Method used

A thermal spray coating method using inorganic materials like metals and ceramics, forming a pattern with a predetermined pitch interval and shape, such as zigzag or coil, to create a durable anti-slip surface without post-treatment, resistant to sunlight degradation.

Benefits of technology

The coating maintains high friction coefficient and continuous anti-slip functionality even under long-term wear and friction, improving durability by reducing contact area and resisting sunlight degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024085558528-PAT00004_ABST
    Figure 112024085558528-PAT00004_ABST
Patent Text Reader

Abstract

The present invention relates to an anti-slip thermal spray coating structure and a method for forming the same. Specifically, the invention relates to a coating structure formed on the surface of a substrate by a thermal spray coating method, comprising one or more types of ceramic and metal, and including a pattern formed repeatedly in the transverse direction in which a predetermined shape protruding from the surface of the substrate is formed, wherein the predetermined shape has a predetermined pitch interval in the transverse direction and the pattern is formed repeatedly at a predetermined interval.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an anti-slip thermal spray coating structure and a method for forming the same. Background Technology

[0003] The decks or working areas of ships transporting cargo or passengers, offshore structures that remain at a point in the sea without being connected to land, and coastal structures such as shipyards, steel mills, estuary dams, and lock docks installed near the sea, are inherently rife with the risk of slipping and falling due to the humid environment. In addition, workplaces in manufacturing industries and construction sites, as well as the interiors and exteriors of transportation equipment, are also areas with a very high risk of slipping and falling due to the nature of the industries.

[0004] In order to protect workers from slipping and falling in such an environment, and to ensure the stability of equipment transport and the securing of loaded goods, appropriate anti-slip means must be provided on the surface of the deck, work area, or workplace.

[0005] Anti-slip coatings are widely used as a means of preventing slippage, and are generally formed by applying epoxy-based resins (paints). In particular, a method is widely used in which sand or hard particles are sprinkled onto the applied paint to impart anti-slip functionality through particles adhering to the paint surface. However, silica-based sand has low inherent hardness, making it vulnerable to friction and wear, and it is highly brittle and tends to crumble easily. Consequently, there is a problem in that its use is limited in the aforementioned deck areas, work areas, or workplaces where wear and impact are frequent.

[0006] To address these issues, a method was introduced in which wear-resistant particles are mixed into epoxy-based paints and applied together. Representative wear-resistant particles include oxide particles such as Al2O3, which are known to resolve the problem to some extent due to their excellent wear resistance and impact resistance. However, since the wear-resistant particles must exist in a protruding form on the surface of the applied paint to provide anti-slip functionality, there is a problem in that the anti-slip function cannot be maintained consistently and continuously.

[0007] To address these issues, a method is used in which large irregularities are formed on the surface of the paint using a roller, brush, or other tool after applying the paint to create a roughness suitable for anti-slip purposes. However, there are still problems to be solved, such as the method of forming roughness using the aforementioned tool being labor-intensive and the results varying depending on the operator's skill.

[0008] In addition, paint-type anti-slip coatings use epoxy-based resins, but since epoxy compound molecules containing benzene rings degrade due to sunlight, there is a problem of reduced friction coefficient or slip resistance over time. To solve this, siloxane-based paints with improved resistance to degradation by sunlight have been developed and are being used, but it is known that degradation by sunlight typically begins after about 2 to 3 years.

[0009] Therefore, there is a need for a new coating material and coating method that is resistant to friction or wear and does not break easily, has an active substance that provides anti-slip functionality always exposed on the surface, forms the roughness required for anti-slip solely through the coating itself without post-processing by tools, and undergoes almost no degradation due to sunlight.

[0010] To this end, a thermal spray coating method has been developed that involves melting and spraying inorganic materials, consisting of metals or a combination of metals and ceramics rather than organic materials. This method allows for the formation of a coating by introducing inorganic wires or powders into a heat source, such as an electric arc or an oxygen-fuel flame, to melt them, and then projecting them onto the surface of a substrate using the force of compressed gas or the flame. Consequently, it has become possible to produce inorganic coatings that possess a roughness capable of providing anti-slip properties without post-treatment, withstand friction and wear, and do not deteriorate due to sunlight.

[0011] In this regard, Korean registered patent No. 10-1528520 discloses an anti-slip moving walkway coated with ceramic using a thermal spray coating method for anti-slip purposes, and a method for manufacturing the same.

[0012] However, the anti-slip coating formed by the above-mentioned thermal spray coating method has a localized roughness capable of preventing slipping, but has a macroscopically flat surface, so when impact or wear occurs, general damage or wear occurs, and when exposed to a long-term wear and friction environment, the anti-slip properties deteriorate.

[0013] Therefore, there is an urgent need to develop an anti-slip coating that protects workers from slippery environments, such as decks and work areas of ships, offshore and coastal structures, as well as workplaces in manufacturing industries and construction sites, and the interiors and exteriors of transport equipment; ensures the stability of equipment transport and the securing of loaded goods; and possesses durability that prevents the deterioration of the overall anti-slip function when exposed to long-term friction and wear environments. Prior art literature

[0015] Republic of Korea Registered Patent No. 10-1528520 The problem to be solved

[0016] The purpose in one aspect is...

[0017] The invention provides an anti-slip thermal spray coating structure and a method for forming the same. means of solving the problem

[0019] In order to achieve the above objective,

[0020] In terms of work

[0021] A coating structure formed on the surface of a substrate by a thermal spray coating method,

[0022] It is composed of one or more types of ceramics and metals, and

[0023] It includes a pattern formed protruding from the surface of the base material and having a predetermined shape repeatedly formed in the transverse direction,

[0024] The above-mentioned predetermined shape has a predetermined pitch interval in the transverse direction, and

[0025] The above pattern is provided to be an anti-slip thermal spray coating structure formed repeatedly at predetermined intervals.

[0027] At this time, the pitch spacing in the transverse direction may preferably be 20 mm or more, preferably 20 mm to 305 mm.

[0028] In addition, the above pattern can be formed at intervals of 20 mm or more, preferably 20 mm to 305 mm.

[0030] In addition, the above pattern may have a zigzag, sawtooth, wave, or coil shape.

[0032] In addition, the height of the pattern from the surface of the base material may be 0.5 mm to 5.0 mm.

[0034] In addition, the above anti-slip thermal spray coating structure may further include a coating layer formed on the surface of the base material.

[0036] In other aspects of work

[0037] As a method for forming the above-mentioned anti-slip thermal spray coating structure,

[0038] A step of melting one or more wires or powders of ceramics and metals using a thermal spray coating device and spraying them onto the surface of a base material, wherein the movement of the spray nozzle head is controlled to form a pattern in which a predetermined shape having a predetermined pitch interval is formed transversely and protrudes from the surface of the base material and is repeated transversely; and

[0039] A method for forming an anti-slip thermal spray coating structure is provided, comprising the step of repeatedly forming the pattern at predetermined intervals on the surface of the base material.

[0041] At this time, the above-mentioned thermal spray coating device is

[0042] A material melting section for melting one or more powder or wire materials among metals and ceramics;

[0043] A spraying unit comprising a body and a spray nozzle head formed at one end of the body, which sprays a molten material melted in the material melting unit toward the surface to be coated of the base material by the pressure of compressed gas; and

[0044] It may include a control unit that controls the movement of the injection body and the injection nozzle head.

[0046] In addition, the step of forming the above pattern

[0047] The step may be to form the pattern in the first direction by moving the spray head in a linear or rotational motion through the control unit of the above-mentioned spray coating device, while simultaneously moving the spray body to move from one end of the base material to the other end (first direction) and spraying the molten material.

[0049] In addition, the material melting section of the above-mentioned thermal spray coating device can melt wire or powder using an arc spray method. Effects of the invention

[0051] The present invention is an anti-slip thermal spray coating structure that can be applied to base materials requiring anti-slip functions, such as decks or work areas of merchant ships, special vessels, offshore structures, and coastal structures, as well as workplaces in the manufacturing, construction, and transportation industries.

[0052] The anti-slip thermal spray coating structure of the present invention does not easily deteriorate from exposure to sunlight, has a predetermined roughness without a separate roughening process after coating, and has the advantage of continuously maintaining the anti-slip function even if a part of the deck or work surface is worn or damaged in a friction or abrasion environment.

[0054] Compared to conventional coating methods that have a locally rough and macroscopically flat shape, resulting in uniform surface wear and significant deterioration of durability under friction and wear environments, the anti-slip thermal spray coating structure of the present invention has the advantage of significantly improving wear resistance performance by forming a pattern consisting of lines such as circular or zigzag shapes. This is achieved by ensuring that a high coefficient of friction is maintained even after wear occurs, as wear occurs along the shape of each pattern.

[0056] The effects of the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by a person skilled in the art from the description below. Brief explanation of the drawing

[0058] FIG. 1 is a schematic diagram illustrating the process of forming an anti-slip coating structure according to one embodiment. Figure 2 is a schematic diagram showing the process of forming an anti-slip coating structure by a conventional thermal spray coating method. Figure 3 is a drawing showing a surface photograph of an anti-slip coating formed by the method of Figure 2. FIG. 4 is a drawing showing the coating shape according to the movement of the spray nozzle head in a method for forming an anti-slip coating structure according to one embodiment. Figure 5 is a schematic diagram (left), a photograph observed with the naked eye (center), and a height profile map (right) of the anti-slip coating structure according to Comparative Example 1. Figure 6 is a schematic diagram (left), a photograph observed with the naked eye (center), and a height profile map (right) of an anti-slip coating structure according to Example 1. Figure 7 is a schematic diagram (left), a photograph observed with the naked eye (center), and a height profile map (right) of an anti-slip coating structure according to Example 2. Figure 8 is a schematic diagram (left), a photograph observed with the naked eye (center), and a height profile map (right) of an anti-slip coating structure according to Example 3. Figure 9 is a schematic diagram (left), a photograph observed with the naked eye (center), and a height profile map (right) of an anti-slip coating structure according to Example 4. Figure 10 is a photograph showing the surface condition of an anti-slip thermal spray coating structure according to an example and a comparative example, observed visually. FIG. 11 is a height profile map (top) and graph (bottom) of an anti-slip thermal spray coating structure according to an example and a comparative example. Figure 12 is a photograph of the surface of an anti-slip thermal spray coating structure according to an example and a comparative example after wear evaluation, observed visually. Figure 13 is a graph showing a comparison of the friction coefficients after wear evaluation of the coating structures formed in the example and comparative example. Figure 14 is a graph comparing the wear resistance performance improvement effect of the coating structure formed in the example and comparative example. Specific details for implementing the invention

[0059] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the specific embodiments described below and should be understood to include all modifications, equivalents, and substitutions that fall within the spirit and scope of the present invention.

[0060] The terms used in this specification are used merely to describe specific embodiments and are not limited thereto.

[0061] Throughout the specification and claims, the terms “first” and “second” are used for distinction purposes in this specification and do not imply or suggest any order or priority in any way. They may be used to describe various components, but said components are not limited by said terms. For example, without departing from the scope of the invention, the first component may be named the second component, and similarly, the second component may be named the first component.

[0062] Furthermore, when it is stated that one component is "connected" or "connected" to another component, it should be understood that while it may be directly connected or connected to that other component, there may also be other components in between. On the other hand, when it is stated that one component is "directly connected" or "directly connected" to another component, it should be understood that there are no other components in between.

[0063] Furthermore, terms such as “include” or “have” are intended merely to indicate the existence of the features, numbers, steps, actions, components, parts, or combinations thereof described in the specification, and do not exclude the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.

[0064] Furthermore, unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this specification.

[0066] In terms of work

[0067] A coating structure formed on the surface of a substrate by a thermal spray coating method,

[0068] It is composed of one or more types of ceramics and metals, and

[0069] It includes a pattern formed protruding from the surface of the base material and having a predetermined shape repeatedly formed in the transverse direction,

[0070] The above-mentioned predetermined shape has a predetermined pitch interval in the transverse direction, and

[0071] The above pattern is provided to be an anti-slip thermal spray coating structure formed repeatedly at predetermined intervals.

[0073] Hereinafter, an anti-slip thermal spray coating structure according to one embodiment will be described in detail with reference to the drawings.

[0075] FIG. 1 is a schematic diagram showing the process of forming an anti-slip coating structure according to one embodiment, FIG. 2 is a schematic diagram showing the process of forming an anti-slip coating structure by a conventional thermal spray coating method, and FIG. 3 is a diagram showing a surface photograph of an anti-slip coating formed by the method of FIG. 2.

[0077] An anti-slip thermal spray coating structure according to one embodiment is a coating structure formed on the surface of a substrate.

[0078] At this time, the surface of the base material may be the surface of various structures requiring anti-slip means, specifically, the surface of a ship transporting cargo or passengers, the surface of an offshore structure that is not connected to land and remains at a point in the sea, the surface of the deck or work area of ​​a coastal structure such as a shipyard, steel mill, estuary dam, or lock-type dock installed near the sea, the work area of ​​a construction site, and the inner and outer surfaces of a transport device.

[0079] The above base material may be composed of a material to which a thermal spray coating can be applied, and specifically, may be composed of materials such as metal, concrete, or tile.

[0081] The anti-slip thermal spray coating structure according to one embodiment is a coating structure formed by a thermal spray coating method.

[0082] Accordingly, the above anti-slip thermal spray coating structure is formed by melting and spraying an inorganic material composed of one or more types of metals and ceramics, rather than organic materials; more specifically, an inorganic wire or powder is introduced into a heat source such as an electric arc or an oxygen-fuel flame to melt it, and then the coating is formed by projecting it onto the surface of a base material using the force of compressed gas or flame.

[0083] Accordingly, the above-mentioned anti-slip thermal spray coating structure has a roughness that enables anti-slip properties solely through the coating itself without post-treatment, withstands friction and wear, and has the advantage of not deteriorating due to sunlight.

[0085] The anti-slip thermal spray coating structure according to one embodiment is composed of one or more types of ceramic and metal.

[0086] In this case, the ceramic may be aluminum oxide (Al2O3), titanium oxide (TiO2), chromium oxide (Cr2O3), zirconium oxide (ZrO2), calcium oxide (CaO), magnesium oxide (MgO), or a mixture thereof, but is not limited thereto.

[0087] In addition, the metal may be aluminum (Al), titanium (Ti), magnesium (Mg), tungsten (W), or a mixture thereof, but is not limited thereto.

[0089] The anti-slip thermal spray coating structure according to one embodiment is

[0090] It includes a pattern formed protruding from the surface of the base material and having a predetermined shape repeatedly formed in the transverse direction,

[0091] The above-mentioned predetermined shape has a predetermined pitch interval in the transverse direction, and

[0092] The above pattern is characterized by being formed repeatedly at predetermined intervals.

[0093] This is intended to improve frictional durability by preventing the deterioration of the anti-slip function.

[0095] A conventional anti-slip thermal spray coating structure includes a pattern composed of a plurality of lines formed protruding from the surface of a substrate, wherein the lines have a continuous straight line shape in the direction in which they are extended, and the pattern composed of the plurality of lines is referred to as a "ladder pattern" (see FIGS. 2 and 3).

[0096] This coating structure has a localized roughness that prevents slipping, but forms a flat surface macroscopically. Consequently, when impact or wear occurs, full-surface damage or wear occurs, and when exposed to long-term wear and friction environments, the anti-slip properties deteriorate.

[0098] The anti-slip thermal spray coating structure according to one embodiment is intended to improve the durability of the anti-slip properties,

[0099] It includes a pattern formed protruding from the surface of the base material and having a predetermined shape repeatedly formed in the transverse direction,

[0100] The above-mentioned predetermined shape has a predetermined pitch interval in the transverse direction, and

[0101] The above pattern is characterized by being formed repeatedly at predetermined intervals.

[0103] The anti-slip thermal spray coating structure according to one embodiment has the advantage of high durability against wear and friction by reducing the contact area with the relative friction material through a structure in which the pattern is repeatedly formed at predetermined intervals.

[0104] The above pattern is, for example, ' A zigzag formed by the repetition of the shape of ' The shape of ' can have a repeating sawtooth, wave, or coiled form.

[0105] Figure 1 shows a coil-shaped pattern and a zigzag-shaped pattern (20).

[0107] The above pattern may preferably be formed by repeating the same shape so as to have a pitch spacing of at least 20 mm in the transverse direction, preferably at least 50 mm. Additionally, the above pattern may preferably be formed at a spacing of at least 20 mm, preferably at least 50 mm.

[0108] Here, "transverse pitch interval" refers to the interval at which a predetermined shape is repeated within the pattern, and specifically, refers to the straight-line distance between the starting points where the predetermined shape is repeated.

[0109] In addition, the “pattern spacing” mentioned above refers to the distance between adjacent patterns, specifically the straight-line distance between starting points where a predetermined shape within an adjacent pattern is repeated.

[0110] The above-mentioned pitch spacing and pattern spacing in the transverse direction are intended to improve the durability of the anti-slip properties. However, if the above-mentioned pitch spacing and pattern spacing are less than 20 mm, the effect of improving the durability of the anti-slip properties may be insufficient.

[0112] In addition, the upper limit of the pitch spacing in the transverse direction and the spacing of the pattern may vary depending on the contact area with the friction counter material, and it is preferable to form the pattern and / or a predetermined shape in the pattern such that at least two are included within the contact area of ​​the friction counter material.

[0114] In addition, the pitch spacing and pattern spacing in the transverse direction may each preferably be 20 mm to 305 mm, preferably 50 mm to 250 mm, preferably 50 mm to 200 mm, and preferably 50 mm to 100 mm.

[0115] At this time, if the pitch spacing and pattern spacing are smaller than 20 mm, the effect of reducing the contact area with the relative friction material is insufficient, and thus the effect of improving the durability of the anti-slip properties may be insufficient. Additionally, if the pitch spacing and pattern spacing exceed 305 mm, the anti-slip effect and the effect of improving durability by the coating structure may be insufficient.

[0117] In addition, the height of the pattern from the surface of the base material may be 0.5 mm to 5.0 mm, and more preferably 1 mm to 3.5 mm.

[0119] This is intended to cause the above pattern to wear down gradually as it wears against the opposing friction material. If the height of the above pattern is less than 0.5 mm, a problem may arise where the anti-slip function is lost due to repeated friction with the opposing friction material. Additionally, if the height of the above pattern exceeds 5.0 mm, a problem may arise where the coating structure is damaged due to friction with the opposing friction material, thereby reducing the anti-slip function.

[0121] An anti-slip thermal spray coating structure according to one embodiment may further include a coating layer formed on the surface of a substrate, and the coating layer may be formed in an area where the pattern is not formed.

[0122] The coating layer can preferably be formed with a thickness of 0.5 mm to 5.0 mm.

[0124] In other aspects of work

[0125] As a method for forming the above-mentioned anti-slip thermal spray coating structure,

[0126] A step of melting one or more wires or powders of ceramics and metals using a thermal spray coating device and spraying them onto the surface of a base material, wherein the movement of the spray nozzle head is controlled to form a pattern in which a predetermined shape having a predetermined pitch interval is formed transversely and protrudes from the surface of the base material and is repeated transversely; and

[0127] A method for forming an anti-slip thermal spray coating structure is provided, comprising the step of repeatedly forming the pattern at predetermined intervals on the surface of the base material.

[0129] Hereinafter, a method for forming an anti-slip thermal spray coating structure according to one embodiment will be described in detail step by step with reference to the drawings.

[0131] A method for forming an anti-slip thermal spray coating structure according to one embodiment includes the step of melting one or more wires or powders of ceramics and metals using a thermal spray coating device and spraying them onto the surface of a base material, and controlling the movement of the spray nozzle to form a pattern in which a predetermined shape having a predetermined pitch interval in the transverse direction is formed repeatedly in the transverse direction and protrudes from the surface of the base material.

[0133] A method for forming an anti-slip thermal spray coating structure according to one embodiment is characterized by using a spraying unit of a thermal spray coating device to spray molten material onto the surface of a substrate for coating, wherein the spraying unit head of the thermal spray coating device is moved in a straight line or rotational motion, and at the same time the spraying unit body is moved in a direction (first direction) from one end of the substrate to the other end perpendicular to the direction of coating progress, and the molten material is sprayed to form a pattern in which a predetermined shape is formed protruding from the surface of the substrate and has a predetermined pitch spacing in the transverse direction and is repeated in the transverse direction.

[0135] FIG. 4 is a drawing showing the coating shape according to the movement of the spray nozzle head in a method for forming an anti-slip coating structure according to one embodiment.

[0136] Referring to FIG. 4, in the conventional case, only the spray body is moved from one end of the substrate to the other without movement of the spray head, thereby forming a straight line. In contrast, the method for forming a thermal spray coating structure according to one embodiment forms a pattern such as a zigzag, sawtooth, wave, or coil shape by moving the spray body in a direction (first direction) from one end of the substrate perpendicular to the coating direction while moving the spray nozzle head in a straight or rotational motion. Here, the pattern may preferably be formed by repeating the same shape to have a pitch spacing of at least 20 mm in the transverse direction, preferably at least 50 mm.

[0137] The above pitch spacing in the transverse direction is intended to improve the durability of the anti-slip properties, and if the above pitch spacing is less than 20 mm, the effect of improving the durability of the anti-slip properties may be insufficient.

[0138] In addition, the upper limit of the pitch spacing in the transverse direction may vary depending on the contact area with the friction counter material, and it is preferable to form it so that at least two of the pattern and / or a predetermined shape in the pattern are included within the contact area of ​​the friction counter material.

[0140] For example, when a predetermined shape in the friction counter material and pattern is repeated in a transverse direction at a distance of 305 mm, the pitch spacing in the transverse direction may be 20 mm to 305 mm, preferably 50 mm to 250 mm, more preferably 50 mm to 200 mm, and more preferably 50 mm to 100 mm.

[0141] At this time, if the above pitch spacing is less than 20 mm, the effect of reducing the contact area with the relative friction material is insufficient, and thus the effect of improving the durability of the anti-slip properties may be insufficient. Also, if the above pitch spacing exceeds 305 mm, the anti-slip effect and the effect of improving durability by the coating structure may be insufficient.

[0142] In addition, the height of the pattern from the surface of the base material may be 0.5 mm to 5.0 mm, and more preferably 1 mm to 3.5 mm.

[0143] A method for forming an anti-slip thermal spray coating structure according to one embodiment includes the step of repeatedly forming the pattern at predetermined intervals.

[0144] A method for forming an anti-slip thermal spray coating structure according to one embodiment can form a coating structure with significantly superior durability against wear and friction by forming a coating structure in which a pattern such as a zigzag, sawtooth, wave, or coil shape is repeatedly formed at predetermined intervals over the entire surface to be coated of a substrate.

[0146] Here, the above-mentioned thermal spray coating device (100) is

[0147] A material melting section (not shown) for melting one or more powder or wire materials among metals and ceramics;

[0148] A spraying unit (100) comprising a body (110) and a spray nozzle head (111) formed at one end of the body (110), and spraying a molten material melted in the material melting unit toward the surface to be coated of the base material by the pressure of compressed gas; and

[0149] It may include a control unit that controls the movement of the injection body (110) and the injection nozzle head (111).

[0151] Referring to FIG. 2, a conventional method for forming a thermal spray coating structure on the entire surface of a coated surface specifically includes the following steps:

[0152] A step of forming a first line by moving the body (110) of the spraying unit (100) of the thermal spraying device in a direction (Y-axis first direction) from one end of the base material to the other end perpendicular to the coating progress direction, and spraying the molten material toward the surface to be coated of the base material (first step);

[0153] A step of forming a second line by moving a predetermined distance in the coating progress direction (a direction perpendicular to the first direction, X-axis direction) and then spraying the molten material toward the surface to be coated of the base material in the reverse direction of the first direction, i.e., the direction from the other end to the end of the base material (Y-axis second direction); and

[0154] Step (3) of moving a predetermined distance in the coating direction (X-axis direction) and then repeating the first and second steps to form a pattern composed of a plurality of lines protruding from the surface of the base material.

[0156] Each line formed by the above-described conventional method has a continuous straight line shape in the direction in which it is extended, and a pattern composed of multiple such lines is referred to as a "ladder pattern."

[0157] As shown in Fig. 3, this coating structure has a localized roughness that prevents slipping, but forms a flat surface macroscopically. Consequently, when impact or wear occurs, full-surface damage or wear occurs, and when exposed to long-term wear and friction environments, the anti-slip properties deteriorate.

[0159] On the other hand, unlike conventional methods, the anti-slip spray coating structure according to one embodiment can be formed by moving the spray head (111) in a linear or rotational motion while moving the spray body (110), and specifically, it can be formed by the following method (see FIG. 1).

[0160] A step of forming a first pattern by moving the spray head (111) of the spraying device in a linear or rotational motion, while moving the spray body (110) in a direction (first direction) from one end of the base material to the other end perpendicular to the direction of coating progress, and spraying the molten material toward the surface to be coated of the base material;

[0161] A step of forming a second pattern by moving a predetermined distance in the coating progress direction (a direction perpendicular to the first direction) and then spraying the molten material toward the surface to be coated of the base material in the reverse direction of the first direction, i.e., in the direction from the other end to the end of the base material (second direction); and

[0162] Step (3) of moving a predetermined distance in the coating direction (a direction perpendicular to the first direction) and then repeating the first and second steps to repeatedly form a pattern protruding from the surface of the substrate at predetermined intervals.

[0164] A method for forming an anti-slip thermal spray coating structure according to one embodiment can significantly improve durability by forming a coating structure in which a pattern having a predetermined pitch interval is repeatedly formed in the transverse direction, such as a zigzag, sawtooth, wave, or coil, by the above method.

[0166] The present invention will be explained in detail below through embodiments and experimental examples.

[0167] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited by the following examples.

[0169] <Example 1>

[0170] An aluminum alloy was spray-coated onto an Fe-based substrate using a spray-coating device, and a coating structure was formed in which a circular shape was repeatedly formed at a height of 100 mm and a pitch interval of 25 mm in the transverse direction, and a coil-shaped pattern formed therein was repeated at a interval of 90 mm.

[0172] <Example 2>

[0173] A coating structure having a pattern in which coil-shaped lines are repeatedly formed was formed by performing the same method as in Example 1, except that the pitch spacing and pattern spacing in Example 1 were different, to 50 mm and 75 mm, respectively.

[0175] <Example 3>

[0176] An aluminum alloy is thermally coated onto an Fe-based substrate using a thermal spraying device, wherein the coating is applied at a height of 100mm and in the lateral direction through the control of the spray head. A zigzag pattern formed by repeating the shape at a pitch interval of 50 mm was formed, and a coating structure formed by repeating the zigzag pattern at a interval of 50 mm was formed.

[0178] <Example 4>

[0179] Except for changing the pitch spacing and pattern spacing to 100mm in the above Example 3, the same method as in Example 2 was performed to form a coating structure in which a zigzag pattern is repeatedly formed.

[0181] <Comparison Example 1>

[0182] An aluminum alloy was thermally coated onto an Fe-based substrate using a thermal spray coating device, and a coating structure was formed in which straight lines with a height of 100 mm were repeatedly formed at intervals of 8 mm.

[0184] <Experiment Example 1>

[0185] In order to compare the surface condition of the anti-slip thermal spray coating structure according to the example and comparative example, the coating structures formed in Comparative Example 1 and Examples 1 to 4 were observed visually, and the results are shown in FIGS. 5 to 9 and compared in FIG. 10. The height profile was measured using a 3D volumetric shape measuring device, and the height map for the entire area is shown in FIGS. 5 to 9. In FIG. 11, the height profile graph (lower drawing) in the line extension direction (Y direction) was compared with the map (upper drawing).

[0186] As shown in FIGS. 5 and FIGS. 10, it can be confirmed that the coating structure formed in Comparative Example 1 has surface protrusion particles of 1 mm or less size generated during the coating process uniformly distributed, and the coating surface is formed smoothly overall.

[0187] On the other hand, as shown in FIGS. 6 to 9 and FIG. 10, it can be seen that the coating structures formed in Examples 1 to 4 have a primary surface structure due to differences in coating thickness by location, and simultaneously have a secondary surface structure through relatively large surface protrusions of about 1.7 mm around the movement path.

[0189] In addition, when comparing the height profile maps in FIGS. 5 to 9 and FIG. 11, it can be seen that in the case of Comparative Example 1, the height difference is negligible across the entire surface of the coating structure and it has a uniform height overall, whereas in Examples 1 to 4, a pattern with a height difference is formed.

[0190] In addition, looking at the height profile graph in the line extension direction in Fig. 6, it can be seen that Comparative Example 1 has a height of almost similar value, whereas the coil pattern or zigzag pattern coatings of Examples 1 and 3 have a sine wave profile shape, although the size or period of the surface shape is different.

[0191] In addition, as a result of analyzing the width (W) and peak-to-peak amplitude (A) in the sine wave according to each surface shape of Examples 1 and 3, for the coil-shaped pattern of Example 1, the maximum width (Wmax) in the sine wave was about 74 cm and the peak-to-peak maximum amplitude (Amax) was about 1.2 mm, and for the zigzag-shaped pattern of Example 2, the maximum width (Wmax) in the sine wave was 90 cm and the peak-to-peak maximum amplitude (Amax) was about 1.1 mm.

[0192] Through the above results, it can be confirmed that the coating structures of Examples 1 to 4 have a height difference in the form of a sine wave and have a dual roughness structure due to surface protrusions.

[0194] <Experiment Example 2>

[0195] In order to evaluate the frictional durability of the anti-slip thermal spray coating structure according to the examples and comparative examples, a wear resistance test was performed on the coating structures formed in Examples 1 and 3 and Comparative Example 1 using a cable wear evaluation device, and the results are shown in FIGS. 12 to 14 and Table 1.

[0196] At this time, the relative wear material and the coating structure were set to be in contact with a width of 150 mm in the transverse direction where a predetermined shape is repeatedly formed, and a wear evaluation was performed while moving the cable in the direction where the pattern is repeatedly formed.

[0198] FIG. 12 is a photograph showing the surface of the coating structure formed in Examples 1 and 3 and Comparative Example 1 after a wear evaluation, and as shown in FIG. 5, in the case of Comparative Example 1, wear occurred over the entire surface area of ​​the coating structure, whereas in the coating structures of Examples 1 and 3, wear occurred along the shape of the pattern formed protruding from the surface of the substrate.

[0199] From the above results, it can be confirmed that in Examples 1 and 3, the contact area between the coating structure and the relative friction material is reduced.

[0201] In addition, Figure 13 and Table 1 compare the friction coefficients after wear evaluation of the coating structures formed in Comparative Example 1 and Examples 1 to 4. Through Table 1, it can be confirmed that the coating structures of Examples 1 to 4 maintain a higher friction coefficient than Comparative Example 1. Through Figure 13, it can be confirmed that the coating structure in which the zigzag pattern of Example 3 and the coil pattern of Example 3 are repeatedly formed maintains a friction coefficient that is 15% and 29% higher, respectively, compared to the trapezoidal pattern of Comparative Example 1, thus confirming that the coil pattern maintains a higher friction coefficient than the zigzag pattern.

[0202] line shape Pitch spacing Pattern spacing coefficient of friction Before wear test After the wear test Example 1 coil 25mm 90mm 1.3 1.08 Example 2 coil 50mm 75mm 1.3 1.13 Example 3 zigzag 50mm 50mm 1.3 0.98 Example 4 zigzag 100mm 100mm 1.3 1.01 Comparison Example 1 beeline - 8mm 1.3 0.87

[0203] Through the above results, it can be confirmed that the coating structure according to the embodiment, which includes a pattern formed protruding from the surface of the base material and having a predetermined shape repeatedly formed in the transverse direction, wherein the predetermined shape has a pitch spacing of at least 20 mm in the transverse direction and the pattern has a three-dimensional structure repeatedly formed at a spacing of at least 20 mm, preferably 50 mm, has high durability against wear and friction compared to a conventional coating structure formed with a trapezoidal pattern, even when exposed to a friction environment for a long time.

[0205] In addition, FIG. 14 compares the wear resistance performance improvement effect of the coating structures formed in Examples 1 and 3 and Comparative Example 1, and calculates the value obtained by subtracting the weight after evaluation from the initial weight, and the smaller the calculated value, the better the durability can be seen.

[0207] As a result of the calculation, it can be confirmed that the coating structure formed in Examples 1 and 3 has more than twice the wear resistance characteristics compared to the coating structure formed in Comparative Example 1.

[0208] Through the above results, it can be confirmed that the coating structure according to the embodiment includes a pattern formed protruding from the surface of the substrate and having a predetermined shape repeatedly formed in the transverse direction, and that the predetermined shape has a pitch spacing of 20 mm or more in the transverse direction, and that the durability is significantly improved through a three-dimensional structure in which the pattern is repeatedly formed at a spacing of 20 mm or more. Explanation of the symbols

[0210] 100: Spraying part of the thermal spraying device 110: Body of the spray unit 111: Head of the spray unit

Claims

Claim 1 A method for forming an anti-slip thermal spray coating structure, comprising: a step of melting one or more types of wire or powder among ceramics and metals using a thermal spray coating device and spraying it onto the surface of a base material, wherein the spraying body is moved to move a spray nozzle head formed at one end of the spraying body in a straight line from one end of the base material to the other end (a first direction), while simultaneously moving the spray nozzle head in a straight line or rotationally and spraying to form a line pattern in which a predetermined shape having a predetermined pitch interval is formed protruding from the surface of the base material and is repeated in the transverse direction; and a step of repeating the line pattern at a predetermined interval on the surface of the base material. Claim 2 A method for forming an anti-slip thermal spray coating structure according to claim 1, wherein the thermal spray coating device comprises: a material melting section for melting one or more powder or wire materials among metals and ceramics; a spraying section including a spraying section body and a spray nozzle head formed at one end of the body, which sprays the molten material melted in the material melting section toward the surface to be coated of a base material by the pressure of compressed gas; and a control section for controlling the movement of the spraying section body and the spray nozzle head. Claim 3 A method for forming an anti-slip thermal spray coating structure according to claim 1, wherein the material melting part of the thermal spray coating device melts a wire or powder using an arc spray method. Claim 4 An anti-slip thermal spray coating structure formed by a thermal spray coating method on the surface of a base material using the forming method of claim 1, comprising one or more types of ceramic and metal, and including a line pattern formed protruding from the surface of the base material and having a predetermined shape repeatedly formed in the transverse direction, wherein the predetermined shape has a predetermined pitch interval in the transverse direction and the line pattern is repeatedly formed at a predetermined interval. Claim 5 In claim 4, the anti-slip thermal spray coating structure wherein the pitch spacing in the transverse direction is 20 mm to 305 mm. Claim 6 In paragraph 4, the above pattern is an anti-slip thermal spray coating structure having a zigzag, sawtooth, wave, or coil shape. Claim 7 In claim 4, the above-mentioned line pattern is an anti-slip thermal spray coating structure having a height of 0.5 mm to 5.0 mm from the surface of the base material. Claim 8 In claim 4, the above pattern is a non-slip thermal spray coating structure formed repeatedly at intervals of 20 mm to 305 mm. Claim 9 In claim 4, an anti-slip thermal spray coating structure further comprising a coating layer formed on a substrate surface where the line pattern is not formed. Claim 10 delete

Citation Information

Patent Citations

  • Roll in hot dip metal coating bath

    JP1993339689A

  • Slip preventing method of surface of steel material

    JP1995100430A

  • Thermal spray gun having a removable nozzle tip and method for manufacturing and using this thermal spray gun

    JP2015514558A

  • Thermal spraying method for manufacturing anti-sliding plate

    US20050281956A1